An aramid sizing agent, modified aramid fibers prepared therefrom, preparation method and application

By introducing acetylacetone complexes into the sizing agent of aramid fibers and using gradient drying technology, a thermally reversible coordination crosslinking network is formed, which solves the problems of poor bonding between aramid fibers and polyoxymethylene matrix and fiber breakage during high-temperature processing, thereby improving the mechanical properties and processing stability of the composite material.

CN123108945APending Publication Date: 2026-11-17SHANDONG HAIHUA GRP CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611627310.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-21
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

The existing aramid fiber has poor interfacial bonding with the polyoxymethylene matrix, conventional sizing agents pollute the environment and are brittle, and short-cut fibers are prone to breakage during high-temperature processing, resulting in a decrease in the reinforcing effect of the composite material.

Method used

A water-based polyurethane resin sizing agent containing acetylacetone complex is used, combined with low-temperature plasma or ultraviolet irradiation pretreatment, and a thermally reversible coordination crosslinking network is formed through gradient drying, which enhances interfacial bonding and protects fiber integrity.

Benefits of technology

Maintaining interface stability during high-temperature processing prevents breakage of chopped fibers, improves the tensile and flexural properties of composite materials, and enables green and environmentally friendly industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

This invention provides an aramid sizing agent, modified aramid fibers prepared therefrom, a preparation method, and applications, relating to the field of aramid sizing agents. The aramid sizing agent, by mass percentage, comprises the following components: waterborne polyurethane resin, acetylacetone complex, internal lubricant, film-forming aid, heat stabilizer, nonionic surfactant, and the balance being deionized water; the acetylacetone complex is one of the following: zinc acetylacetone, aluminum acetylacetone, or zirconium acetylacetone. The aramid sizing agent of this invention effectively overcomes the problems of poor interfacial bonding between aramid fibers and polyoxymethylene matrix, environmental pollution from organic solvents, brittle and easily broken sizing films, and easy breakage of chopped fibers during melt blending in existing technologies. Under the premise of being water-based and environmentally friendly, it can maintain interfacial stability during high-temperature processing, is not easily broken or detached during the chopped aramid fibers and the blending and extrusion of composite materials, and effectively protects the integrity of the chopped fibers.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of aramid sizing agents, and in particular to an aramid sizing agent, modified aramid fibers prepared therefrom, preparation methods therefrom, and applications. Background Technology

[0002] Aramid fibers (poly(p-phenylene terephthalamide), PPTA) are widely used as reinforcements in high-performance composite materials due to their high strength, high modulus, low density, and excellent heat resistance. Polyoxymethylene (POM), as an engineering plastic with excellent comprehensive properties, possesses advantages such as high rigidity, fatigue resistance, and creep resistance, and is widely used in automotive parts, electronics, and precision machinery. Combining aramid fibers with POM holds promise for obtaining high-performance composite materials that combine high strength, high rigidity, and good wear resistance.

[0003] However, aramid fibers have a smooth surface, strong chemical inertness, and lack active functional groups, resulting in extremely weak interfacial bonding with the polyoxymethylene (POM) matrix. Furthermore, POM is a non-polar crystalline polymer with a high melt processing temperature. At this temperature, conventional sizing agents applied to the surface of aramid fibers are prone to thermal decomposition or desorption, leading to interfacial failure. Existing technologies typically employ epoxy sizing agents or isocyanate coupling agents to surface-treat aramid fibers in an attempt to improve the interfacial bonding between the aramid fibers and the POM matrix. However, these sizing agents contain organic solvents, causing significant environmental pollution. After curing, they form a highly cross-linked three-dimensional network structure with a high cross-linking density and a glass transition temperature far exceeding room temperature. This results in the sizing film remaining in a glassy state at room temperature, exhibiting hard and brittle characteristics. The cross-linked film is highly brittle and easily breaks and detaches during the chopped aramid fibers and the blending and extrusion of composite materials.

[0004] Furthermore, when chopped aramid fibers are melt-blended with polyoxymethylene (POM) using a twin-screw extruder, existing aramid sizing agents cannot effectively protect the fibers. The aramid fibers are highly susceptible to breakage under the high shear stress of the screw, resulting in a significant decrease in their reinforcing effect on the composite material. Currently, there is a lack of a sizing agent system that can provide both strong interfacial bonding and effectively protect chopped aramid fibers from shear breakage during processing.

[0005] Based on this, we provide an aramid sizing agent that is water-based and environmentally friendly, can maintain interface stability during high-temperature processing, is not easily broken or detached during the chopped aramid fiber and composite material blending and extrusion process, and can effectively protect the integrity of the chopped fiber, which has important industrial application value. Summary of the Invention

[0006] To address the technical problems existing in the prior art, this invention provides an aramid sizing agent that effectively overcomes the problems of poor interfacial bonding between aramid fibers and polyoxymethylene matrix, environmental pollution from organic solvents, brittle and easily broken sizing film, and easy breakage of chopped fibers during melt blending. Under the premise of being water-based and environmentally friendly, it can maintain interface stability during high-temperature processing, is not easily broken or detached during the chopped aramid fibers and the blending and extrusion of composite materials, and can effectively protect the integrity of chopped fibers.

[0007] The present invention also provides modified aramid fibers prepared using the aramid sizing agent; This invention also provides a method for preparing modified aramid fibers using the aramid sizing agent; The present invention also provides the application of the modified aramid fiber in the preparation of aramid polyoxymethylene composite materials.

[0008] To solve the above technical problems, the technical solution adopted by the present invention is as follows: An aramid sizing agent, comprising the following components by weight percentage: Waterborne polyurethane resin, with a solid content of 8.76-16.41%; Acetylacetone complex: 0.04-0.82%; Internal lubricant: 0.18-1.31%; Film-forming aids: 0.44-3.28%; Heat stabilizer 0.03-0.16%; Nonionic surfactants: 0.04-0.49%; The remainder is deionized water; The acetylacetone complex is one of the following: zinc acetylacetone, aluminum acetylacetone, and zirconium acetylacetone.

[0009] Preferably, the internal lubricant is one of the following: ethylene bis-stearamide, glyceryl monostearate, or pentaerythritol stearate; The film-forming aid is one of the following: dipropylene glycol methyl ether, dipropylene glycol butyl ether, or propylene glycol methyl ether acetate. The heat stabilizer is one of the following: antioxidant 168, antioxidant 626, antioxidant 9228; The nonionic surfactant is one of the following: AEO-9, AEO-10, or Pingpingjia O-10.

[0010] A method for preparing modified aramid fibers using the aforementioned aramid sizing agent includes the following steps: pretreatment, impregnation sizing, and gradient drying; The pretreatment method is to subject the aramid fiber precursor to low-temperature plasma treatment or ultraviolet irradiation treatment to obtain pretreated aramid fiber precursor. The method of impregnation and sizing is to impregnate the pretreated aramid fiber raw yarn into the aramid sizing agent, and then take it out to obtain the impregnated aramid fiber. The gradient drying method involves drying the impregnated aramid fibers in a first stage and then in a second stage to obtain modified aramid fibers.

[0011] Preferably, the immersion time in the sizing process is 10-30 seconds; In the gradient drying process, the temperature of the first stage of drying is 80-100℃, and the holding time for the first stage of drying is 5-10 minutes; the temperature of the second stage of drying is 130-150℃, and the holding time for the second stage of drying is 3-8 minutes.

[0012] Preferably, in the pretreatment, the processing atmosphere of the low-temperature plasma treatment is at least one of the following: air, argon, oxygen, and nitrogen; The processing temperature for low-temperature plasma treatment is 20-40℃, the processing power is 1000-2000W, and the processing time is 30-180s.

[0013] Preferably, in the pretreatment, the treatment atmosphere for ultraviolet irradiation is air or ozone; The ultraviolet irradiation treatment temperature is 20-40℃, the treatment power is 100-1000W, and the treatment time is 5-30min.

[0014] A modified aramid fiber is prepared using the aforementioned method.

[0015] An aramid polyoxymethylene composite material is prepared by melt blending and extrusion of the aforementioned modified aramid fibers and polyoxymethylene resin.

[0016] Preferably, the length of the modified aramid fiber used is 3-6 mm; The weight ratio of modified aramid fiber to polyoxymethylene resin is (2-3):(16-17).

[0017] Preferably, the melt blending temperature is 190-210℃; the extrusion temperature is 190-210℃.

[0018] Compared with the prior art, the beneficial effects of the present invention are as follows: This invention introduces a specific acetylacetone complex into an aramid sizing agent. During the drying process of modified aramid fibers prepared using this sizing agent, the metal ions of the acetylacetone complex form coordination crosslinks with the carboxyl groups (-COOH) on the waterborne polyurethane segments, forming a stable three-dimensional coordination crosslink network. The bond energy of this coordination bond is between that of a hydrogen bond and a covalent bond, exhibiting excellent stability at room temperature, ensuring a firm coating of the fiber by the sizing film. In the subsequent melt blending and extrusion (190-210℃) of the modified aramid fiber and polyoxymethylene resin, the coordination bonds undergo thermally reversible dissociation, absorbing shear energy and preventing fiber brittleness caused by stress concentration, thus improving the mechanical properties of the composite material. During the cooling stage, the coordination bonds reform, restoring the interfacial bonding force and ensuring further improvement in the mechanical properties of the composite material. This allows the modified aramid fiber to maintain interfacial stability during high-temperature processing, preventing breakage and detachment during the chopped modified aramid fiber and blending extrusion of the composite material, and effectively protecting the integrity of the chopped fiber. Specifically: (1) The present invention introduces an acetylacetone complex into the sizing agent, which has good compatibility with the aqueous polyurethane dispersion system and can be dispersed in polyurethane at the molecular level. The thermal dissociation temperature (130-150℃) is perfectly matched with the second stage of gradient drying. During the drying process, the unsaturated metal ions are released and form a three-dimensional coordination crosslinking network with the carboxyl groups and other groups on the molecular chain of aqueous polyurethane.

[0019] In the shear field of the extrusion process, the coordination bonds are in a dynamic equilibrium of "dissociation-recombination." Each dissociation absorbs shear energy, protecting the fiber from breakage damage caused by stress concentration, thus maintaining fiber length. Each recombination restores interfacial bonding, maintaining the integrity of the sizing film and effectively resisting the erosion of the fiber surface coating by the polyoxymethylene melt. This facilitates the reaction between polyurethane and aramid fibers, as well as the polar groups on the polyoxymethylene surface, enhancing interfacial bonding and thus improving mechanical properties. Compared to traditional transition metal ions (such as Fe), 3+ Cu 2+ The Zn selected in this invention 2+ Al 3+ and Zr 4+ The complex exhibits extremely low catalytic activity for the thermal degradation of polyoxymethylene, minimizing its impact on mechanical properties. Without a coordination crosslinking network, waterborne polyurethane will completely melt into a low-viscosity fluid during the high-temperature shearing process of melt blending and extrusion, relying solely on van der Waals forces and weak hydrogen bonds for connection. The sizing film layer on the entire fiber surface is easily washed away by the polyoxymethylene melt, ultimately leaving the fiber surface unprotected by the sizing film and directly exposed to the shear field, making it more prone to fiber breakage and reducing mechanical properties.

[0020] (2) In the process of preparing modified aramid fibers using the aforementioned aramid sizing agent, low-temperature plasma treatment or ultraviolet irradiation pretreatment can significantly improve the interfacial compatibility between aramid fibers and water-based sizing agents. Low-temperature plasma treatment or ultraviolet irradiation pretreatment can introduce polar groups such as hydroxyl and carboxyl groups on the surface of aramid fibers, which can form hydrogen bonds with water-based polyurethane molecular chains, which is beneficial to the uniform spreading of subsequent water-based sizing agents, improves interfacial bonding force, and improves mechanical properties. Compared with the silane coupling agent treatment and alkaline etching treatment in the prior art, which introduce amino groups (-NH2), amino groups have a greater impact on Zn. 2+ Its coordination ability is higher than that of the carboxyl group, and it will preferentially bind to Zn. 2+ Stable Zn-NH2 coordination bonds are formed, preventing the formation of cross-linked networks with carboxyl groups in waterborne polyurethane. Furthermore, the low-temperature plasma treatment or ultraviolet irradiation pretreatment in this invention does not introduce strong coordinating groups such as amino groups, thus preventing them from complexing with Zn in acetylacetone compounds. 2+ / Al 3+ / Zr 4+ Competitive coordination occurs, which does not interfere with the formation of the coordination crosslinking network between metal ions and waterborne polyurethane carboxyl groups.

[0021] (3) In the process of preparing modified aramid fibers using the aforementioned aramid sizing agent, the first stage of gradient drying is performed at 80-100℃ for 5-10 minutes to completely remove free water and allow the polyurethane micelles to initially fuse into a film; the second stage of gradient drying is performed at 130-150℃ for 3-8 minutes to match the thermal dissociation temperature range of the acetylacetone complex, ensuring that the ligand dissociation rate and coordination reaction rate are balanced, thus ensuring that the metal ions and the carboxyl groups of the polyurethane undergo coordination crosslinking reactions to form a crosslinked network, while avoiding excessive crosslinking that would cause the film to become brittle, and ensuring the maintenance of mechanical properties. If the impregnated fibers are directly placed in an oven at 130-150℃ for one-step drying, the sizing film will be discontinuous, unable to form a continuous coating layer, and the coordination crosslinking points will be unevenly distributed, resulting in local over-crosslinking or insufficient crosslinking, which will reduce the strength of the sizing fibers.

[0022] (4) This invention uses acetylacetone complex as the core and utilizes the matching of its thermal dissociation temperature with the second stage of gradient drying to construct a thermally reversible coordination crosslinking network on the fiber surface: during melt blending and extrusion, the coordination bonds dissociate and metal ions are anchored to the fiber surface through ionic bonds to resist the scouring of polyoxymethylene melt. At the same time, the dynamic equilibrium of "dissociation-recombination" absorbs shear energy, protects fiber length, restores interfacial bonding, and enhances mechanical properties; Zn is selected. 2+ / Al 3+ / Zr 4+To avoid catalytic degradation of polyoxymethylene (POM), hydroxyl and carboxyl groups are introduced through low-temperature plasma treatment or UV irradiation pretreatment to avoid competitive coordination with amino groups. A two-stage gradient drying process—film formation and dehydration at 80-100℃ followed by coordination crosslinking at 130-150℃—ensures the continuous integrity and appropriate crosslinking of the coated film. These three factors synergistically result in a composite material with a tensile strength of 73.21 MPa and a flexural strength of 105.61 MPa, achieving simultaneous improvement in interfacial reinforcement and the tensile and flexural properties of the composite material.

[0023] (5) The aramid sizing agent of the present invention and its application process are simple, the raw materials are green and environmentally friendly, and it is suitable for the industrial-scale production of high-performance aramid / polyoxymethylene composite materials. Detailed Implementation

[0024] To provide a clearer understanding of the technical features, objectives, and effects of this invention, specific embodiments are now described. It should be noted that the following detailed descriptions are exemplary and intended to provide further explanation of the invention. Unless otherwise specified, all technical and scientific terms used in this invention have the same meaning as commonly understood by one of ordinary skill in the art to which this invention pertains.

[0025] It should be noted that the terminology used herein is for the purpose of describing particular embodiments only and is not intended to limit the exemplary embodiments of the present invention. As used herein, "first," "second," etc., are used to distinguish similar objects and are not used to describe a particular order or sequence. Furthermore, it should be understood that when the terms "comprising" and / or "including" are used in this specification, they indicate the presence of features, steps, operations, devices, components, and / or combinations thereof.

[0026] This invention provides an aramid sizing agent, comprising the following components by mass percentage: Waterborne polyurethane resin (based on solid content): 8.76-16.41%; Acetylacetone complex: 0.04-0.82%; Internal lubricant: 0.18-1.31%; Film-forming aids: 0.44-3.28%; Heat stabilizer 0.03-0.16%; Nonionic surfactants: 0.04-0.49%; The remainder is deionized water.

[0027] In this embodiment of the invention, the waterborne polyurethane resin used has a glass transition temperature below 0°C. At this temperature, the coated film at room temperature (25°C) is in a rubbery state, absorbing energy through elastic deformation during cutting rather than undergoing brittle fracture. Furthermore, the softening temperature range of the waterborne polyurethane is 140-190°C. During the second drying stage (130-150°C), it begins to soften but does not flow, which is conducive to the coordination reaction between the acetylacetone complex and the polyurethane.

[0028] The acetylacetone complex used has good compatibility with the aqueous polyurethane dispersion system and can be dispersed in polyurethane at the molecular level. The thermal dissociation temperature of acetylacetone (130-150℃) is perfectly matched with the second stage of gradient drying. During the drying process, the unsaturated metal ions are released and efficiently coordinate with the carboxyl groups in the aqueous polyurethane to form carboxylic acid metal salt bonds (-COO-M-) to construct a three-dimensional cross-linked network. The mechanical properties of the resulting sized fiber membrane are improved, and the coordination bonds are stable at room temperature. The surface stickiness of the cross-linked sized membrane is reduced, so that the short-cut fibers will not clump due to the stickiness of the membrane during storage and transportation. The coordination bonds dissociate and absorb shear energy during high-temperature extrusion at 190-210℃, and can reform after cooling, restoring the interfacial bonding force, maintaining the integrity of the sized membrane, and improving mechanical properties.

[0029] In this embodiment of the invention, preferably, the acetylacetone complex is one of the following: zinc acetylacetone, aluminum acetylacetone, or zirconium acetylacetone. Wherein, Zn 2+ It exhibits extremely low catalytic activity towards polyoxymethylene (POM), a rapid coordination reaction rate, and can achieve rapid crosslinking during the drying stage; the coordination bond exhibits moderate thermal reversibility. Al 3+ and Zr 4+ It also exhibits low redox activity and high coordination bond strength.

[0030] In this embodiment of the invention, preferably, the internal lubricant is one of the following: ethylene bis-stearamide, glyceryl monostearate, or pentaerythritol stearate.

[0031] In this embodiment of the invention, preferably, the film-forming aid is one of the following: dipropylene glycol methyl ether, dipropylene glycol butyl ether, or propylene glycol methyl ether acetate.

[0032] In this embodiment of the invention, preferably, the heat stabilizer is one of the following: antioxidant 168, antioxidant 626, or antioxidant 9228.

[0033] In this embodiment of the invention, preferably, the nonionic surfactant is one of the following: fatty alcohol polyoxyethylene (9) ether AEO-9, fatty alcohol polyoxyethylene (10) ether AEO-10, or fatty alcohol polyoxyethylene ether Pingpingjia O-10.

[0034] This invention also provides a method for preparing modified aramid fibers using the aforementioned aramid sizing agent, comprising the following steps: (1) Pretreatment: The aramid fiber precursor is subjected to low-temperature plasma treatment or ultraviolet irradiation treatment to obtain pretreated aramid fiber precursor; (2) Impregnation and sizing: The pretreated aramid fiber raw yarn is impregnated in an impregnation tank containing the aforementioned aramid sizing agent for 10-30 seconds to obtain impregnated aramid fiber; (3) Gradient drying: The impregnated aramid fibers are subjected to gradient drying. The temperature of the first stage of drying is controlled at 80-100℃ and the temperature is kept warm for 5-10 minutes to remove free moisture. The temperature of the second stage of drying is 130-150℃ and the temperature is kept warm for 3-8 minutes to allow the acetylacetone complex to coordinate with the carboxyl groups on the waterborne polyurethane molecular chain to form a cross-linked network, thereby obtaining modified aramid fibers with a sizing amount (the percentage increase in fiber weight after sizing relative to the weight of unsizing fibers) of 3-6 wt%.

[0035] In this embodiment of the invention, the low-temperature plasma treatment atmosphere is at least one of the following: air, argon, oxygen, or nitrogen; the treatment temperature is 20-40°C; the treatment power is 1000-2000W; and the treatment time is 30-180s. The ultraviolet irradiation treatment atmosphere is air or ozone; the treatment temperature is 20-40°C; the treatment power is 100-1000W; and the treatment time is 5-30min. After plasma or ultraviolet irradiation treatment, polar groups such as hydroxyl and carboxyl groups are introduced onto the surface of the aramid fiber, which is beneficial for the uniform spreading of the subsequent aqueous sizing agent. Furthermore, these polar groups can form more coordination bonds and hydrogen bonds with the polyurethane segments in the aramid sizing agent, further enhancing the interfacial bonding strength between the two.

[0036] The present invention also provides modified aramid fibers prepared using the aforementioned aramid sizing agent.

[0037] The present invention also provides a method for preparing aramid polyoxymethylene composite material using the modified aramid fiber, which is obtained by melt blending and extrusion of chopped modified aramid fiber and polyoxymethylene resin.

[0038] In this embodiment of the invention, preferably, the weight ratio of modified aramid fiber to polyoxymethylene resin is (2-3):(16-17).

[0039] In this embodiment of the invention, preferably, the chopped modified aramid fiber is obtained by cutting the modified aramid fiber using a cutting machine; the length of the chopped modified aramid fiber is 3-6 mm.

[0040] In this embodiment of the invention, preferably, the melt blending is carried out in a twin-screw extruder, and the temperature of melt blending and extrusion is 190-210°C, and the screw speed is 150-250 RPM.

[0041] The mechanism of action of modified aramid fibers treated with aramid sizing agent on aramid polyoxymethylene composite materials in this embodiment of the invention is as follows: This invention introduces a specific acetylacetone complex into the sizing agent. During the second stage of gradient drying (130-150℃), the metal ions of the acetylacetone complex form coordination crosslinks with the carboxyl groups (-COOH) on the waterborne polyurethane segments, creating a stable three-dimensional coordination crosslink network. The bond energy of this coordination bond lies between that of a hydrogen bond and a covalent bond, exhibiting excellent stability at room temperature, ensuring a firm coating of the fiber by the sizing film. In the subsequent melt blending and extrusion (190-210℃) of the modified aramid fiber and polyoxymethylene resin, the coordination bonds undergo thermally reversible dissociation, absorbing shear energy and preventing fiber brittleness caused by stress concentration, thus improving the mechanical properties of the composite material. During the cooling stage, the coordination bonds reform, restoring the interfacial bonding force and ensuring further improvement in the mechanical properties of the composite material.

[0042] Meanwhile, the internal lubricant in the sizing agent (such as ethylene bis-stearamide) migrates to the fiber surface during extrusion, reducing the coefficient of friction between the fiber and the screw wall and melt, effectively reducing mechanical damage to chopped fibers caused by high shear forces. The active groups (such as hydroxyl groups) on the waterborne polyurethane molecular chain can form intermolecular hydrogen bonds with the end groups (-OH) of the polyoxymethylene molecular chain, enhancing the interfacial bonding between the modified aramid fiber and polyoxymethylene.

[0043] The addition of heat stabilizers effectively quenches free radical degradation reactions that may be initiated by metal ions, preventing the catalytic degradation of the polyoxymethylene matrix by metal ions. This, combined with the low catalytic activity of Zn... 2+ Al 3+ and Zr 4+ The use of complexes ensures the stability of the mechanical properties of composite materials.

[0044] To enable those skilled in the art to more clearly understand the technical solution of the present invention, the present invention will be further described below with reference to some specific embodiments. Unless otherwise specified, the experimental methods used in each embodiment are conventional methods; unless otherwise specified, the reagents and materials used in each embodiment are commercially available products.

[0045] Example 1 This embodiment provides an aramid sizing agent, which, by mass percentage, comprises the following components: 15.5% waterborne polyurethane resin (based on solid content); 0.25% zinc acetylacetonate; 0.75% ethylene bis-stearamide; 2.5% dipropylene glycol methyl ether; 0.08% antioxidant 168; 0.3% nonionic surfactant AEO-9; and 80.62% deionized water.

[0046] In this embodiment, the waterborne polyurethane resin is added using a commercially available waterborne polyurethane dispersion. The manufacturer of the waterborne polyurethane dispersion used is Covestro UH2558, with a solid content of 37 wt%, and the dispersion medium is deionized water. In the formulation process of the above-mentioned aramid sizing agent, the waterborne polyurethane dispersion of the above-mentioned brand is added according to the solid content of the polyurethane, and the dispersion medium (deionized water) contained in the waterborne polyurethane dispersion is included in the amount of deionized water used in the aramid sizing agent.

[0047] This embodiment also provides a method for preparing modified aramid fibers using the aforementioned aramid sizing agent, the specific steps of which are as follows: (1) Pretreatment of aramid fiber: The aramid fiber is treated by a low-temperature plasma treatment device under normal pressure. The temperature of the low-temperature plasma treatment is controlled at 25°C, the treatment atmosphere is air, the treatment power is 1000W, and the treatment time is 120s to obtain the pretreated aramid fiber fiber. (2) Impregnation and sizing: Mix the raw materials of aramid sizing agent according to the aforementioned mass percentages, stir until completely dispersed, and obtain a uniform and stable water-based sizing agent; pass the pretreated aramid fiber raw yarn through an impregnation tank containing the above-mentioned aramid sizing agent, and control the impregnation time to 20s.

[0048] (3) Gradient drying: The impregnated aramid fibers are subjected to gradient drying. The temperature of the first stage of drying is controlled at 80℃ and the temperature is kept warm for 8 minutes. The temperature of the second stage of drying is 140℃ and the temperature is kept warm for 5 minutes. Modified aramid fibers with a sizing amount (the percentage of the weight increase of the sizing fiber to the weight of the unsizing fiber) of 5wt% are obtained.

[0049] This embodiment also provides modified aramid fibers prepared by the aforementioned aramid sizing agent according to the aforementioned method.

[0050] Example 2 This embodiment provides an aramid sizing agent, which, by mass percentage, comprises the following components: 9.5% waterborne polyurethane resin (based on solid content); 0.15% aluminum acetylacetonate; 0.5% glyceryl monostearate; 1.5% dipropylene glycol butyl ether; 0.05% antioxidant 626; 0.2% nonionic surfactant Pingpingjia O-10; and 88.1% deionized water.

[0051] In this embodiment, the waterborne polyurethane resin is added using a commercially available waterborne polyurethane dispersion. The manufacturer of the waterborne polyurethane dispersion is Covestro DLN-SD, with a solid content of 40 wt% and deionized water as the dispersion medium. In the formulation process of the above-mentioned aramid sizing agent, the waterborne polyurethane dispersion of the above-mentioned brand is added according to the solid content of the polyurethane, and the dispersion medium (deionized water) contained in the waterborne polyurethane dispersion is included in the amount of deionized water used in the aramid sizing agent.

[0052] This embodiment also provides a method for preparing modified aramid fibers using the aforementioned aramid sizing agent, the specific steps of which are as follows: (1) Pretreatment of aramid fiber: The aramid fiber is treated by an ultraviolet irradiation treatment device. The temperature of the ultraviolet irradiation treatment is controlled at 30℃, the treatment atmosphere is air, the treatment power is 500W, and the treatment time is 5min to obtain the pretreated aramid fiber fiber. (2) Impregnation and sizing: Mix the raw materials of aramid sizing agent according to the aforementioned mass percentages, stir until completely dispersed, and obtain a uniform and stable water-based sizing agent; pass the pretreated aramid fiber raw yarn through an impregnation tank containing the above-mentioned aramid sizing agent, and control the impregnation time to 30s.

[0053] (3) Gradient drying: The impregnated aramid fibers are subjected to gradient drying. The temperature of the first stage of drying is controlled at 90℃ and the temperature is kept warm for 5 minutes. The temperature of the second stage of drying is 145℃ and the temperature is kept warm for 3 minutes. Modified aramid fibers with a sizing amount (the percentage of the weight increase of the sizing fiber to the weight of the unsizing fiber) of 3wt% are obtained.

[0054] This embodiment also provides modified aramid fibers prepared by the aforementioned aramid sizing agent according to the aforementioned method.

[0055] Comparative Example 1 Comparative Example 1 uses the technical solution of Example 1, except that an equal amount of EDTA-zinc is used instead of zinc acetylacetone in the aramid sizing agent; the other components and amounts of the aramid sizing agent are the same as in Example 1. Specifically: The aramid sizing agent of Comparative Example 1, by mass percentage, comprises the following components: 15.5% waterborne polyurethane resin (by solids content); 0.25% EDTA-zinc; 0.75% ethylene bis-stearamide; 2.5% dipropylene glycol methyl ether; 0.08% antioxidant 168; 0.3% nonionic surfactant AEO-9; and 80.62% deionized water.

[0056] The method for preparing modified aramid fibers using the aramid sizing agent in Comparative Example 1 is the same as that in Example 1.

[0057] Comparative Example 2 Comparative Example 2 used the aramid sizing agent of Example 1, but differed in that a one-step drying process was used instead of gradient drying in the preparation of modified aramid fibers using this aramid sizing agent; other operations and process parameters were the same as in Example 1. Specifically: (1) Pretreatment of aramid fiber: The aramid fiber is treated by a low-temperature plasma treatment device under normal pressure. The temperature of the low-temperature plasma treatment is controlled at 25°C, the treatment atmosphere is air, the treatment power is 1000W, and the treatment time is 120s to obtain the pretreated aramid fiber fiber. (2) Impregnation and sizing: Mix the raw materials of aramid sizing agent according to the aforementioned mass percentages, stir until completely dispersed, and obtain a uniform and stable water-based sizing agent; pass the pretreated aramid fiber raw yarn through an impregnation tank containing the above-mentioned aramid sizing agent, and control the impregnation time to 20s.

[0058] (3) One-step drying: The impregnated aramid fiber is dried at a temperature of 140°C and kept warm for 10 minutes to obtain modified aramid fiber with a sizing amount (the percentage of the weight increase of the fiber after sizing to the weight of the unsizing fiber) of 5wt%.

[0059] Comparative Example 3 Comparative Example 3 uses the technical solution of Example 1, except that an equal amount of iron acetylacetone is used instead of zinc acetylacetone in the aramid sizing agent; the other components and amounts of the aramid sizing agent are the same as in Example 1. Specifically: The aramid sizing agent of Comparative Example 3, by mass percentage, comprises the following components: 15.5% waterborne polyurethane resin (by solids content); 0.25% acetylacetone iron; 0.75% ethylene bis-stearamide; 2.5% dipropylene glycol methyl ether; 0.08% antioxidant 168; 0.3% nonionic surfactant AEO-9; and 80.62% deionized water.

[0060] The method for preparing modified aramid fibers using the aramid sizing agent in Comparative Example 3 is the same as that in Example 1.

[0061] The modified aramid fibers of Examples 1-2 and Comparative Examples 1-3 were cut to a length of 6 mm using a cutting machine to obtain short modified aramid fibers. Then, the short modified aramid fibers of Examples 1-2 and Comparative Examples 1-3 were melt-blended and extruded with polyoxymethylene resin at a mass ratio of 3:17 using a twin-screw extruder. The temperature of melt blending and extrusion was controlled at 210°C and the twin-screw speed was 150 RPM to obtain aramid polyoxymethylene composite materials.

[0062] The aramid polyoxymethylene composite materials prepared in each embodiment and comparative example were made into test strips and tested according to the following relevant performance standards: 1. Tensile strength test method: according to GB / T 1040.2-2022 "Determination of tensile properties of plastics - Part 2: Test conditions for molded and extruded plastics". 2. Flexural strength test method: according to GB / T 9341-2008 "Determination of flexural properties of plastics". The test results are shown in Table 1: Table 1. Summary of the properties of composite materials prepared in each example and comparative example.

[0063] As can be seen from the data in the table above, the modified aramid short fibers prepared in Examples 1-2 have the best reinforcing and modifying effect on polyoxymethylene composites.

[0064] As shown in the table above, compared with Examples 1-2, the tensile strength and flexural strength of the aramid short fiber modified polyoxymethylene resin prepared in Comparative Example 1 decreased. Analysis revealed that this was because in Comparative Example 1, EDTA and Zn... 2+ Zn exhibits high coordination stability; the ligands do not undergo thermal dissociation during the second stage of gradient drying (130-150℃). 2+ It cannot release and coordinate with the carboxyl groups of waterborne polyurethane, and a three-dimensional coordination crosslinking network cannot be formed. The sizing film is only a thermoplastic waterborne polyurethane film, which is partially washed away from the fiber surface by the polyoxymethylene melt during extrusion, causing some fibers to lose protection and break, thereby reducing tensile and flexural strength.

[0065] As shown in the table above, compared with Examples 1-2, the tensile strength and flexural strength of the aramid short fiber modified polyoxymethylene resin prepared in Comparative Example 2 decreased. Analysis revealed that this was because in Comparative Example 2, the water vaporized rapidly during the one-step drying process, generating a large number of bubbles inside the sizing film. The film layer was discontinuous, and the coordination reaction was carried out in a water-containing environment, resulting in uneven distribution of crosslinking points, local over-crosslinking or under-crosslinking. This led to weak adhesion of the sizing film, causing some fibers to peel off during extrusion, resulting in some fibers losing protection and being broken, thus reducing the tensile and flexural strength.

[0066] As shown in the table above, compared with Examples 1-2, the tensile strength and flexural strength of the aramid short fiber modified polyoxymethylene resin prepared in Comparative Example 3 decreased. Analysis revealed that this was because in Comparative Example 3, Fe... 3+ As a strong Lewis acid, it has extremely strong catalytic activity for the thermal degradation of polyoxymethylene (POM). During the extrusion process, it accelerates the degradation of POM molecular chains, leading to a deterioration in the tensile and flexural strength of the composite material.

[0067] Unless otherwise stated, all percentages used in this invention are mass percentages.

[0068] Finally, it should be noted that the above descriptions are merely preferred embodiments of the present invention and are not intended to limit the present invention. Although the present invention has been described in detail with reference to the foregoing embodiments, those skilled in the art can still modify the technical solutions described in the foregoing embodiments or make equivalent substitutions for some of the technical features. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the protection scope of the present invention.

Claims

1. An aramid sizing agent characterized by, By mass percentage, it includes the following components: Waterborne polyurethane resin, with a solid content of 8.76-16.41%; Acetylacetone complex: 0.04-0.82%; Internal lubricant: 0.18-1.31%; Film-forming aids: 0.44-3.28%; Heat stabilizer 0.03-0.16%; Nonionic surfactants: 0.04-0.49%; The remainder is deionized water; The acetylacetone complex is one of the following: zinc acetylacetone, aluminum acetylacetone, and zirconium acetylacetone.

2. The aramid sizing agent according to claim 1, characterized in that, The internal lubricant is one of the following: ethylene bis-stearamide, glyceryl monostearate, or pentaerythritol stearate; The film-forming aid is one of the following: dipropylene glycol methyl ether, dipropylene glycol butyl ether, or propylene glycol methyl ether acetate. The heat stabilizer is one of the following: antioxidant 168, antioxidant 626, antioxidant 9228; The nonionic surfactant is one of the following: AEO-9, AEO-10, or Pingpingjia O-10.

3. A method for preparing modified aramid fibers using the aramid sizing agent according to claim 1 or 2, characterized in that, Includes the following steps: Pretreatment, impregnation and sizing, gradient drying; The pretreatment method is to subject the aramid fiber precursor to low-temperature plasma treatment or ultraviolet irradiation treatment to obtain pretreated aramid fiber precursor. The method of impregnation and sizing is to impregnate the pretreated aramid fiber raw yarn into the aramid sizing agent, and then take it out to obtain the impregnated aramid fiber. The gradient drying method involves drying the impregnated aramid fibers in a first stage and then in a second stage to obtain modified aramid fibers.

4. The method for preparing modified aramid fibers according to claim 3, characterized in that, In the sizing process, the immersion time is 10-30 seconds; In the gradient drying process, the temperature of the first stage of drying is 80-100℃, and the holding time for the first stage of drying is 5-10 minutes; the temperature of the second stage of drying is 130-150℃, and the holding time for the second stage of drying is 3-8 minutes.

5. The method for preparing modified aramid fibers according to claim 3, characterized in that, In the pretreatment, the processing atmosphere of the low-temperature plasma treatment is at least one of the following: air, argon, oxygen, and nitrogen; The processing temperature for low-temperature plasma treatment is 20-40℃, the processing power is 1000-2000W, and the processing time is 30-180s.

6. The method for preparing modified aramid fibers according to claim 3, characterized in that, In the pretreatment, the treatment atmosphere for ultraviolet irradiation is air or ozone; The ultraviolet irradiation treatment temperature is 20-40℃, the treatment power is 100-1000W, and the treatment time is 5-30min.

7. A modified aramid fiber, characterized in that, It is prepared by the method described in claim 3.

8. An aramid polyoxymethylene composite material, characterized in that, It is prepared by melt blending and extrusion of the modified aramid fiber as described in claim 7 and polyoxymethylene resin.

9. The aramid polyoxymethylene composite material according to claim 8, characterized in that, The length of the modified aramid fiber used is 3-6 mm; The weight ratio of modified aramid fiber to polyoxymethylene resin is (2-3):(16-17).