A method for preparing cashmere composite fabric with far-infrared and negative oxygen ion emission functions and its product.

By using a core-sheath composite fiber structure and a porous connecting layer, the durability and breathability issues of cashmere fabrics in achieving far-infrared and negative oxygen ion functions while maintaining a soft feel are solved, thus achieving highly efficient functional emission and ion generation effects.

CN123108946APending Publication Date: 2026-11-17INNER MONGOLIA PALANTI TECH DEV CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611458840.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-19
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing technologies struggle to simultaneously achieve far-infrared and negative ion functions in cashmere fabrics without compromising their softness, and the functional layers lack durability and breathability.

Method used

The core-sheath composite fiber structure is adopted. Functional powder with surface modification is mixed with polyester chips to form core-sheath composite fiber. The outer layer is woven with water-soluble vinylon fiber through alkali reduction and pore opening treatment, combined with reactive hot melt adhesive bonding and supercritical CO2 foaming treatment to form a porous connecting layer. Finally, the functional powder is fixed by hyperbranched polymer chemical modification.

Benefits of technology

It achieves the goal of maintaining the soft feel of cashmere fabric while possessing efficient far-infrared and negative oxygen ion functions, and significantly improving functional durability and breathability, with a breathability rate of 155-183mm/s, and functional emissivity and ion generation retention rates of 86.2% and 83.5%, respectively.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123108946A_ABST
    Figure CN123108946A_ABST
Patent Text Reader

Abstract

This invention discloses a method for preparing a cashmere composite fabric with far-infrared and negative oxygen ion emission functions, and the product thereof, relating to the field of functional textile fabric technology. The method includes: 1. Preparing a core-sheath composite fiber using nano-tourmaline powder and nano-silicon carbide powder with polyester chips as the core layer and polyester chips as the sheath layer; 2. Alkali reduction and pore opening of the inner fabric layer to form pits exposing the functional powder; 3. Spinning water-soluble vinylon with cashmere to create a fluffy microporous outer layer; 4. Applying reactive hot melt adhesive to the inner and outer layers in a discrete lattice manner; 5. Supercritical CO2 rapid pressure release foaming to form a porous connecting layer with the hot melt adhesive; 6. Chemical modification treatment with hyperbranched polymers, resulting in a three-layer composite fabric with a far-infrared emissivity ≥0.85 and a negative oxygen ion generation ≥1352 ions / cm². 3 Air permeability ≥155mm / s, and functional retention rate ≥83.5% after 50 washes.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of functional textile fabric technology, specifically to a method for preparing a cashmere composite fabric with far-infrared and negative oxygen ion emission functions and its product. Background Technology

[0002] In the field of functional textiles, imbuing high-end fabrics with health-promoting functions has always been a hot research topic. Cashmere, as a top-grade natural fiber, is known as "soft gold" for its softness, lightness, and warmth, making it the preferred raw material for high-end intimate apparel. If it could simultaneously possess far-infrared emission and negative ion generation functions, it would undoubtedly significantly enhance the added value of the product. However, existing technologies for achieving these functions fundamentally conflict with the inherent comfort of cashmere fabrics. For example, to achieve an effective level of functionality, the amount of functional powder added must be sufficiently high, but this compromises the soft feel of cashmere. Furthermore, coatings or impregnation-type functional layers have poor durability, rapidly diminishing their functionality after washing. Additionally, the dense adhesive layer formed by traditional lamination methods blocks breathability, leading to stuffiness and discomfort when worn.

[0003] To address the aforementioned issues, this invention provides a method for preparing a cashmere composite fabric with far-infrared and negative oxygen ion emission functions, as well as the resulting product. This method aims to balance functional efficiency with the soft feel of cashmere, enhance functional durability, and impart good breathability to the fabric. Summary of the Invention

[0004] To address the aforementioned technical problems, this invention provides a method for preparing a cashmere composite fabric with far-infrared and negative oxygen ion emission functions, as well as the product thereof, as detailed below: A method for preparing a cashmere composite fabric with far-infrared and negative oxygen ion emission functions includes the following steps: (1) Preparation of core-sheath composite fiber: The surface-modified functional powder is mixed with polyester chips as the core spinning raw material; the polyester chips are used as the sheath spinning raw material, and the core-sheath composite fiber with sheath covering core layer is obtained by core-sheath composite spinning process; wherein, the functional powder includes nano tourmaline powder and nano silicon carbide powder. (2) The inner fabric woven from the core-sheath composite fiber is subjected to alkali reduction and pore opening treatment to form nanoscale pits on the surface of the sheath layer, exposing part of the core layer spinning raw material. (3) Water-soluble vinylon fiber is spun together with cashmere yarn and woven into an outer fabric. The water-soluble vinylon fiber is removed by water-soluble treatment, so that the outer fabric forms a fluffy microporous structure. (4) A reactive hot melt adhesive is applied between the inner fabric and the outer fabric in a discrete dot matrix manner to bond the two together to form a composite fabric. (5) The composite fabric is placed in a supercritical CO2 environment and subjected to pressure swelling followed by rapid pressure release foaming treatment, so that the hot melt adhesive forms a porous connecting layer in the glue-free area between the inner fabric and the outer fabric. (6) The composite fabric is immersed in a finishing solution containing hyperbranched polymer for chemical modification treatment, and then dried and set to obtain the cashmere composite fabric. Figure 1 The chemical modification treatment causes the hyperbranched polymer to be fixed on the fiber surface and inside the nanoscale pits through physical adsorption, hydrogen bonding and ionic bonding. Under baking conditions, some amino groups react with the carboxyl groups on the keratin molecular chain of cashmere fibers to form amide bonds (—CONH—), thereby fixing the hyperbranched polymer and the functional powder exposed in the core layer together on the fiber surface.

[0005] It should be noted that in actual large-scale continuous production, the porous connecting layer can be prepared using chemical foaming instead of supercritical CO2 physical foaming to reduce production costs. Specifically: In the formulation stage of the reactive hot melt adhesive, a chemical foaming agent with a mass percentage of 0.5%-1.0% is added to the polyurethane hot melt adhesive system. The chemical foaming agent is selected from any one or more combinations of azodicarbonamide, azobisisobutyronitrile, or sodium bicarbonate. At the same time, an appropriate amount of foaming aid (such as zinc oxide or zinc stearate) is added to adjust the foaming temperature and rate.

[0006] After the adhesive is applied and bonded, the composite fabric is directly sent into a continuous hot air oven and baked at 140℃-190℃ for 3-5 minutes. At this temperature, the chemical foaming agent decomposes and releases gas, forming a porous structure inside the hot melt adhesive points, thereby achieving microporous bonding layer.

[0007] This chemical foaming solution does not require high-pressure autoclave equipment and can be completed directly on a conventional composite production line. The equipment investment is only 10%-20% of that of the supercritical solution, and the production efficiency can be improved to a continuous production mode. The overall processing cost is reduced by about 60%-70% compared with the supercritical solution.

[0008] Further, in step (1), the surface modification treatment of the functional powder is carried out using a silane coupling agent, wherein the silane coupling agent is any one or more combinations of KH-550, KH-560 or KH-570; the mass ratio of the functional powder to the polyester chips in the core layer is (20-40):(80-60). The specific method is as follows: Step 1: Prepare the modified solution: Add the silane coupling agent to the ethanol / water mixed solvent to prepare a solution with a mass concentration of 1%-3%; Adjust the pH to 4.0-5.5 with glacial acetic acid and stir for about 30 minutes to hydrolyze.

[0009] Step 2, Soaking Modification: Mix nano-tourmaline powder and nano-silicon carbide powder at a mass ratio of 1:1-3:1 and add them to the above hydrolysate; Disperse at high speed for 1-3 hours at 60℃-80℃.

[0010] Step 3, Drying and Pulverizing: The modified powder suspension is filtered and repeatedly washed with deionized water to remove unreacted coupling agent; dried at 80℃-105℃, and then the aggregates are broken up by air jet pulverization to obtain surface organic modified nano-functional powder.

[0011] Further, in step (1), the sheath of the core-sheath composite fiber accounts for 60%-80% of the total fiber mass, and the core accounts for 20%-40% of the total fiber mass; the functional powder content in the core is 15%-25% by mass.

[0012] Further, in step (2), the conditions for the alkali reduction and pore opening treatment are: alkali concentration of 2%-5%, treatment temperature of 70℃-80℃, and treatment time of 15-30 minutes; the alkali solution used is sodium hydroxide solution or potassium hydroxide solution.

[0013] The specific operating method is as follows: Place the woven inner layer fabric in a relaxed state into a continuous alkali reduction machine or an intermittent dyeing vat, add water first, then add the calculated sodium hydroxide or potassium hydroxide according to the weight of the fabric to prepare an alkali solution of a specified concentration, heat to the set temperature, and soak for 15-30 minutes.

[0014] Furthermore, in step (2), the pore size of the nanoscale pit is 100nm-200nm, and the pit depth is 40%-50% of the skin thickness.

[0015] Further, in step (3), the mass ratio of the water-soluble vinylon fiber to the cashmere yarn is 15-25:75-85; the conditions for the water-soluble treatment are: water temperature 85℃-100℃, treatment time 30-40 minutes.

[0016] Further, in step (4), the discrete dot matrix is ​​a rhombic dot matrix, a square dot matrix, or a hexagonal dot matrix; the spacing between adjacent dots in the dot matrix is ​​1.0 mm to 3.0 mm, and the diameter of each dot is 0.5 mm to 1.0 mm; the reactive hot melt adhesive is a moisture-curing polyurethane hot melt adhesive; the application area of ​​the hot melt adhesive accounts for 15% to 20% of the total area between the inner and outer fabric layers.

[0017] Further, in step (5), the conditions for the supercritical CO2 foaming treatment are: pressurization to 8MPa-10MPa, swelling temperature of 40℃-50℃, swelling time of 30-50 minutes, and depressurization rate of 0.5MPa / s-1.0MPa / s.

[0018] Further, in step (6), the hyperbranched polymer is any one of terminal amino hyperbranched polyamide, terminal hydroxyl hyperbranched polyester, or terminal mercapto hyperbranched polyether; the molecular weight of the hyperbranched polymer is 2000-3000, and the mass percentage of the hyperbranched polymer in the finishing solution is 5%-8%; the conditions for the chemical modification treatment are: impregnation temperature 40℃-80℃, impregnation time 20-120 minutes, bath ratio 1:8-20, and after modification, pre-baking at 80℃-100℃ and curing at 160℃-180℃. Specifically, the terminal group of the terminal amino hyperbranched polyamide is a primary amino group (-NH2), and the cashmere keratin molecular chain contains side chain carboxyl groups (-COOH) from acidic amino acid residues such as aspartic acid and glutamic acid. Under baking conditions (160℃–180℃), the primary amino groups of the terminal amino hyperbranched polyamide undergo a condensation dehydration reaction with the carboxyl groups of the cashmere keratin side chain to generate amide bonds (-CONH-), thereby fixing the hyperbranched polymer and the core layer exposed functional powder together on the fiber surface.

[0019] On the other hand, the present invention provides a cashmere composite fabric with far-infrared and negative oxygen ion emission functions prepared by the aforementioned method, wherein the cashmere composite fabric has a three-layer composite structure, comprising: The inner layer is a functional layer composed of core-skin composite fibers with nanoscale pits in the skin, which provides far-infrared and negative oxygen ion emission functions. The outer layer is a fluffy microporous layer made of pure cashmere fibers, providing a soft feel; The intermediate connecting layer is a porous lattice connecting layer made of foamed hot melt adhesive, providing breathable channels.

[0020] Furthermore, in the dot matrix of the intermediate connecting layer, the glue-free areas between adjacent dots form a continuous air channel.

[0021] Compared with the prior art, the beneficial effects of the present invention are as follows: 1. This invention concentrates functional powders in the core layer of a core-sheath composite fiber, which is then completely covered by a polyester sheath. The actual contact surface with the skin is the smooth polyester sheath, not exposed inorganic powder particles. After alkali reduction and pore-opening treatment, nanoscale pits of 100nm-200nm are formed on the surface of the sheath, allowing the functional powders in the core layer to be exposed and function. Simultaneously, the pit size is much smaller than the tactile perception threshold (typically >50μm), thus completely eliminating any itching sensation. Furthermore, the outer fabric uses pure cashmere yarn and is woven with water-soluble vinylon to create a fluffy microporous structure, fully preserving the soft feel of cashmere. Therefore, the functional layer and the comfort layer are structurally completely separated, and the amount of functional powder added is no longer limited by feel requirements; the functional powder content in the core layer can reach 15%-25%.

[0022] 2. This invention achieves functional durability through a dual mechanism. On one hand, the functional powder is encapsulated within the core layer of the core-sheath fiber. The nano-pits formed after the sheath layer is alkali-reduced and opened up act as physical confinements for the powder in the core layer, effectively inhibiting mechanical loss of the powder during the washing process. On the other hand, the hyperbranched polymer forms a covalent bond with the fiber through chemical modification, creating a molecular-level protective and fixing network on the fiber surface, further fixing the functional powder within the pits. In addition, the hyperbranched polymer itself is rich in polar groups, which can actively ionize water molecules in the air to generate negative oxygen ions, providing an organic negative ion supplementary source in addition to the inorganic powder, thus forming functional redundancy. After the above treatment, the fabric retains 86.2% of the far-infrared emissivity, 83.5% of the negative oxygen ion generation, and 91.2% of the air permeability after 50 standard washes.

[0023] 3. This invention abandons the traditional method of continuous application of adhesive across the entire surface in lamination processes. Instead, it uses a discrete dot matrix method to apply reactive hot melt adhesive. The application area of ​​the hot melt adhesive accounts for only 15%-20% of the total area between the inner and outer layers. The adhesive-free areas between adjacent points form continuous and interconnected air channels, and the air permeability of the composite fabric can reach 155-183 mm / s. This solves the problem of stuffiness and dampness caused by the loss of air permeability in traditional lamination composite fabrics. At the same time, the supercritical CO2 foaming treatment creates a porous structure with increasing pore size from the inside to the outside of the hot melt adhesive dots, resulting in good air permeability. Attached Figure Description

[0024] Figure 1 This is a schematic diagram of the cashmere composite fabric structure prepared according to the present invention. Detailed Implementation

[0025] The present invention will be further described in detail below with reference to embodiments and comparative examples. However, it should be understood that these embodiments are for illustrative purposes only and are not intended to limit the scope of the invention. All technical solutions implemented based on the above description of the present invention fall within the protection scope of the present invention.

[0026] Example 1 This embodiment provides a method for preparing a cashmere composite fabric with far-infrared and negative oxygen ion emission functions. The specific steps are as follows: (1) Surface modification of functional powders Nano-tourmaline powder (average particle size 80 nm) and nano-silicon carbide powder (average particle size 50 nm) were mixed uniformly at a mass ratio of 1:1 to obtain a mixed powder. KH-550 silane coupling agent was added to an ethanol / water mixed solvent to prepare a 1% mass concentration solution. The pH was adjusted to 4.0 with glacial acetic acid, and the solution was stirred and hydrolyzed for 30 minutes to obtain a hydrolysate. The mixed powder was added to the hydrolysate at a mass ratio of 1:10, and the mixture was stirred at high speed (2000 r / min) in a 60℃ water bath for 3 hours. After the reaction, the mixture was filtered, washed three times with anhydrous ethanol, dried in an 80℃ oven for 6 hours, and then pulverized by air jet milling and sieved (300 mesh) to obtain the surface-modified functional powder.

[0027] (2) Preparation of core-sheath composite fibers The surface-modified functional powder obtained in step (1) was mixed with polyester chips (PET) at a mass ratio of 25:100 to serve as the core spinning raw material; pure PET chips were used as the sheath spinning raw material. Core-sheath composite spinning equipment was used to produce a core-sheath composite fiber with a sheath layer accounting for 60% of the total fiber mass and a core layer accounting for 40%. The fiber specifications were 2.5 dtex × 38 mm, and the sheath thickness was approximately 1.0 μm.

[0028] (3) Alkali reduction treatment The core-sheath composite fiber obtained in step (2) is woven into an inner layer fabric on a circular knitting machine (area density 120 g / m²). 2 The inner layer fabric is placed into the overflow dyeing machine in a relaxed state. Deionized water is added at a liquor ratio of 1:15, and sodium hydroxide flakes at 2% of the fabric weight are added. The temperature is increased to 70℃ at a rate of 1.5℃ / min and kept warm for 15 minutes. After treatment, the alkali solution is drained immediately, and the fabric is washed in 80℃ hot water for 10 minutes (twice), then in cold water for 10 minutes (twice). The fabric is then neutralized with 0.8% acetic acid solution at 40℃ for 10 minutes. Finally, the fabric is washed with water until neutral (pH 6.5-7.0) and dried and set in a 150℃ hot air setting machine.

[0029] (4) Hole-making treatment Water-soluble vinylon fiber (vinylon, 1.2 dtex × 38 mm) and pure cashmere yarn (fineness 15.5 μm, count 26 Nm / 2) are mixed and spun together at a mass ratio of 15:85. The resulting yarn is then spun on a spinning machine and woven on a circular knitting machine to form the outer fabric (area density 110 g / m²). 2The outer fabric is immersed in 85°C hot water for 40 minutes to completely dissolve the vinylon fibers. After washing, dehydration, and drying at 120°C, a fluffy, microporous pure cashmere outer fabric is obtained.

[0030] (5) Inner and outer layer bonding composite A rotary screen transfer coating device is used to apply moisture-curing polyurethane hot melt adhesive (PUR adhesive) between the inner and outer fabrics in a diamond dot matrix pattern (1.0 mm between adjacent dots and 0.5 mm in diameter per dot). After bonding, the area of ​​hot melt adhesive applied is 15% of the total area between the inner and outer layers. The two are then pressed together to form a composite fabric.

[0031] (6) Supercritical CO2 foaming treatment The composite fabric obtained in step (5) was placed in a supercritical CO2 foaming autoclave, pressurized to 8 MPa, heated to 40°C, and swollen for 30 minutes to allow CO2 to fully penetrate into the hot melt adhesive points. Then, the pressure was rapidly released to atmospheric pressure at a rate of 0.5 MPa / s, and the fabric was removed.

[0032] (7) Chemical modification treatment of hyperbranched polymers The composite fabric obtained in step (6) is immersed in a finishing solution containing terminal amino hyperbranched polyamide (molecular weight 2000). The mass percentage of the hyperbranched polymer in the finishing solution is 5%, the liquor ratio is 1:8, the immersion temperature is 40°C, and the immersion time is 120 minutes. After removal, it is pre-dried at 80°C for 5 minutes, then baked and cured at 160°C for 5 minutes. After washing, dehydration, and drying and shaping at 120°C, the cashmere composite fabric of this embodiment is obtained.

[0033] Example 2 This embodiment provides a method for preparing a cashmere composite fabric with far-infrared and negative oxygen ion emission functions. The specific steps are as follows: (1) Surface modification of functional powders Nano-tourmaline powder (average particle size 80 nm) and nano-silicon carbide powder (average particle size 50 nm) were mixed evenly at a mass ratio of 2:1. KH-550 silane coupling agent was added to an ethanol / water mixed solvent to prepare a 2% mass concentration solution. The pH was adjusted to 4.5 with glacial acetic acid, and the mixture was stirred and hydrolyzed for 30 minutes. The mixed powder was added to the hydrolysate at a mass ratio of 1:10, and the mixture was stirred at high speed (2000 r / min) in a 70℃ water bath for 2 hours. After the reaction, the mixture was filtered, washed three times with anhydrous ethanol, dried in a 100℃ oven for 4 hours, and then pulverized by air jet milling and sieved (300 mesh) to obtain the surface-modified functional powder.

[0034] (2) Preparation of core-sheath composite fibers The surface-modified functional powder obtained in step (1) was mixed with polyester chips (PET) at a mass ratio of 15:100 to serve as the core layer spinning raw material; pure PET chips were used as the sheath layer spinning raw material. Core-sheath composite spinning equipment was used to produce a core-sheath composite fiber with a sheath layer accounting for 75% of the total fiber mass and a core layer accounting for 25%, with a fiber specification of 2.5 dtex × 38 mm. The sheath layer thickness was approximately 0.8 μm.

[0035] (3) Alkali reduction treatment The core-sheath composite fiber obtained in step (2) is woven into an inner layer fabric on a circular knitting machine (area density 120 g / m²). 2 The inner layer fabric is placed in an overflow dyeing machine in a relaxed state. Deionized water is added at a liquor ratio of 1:15, and sodium hydroxide flakes (5% of the fabric weight) are added. The mixture is heated to 80°C at a heating rate of 1.5°C / min and held for 22 minutes. Immediately after treatment, the alkali solution is drained, and the fabric is washed sequentially with 80°C hot water for 10 minutes (twice), followed by cold water for 10 minutes (twice). Then, it is neutralized with 0.8% acetic acid solution at 40°C for 10 minutes. Finally, it is washed with water until neutral (pH 6.5-7.0) and dried and set in a 150°C hot air setting machine.

[0036] (4) Hole-making treatment Water-soluble vinylon fiber (vinylon, 1.2 dtex × 38 mm) and pure cashmere yarn (fineness 15.5 μm, count 26 Nm / 2) are mixed and spun together at a mass ratio of 20:80. The spun yarn is then spun on a spinning machine and woven on a circular knitting machine to form the outer fabric (area density 110 g / m²). 2 The outer fabric is immersed in 92℃ hot water for 35 minutes to completely dissolve the vinylon fibers. After washing, dehydration, and drying at 120℃, a fluffy, microporous pure cashmere outer fabric is obtained.

[0037] (5) Inner and outer layer bonding composite A rotary screen transfer coating device is used to apply moisture-curing polyurethane hot melt adhesive (PUR adhesive) between the inner and outer fabrics in a diamond dot matrix pattern (2.0 mm between adjacent dots and 0.8 mm in diameter per dot). After bonding, the area of ​​hot melt adhesive applied is 18% of the total area between the inner and outer layers. The two are then pressed together to form a composite fabric.

[0038] (6) Supercritical CO2 foaming treatment The composite fabric obtained in step (5) was placed in a supercritical CO2 foaming autoclave, pressurized to 10 MPa, heated to 45°C, and swollen for 40 minutes to allow CO2 to fully penetrate into the hot melt adhesive points. Then, the pressure was rapidly released to atmospheric pressure at a rate of 0.8 MPa / s, and the fabric was removed.

[0039] (7) Chemical modification treatment of hyperbranched polymers The composite fabric obtained in step (6) was immersed in a finishing solution containing terminal amino hyperbranched polyamide (molecular weight 2500). The mass percentage of the hyperbranched polymer in the finishing solution was 6.5%, the bath ratio was 1:15, the immersion temperature was 60°C, and the immersion time was 70 minutes. After removal, it was pre-dried at 90°C for 5 minutes, then baked and cured at 170°C for 4 minutes. After washing, dehydration, and drying and shaping at 120°C, the cashmere composite fabric of this embodiment was obtained.

[0040] Example 3 This embodiment provides a method for preparing a cashmere composite fabric with far-infrared and negative oxygen ion emission functions. The specific steps are as follows: (1) Surface modification of functional powders Nano-tourmaline powder (average particle size 80 nm) and nano-silicon carbide powder (average particle size 50 nm) were mixed evenly at a mass ratio of 3:1. KH-550 silane coupling agent was added to an ethanol / water mixed solvent to prepare a 3% mass concentration solution. The pH was adjusted to 5.5 with glacial acetic acid, and the mixture was stirred and hydrolyzed for 30 minutes. The mixed powder was added to the hydrolysate at a mass ratio of 1:10, and the mixture was stirred at high speed (2000 r / min) in an 80℃ water bath for 1 hour. After the reaction, the mixture was filtered, washed three times with anhydrous ethanol, dried in an oven at 105℃ for 4 hours, and then pulverized by air jet milling and sieved (300 mesh) to obtain the surface-modified functional powder.

[0041] (2) Preparation of core-sheath composite fibers The surface-modified functional powder obtained in step (1) was mixed with polyester chips (PET) at a mass ratio of 20:100 to serve as the core layer spinning raw material; pure PET chips were used as the sheath layer spinning raw material. Core-sheath composite spinning equipment was used to produce a core-sheath composite fiber with a sheath layer accounting for 80% of the total fiber mass and a core layer accounting for 20%, with a fiber specification of 2.5 dtex × 38 mm. The sheath layer thickness was approximately 0.6 μm.

[0042] (3) Alkali reduction treatment The core-sheath composite fiber obtained in step (2) is woven into an inner layer fabric on a circular knitting machine (area density 120 g / m²). 2 The inner layer fabric is placed in an overflow dyeing machine in a relaxed state. Deionized water is added at a liquor ratio of 1:15, and sodium hydroxide flakes (5% of the fabric weight) are added. The mixture is heated to 80°C at a heating rate of 1.5°C / min and held for 30 minutes. Immediately after treatment, the alkali solution is drained, and the fabric is washed sequentially with 80°C hot water for 10 minutes (twice), followed by cold water for 10 minutes (twice). Then, it is neutralized with 0.8% acetic acid solution at 40°C for 10 minutes. Finally, it is washed with water until neutral (pH 6.5-7.0) and dried and set in a 150°C hot air setting machine.

[0043] (4) Hole-making treatment Water-soluble vinylon fiber (vinylon, 1.2 dtex × 38 mm) and pure cashmere yarn (fineness 15.5 μm, count 26 Nm / 2) are mixed and spun together at a mass ratio of 30:70. The spun yarn is then spun on a spinning machine and woven on a circular knitting machine to form the outer fabric (area density 110 g / m²). 2 The outer fabric is immersed in 100°C hot water for 30 minutes to completely dissolve the vinylon fibers. After washing, dehydration, and drying at 120°C, a fluffy, microporous pure cashmere outer fabric is obtained.

[0044] (5) Inner and outer layer bonding composite A rotary screen transfer coating device is used to apply moisture-curing polyurethane hot melt adhesive (PUR adhesive) between the inner and outer fabrics in a hexagonal dot matrix pattern (3.0 mm spacing between adjacent dots and 1.0 mm diameter per dot). After bonding, the area of ​​hot melt adhesive applied is 20% of the total area between the inner and outer layers. The two are then pressed together to form a composite fabric.

[0045] (6) Supercritical CO2 foaming treatment The composite fabric obtained in step (5) was placed in a supercritical CO2 foaming autoclave, pressurized to 12 MPa, heated to 50 °C, and swollen for 50 minutes to allow CO2 to fully penetrate into the hot melt adhesive points. Then, the pressure was rapidly released to atmospheric pressure at a rate of 1.0 MPa / s, and the fabric was removed.

[0046] (7) Chemical modification treatment of hyperbranched polymers The composite fabric obtained in step (6) is immersed in a finishing solution containing hydroxyl-terminated hyperbranched polyester (molecular weight 3000). The mass percentage of the hyperbranched polymer in the finishing solution is 5%, the liquor ratio is 1:20, the immersion temperature is 80°C, and the immersion time is 20 minutes. After removal, it is pre-dried at 100°C for 5 minutes, then baked and cured at 180°C for 3 minutes. After washing, dehydration, and drying and shaping at 120°C, the cashmere composite fabric of this embodiment is obtained.

[0047] Example 4 This embodiment provides a method for preparing a cashmere composite fabric with far-infrared and negative oxygen ion emission functions. The specific steps are as follows: (1) Surface modification of functional powders Nano-tourmaline powder (average particle size 80 nm) and nano-silicon carbide powder (average particle size 50 nm) were mixed evenly at a mass ratio of 2:1. KH-550 silane coupling agent was added to an ethanol / water mixed solvent to prepare a 2% mass concentration solution. The pH was adjusted to 4.5 with glacial acetic acid, and the mixture was stirred and hydrolyzed for 30 minutes. The mixed powder was added to the hydrolysate at a mass ratio of 1:10, and the mixture was stirred at high speed (2000 r / min) in a 70℃ water bath for 2 hours. After the reaction, the mixture was filtered, washed three times with anhydrous ethanol, dried in a 100℃ oven for 4 hours, and then pulverized by air jet milling and sieved (300 mesh) to obtain the surface-modified functional powder.

[0048] (2) Preparation of core-sheath composite fibers The surface-modified functional powder obtained in step (1) was mixed with polyester chips (PET) at a mass ratio of 20:100 to serve as the core spinning raw material; pure PET chips were used as the sheath spinning raw material. Core-sheath composite spinning equipment was used to spin the fibers, resulting in a core-sheath composite fiber with a sheath layer accounting for 70% of the total fiber mass and a core layer accounting for 30%, with a fiber specification of 2.5 dtex × 38 mm.

[0049] (3) Alkali reduction treatment The core-sheath composite fiber obtained in step (2) is woven into an inner layer fabric on a circular knitting machine (area density 120 g / m²). 2 The inner layer fabric is placed in an overflow dyeing machine in a relaxed state. Deionized water is added at a liquor ratio of 1:15, and sodium hydroxide flakes (5% of the fabric weight) are added. The mixture is heated to 80°C at a heating rate of 1.5°C / min and held for 22 minutes. Immediately after treatment, the alkali solution is drained, and the fabric is washed sequentially with 80°C hot water for 10 minutes (twice), followed by cold water for 10 minutes (twice). Then, it is neutralized with 0.8% acetic acid solution at 40°C for 10 minutes. Finally, it is washed with water until neutral (pH 6.5-7.0) and dried and set in a 150°C hot air setting machine.

[0050] (4) Hole-making treatment Water-soluble vinylon fiber (vinylon, 1.2 dtex × 38 mm) and pure cashmere yarn (fineness 15.5 μm, count 26 Nm / 2) are mixed and spun together at a mass ratio of 20:80. The spun yarn is then spun on a spinning machine and woven on a circular knitting machine to form the outer fabric (area density 110 g / m²). 2 The outer fabric is immersed in 92℃ hot water for 35 minutes to completely dissolve the vinylon fibers. After washing, dehydration, and drying at 120℃, a fluffy, microporous pure cashmere outer fabric is obtained.

[0051] (5) Inner and outer layer bonding composite In the formulation stage of moisture-curing polyurethane hot melt adhesive (PUR adhesive), 0.8% by weight of azodicarbonamide (AC foaming agent) and 0.3% by weight of zinc oxide foaming aid are added to the hot melt adhesive system and stirred evenly. Using a rotary screen transfer coating device, the PUR adhesive containing the foaming agent is applied between the inner and outer fabrics in a diamond-shaped dot matrix pattern (2.0 mm spacing between adjacent dots, 0.8 mm diameter per dot). After lamination, the application area of ​​the hot melt adhesive is 18% of the total area between the inner and outer layers. The two are then pressed together to form a composite fabric.

[0052] (6) Chemical foaming treatment The composite fabric obtained in step (5) is placed in a continuous hot air oven and baked at 170°C for 4 minutes. At this temperature, azodicarbonamide decomposes to release nitrogen and carbon dioxide gases, forming a porous structure inside the hot melt adhesive points. The fabric is then removed.

[0053] (7) Chemical modification treatment of hyperbranched polymers The composite fabric obtained in step (6) was immersed in a finishing solution containing terminal amino hyperbranched polyamide (molecular weight 2500). The mass percentage of the hyperbranched polymer in the finishing solution was 6.5%, the bath ratio was 1:15, the immersion temperature was 60°C, and the immersion time was 70 minutes. After removal, it was pre-dried at 90°C for 5 minutes, then baked and cured at 175°C for 4 minutes. After washing, dehydration, and drying and shaping at 120°C, the cashmere composite fabric of this embodiment was obtained.

[0054] Comparative Example 1 The difference between this comparative example and Example 1 is that: in step (2), the core-sheath composite spinning is not used, but the surface-modified functional powder and PET chips are directly blended at a mass ratio of 10:90, and ordinary blended fibers are obtained by conventional melt spinning and woven into inner layer fabric; the remaining steps are the same as in Example 1.

[0055] Comparative Example 2 The difference between this comparative example and Example 1 is that: in step (3), the inner layer fabric is not subjected to alkali reduction and pore opening treatment after weaving, that is, the skin surface is kept smooth and without nano-pits, the functional powder is completely covered inside the skin and not exposed, and step (6) is not performed. The remaining steps are the same as in Example 1.

[0056] Comparative Example 3 The difference between this comparative example and Example 1 is that: in step (5), instead of using a discrete dot matrix method for applying adhesive, a traditional method of continuous hot melt adhesive coating is used to bond the inner and outer fabrics together across the entire width, with the hot melt adhesive covering 100% of the area and leaving no gaps. The remaining steps are the same as in Example 1.

[0057] Comparative Example 4 The difference between this comparative example and Example 1 is that step (7) is omitted, that is, the composite fabric after foaming is not subjected to hyperbranched polymer chemical modification treatment, and is directly washed, dried and shaped. The remaining steps are the same as in Example 1.

[0058] Comparative Example 5 This comparative example uses the conventional functional powder blending and spinning method in existing technology to prepare cashmere functional fabrics, as detailed below: Nano-tourmaline powder (average particle size 80 nm) was directly blended with polyester chips at a mass ratio of 15:85, and functional fibers (2.5 dtex × 38 mm) were obtained by melt spinning. The functional powder was uniformly distributed throughout the fiber cross-section. This functional fiber was then blended with pure cashmere yarn (fineness 15.5 μm, count 26 Nm / 2) at a mass ratio of 50:50 and woven into a single-knitted fabric (area density 230 g / m²). 2 After routine dyeing, setting and finishing, the fabric sample of Comparative Example 5 is obtained.

[0059] Comparative Example 6 This comparative example uses a conventional coating finishing method in the prior art to prepare cashmere functional fabrics, as detailed below: A functional coating slurry was prepared by mixing nano-tourmaline powder (average particle size 80 nm) with polyurethane binder, dispersant, thickener, etc., at a mass ratio of 20:65:5:10. A pure cashmere knitted fabric (area density 230 g / m²) was used as the base material. 2 Using a base fabric, a coating slurry was uniformly coated onto the fabric surface using a scraping method. The coating thickness was approximately 50 μm. After pre-baking at 100℃ and curing at 150℃, the fabric sample of Comparative Example 6 was obtained.

[0060] Experimental Section The main raw materials used in the following experiments, including nano-tourmaline powder (average particle size 80nm), nano-silicon carbide powder (average particle size 50nm), polyester chips (spinning grade, intrinsic viscosity 0.68dL / g), cashmere yarn (fineness 15.5μm, 26Nm / 2), water-soluble vinylon fiber (1.2dtex×38mm), silane coupling agent KH-550 (analytical grade), sodium hydroxide (analytical grade), moisture-curing polyurethane hot melt adhesive (single component, NCO content 8%-12%), amino-terminated hyperbranched polyamide (molecular weight 2000-3000), and hydroxyl-terminated hyperbranched polyester (molecular weight 3000), were all commercially available industrial-grade or commonly used laboratory reagents, used directly without further purification.

[0061] Experiment 1 Instrument: YG461E fully automatic air permeability tester; Test area: 20cm 2 ; Pressure drop setting: 100Pa; Samples: Fabric samples prepared for each embodiment and comparative example, with a size of not less than 30cm×30cm, 5 samples of each type; Standard atmospheric conditions: temperature (20±2)℃, relative humidity (65±4)%.

[0062] The test samples were laid flat and equilibrated under standard atmospheric conditions for 24 hours. Five specimens were cut from different parts of each sample, each specimen measuring no less than 30cm × 30cm. The specimens were free of wrinkles, creases, and damage. Before powering on, the zero point of the differential pressure sensor was checked to confirm that the differential pressure display was 0Pa. The instrument was calibrated using a standard calibration plate.

[0063] Clamp the sample flat onto the circular sample holder of the air permeability tester, ensuring the sample is naturally flat and free from tension. After confirming there is no air leakage from the holder's sealing gasket, close the test chamber cover, set the pressure difference to 100 Pa, and start the instrument. Once the pressure difference stabilizes at 100 Pa, continue testing until the reading stabilizes. Record the average of five stable readings. Repeat the test five times for each sample at different locations. After each test, release the sample and re-clamp it to avoid continuous testing at the same location.

[0064] Air permeability calculation formula: R = Q / A × t, where, R: air permeability, mm / s; Q: gas volume passing through the sample, mm. 3 A: Test area, mm 2 (2000mm) 2 ); t: test time, s. The arithmetic mean of 5 samples for each sample is taken as the air permeability measurement value of that sample.

[0065] Table 1. Air permeability test results for each embodiment and comparative example.

[0066] As shown in Table 1, the air permeability range of Examples 1-3 is 155-183 mm / s, with Example 2 having the highest. This may be because Example 2 has a relatively balanced dot matrix spacing of 2.0 mm and an adhesive application area of ​​18%, and the air channel area formed in the adhesive-free area has the best synergistic effect with the pore structure of the hot melt adhesive after foaming. Example 1 has the smallest adhesive application area, but the lowest content of functional powder, and the inner layer structure is relatively loose.

[0067] Comparative Example 3 uses a full-surface adhesive application method, with hot melt adhesive continuously covering the fabric surface. Although foaming treatment was performed, the continuous adhesive film still severely obstructed air channels, resulting in an air permeability of only 38 mm / s. Comparative Example 6 uses a coating method, where the coating slurry forms a dense film on the fabric surface, resulting in an air permeability of only 26 mm / s, almost non-existent. Comparative Example 5 is a blended yarn fabric. Due to the absence of an adhesive layer and its simple structure, it boasts an air permeability as high as 211 mm / s. However, this comes at the cost of sacrificing functionality, durability, and hand feel; this high air permeability does not bring any substantial improvement in comfort.

[0068] It's important to note that higher breathability isn't always better. Excessively high breathability means the fabric structure is too loose, resulting in reduced warmth in winter and poor liquid water management due to the lack of differential capillary effect.

[0069] Experiment 2 The far-infrared emissivity was tested in accordance with GB / T 30127—2013 "Test and Evaluation of Far-Infrared Performance of Textiles".

[0070] Instrument: Far-infrared emissivity testing device, mainly including blackbody chamber, test hot plate (circular surface with effective area not less than 60mm in diameter, temperature (34±0.1)℃), and far-infrared detection sensor (detection wavelength range 5μm-14μm, radiation intensity measurement accuracy ±0.1%).

[0071] Standard blackbody plate: cavity blackbody radiation source, emissivity ≥0.995.

[0072] Samples: Fabric samples prepared for each embodiment and comparative example, 50mm×50mm in size, 5 samples of each type.

[0073] Conditioning conditions: According to GB / T 6529, lay flat and equilibrate for 24 hours under standard atmospheric conditions of temperature (20±2)℃ and relative humidity (65±4)%.

[0074] Five specimens, each 50mm x 50mm, are cut from different parts of each sample. The specimens should have a smooth, wrinkle-free, and uncontaminated surface. During testing, the specimens should be placed with the inner surface facing upwards.

[0075] A standard blackbody plate was placed on a hot plate, and the temperature of the hot plate was set to (34±0.1)℃. After the temperature stabilized, the radiation intensity I0 of the standard blackbody plate in the 5μm-14μm band was measured using a far-infrared detection sensor. The sample was flatly attached to the hot plate of the test. The temperature of the hot plate was set to (34±0.1)℃. After the temperature stabilized, the radiation intensity I of the sample in the 5μm-14μm band was measured with a far-infrared detection sensor at an incident angle of 0°. Five samples were replaced for each sample and the test was repeated.

[0076] Calculation result: η = I / I0, where η: far-infrared emissivity of the sample; I0: far-infrared radiation intensity of the standard blackbody plate, unit W / m². 2 I: Far-infrared radiation intensity of the sample, unit W / m 2 .

[0077] Table 2. Far-infrared emissivity test results for each embodiment and comparative example.

[0078] As shown in Table 2, the far-infrared emissivity of Examples 1-4 all reached above 0.88. The emissivity increased with the increase of the content of functional powder in the core layer, showing a good positive correlation. This is because both tourmaline powder and silicon carbide powder have high far-infrared emission capabilities. The higher the powder concentration in the core layer, the greater the density of active emission points exposed on the surface of the pit after alkali reduction and pore opening, and the higher the far-infrared radiation efficiency.

[0079] Comparative Example 2, without alkali reduction and pore opening treatment, had a complete skin layer covering the core layer, with the functional powder completely sealed inside the skin layer. Its far-infrared emissivity was only 0.48, far below the acceptable level, essentially lacking far-infrared functionality. Comparative Example 1 used blended fibers, with functional powder evenly distributed across the entire fiber cross-section. The proportion of powder effectively exposed on the fiber surface was far lower than the core layer enrichment design, resulting in a far-infrared emissivity of only 0.72, higher than Comparative Example 2 but still significantly lower than Example 1. Comparative Example 4, without hyperbranched polymer modification treatment, had an initial far-infrared emissivity of 0.84, slightly lower than Example 1, indicating that hyperbranched polymer modification has a certain gain on the initial emissivity, but the difference is small, and its main effect is reflected in functional durability (see Experiment 4). Comparative Example 5 had an emissivity of 0.65, and Comparative Example 6 had an emissivity of 0.78, both failing to reach the acceptable level of 0.88. Although the absolute content of functional powder in the coating of Comparative Example 6 is higher than that in the core layer of Example 1, its far-infrared emissivity is still significantly lower than that of Example 1 because the powder in the coating is excessively wrapped by polyurethane adhesive and the effective exposed surface is reduced.

[0080] Experiment 3 Instrument: Negative oxygen ion tester, ion mobility ≥ 0.15cm 2 / (V·s), measuring range 0-50000 pieces / cm 3 ; Test chamber: Sealed acrylic glass chamber, 1m³ volume 3 The inner wall is treated with anti-static agents; Sampler: Air circulation sampling pump with constant flow rate; Samples: Fabric samples prepared for each embodiment and comparative example, 50cm×50cm in size, 5 samples of each type; Test conditions: Temperature (20±2)℃, relative humidity (40±5)%, background negative ion concentration ≤50 ions / cm³3 .

[0081] The test samples were laid flat and equilibrated for 24 hours under standard atmospheric conditions. 50cm x 50cm specimens were cut from different parts of each sample; the specimens should be free of wrinkles and contamination. Before testing, the surface of the specimens was electrostatically removed using an ion blower (30cm distance, 10s) to eliminate interference from electrostatic adsorption on ion concentration measurement. Before starting the instrument, the negative ion meter was calibrated using a standard ion generator to ensure the instrument reading deviation was within ±5%. The test chamber was sealed, and the air circulation sampling pump was started to purge the chamber with purified, dry air for 3 minutes to stabilize the background negative ion concentration at ≤50 ions / cm³. 3 Open the test chamber door, lay the sample flat on the central sample rack inside the chamber, quickly close the door to seal it, and start the negative oxygen ion meter. Begin recording 30 seconds after the sample is placed in, continuously collecting the negative ion concentration change over 30 minutes at a sampling frequency of 1 time / min. Take the peak value as the negative oxygen ion generation of the sample. Repeat the test with 5 samples for each sample. After each test, thoroughly clean the test chamber with zero air until the background concentration returns to ≤50 ions / cm³. 3 Then proceed with the next test.

[0082] Table 3. Test results of negative oxygen ion generation in each embodiment and comparative example.

[0083] As shown in Table 3, the negative oxygen ion generation range of Examples 1-4 is 1352-1822 ions / cm³. 3 It reaches the superior level. The generation amount increases significantly with the increase of tourmaline powder content in the core layer. Tourmaline is the core component for negative ion generation. The higher the proportion of tourmaline and the total powder content, the more effective polarization electrode points per unit area, and the stronger the ability to ionize water molecules.

[0084] Comparative Example 2, without alkali reduction and pore opening, had a negative oxygen ion generation rate of only 180 ions / cm³. 3 Functional powders cannot function when the skin layer is sealed. Comparative Example 1: 985 particles / cm² 3 Comparative Example 5 has 823 cells / cm² 3 Comparative Example 6 has 1059 cells / cm². 3 The values ​​were all significantly lower than in the embodiments. It is worth noting that, although Comparative Example 6 had an initial generation of 1050 cells / cm², the results were significantly lower. 3 However, this comes at the cost of the coating clogging the fabric pores and causing the fabric to become severely stiff, and the amount of coating decreases very rapidly after washing (see Experiment 5).

[0085] The negative oxygen ion generation rate in Example 4 was 1520 ions / cm³. 3The result was slightly lower than in Example 2, which may be because the high-temperature baking during the chemical foaming process had some impact on the exposure state of the functional powder of the inner fiber, but it was still at a relatively high level.

[0086] Experiment 4 Water Washing Durability Test Instrument: Fully automatic washing machine; Detergent: Standard detergent ECE, dosage is 20g per kilogram of clothing; Washing cloth: Pure cotton bleached cloth sheet, size 20cm×20cm, total weight makes the total washing load reach 2.0±0.1kg; Samples: Fabric samples prepared in Example 1 and Comparative Examples 1, 4, 5 and 6, each measuring 50cm × 50cm, with sufficient quantity of each sample; Drying method: Hang to air dry.

[0087] Water wash durability was tested using Example 1 and Comparative Examples 1, 4, 5, and 6. Comparative Examples 2 and 3 were not tested again because their initial function was extremely low or their durability mechanism could be inferred from the above samples.

[0088] 50cm×50cm samples were cut from different parts of each sample. After equilibration under standard atmospheric conditions for 24 hours, the air permeability, far-infrared emissivity and negative oxygen ion generation were measured according to the methods of Experiments 1, 2 and 3, respectively, as the baseline value for 0 washes. The washing temperature was 40℃, the water level was about 18L, the main wash time was 15min, the rinsing was 3 times, each time for 3min, and the dehydration speed was 800r / min. Each 5 washes were counted as 1 cycle.

[0089] Samples were taken at 0, 10, 20, 30, and 50 water washes. After each sampling, the samples were equilibrated under standard atmospheric conditions for 24 hours. The properties were measured according to the methods in Experiments 1, 2, and 3. The retention rate of each property relative to the initial value was calculated. Five samples were measured for each property, and the average value was taken.

[0090] Table 4. Far-infrared emissivity retention rate (%) after different number of water washes

[0091] Table 5. Retention rate of negative oxygen ion generation after different number of water washes (%)

[0092] As shown in Tables 4-5, after 50 water washes, the far-infrared emissivity retention rate of Example 1 was 86.2%, and the negative oxygen ion generation retention rate was 83.5%, both significantly better than all comparative examples. After 10 water washes, the retention rates were 96.5% and 95.8%, respectively, and after 20 washes, they were 93.1% and 92.0%, respectively. The attenuation mainly occurred during the initial stage of unstable powder loss. The fact that the remaining powder remained at a high level after 50 washes indicates that the remaining powder was firmly fixed.

[0093] After 50 washes, Comparative Example 4 showed a decrease in far-infrared retention rate and negative ion retention rate compared to Example 1, demonstrating that the skin layer alone is insufficient to fully fix the powder; the chemical modification and fixation of the hyperbranched polymer is the decisive factor for durability. Although Comparative Example 1 underwent modification treatment, the powder was distributed across the entire fiber cross-section rather than concentrated in the core layer, lacking skin layer protection. After 50 washes, the retention rates for both far-infrared and negative ions were only 62.5% and 58.0%, respectively, significantly lower than Example 1. After 50 washes, Comparative Examples 5 and 6 showed far-infrared retention rates of only 48.6% and 31.2%, and negative ion retention rates of only 43.0% and 25.0%, respectively. The coating method showed significant degradation after only 10 washes, indicating that traditional physical adhesion methods cannot solve the problem of durability after washing.

Claims

1. A method for preparing a cashmere composite fabric with far-infrared and negative oxygen ion emission functions, characterized in that, Includes the following steps: (1) Preparation of core-sheath composite fiber: The surface-modified functional powder is mixed with polyester chips as the core spinning raw material; the polyester chips are used as the sheath spinning raw material, and the core-sheath composite fiber with sheath covering core layer is obtained by core-sheath composite spinning process; wherein, the functional powder includes nano tourmaline powder and nano silicon carbide powder. (2) The inner fabric woven from the core-sheath composite fiber is subjected to alkali reduction and pore opening treatment to form nanoscale pits on the surface of the sheath layer, exposing part of the core layer. (3) Water-soluble vinylon fiber is spun together with cashmere yarn and woven into an outer fabric. The water-soluble vinylon fiber is removed by water-soluble treatment, so that the outer fabric forms a fluffy microporous structure. (4) A reactive hot melt adhesive is applied between the inner fabric and the outer fabric in a discrete dot matrix manner to bond the two together to form a composite fabric. (5) The composite fabric is placed in a supercritical CO2 environment and subjected to pressure swelling followed by pressure release foaming treatment, so that the hot melt adhesive forms a porous connecting layer in the glue-free area between the inner fabric and the outer fabric. (6) The composite fabric is immersed in a finishing solution containing hyperbranched polymer for chemical modification treatment, and then dried and shaped to obtain the cashmere composite fabric.

2. The method for preparing cashmere composite fabric with far-infrared and negative oxygen ion emission functions according to claim 1, characterized in that, In step (1), the surface modification treatment of the functional powder is carried out using a silane coupling agent, wherein the silane coupling agent is any one or more combinations of KH-550, KH-560 or KH-570.

3. The method for preparing cashmere composite fabric with far-infrared and negative oxygen ion emission functions according to claim 1, characterized in that, In step (1), the sheath of the core-sheath composite fiber accounts for 60%-80% of the total fiber mass, and the core accounts for 20%-40% of the total fiber mass; the functional powder in the core layer has a mass percentage of 15%-25%; and the nano-tourmaline powder and nano-silicon carbide powder are in a mass ratio of 1:1-3:

1.

4. The method for preparing cashmere composite fabric with far-infrared and negative oxygen ion emission functions according to claim 1, characterized in that, In step (2), the conditions for the alkali reduction and pore opening treatment are: alkali concentration of 2%-5%, treatment temperature of 70℃-80℃, and treatment time of 15-30 minutes; the alkali solution used is sodium hydroxide solution or potassium hydroxide solution.

5. The method for preparing cashmere composite fabric with far-infrared and negative oxygen ion emission functions according to claim 1, characterized in that, In step (2), the pore size of the nanoscale pit is 100nm-200nm, and the pit depth is 40%-50% of the skin thickness.

6. The method for preparing cashmere composite fabric with far-infrared and negative oxygen ion emission functions according to claim 1, characterized in that, In step (3), the mass ratio of the water-soluble vinylon fiber to the cashmere yarn is 15-25:75-85; the conditions for the water-soluble treatment are: water temperature 85℃-100℃, treatment time 30-40 minutes.

7. The method for preparing cashmere composite fabric with far-infrared and negative oxygen ion emission functions according to claim 1, characterized in that, In step (4), the discrete dot matrix is ​​a rhombus dot matrix, a square dot matrix, or a hexagonal dot matrix; the spacing between adjacent points of the dot matrix is ​​1.0mm-3.0mm, and the diameter of each point is 0.5mm-1.0mm.

8. The preparation method according to claim 1, characterized in that, In step (4), the reactive hot melt adhesive is a moisture-curing polyurethane hot melt adhesive; the application area of ​​the hot melt adhesive accounts for 15%-20% of the total area between the inner and outer fabric layers.

9. The method for preparing cashmere composite fabric with far-infrared and negative oxygen ion emission functions according to claim 1, characterized in that, In step (6), the hyperbranched polymer is any one of amino-terminated hyperbranched polyamide, hydroxyl-terminated hyperbranched polyester, or mercapto-terminated hyperbranched polyether; the molecular weight of the hyperbranched polymer is 2000-3000, and the mass percentage of the hyperbranched polymer in the finishing solution is 5%-8%; the conditions for the chemical modification treatment are: impregnation temperature 40℃-80℃, impregnation time 20-120 minutes, bath ratio 1:8-20, and after impregnation, pre-drying at 80℃-100℃ and curing at 160℃-180℃.

10. A cashmere composite fabric with far-infrared and negative oxygen ion emission functions prepared by the preparation method according to any one of claims 1 to 9, characterized in that, The cashmere composite fabric has a three-layer composite structure, including: The inner layer is a functional layer composed of core-skin composite fibers with nanoscale pits in the skin, which provides far-infrared and negative oxygen ion emission functions. The outer layer is a fluffy microporous layer made of pure cashmere fibers, providing a soft feel; The intermediate connecting layer is a porous lattice connecting layer made of foamed hot melt adhesive, providing breathable channels.