A heat-insulating and cooling umbrella fabric and its preparation method
By setting a reflective radiation layer and a dark absorption layer on the umbrella fabric, and utilizing a combination of hollow silica microspheres and porous carbon microspheres, the umbrella fabric can reduce the temperature under the umbrella while blocking ultraviolet rays, thus solving the problems of functional interference and easy damage to the coating in the prior art.
Patent Information
- Application Number
- CN202611580749.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-10-13
- Publication Date
- 2026-11-17
AI Technical Summary
Existing umbrella fabrics, while blocking ultraviolet rays, are difficult to simultaneously reflect sunlight, prevent heat from being conducted under the umbrella, and store peak heat during midday. Furthermore, the coating is easily damaged during high-temperature processing and daily use.
A reflective radiation layer is set on the outer surface of the polyester base fabric and a dark absorption layer is set on the inner surface. The reflective radiation layer is composed of reflective radiation core-shell particles. The core is a hollow silica microsphere encapsulated with phase change core material, and the shell is barium sulfate composite with strontium titanate nanocrystals. The dark absorption layer is composed of porous carbon microspheres. The umbrella surface temperature is reduced through the combined effects of reflection, heat insulation, heat storage and radiation functions.
It achieves the effect of effectively reflecting sunlight while blocking ultraviolet rays, preventing heat from being conducted to the umbrella, storing heat during the midday period, and maintaining the integrity of the coating during high-temperature processing and daily use, thus solving the problems of functional interference and easy damage to the coating in the prior art.
Smart Images

Figure CN123108952A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of umbrella material technology, specifically relating to a heat-insulating and cooling umbrella fabric and its preparation method. Background Technology
[0002] Sun umbrellas are among the most widely used outdoor protective products in summer, and the canopy fabric is the core component that determines the protective performance of a sun umbrella. Canopy fabric is typically made with a polyester base fabric as the skeleton, coated with a functional coating. It is widely used in umbrellas, sun umbrellas, beach umbrellas, and the tops of outdoor tents. Polyester base fabric itself is lightweight, strong, and fold-resistant, making it an ideal skeleton material for canopy fabrics. However, polyester fibers have limited ability to block sunlight; ultraviolet rays can penetrate the fabric and reach human skin, causing sunburn and aging with prolonged exposure. Therefore, functional coatings are needed on the base fabric to provide protection. The main functions of canopy fabric are twofold: first, to block ultraviolet rays from sunlight, protecting the person under the umbrella; and second, to reduce the amount of solar heat absorbed by the canopy, lowering the temperature of the space under the umbrella and providing a cool, shaded environment.
[0003] In practical applications, umbrella fabrics face a long-standing unresolved contradiction. During midday in summer, direct sunlight hits the umbrella surface, with the energy concentrated in the 300-2500 nm wavelength range. The umbrella surface absorbs this light energy and converts it into heat. Currently, most commercially available high-protection sun umbrellas use a black coating. While this black coating absorbs most visible light and ultraviolet rays, providing good UV protection, all the absorbed light energy is converted into heat and accumulates on the umbrella surface, raising its temperature to over 60°C. This high temperature then radiates heat into the space beneath the umbrella, making people feel stuffy and uncomfortable. In other words, the needs for UV protection and cooling are conflicting when using a black coating; the more the light is absorbed, the hotter the umbrella surface becomes, and the more uncomfortable it is for those under it.
[0004] To address the issue of heat absorption and temperature rise in umbrella surfaces, existing technologies offer several solutions. One approach involves adding white reflective fillers such as titanium dioxide and barium sulfate to the coating. These fillers, with their high refractive index, reflect sunlight back to the outside, reducing heat absorption by the umbrella surface. However, these reflective fillers are solid particles with a dense internal structure, resulting in rapid thermal conductivity. Heat that cannot be reflected is quickly transferred along the particles to the inner side of the umbrella surface, limiting its heat insulation capacity. Furthermore, a single reflective layer cannot block all sunlight; residual transmitted light passes through the umbrella surface and undergoes multiple diffuse reflections in the space beneath, creating secondary radiation and compromising UV protection.
[0005] Another approach involves incorporating phase change microcapsules into the coating. These utilize the properties of paraffin-based phase change core materials—melting and absorbing heat during the day, then solidifying and releasing heat as the temperature decreases—to regulate the umbrella surface temperature. However, the wall material of these microcapsules is an organic polymer. The drying temperature during coating processing typically requires 80-110℃. Under the combined effects of high temperature and the expansion of the internal molten paraffin, the wall material is prone to cracking. Paraffin leakage contaminates the coating, and the phase change temperature regulation function quickly diminishes. Furthermore, the organic wall material ages and becomes brittle under prolonged outdoor ultraviolet radiation, leading to leakage after a period of use. Yet another approach borrows from radiative cooling coatings used in the construction industry. These coatings utilize the infrared emission capability of the coating in the 8-13 μm atmospheric window band to dissipate heat to the outside environment as infrared radiation. These coatings are often designed for rigid building substrates, making them hard and brittle. After daily folding and unfolding, the coating cracks and peels off, making them unsuitable for long-term use on umbrella fabrics.
[0006] In summary, in existing technologies, the three functions of reflection, heat insulation, and heat storage are performed by different materials. Simply stacking them in the same coating can cause mutual interference. Reflective fillers conduct heat quickly, phase change microcapsules are susceptible to leakage at high temperatures, and radiation cooling coatings are not resistant to folding. Furthermore, the coating can cause secondary irradiation under the umbrella after absorbing residual transmitted light. Therefore, how to make the umbrella fabric block ultraviolet rays while simultaneously reflecting sunlight, preventing heat conduction under the umbrella, storing peak heat during midday, and absorbing residual transmitted light, and also withstand the high temperatures of coating processing and repeated folding during daily use, is a technical problem that urgently needs to be solved in this field. Therefore, this application designs a heat-insulating and cooling umbrella fabric and its preparation method. Summary of the Invention
[0007] To overcome the shortcomings of the existing technology, a heat-insulating and cooling umbrella fabric and its preparation method are provided.
[0008] To achieve the above objectives, the present invention provides the following technical solution:
[0009] A heat-insulating and cooling umbrella fabric, comprising a polyester base fabric, a reflective radiation layer on the outer surface of the polyester base fabric, and a dark-colored absorbent layer on the inner surface of the polyester base fabric.
[0010] The reflective radiation layer is formed by drying a reflective radiation slurry. The mass ratio of reflective radiation core-shell particles, water-based acrylic resin, and sodium polyacrylate in the reflective radiation slurry is 1:(2-5):(0.02-0.06), and the solid content of the reflective radiation slurry is 35-50%. The reflective radiation core-shell particles have hollow silica microspheres encapsulated with phase change core material as the core and barium sulfate composited with strontium titanate nanocrystals as the shell.
[0011] The dark absorbent layer is formed by drying a dark absorbent slurry. The mass ratio of porous carbon microspheres to water-based acrylic resin in the dark absorbent slurry is 1:(6-12), and the solid content of the dark absorbent slurry is 20-35%.
[0012] The method for preparing the reflected radiation core-shell particles is as follows: Piece wax is heated to 60-70℃ to melt, hollow silica microspheres are added, and the mass ratio of the piece wax to the hollow silica microspheres is (1.5-3):1. A vacuum is drawn to a vacuum degree of 0.06-0.09 MPa and maintained for 30-60 min. During this period, the pressure is released and the vacuum is drawn again every 10 min, repeated 2-3 times. After restoring to normal pressure, the particles are centrifuged to remove the piece wax adhering to the surface, and then cooled to obtain wax-loaded hollow silica microspheres. The mass ratio of the piece wax to the hollow silica microspheres in the wax-loaded hollow silica microspheres is (0.5-1.2):1.
[0013] Wax-loaded hollow silica microspheres were dispersed in deionized water, and strontium titanate nanocrystals were added. The mass ratio of strontium titanate nanocrystals to hollow silica microspheres was (0.05-0.2):1. The mixture was ultrasonically dispersed until uniform. 0.1-0.5 mol / L barium chloride solution and 0.1-0.5 mol / L sodium sulfate solution were added dropwise, with a molar ratio of barium chloride to sodium sulfate of 1:1. The dropping rate for both solutions was 2-5 mL / min. The amount added was based on the theoretical production amount of barium sulfate to the mass ratio of hollow silica microspheres of (0.5-1.5):1. The pH was controlled at 6-7, and the reaction was carried out at 40-50℃ for 1-3 h. The mixture was washed with deionized water at 10-20℃ and vacuum dried at 30-40℃ to obtain reflective radiation core-shell particles.
[0014] The hollow silica microspheres have a particle size of 300-600 nm; the strontium titanate nanocrystals have a particle size of 20-50 nm; and the sliced paraffin has a melting point of 52-54 °C.
[0015] The hollow silica microspheres are prepared as follows: polystyrene microspheres with a particle size of 250-500 nm are dispersed in a mixture of anhydrous ethanol and deionized water in a volume ratio of (2-4):1. Ammonia is added to adjust the pH value to 8-9. Tetraethyl orthosilicate is added dropwise, with a mass ratio of polystyrene microspheres to tetraethyl orthosilicate of 1:(1-2). The mixture is reacted at room temperature for 12-24 h, centrifuged, dried, and calcined at 500-600℃ for 2-4 h in an air atmosphere at a rate of 2-5℃ / min to obtain hollow silica microspheres.
[0016] The preparation method of the strontium titanate nanocrystals is as follows: Tetrabutyl titanate and acetylacetone are mixed in a molar ratio of 1:(1-2), complexed at room temperature for 30-60 min, and then dissolved in anhydrous ethanol. The mass ratio of tetrabutyl titanate to anhydrous ethanol is 1:(10-15) to obtain a titanium source solution. Strontium nitrate is dissolved in 0.5-2 mol / L potassium hydroxide aqueous solution. The titanium source solution is added dropwise to the strontium nitrate solution. The molar ratio of tetrabutyl titanate to strontium nitrate is 1:1. The mixture is stirred to form a suspension and subjected to hydrothermal reaction at 180-220℃ for 12-24 h. After washing and drying, strontium titanate nanocrystals are obtained.
[0017] The porous carbon microspheres are prepared as follows: sucrose is prepared into a 0.5-1.0 mol / L aqueous solution, hydrothermally carbonized at 180-220℃ for 6-12 h, filtered, dried, and carbonized at 500-700℃ for 1-3 h under nitrogen protection. The carbonized product is mixed with potassium hydroxide at a mass ratio of 1:(1-3), activated at 700-900℃ for 1-2 h under nitrogen protection, washed until neutral, dried, ground and dispersed, and then passed through a 200-mesh sieve to obtain porous carbon microspheres.
[0018] A method for preparing a heat-insulating and cooling umbrella fabric, the method comprising the following steps:
[0019] S1. Using polystyrene microspheres as templates, hollow silica microspheres are obtained by hydrolyzing and coating with tetraethyl orthosilicate and then calcining to remove the template.
[0020] S2, tetrabutyl titanate, after being complexed with acetylacetone, reacts with strontium nitrate in an aqueous potassium hydroxide solution via hydrothermal reaction to obtain strontium titanate nanocrystals;
[0021] S3. Mix the molten sliced paraffin wax with the hollow silica microspheres obtained in S1, impregnate under vacuum, centrifuge, and cool to obtain wax-loaded hollow silica microspheres.
[0022] S4. Add the wax-loaded hollow silica microspheres obtained in S3 and the strontium titanate nanocrystals obtained in S2 to deionized water, disperse them evenly by ultrasonication, add barium chloride solution and sodium sulfate solution dropwise, react at 40-50℃, wash and dry to obtain core-shell particles that reflect radiation.
[0023] S5. The sucrose aqueous solution was hydrothermally carbonized, then carbonized again under nitrogen protection and activated by mixing with potassium hydroxide. After washing, drying, grinding and dispersing, it was sieved to obtain porous carbon microspheres.
[0024] S6. Mix the reflective core-shell particles obtained in S4 with water-based acrylic resin and sodium polyacrylate, add deionized water to make a slurry, and apply the reflective slurry to the outer surface of polyester base fabric. After pre-baking at 40-50℃, dry at 80-110℃ to form a reflective layer.
[0025] S7. Mix the porous carbon microspheres obtained in S5 with water-based acrylic resin, add deionized water to adjust the slurry, and obtain a dark-colored absorbent slurry. Apply the slurry to the inner surface of the polyester base fabric, dry it, and form a dark-colored absorbent layer to obtain a heat-insulating and cooling umbrella fabric.
[0026] In S4, the power of the ultrasonic dispersion is 200-400 W, and the time is 10-30 min.
[0027] In S6, the wet film thickness of the reflective radiation slurry is 30-60 μm, the pre-baking time is 10-20 min, and the drying time is 5-15 min.
[0028] In S7, the wet film thickness of the dark absorbent slurry is 15-30 μm, the drying temperature is 80-110℃, and the drying time is 5-15 min.
[0029] Compared with the prior art, the advantages and beneficial effects of the present invention are as follows:
[0030] 1. The heat-insulating and cooling umbrella fabric provided in this application has a reflective radiation layer on the outer surface of a polyester base fabric. The reflective radiation core-shell particles in the reflective radiation layer have hollow silica microspheres encapsulated with phase change core material as the core and barium sulfate composited with strontium titanate nanocrystals as the shell. The barium sulfate shell has a high refractive index, which can reflect most of the sunlight back to the outside, reducing the light energy absorption of the umbrella surface; the cavity of the hollow silica microspheres reduces the thermal conductivity of the particles, and the residual heat after reflection is difficult to be transferred to the inside of the umbrella surface along the particles; the sliced paraffin encapsulated in the cavity melts and absorbs heat when the umbrella surface is heated by strong midday sunlight, temporarily storing the heat during the peak period, so that the temperature of the umbrella surface will not rise rapidly; the strontium titanate nanocrystals and silica have infrared emission capabilities in the atmospheric window band, and the heat accumulated on the umbrella surface can be dissipated to the outside in the form of infrared radiation. The four functions of reflection, heat insulation, heat storage, and radiation are all accomplished by a single particle. The heat entering the umbrella surface is reduced layer by layer, and the temperature of the space under the umbrella is reduced accordingly, thus solving the problem of conflict between UV protection and cooling in existing black glue coatings.
[0031] 2. The reflective radiation core-shell particles of this application are prepared by first filling the phase change core material and then depositing the shell layer. After the sliced paraffin wax is vacuum impregnated into the cavity of the hollow silica microspheres, the barium sulfate shell layer is deposited on the outer surface of the microspheres and seals the pores of the shell layer, thus confining the phase change core material within the rigid shell. Compared with phase change microcapsules with organic wall materials, silica and barium sulfate are both inorganic materials, which are resistant to high temperatures and UV aging. Even if the sliced paraffin wax melts during the drying and forming of the slurry, it is sealed within the shell and will not leak out. The cavity allowance left by the filling amount can accommodate the volume expansion caused by the melting of paraffin wax. The gradient heating method of pre-baking and drying allows residual moisture to be discharged before the paraffin wax melts. The particles remain intact during coating processing and long-term outdoor use, and the temperature regulation function does not decay with the use time, overcoming the defects of existing phase change microcapsule wall materials being prone to cracking and core material leakage.
[0032] 3. This application incorporates a dark-colored absorption layer on the inner surface of the polyester base fabric. The porous carbon microspheres within this layer possess a rich pore structure. Residual light passing through the reflective radiation layer enters the pores and undergoes multiple reflections between the pore walls. Each reflection results in partial absorption, and residual visible light and ultraviolet radiation are consumed within the pores. This not only prevents ultraviolet radiation from reaching the human body but also avoids secondary irradiation caused by light reflection back into the space under the umbrella. The porous carbon microspheres have low thermal conductivity, and the absorbed heat is slowly conducted to the human body side, allowing it to be transferred back along the polyester base fabric to the reflective radiation layer and discharged through the radiation channel in the atmospheric window band. The inner layer absorption and the outer layer reflection of radiation are seamlessly integrated, simultaneously achieving both ultraviolet protection and cooling functions.
[0033] 4. The heat-insulating and cooling umbrella fabric of this application also has excellent folding resistance. The hollow structure of the reflective radiation core-shell particles reduces the effective density and modulus of the particles. When the umbrella is folded and bent, the stress on the particle shell is dispersed through the cavity, making it difficult for cracks to propagate. After the water-based acrylic resin cures into a film, it encapsulates and fixes the particles. The coating is not easy to crack or peel off during repeated folding and can be used on the umbrella fabric for a long time. Compared with existing black glue coatings, solid reflective filler coatings, phase change microcapsule coatings, and hard radiation cooling coatings, this application reduces the temperature under the umbrella while blocking ultraviolet rays, and takes into account the coating processing temperature and folding wear during daily use. It solves the problems of mutual interference between reflection, heat insulation, and heat storage functions, easy leakage of phase change core material, and poor folding resistance of coatings in the prior art. Attached Figure Description
[0034] Figure 1 This is a process flow diagram of the preparation method of a heat-insulating and cooling umbrella fabric according to the present invention. Detailed Implementation
[0035] The technical solutions in the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.
[0036] The technical solution of this application is as follows:
[0037] A heat-insulating and cooling umbrella fabric, comprising a polyester base fabric, a reflective radiation layer on the outer surface of the polyester base fabric, and a dark-colored absorbent layer on the inner surface of the polyester base fabric.
[0038] The reflective radiation layer is formed by drying a reflective radiation slurry. The mass ratio of reflective radiation core-shell particles, water-based acrylic resin, and sodium polyacrylate in the reflective radiation slurry is 1:(2-5):(0.02-0.06), and the solid content of the reflective radiation slurry is 35-50%. The reflective radiation core-shell particles have hollow silica microspheres encapsulated with phase change core material as the core and barium sulfate composited with strontium titanate nanocrystals as the shell.
[0039] The dark absorbent layer is formed by drying a dark absorbent slurry. The mass ratio of porous carbon microspheres to water-based acrylic resin in the dark absorbent slurry is 1:(6-12), and the solid content of the dark absorbent slurry is 20-35%.
[0040] The method for preparing the reflected radiation core-shell particles is as follows: Piece wax is heated to 60-70℃ to melt, hollow silica microspheres are added, and the mass ratio of the piece wax to the hollow silica microspheres is (1.5-3):1. A vacuum is drawn to a vacuum degree of 0.06-0.09 MPa and maintained for 30-60 min. During this period, the pressure is released and the vacuum is drawn again every 10 min, repeated 2-3 times. After restoring to normal pressure, the particles are centrifuged to remove the piece wax adhering to the surface, and then cooled to obtain wax-loaded hollow silica microspheres. The mass ratio of the piece wax to the hollow silica microspheres in the wax-loaded hollow silica microspheres is (0.5-1.2):1.
[0041] Wax-loaded hollow silica microspheres were dispersed in deionized water, and strontium titanate nanocrystals were added. The mass ratio of strontium titanate nanocrystals to hollow silica microspheres was (0.05-0.2):1. The mixture was ultrasonically dispersed until uniform. 0.1-0.5 mol / L barium chloride solution and 0.1-0.5 mol / L sodium sulfate solution were added dropwise, with a molar ratio of barium chloride to sodium sulfate of 1:1. The dropping rate for both solutions was 2-5 mL / min. The amount added was based on the theoretical production amount of barium sulfate to the mass ratio of hollow silica microspheres of (0.5-1.5):1. The pH was controlled at 6-7, and the reaction was carried out at 40-50℃ for 1-3 h. The mixture was washed with deionized water at 10-20℃ and vacuum dried at 30-40℃ to obtain reflective radiation core-shell particles.
[0042] After a period of use under the midday sun, a parasol heats up and radiates heat downwards. Existing coatings with solid reflective fillers conduct heat quickly, and the heat that cannot be reflected still transfers to the parasol surface. This application employs reflective radiation core-shell particles in the reflective radiation layer, using barium sulfate composited with strontium titanate nanocrystals as the shell. The wide band gap between the valence and conduction bands of barium sulfate crystals means that the energy of visible and near-infrared photons in sunlight is insufficient to excite electron transitions. The light energy cannot be absorbed by the shell and returns to the outside world through reflection and scattering. Furthermore, barium sulfate has a high refractive index, which differs significantly from that of water-based acrylic resin. As light passes through the coating, its propagation direction repeatedly changes at the particle-resin interface, increasing the scattering paths and further improving reflection efficiency. The size of the barium sulfate grains in the shell is on the same order of magnitude as the wavelength of sunlight, resulting in strong scattering. Most sunlight is reflected back to the outside world before reaching the parasol surface, thus reducing light energy absorption at the source.
[0043] The hollow silica microspheres have a particle size of 300-600 nm; the strontium titanate nanocrystals have a particle size of 20-50 nm; and the sliced paraffin has a melting point of 52-54 °C.
[0044] The hollow silica microspheres are prepared as follows: polystyrene microspheres with a particle size of 250-500 nm are dispersed in a mixture of anhydrous ethanol and deionized water in a volume ratio of (2-4):1. Ammonia is added to adjust the pH value to 8-9. Tetraethyl orthosilicate is added dropwise, with a mass ratio of polystyrene microspheres to tetraethyl orthosilicate of 1:(1-2). The mixture is reacted at room temperature for 12-24 h, centrifuged, dried, and calcined at 500-600℃ for 2-4 h in an air atmosphere at a rate of 2-5℃ / min to obtain hollow silica microspheres.
[0045] Reflection cannot completely block sunlight from entering the umbrella; residual heat will still be conducted downwards along the coating. The reflective core-shell particles of this application use hollow silica microspheres as the core. These hollow silica microspheres are obtained by using polystyrene microspheres as a template, which are then coated with tetraethyl orthosilicate via hydrolysis and calcined to remove the template, resulting in a closed cavity inside. The gas molecules within the cavity are sparse, and the frequency of energy transfer through intermolecular collisions is much lower than that of solids, leading to very weak thermal conductivity. The cavity interrupts the continuous solid-phase heat transfer path within the particles, forcing heat transferred along the shell to bypass the silica shell wall. This lengthens the heat transfer path, reduces the effective heat transfer cross-sectional area, and makes it difficult for heat to penetrate the cavity and continue to transfer to the inner side of the umbrella surface. The particle size of the template polystyrene microspheres determines the cavity size, and the amount of tetraethyl orthosilicate hydrolysis coating determines the shell wall thickness. After calcination to remove the template, the cavity is sealed, further reducing heat transfer during the conduction phase following reflection.
[0046] Reflection and heat insulation can only reduce heat, not eliminate the continuous accumulation of heat on the umbrella surface during midday. This application encapsulates sliced paraffin wax as a phase change core material within the cavity of hollow silica microspheres. When the sliced paraffin wax melts, the molecules transform from an ordered lattice state to a disordered liquid state. This process requires the absorption of a large amount of heat while maintaining a constant temperature. The absorbed heat is stored as latent heat of phase change and does not manifest as a temperature rise on the umbrella surface. Consequently, the umbrella surface temperature is stabilized near the melting temperature. After the light intensity decreases, the sliced paraffin wax solidifies, and the heat is released slowly. During preparation, the sliced paraffin wax is first heated and melted, then mixed with hollow silica microspheres and evacuated. The gas inside the cavity is extracted, and after restoring normal pressure, the external air pressure forces the molten sliced paraffin wax into the cavity. Capillary action assists its penetration into the micropores of the shell wall. During this process, repeated depressurization and evacuation gradually remove residual air bubbles deep within the cavity, resulting in more thorough filling. Encapsulation robustness is a prerequisite for the long-term function of phase change core materials. This application adopts a sequence of filling first and then sealing. After filling, a barium sulfate shell is deposited on the outer surface of the wax-loaded hollow silica microspheres. The shell seals the pores of the cavity, and the temperature throughout the deposition, washing, and drying processes is controlled below the melting point of the sliced paraffin wax. The core material remains solid and does not leak during the preparation process. The filling volume does not completely fill the cavity, and the reserved cavity margin can accommodate the volume expansion generated when the sliced paraffin wax melts. The shell does not bear additional internal pressure. During the subsequent slurry drying, it is first pre-dried at a low temperature. At this time, the sliced paraffin wax is still solid, and the residual moisture in the coating is discharged first in the form of water vapor. Then, the temperature is raised for drying. When the paraffin wax melts, the moisture has been discharged. The moisture evaporation pressure and melting expansion do not overlap. The rigid shell remains intact during processing and use, and the core material will not leak.
[0047] The preparation method of the strontium titanate nanocrystals is as follows: Tetrabutyl titanate and acetylacetone are mixed in a molar ratio of 1:(1-2), complexed at room temperature for 30-60 min, and then dissolved in anhydrous ethanol. The mass ratio of tetrabutyl titanate to anhydrous ethanol is 1:(10-15) to obtain a titanium source solution. Strontium nitrate is dissolved in 0.5-2 mol / L potassium hydroxide aqueous solution. The titanium source solution is added dropwise to the strontium nitrate solution. The molar ratio of tetrabutyl titanate to strontium nitrate is 1:1. The mixture is stirred to form a suspension and subjected to hydrothermal reaction at 180-220℃ for 12-24 h. After washing and drying, strontium titanate nanocrystals are obtained.
[0048] The heat accumulated on the umbrella surface still needs a channel to dissipate to the outside. This application composites strontium titanate nanocrystals in a barium sulfate shell. During the preparation of strontium titanate nanocrystals, the titanium atoms in tetrabutyl titanate are highly susceptible to attack by water molecules and undergo violent hydrolysis, making it impossible to react normally with strontium nitrate. In this application, tetrabutyl titanate is first mixed with acetylacetone. Acetylacetone coordinates with titanium atoms to form a stable cyclic chelate, making it difficult for water molecules to approach the titanium atoms, thus inhibiting hydrolysis. The complexed titanium source remains stable in water and then undergoes a hydrothermal reaction with strontium nitrate in a potassium hydroxide aqueous solution. Strontium ions and titanium oxide species co-crystallize under a strongly alkaline environment to obtain strontium titanate nanocrystals with uniform particle size. During shell deposition, strontium titanate nanocrystals have high density and surface energy, making them prone to aggregation. If the aggregates remain free in the dispersion, the generated barium sulfate will preferentially nucleate on the surface of the aggregates, preventing the formation of the shell. In this application, after adding strontium titanate nanocrystals, ultrasonic dispersion is performed. The local jet and shock wave generated by ultrasonic cavitation break up the aggregates, and the strontium titanate nanocrystals are uniformly distributed with the wax-loaded hollow silica microspheres. Barium chloride solution and sodium sulfate solution are slowly added to maintain the supersaturation of barium sulfate in the dispersion at a low level. At this time, the energy barrier required for nucleation on the surface of the microspheres is lower than that for homogeneous nucleation inside the solution. Barium sulfate preferentially nucleates on the outer surface of the microspheres and grows layer by layer, and the strontium titanate nanocrystals are then uniformly incorporated into the shell. Both the silicon-oxygen bond vibration in silicon dioxide and the titanium-oxygen bond vibration in strontium titanate can produce infrared emission in the atmospheric window band. The two have different vibration frequencies and their emission peak positions are staggered. The emission band of the composite shell is wider, while the atmospheric absorption in the atmospheric window band is very weak. The heat stored on the umbrella surface is dissipated to the outside through the atmosphere in the form of infrared radiation, adding a continuous heat dissipation channel in addition to reflection, heat insulation and heat storage.
[0049] The porous carbon microspheres are prepared as follows: sucrose is prepared into a 0.5-1.0 mol / L aqueous solution, hydrothermally carbonized at 180-220℃ for 6-12 h, filtered, dried, and carbonized at 500-700℃ for 1-3 h under nitrogen protection. The carbonized product is mixed with potassium hydroxide at a mass ratio of 1:(1-3), activated at 700-900℃ for 1-2 h under nitrogen protection, washed until neutral, dried, ground and dispersed, and then passed through a 200-mesh sieve to obtain porous carbon microspheres.
[0050] After the outer reflective radiation layer blocks most of the sunlight, a small amount of residual light still passes through the umbrella surface. This application incorporates a dark-colored absorption layer on the inner surface of the polyester base fabric. The porous carbon microspheres in this layer are formed by hydrothermal carbonization of sucrose to create a spherical carbon skeleton. Further carbonization aromaticates the carbon skeleton. During activation with potassium hydroxide, the potassium hydroxide reacts with the carbon at high temperature and etches the carbon skeleton, forming well-developed micropores and mesopores. Residual light entering the pores undergoes multiple reflections between the pore walls. Carbon has a strong light absorption capacity, absorbing a portion of the light with each reflection. The depth of the pores makes it difficult for the light to return along its original path, lengthening the equivalent optical path. The light gradually dissipates within the pores, failing to reach the human body or be reflected back into the space under the umbrella to form secondary irradiation. The gas within the pores blocks the solid-phase heat transfer path. The porous carbon microspheres have low thermal conductivity, resulting in slow heat conduction towards the human body. The absorbed heat can be transferred back along the fiber axis of the polyester base fabric to the reflective radiation layer and discharged through the radiation channel in the atmospheric window band.
[0051] The umbrella surface is opened and closed daily, and the coating needs to withstand repeated bending. The reflective core-shell particles of this application have a hollow structure with low effective density and modulus. When bent, the stress on the shell layer is dispersed through the deformation of the cavity, and the edge of the cavity can also blunt the crack tip, making it difficult for cracks to be generated and propagate. After the water-based acrylic resin is cured into a film, the particles are wrapped and fixed on the surface of the polyester base fabric. The film layer has good flexibility, and the resin film layer bears the main deformation when folded. The bond between the particles and the resin remains stable during repeated folding, the coating is not easy to crack and peel off, and the heat insulation and cooling function can be maintained for a long time.
[0052] A method for preparing a heat-insulating and cooling umbrella fabric, such as... Figure 1 As shown, the preparation method includes the following steps:
[0053] S1. Using polystyrene microspheres as templates, hollow silica microspheres are obtained by hydrolyzing and coating with tetraethyl orthosilicate and then calcining to remove the template.
[0054] S2, tetrabutyl titanate, after being complexed with acetylacetone, reacts with strontium nitrate in an aqueous potassium hydroxide solution via hydrothermal reaction to obtain strontium titanate nanocrystals;
[0055] S3. Mix the molten sliced paraffin wax with the hollow silica microspheres obtained in S1, impregnate under vacuum, centrifuge, and cool to obtain wax-loaded hollow silica microspheres.
[0056] S4. Add the wax-loaded hollow silica microspheres obtained in S3 and the strontium titanate nanocrystals obtained in S2 to deionized water, disperse them evenly by ultrasonication, add barium chloride solution and sodium sulfate solution dropwise, react at 40-50℃, wash and dry to obtain core-shell particles that reflect radiation.
[0057] S5. The sucrose aqueous solution was hydrothermally carbonized, then carbonized again under nitrogen protection and activated by mixing with potassium hydroxide. After washing, drying, grinding and dispersing, it was sieved to obtain porous carbon microspheres.
[0058] S6. Mix the reflective core-shell particles obtained in S4 with water-based acrylic resin and sodium polyacrylate, add deionized water to make a slurry, and apply the reflective slurry to the outer surface of polyester base fabric. After pre-baking at 40-50℃, dry at 80-110℃ to form a reflective layer.
[0059] S7. Mix the porous carbon microspheres obtained in S5 with water-based acrylic resin, add deionized water to adjust the slurry, and obtain a dark-colored absorbent slurry. Apply the slurry to the inner surface of the polyester base fabric, dry it, and form a dark-colored absorbent layer to obtain a heat-insulating and cooling umbrella fabric.
[0060] In S4, the power of the ultrasonic dispersion is 200-400 W, and the time is 10-30 min.
[0061] In S6, the wet film thickness of the reflective radiation slurry is 30-60 μm, the pre-baking time is 10-20 min, and the drying time is 5-15 min.
[0062] In S7, the wet film thickness of the dark absorbent slurry is 15-30 μm, the drying temperature is 80-110℃, and the drying time is 5-15 min.
[0063] The present invention will be described in detail below through examples and comparative examples, but the scope of protection of the present invention is not limited to these examples. Unless otherwise specified, the chemical reagents and raw materials used in the following examples and comparative examples are all conventional commercially available products.
[0064] Example 1
[0065] Polystyrene microspheres with a particle size of 500 nm were dispersed in a mixture of anhydrous ethanol and deionized water in a volume ratio of 3:1. Ammonia was added to adjust the pH to 8, and tetraethyl orthosilicate was added dropwise. The mass ratio of polystyrene microspheres to tetraethyl orthosilicate was 1:2. The mixture was reacted at room temperature for 18 h, centrifuged, dried, and calcined at 600 °C for 3 h in air at a rate of 2 °C / min to obtain hollow silica microspheres.
[0066] Tetrabutyl titanate and acetylacetone were mixed in a molar ratio of 1:1 and complexed at room temperature for 60 min. The mixture was then dissolved in anhydrous ethanol at a mass ratio of 1:12.5 to obtain a titanium source solution. Strontium nitrate was dissolved in a 0.5 mol / L potassium hydroxide aqueous solution. The titanium source solution was added dropwise to the strontium nitrate solution at a molar ratio of 1:1 to tetrabutyl titanate. The mixture was stirred to form a suspension and subjected to hydrothermal reaction at 220℃ for 18 h. After washing and drying, strontium titanate nanocrystals were obtained.
[0067] Chip-coated paraffin wax was heated to 60°C to melt, and hollow silica microspheres were added. The mass ratio of chip-coated paraffin wax to hollow silica microspheres was 3:1. The vacuum was evacuated to a degree of 0.075 MPa and maintained for 30 min. During this period, the pressure was released and the vacuum was evacuated again every 10 min, and this process was repeated 3 times. After restoring to normal pressure, the microspheres were centrifuged to remove the chip-coated paraffin wax adhering to the surface. The microspheres were then cooled to obtain wax-loaded hollow silica microspheres with a mass ratio of chip-coated paraffin wax to hollow silica microspheres of 0.85:1.
[0068] Wax-loaded hollow silica microspheres were dispersed in deionized water, and strontium titanate nanocrystals were added. The mass ratio of strontium titanate nanocrystals to hollow silica microspheres was 0.05:1. The mixture was ultrasonically dispersed at 400 W for 20 min. Then, 0.1 mol / L barium chloride solution and 0.1 mol / L sodium sulfate solution were added dropwise, with a molar ratio of barium chloride to sodium sulfate of 1:1. The dropwise addition rate was 5 mL / min, and the amount added was based on a theoretical barium sulfate production to hollow silica microsphere mass ratio of 1.0:1. The pH was controlled at 6, and the reaction was carried out at 50 °C for 2 h. The mixture was washed with deionized water at 10 °C and dried under vacuum at 40 °C to obtain reflective radiation core-shell particles.
[0069] Sucrose was prepared into a 0.75 mol / L aqueous solution and hydrothermally carbonized at 180℃ for 12 h. After filtration and drying, the product was carbonized at 600℃ for 1 h under nitrogen protection. The carbonized product was mixed with potassium hydroxide at a mass ratio of 1:3 and activated at 800℃ for 1 h under nitrogen protection. The product was washed until neutral, dried, ground and dispersed, and then passed through a 200-mesh sieve to obtain porous carbon microspheres.
[0070] In this embodiment, 200T polyester pongee is selected as the polyester base fabric. Reflective radiation core-shell particles, water-based acrylic resin, and sodium polyacrylate are mixed in a mass ratio of 1:5:0.04. Deionized water is added to adjust the slurry solid content to 35% to obtain a reflective radiation slurry. This slurry is then coated onto the outer surface of the 200T polyester pongee fabric with a wet film thickness of 60 μm. The slurry is pre-dried at 45℃ for 10 min and then heated to 110℃ for 10 min to form a reflective radiation layer.
[0071] Porous carbon microspheres and water-based acrylic resin were mixed at a mass ratio of 1:6, and deionized water was added to adjust the slurry solid content to 35% to obtain a dark-colored absorbent slurry. This slurry was then coated onto the inner surface of polyester pongee fabric with a wet film thickness of 22.5 μm. The fabric was dried at 80°C for 15 min to form a dark-colored absorbent layer, thus obtaining a heat-insulating and cooling umbrella fabric.
[0072] Example 2
[0073] In this embodiment, the similarities to those in Embodiment 1 will not be repeated, and the differences are as follows:
[0074] Polystyrene microspheres with a particle size of 250 nm were dispersed in a mixture of anhydrous ethanol and deionized water in a volume ratio of 4:1. Ammonia was added to adjust the pH to 8.5, and tetraethyl orthosilicate was added dropwise. The mass ratio of polystyrene microspheres to tetraethyl orthosilicate was 1:1. The mixture was reacted at room temperature for 24 h, centrifuged, dried, and calcined at 500 °C for 4 h in air at a rate of 3.5 °C / min to obtain hollow silica microspheres.
[0075] Tetrabutyl titanate and acetylacetone were mixed in a molar ratio of 1:1.5 and complexed at room temperature for 30 min. The mixture was then dissolved in anhydrous ethanol at a mass ratio of 1:15 to obtain a titanium source solution. Strontium nitrate was dissolved in a 1.25 mol / L potassium hydroxide aqueous solution. The titanium source solution was added dropwise to the strontium nitrate solution at a molar ratio of 1:1 to tetrabutyl titanate. The mixture was stirred to form a suspension and subjected to hydrothermal reaction at 180℃ for 24 h. After washing and drying, strontium titanate nanocrystals were obtained.
[0076] Chip-coated paraffin wax was heated to 65°C to melt, and hollow silica microspheres were added. The mass ratio of chip-coated paraffin wax to hollow silica microspheres was 1.5:1. The vacuum was evacuated to a vacuum degree of 0.09 MPa and maintained for 45 min. During this period, the pressure was released and the vacuum was evacuated again every 10 min, and this process was repeated twice. After restoring to normal pressure, the microspheres were centrifuged to remove the chip-coated paraffin wax adhering to the surface. The microspheres were then cooled to obtain wax-loaded hollow silica microspheres. The mass ratio of chip-coated paraffin wax to hollow silica microspheres in the wax-loaded hollow silica microspheres was 1.2:1.
[0077] Wax-loaded hollow silica microspheres were dispersed in deionized water, and strontium titanate nanocrystals were added. The mass ratio of strontium titanate nanocrystals to hollow silica microspheres was 0.125:1. The mixture was ultrasonically dispersed at 200 W for 30 min. Then, 0.3 mol / L barium chloride solution and 0.3 mol / L sodium sulfate solution were added dropwise, with a molar ratio of barium chloride to sodium sulfate of 1:1. The dropwise addition rate was 2 mL / min, and the amount added was based on a theoretical barium sulfate production to hollow silica microsphere mass ratio of 1.5:1. The pH was controlled at 6.5, and the reaction was carried out at 40 °C for 3 h. The mixture was washed with deionized water at 15 °C and vacuum dried at 30 °C to obtain reflective radiation core-shell particles.
[0078] Sucrose was prepared into a 1.0 mol / L aqueous solution, hydrothermally carbonized at 200℃ for 6 h, filtered, dried, and carbonized at 700℃ for 2 h under nitrogen protection. The carbonized product was mixed with potassium hydroxide at a mass ratio of 1:1, activated at 900℃ for 1.5 h under nitrogen protection, washed until neutral, dried, ground and dispersed, and passed through a 200-mesh sieve to obtain porous carbon microspheres.
[0079] Reflective radiation core-shell particles, water-based acrylic resin, and sodium polyacrylate were mixed in a mass ratio of 1:2:0.06. Deionized water was added to adjust the slurry solid content to 42.5% to obtain a reflective radiation slurry. This slurry was then coated onto the outer surface of a 200T polyester pongee fabric with a wet film thickness of 30 μm. The fabric was pre-dried at 50℃ for 15 min and then heated to 80℃ for 15 min to form a reflective radiation layer.
[0080] Porous carbon microspheres and water-based acrylic resin were mixed at a mass ratio of 1:9. Deionized water was added to adjust the slurry solid content to 20% to obtain a dark-colored absorbent slurry. This slurry was then coated onto the inner surface of polyester pongee fabric with a wet film thickness of 30 μm. The fabric was dried at 95°C for 5 minutes to form a dark-colored absorbent layer, thus obtaining a heat-insulating and cooling umbrella fabric.
[0081] Example 3
[0082] In this embodiment, the similarities to those in Embodiment 1 will not be repeated, and the differences are as follows:
[0083] Polystyrene microspheres with a particle size of 375 nm were dispersed in a mixture of anhydrous ethanol and deionized water in a volume ratio of 2:1. Ammonia was added to adjust the pH to 9, and tetraethyl orthosilicate was added dropwise. The mass ratio of polystyrene microspheres to tetraethyl orthosilicate was 1:1.5. The mixture was reacted at room temperature for 12 h, centrifuged, dried, and calcined at 550 °C for 2 h in air at a rate of 5 °C / min to obtain hollow silica microspheres.
[0084] Tetrabutyl titanate and acetylacetone were mixed in a molar ratio of 1:2 and complexed at room temperature for 45 min. The mixture was then dissolved in anhydrous ethanol at a mass ratio of 1:10 to obtain a titanium source solution. Strontium nitrate was dissolved in a 2 mol / L potassium hydroxide aqueous solution. The titanium source solution was added dropwise to the strontium nitrate solution at a molar ratio of 1:1 to tetrabutyl titanate. The mixture was stirred to form a suspension and subjected to hydrothermal reaction at 200℃ for 12 h. After washing and drying, strontium titanate nanocrystals were obtained.
[0085] Melt paraffin slices at 70°C, add hollow silica microspheres (mass ratio of paraffin slices to hollow silica microspheres 2.25:1), evacuate to 0.06 MPa and maintain for 60 min, depressurize and evacuate again every 10 min, repeat twice, restore to normal pressure, centrifuge to remove paraffin slices adhering to the surface, cool to obtain wax-loaded hollow silica microspheres (mass ratio of paraffin slices to hollow silica microspheres 0.5:1).
[0086] Wax-loaded hollow silica microspheres were dispersed in deionized water, and strontium titanate nanocrystals were added. The mass ratio of strontium titanate nanocrystals to hollow silica microspheres was 0.2:1. The mixture was ultrasonically dispersed at 300 W for 10 min. Then, 0.5 mol / L barium chloride solution and 0.5 mol / L sodium sulfate solution were added dropwise, with a molar ratio of barium chloride to sodium sulfate of 1:1. The dropwise addition rate was 3.5 mL / min, and the amount added was based on the theoretical production amount of barium sulfate to the mass ratio of hollow silica microspheres of 0.5:1. The pH was controlled at 7, and the reaction was carried out at 45 °C for 1 h. The mixture was washed with deionized water at 20 °C and dried under vacuum at 35 °C to obtain reflective radiation core-shell particles.
[0087] Sucrose was prepared into a 0.5 mol / L aqueous solution and hydrothermally carbonized at 220℃ for 9 h. After filtration and drying, the product was carbonized at 500℃ for 3 h under nitrogen protection. The carbonized product was mixed with potassium hydroxide at a mass ratio of 1:2 and activated at 700℃ for 2 h under nitrogen protection. The product was washed until neutral, dried, ground and dispersed, and then passed through a 200-mesh sieve to obtain porous carbon microspheres.
[0088] Reflective radiation core-shell particles, water-based acrylic resin, and sodium polyacrylate were mixed in a mass ratio of 1:3.5:0.02. Deionized water was added to adjust the slurry solid content to 50% to obtain a reflective radiation slurry. This slurry was then coated onto the outer surface of a 200T polyester pongee fabric with a wet film thickness of 45 μm. The fabric was pre-dried at 40℃ for 20 min and then heated to 95℃ for 5 min to form a reflective radiation layer.
[0089] Porous carbon microspheres and water-based acrylic resin were mixed at a mass ratio of 1:12. Deionized water was added to adjust the slurry solid content to 27.5% to obtain a dark-colored absorbent slurry. This slurry was then coated onto the inner surface of polyester pongee fabric with a wet film thickness of 15 μm. The fabric was dried at 110℃ for 10 min to form a dark-colored absorbent layer, thus obtaining a heat-insulating and cooling umbrella fabric.
[0090] Example 4
[0091] In this embodiment, the similarities to those in Embodiment 1 will not be repeated, and the differences are as follows:
[0092] Polystyrene microspheres with a particle size of 375 nm were dispersed in a mixture of anhydrous ethanol and deionized water in a volume ratio of 3:1. Ammonia was added to adjust the pH to 8.5, and tetraethyl orthosilicate was added dropwise. The mass ratio of polystyrene microspheres to tetraethyl orthosilicate was 1:1.5. The mixture was reacted at room temperature for 18 h, centrifuged, dried, and calcined at 550 °C for 3 h in air at a rate of 3 °C / min to obtain hollow silica microspheres.
[0093] Tetrabutyl titanate and acetylacetone were mixed in a molar ratio of 1:1.5 and complexed at room temperature for 45 min. The mixture was then dissolved in anhydrous ethanol at a mass ratio of 1:12 to obtain a titanium source solution. Strontium nitrate was dissolved in a 1.2 mol / L potassium hydroxide aqueous solution. The titanium source solution was added dropwise to the strontium nitrate solution at a molar ratio of 1:1 to tetrabutyl titanate. The mixture was stirred to form a suspension and subjected to hydrothermal reaction at 200℃ for 18 h. After washing and drying, strontium titanate nanocrystals were obtained.
[0094] Chip-coated paraffin wax was heated to 65°C to melt, and hollow silica microspheres were added. The mass ratio of chip-coated paraffin wax to hollow silica microspheres was 2.5:1. The vacuum was evacuated to a degree of 0.08 MPa and maintained for 45 min. During this period, the pressure was released and the vacuum was evacuated again every 10 min, and this process was repeated 3 times. After restoring to normal pressure, the mixture was centrifuged to remove the chip-coated paraffin wax adhering to the surface. The mixture was then cooled to obtain wax-loaded hollow silica microspheres. The mass ratio of chip-coated paraffin wax to hollow silica microspheres in the wax-loaded hollow silica microspheres was 1.0:1.
[0095] Wax-loaded hollow silica microspheres were dispersed in deionized water, and strontium titanate nanocrystals were added. The mass ratio of strontium titanate nanocrystals to hollow silica microspheres was 0.12:1. The mixture was ultrasonically dispersed at 300 W for 20 min. Then, 0.3 mol / L barium chloride solution and 0.3 mol / L sodium sulfate solution were added dropwise, with a molar ratio of barium chloride to sodium sulfate of 1:1. The dropwise addition rate was 3 mL / min, and the amount added was based on a theoretical barium sulfate production to hollow silica microsphere mass ratio of 1.0:1. The pH was controlled at 6.5, and the reaction was carried out at 45 °C for 2 h. The mixture was washed with deionized water at 15 °C and vacuum dried at 35 °C to obtain reflective radiation core-shell particles.
[0096] Sucrose was prepared into a 0.8 mol / L aqueous solution, hydrothermally carbonized at 200℃ for 10 h, filtered, dried, and carbonized at 600℃ for 2 h under nitrogen protection. The carbonized product was mixed with potassium hydroxide at a mass ratio of 1:2, activated at 800℃ for 1.5 h under nitrogen protection, washed until neutral, dried, ground and dispersed, and passed through a 200-mesh sieve to obtain porous carbon microspheres.
[0097] Reflective radiation core-shell particles, water-based acrylic resin, and sodium polyacrylate were mixed in a mass ratio of 1:3.5:0.04. Deionized water was added to adjust the slurry solid content to 45% to obtain a reflective radiation slurry. This slurry was then coated onto the outer surface of a 200T polyester pongee fabric with a wet film thickness of 45 μm. The fabric was pre-dried at 45℃ for 15 min and then heated to 95℃ for 10 min to form a reflective radiation layer.
[0098] Porous carbon microspheres and water-based acrylic resin were mixed at a mass ratio of 1:9, and deionized water was added to adjust the slurry solid content to 28% to obtain a dark-colored absorbent slurry. This slurry was then coated onto the inner surface of polyester pongee fabric with a wet film thickness of 20 μm. The fabric was dried at 95°C for 10 min to form a dark-colored absorbent layer, thus obtaining a heat-insulating and cooling umbrella fabric.
[0099] Comparative Example 1: The difference from Example 4 is that commercially available solid silica microspheres are used instead of hollow silica microspheres, and vacuum impregnation and filling with sliced paraffin is not performed. The solid silica microspheres are directly deposited with strontium titanate nanocrystals. The remaining steps are the same as in Example 4 to obtain the umbrella fabric.
[0100] Comparative Example 2: The difference from Example 4 is that the preparation of strontium titanate nanocrystals is omitted, and strontium titanate nanocrystals are not added during the deposition of the shell layer. The shell layer is only barium sulfate. The remaining steps are the same as in Example 4, and the umbrella fabric is obtained.
[0101] Comparative Example 3: The difference from Example 4 is that the hollow silica microspheres are not filled with sliced paraffin, but directly deposited with shell. The remaining steps are the same as in Example 4 to obtain the umbrella fabric.
[0102] Comparative Example 4: The difference from Example 4 is that carbon black is used instead of porous carbon microspheres. The mass ratio of carbon black to waterborne acrylic resin is the same as in Example 4. The remaining steps are the same as in Example 4 to obtain umbrella fabric.
[0103] Comparative Example 5: The difference from Example 4 is that the coating of dark absorbent slurry is omitted, and no dark absorbent layer is provided on the inner surface of the polyester pongee. The remaining steps are the same as in Example 4, and the umbrella fabric is obtained.
[0104] Comparative Example 6: The difference from Example 4 is that commercially available paraffin phase change microcapsules are used instead of reflective radiation core-shell particles. The wall material of the paraffin phase change microcapsules is melamine-formaldehyde resin and the core material is sliced paraffin. The remaining steps are the same as in Example 4 to obtain umbrella fabric.
[0105] Comparative Example 7: The difference from Example 4 is that the reflective radiation paste was not pre-dried after being scraped and was directly dried at 110°C for 10 min. The remaining steps were the same as in Example 4, and the umbrella fabric was obtained.
[0106] Performance Test Results and Analysis
[0107] The umbrella fabrics obtained in Examples 1-4 and Comparative Examples 1-7 were cut into samples and subjected to the following tests. For the UPF test, four samples were taken according to GB / T18830. For the other tests, three parallel samples were taken from each group of samples, and the average value of the test results was used. The sample size for solar reflectivity and visible light transmittance testing was 50 mm × 50 mm; the sample size for atmospheric window emissivity testing was 20 mm × 20 mm; the sample size for cooling performance testing was 500 mm × 500 mm; the sample size for UPF testing was 100 mm × 100 mm; the sample size for heat leakage resistance testing was 50 mm × 50 mm; and the sample size for folding resistance testing was 150 mm × 20 mm.
[0108] Solar reflectance was measured using a UV-Vis-NIR spectrophotometer equipped with an integrating sphere, with a measurement band of 300-2500 nm; atmospheric window emissivity was measured using a Fourier transform infrared spectrometer, with a measurement band of 8-13 μm; visible light transmittance was measured using a spectrophotometer to determine the average transmittance in the 380-780 nm band; during the cooling performance test, the sample was fixed on a simulated umbrella frame and irradiated vertically from one side of the sample's outer surface with a 500 W xenon lamp, with a distance of 30 cm between the light source and the sample, and an irradiance of 1000 W / m² at the sample's outer surface. 2 The ambient temperature was maintained at 26℃. The temperature at 5 cm below the inner surface of the sample was measured using a thermocouple. After irradiation for 30 min, the equilibrium temperature was recorded as the temperature under the umbrella. Simultaneously, the highest temperature of the outer surface of the sample was measured using an infrared thermometer. The UV protection performance was determined according to GB / T 18830, using the UV protection factor (UPF). For the heat leakage resistance test, the sample was weighed and placed in a 110℃ forced-air drying oven for 30 min. After cooling, it was weighed again, and the mass loss rate was calculated. For the folding resistance test, the sample was folded 500 times on a folding resistance tester. The mass of the sample before and after folding was weighed, and the mass loss rate before and after folding was used to characterize the coating peeling. The coating mass retention rate was calculated. The test results are shown in Tables 1, 2, and 3.
[0109] Table 1 Optical performance test results
[0110] sample Solar reflectance, % Atmospheric window emissivity, % Visible light transmittance, % Example 1 84.8 90.2 0.6 Example 2 85.9 91.5 0.5 Example 3 86.4 91.8 0.5 Example 4 89.3 94.2 0.3 Comparative Example 1 83.5 89.8 0.7 Comparative Example 2 85.1 83.6 0.6 Comparative Example 3 85.6 91.0 0.6 Comparative Example 4 85.0 90.8 1.8 Comparative Example 5 85.2 90.9 12.6 Comparative Example 6 82.9 89.2 0.8 Comparative Example 7 84.2 90.1 0.7
[0111] The solar reflectivity is mainly determined by the barium sulfate shell. As shown in Table 1, the shell thickness and uniformity of Example 4 are optimal, achieving a reflectivity of 89.3%. Examples 1-3 show slightly lower reflectivity due to differences in shell formation and deposition conditions, but all remain above 84%. Comparative Example 2, with a shell consisting only of barium sulfate and lacking strontium titanate nanocrystals, exhibits an atmospheric window emissivity of 83.6%, showing the most significant difference from the examples. This indicates that the composite of strontium titanate nanocrystals broadens the emission band of the shell in the atmospheric window wavelength range, consistent with the analysis that the emission peaks of silica and strontium titanate are staggered in the beneficial effect. Comparative Example 5, without a dark absorption layer, achieved a visible light transmittance of 12.6%, with residual light passing directly through the umbrella surface. Comparative Example 4, using carbon black instead of porous carbon microspheres, achieved a transmittance of 1.8%, higher than the other examples. The dense internal structure of carbon black particles causes light to be absorbed only once at the particle surface, while the porous structure of the carbon microspheres results in multiple reflections and gradual depletion of light within the pores, leading to a longer equivalent optical path and achieving a lower transmittance with the same amount of carbon black. The reflective radiation shell composition of Comparative Examples 3-5 is the same as that of Example 4. Solar reflectivity and atmospheric window emissivity are mainly determined by the shell, thus these two indicators are close to those of Example 4. The main differences between Comparative Examples 3-5 and the present application are reflected in the cooling performance (Table 2) and durability performance (Table 3).
[0112] Table 2. Test results of cooling and UV protection performance
[0113] sample Temperature under the umbrella, ℃ Maximum temperature on the outer surface of the umbrella canopy, ℃ UPF Example 1 35.8 57.8 50+ Example 2 35.2 57.1 50+ Example 3 34.9 56.6 50+ Example 4 33.6 55.8 50+ Comparative Example 1 38.6 63.5 50+ Comparative Example 2 37.9 62.8 50+ Comparative Example 3 38.2 64.2 50+ Comparative Example 4 37.6 61.9 50+ Comparative Example 5 37.3 61.2 35 Comparative Example 6 38.4 63.8 50+ Comparative Example 7 38.0 62.4 50+
[0114] Table 2 shows the test results of cooling and UV protection performance. In Table 2, the temperature under the umbrella is the result of the combined effect of four heat channels: reflection, insulation, heat storage, and radiation. The temperature under the umbrella in Example 4 was 33.6℃, which was only 7.6℃ higher than the ambient temperature. Background art records indicate that the temperature of a black-coated umbrella surface can rise above 60℃. The black-coated surface absorbs most of the visible light and ultraviolet rays, and its solar reflectivity is usually less than 10%, meaning that more than 90% of the solar energy is absorbed by the umbrella surface and converted into heat. As shown in Table 1, the solar reflectivity of Examples 1-4 is 84.8%-89.3%, and the visible light transmittance is less than 1%. The absorption rate of sunlight by the umbrella surface is only about 10%, and the heat absorption of the umbrella surface under the same irradiation conditions is less than 20% of that of the black-coated umbrella surface. This is the fundamental reason why the highest surface temperature of the umbrella surface in this application is only 55.8-57.8℃, and the temperature under the umbrella is significantly lower than that of the black-coated umbrella surface.
[0115] Comparative Example 1 used solid silica microspheres, eliminating the heat transfer barrier effect of the cavity. Heat was transferred along the solid particles to the inner side of the umbrella surface, and the temperature under the umbrella rose to 38.6℃. Comparative Example 3 lacked sliced paraffin wax, so the peak heat at noon had nowhere to be stored, and both the highest temperature on the outer surface of the umbrella and the temperature under the umbrella increased, indicating the smoothing effect of the phase change core material on peak heat. Comparative Example 2 had the lowest atmospheric window emissivity, and lacked a radiation outlet channel for stored heat, resulting in a corresponding increase in the temperature under the umbrella. Comparative Example 6 used paraffin phase change microcapsules with organic wall materials. Although it initially had heat storage capacity, its temperature under the umbrella was still higher than that of the other examples. This was because some of the microcapsule wall materials had cracked during the drying process, resulting in the loss of sliced paraffin wax and a decrease in heat storage capacity. The UPF of all examples reached 50+. Comparative Example 5, lacking a dark absorption layer, did not absorb the transmitted ultraviolet light, and its UPF dropped to 35, verifying the necessity of the inner and outer layers working together for UV protection.
[0116] In Table 3, the mass loss rate of Examples 1-4 after treatment at 110℃ for 30 min was less than 1%, indicating that the sealing effect of the inorganic shell on the sliced paraffin remained reliable at the coating processing temperature. Comparative Example 6 had a mass loss rate of 4.3%, indicating that the organic wall material cracked under the combined effects of high temperature and the melting and expansion of paraffin, resulting in a large amount of sliced paraffin seeping out. Comparative Example 7 was directly dried at high temperature without pre-drying; the residual moisture evaporation and the melting and expansion of paraffin caused some shells to crack, resulting in a mass loss rate of 1.6%, demonstrating the protective effect of the gradient heating pre-drying step on the integrity of the shell. Regarding folding resistance, the coating mass retention rate of the examples was all above 96.8%. The hollow structure reduced the effective modulus of the reflective core-shell particles, and the bending stress was dispersed through the cavity, making the coating less prone to cracking. Comparative Example 1 used solid particles, and the stress concentrated at the particle-resin interface during bending, reducing the coating mass retention rate to 92.1%. In Comparative Example 6, defects appeared inside the coating after the microcapsules ruptured, making it more prone to peeling during folding. Based on Tables 1 to 3, Example 1, which showed the weakest effect, still outperformed the best-performing comparative example in all indicators.
[0117] Table 3 Durability test results
[0118] sample Mass loss rate (%) after treatment at 110℃ for 30 min Coating quality retention rate after 500 folds, % Example 1 0.9 96.8 Example 2 0.7 97.3 Example 3 0.6 97.6 Example 4 0.2 98.4 Comparative Example 1 - 92.1 Comparative Example 2 0.5 93.5 Comparative Example 3 - 94.0 Comparative Example 4 0.5 91.8 Comparative Example 5 0.4 91.6 Comparative Example 6 4.3 88.6 Comparative Example 7 1.6 90.4
[0119] Note: The coatings of the umbrella fabrics obtained in Comparative Examples 1 and 3 do not contain sliced paraffin and have no core material for leakage, so heat leakage resistance performance tests were not conducted, and are indicated by - in the table.
[0120] Test results show that the present invention uses hollow silica microspheres encapsulated with sliced paraffin as the core and barium sulfate composited with strontium titanate nanocrystals as the shell to create a reflective radiation core-shell particle. Combined with the dark inner layer of porous carbon microspheres, the umbrella fabric simultaneously possesses five heat channels: reflecting sunlight, cavity heat insulation, phase change peak reduction, atmospheric window radiation heat dissipation, and residual light absorption. Compared with the black glue coating, the heat absorption of the umbrella surface is reduced by about 80%, and the inorganic shell is firmly encapsulated and does not leak wax, the hollow structure is fold-resistant, and the cooling effect is long-lasting and stable.
[0121] The above description represents the preferred embodiments of the present invention. It should be noted that those skilled in the art can make various improvements and modifications without departing from the principles of the present invention, and these improvements and modifications should also be considered within the scope of protection of the present invention.
Claims
1. A heat-insulating and cooling umbrella fabric, characterized in that, The umbrella fabric includes a polyester base fabric, a reflective radiation layer on the outer surface of the polyester base fabric, and a dark-colored absorbent layer on the inner surface of the polyester base fabric. The reflective radiation layer is formed by drying a reflective radiation slurry. The mass ratio of reflective radiation core-shell particles, water-based acrylic resin, and sodium polyacrylate in the reflective radiation slurry is 1:(2-5):(0.02-0.06), and the solid content of the reflective radiation slurry is 35-50%. The reflective radiation core-shell particles have hollow silica microspheres encapsulated with phase change core material as the core and barium sulfate composited with strontium titanate nanocrystals as the shell. The dark absorbent layer is formed by drying a dark absorbent slurry. The mass ratio of porous carbon microspheres to water-based acrylic resin in the dark absorbent slurry is 1:(6-12), and the solid content of the dark absorbent slurry is 20-35%.
2. The heat-insulating and cooling umbrella fabric according to claim 1, characterized in that, The method for preparing the reflected radiation core-shell particles is as follows: Piece wax is heated to 60-70℃ to melt, hollow silica microspheres are added, and the mass ratio of the piece wax to the hollow silica microspheres is (1.5-3):
1. A vacuum is drawn to a vacuum degree of 0.06-0.09 MPa and maintained for 30-60 min. During this period, the pressure is released and the vacuum is drawn again every 10 min, repeated 2-3 times. After restoring to normal pressure, the particles are centrifuged to remove the piece wax adhering to the surface, and then cooled to obtain wax-loaded hollow silica microspheres. The mass ratio of the piece wax to the hollow silica microspheres in the wax-loaded hollow silica microspheres is (0.5-1.2):
1. Wax-loaded hollow silica microspheres were dispersed in deionized water, and strontium titanate nanocrystals were added. The mass ratio of strontium titanate nanocrystals to hollow silica microspheres was (0.05-0.2):
1. The mixture was ultrasonically dispersed until uniform. 0.1-0.5 mol / L barium chloride solution and 0.1-0.5 mol / L sodium sulfate solution were added dropwise, with a molar ratio of barium chloride to sodium sulfate of 1:
1. The dropping rate for both solutions was 2-5 mL / min. The amount added was based on the theoretical production amount of barium sulfate to the mass ratio of hollow silica microspheres of (0.5-1.5):
1. The pH was controlled at 6-7, and the reaction was carried out at 40-50℃ for 1-3 h. The mixture was washed with deionized water at 10-20℃ and vacuum dried at 30-40℃ to obtain reflective radiation core-shell particles.
3. The heat-insulating and cooling umbrella fabric according to claim 2, characterized in that, The hollow silica microspheres have a particle size of 300-600 nm; the strontium titanate nanocrystals have a particle size of 20-50 nm; and the sliced paraffin has a melting point of 52-54℃.
4. The heat-insulating and cooling umbrella fabric according to claim 2, characterized in that, The hollow silica microspheres are prepared as follows: polystyrene microspheres with a particle size of 250-500 nm are dispersed in a mixture of anhydrous ethanol and deionized water in a volume ratio of (2-4):
1. Ammonia is added to adjust the pH value to 8-9. Tetraethyl orthosilicate is added dropwise, with a mass ratio of polystyrene microspheres to tetraethyl orthosilicate of 1:(1-2). The mixture is reacted at room temperature for 12-24 h, centrifuged, dried, and calcined at 500-600℃ for 2-4 h in an air atmosphere at a rate of 2-5℃ / min to obtain hollow silica microspheres.
5. The heat-insulating and cooling umbrella fabric according to claim 2, characterized in that, The preparation method of the strontium titanate nanocrystals is as follows: Tetrabutyl titanate and acetylacetone are mixed in a molar ratio of 1:(1-2), complexed at room temperature for 30-60 min, and then dissolved in anhydrous ethanol. The mass ratio of tetrabutyl titanate to anhydrous ethanol is 1:(10-15) to obtain a titanium source solution. Strontium nitrate is dissolved in a 0.5-2 mol / L potassium hydroxide aqueous solution. The titanium source solution is added dropwise to the strontium nitrate solution. The molar ratio of tetrabutyl titanate to strontium nitrate is 1:
1. The mixture is stirred to form a suspension and subjected to hydrothermal reaction at 180-220℃ for 12-24 h. After washing and drying, strontium titanate nanocrystals are obtained.
6. The heat-insulating and cooling umbrella fabric according to claim 1, characterized in that, The porous carbon microspheres are prepared as follows: sucrose is prepared into a 0.5-1.0 mol / L aqueous solution, hydrothermally carbonized at 180-220℃ for 6-12 h, filtered, dried, and carbonized at 500-700℃ for 1-3 h under nitrogen protection. The carbonized product is mixed with potassium hydroxide at a mass ratio of 1:(1-3), activated at 700-900℃ for 1-2 h under nitrogen protection, washed until neutral, dried, ground and dispersed, and then passed through a 200-mesh sieve to obtain porous carbon microspheres.
7. A method for preparing a heat-insulating and cooling umbrella fabric as described in any one of claims 1-6, characterized in that, The preparation method includes the following steps: S1. Using polystyrene microspheres as templates, hollow silica microspheres are obtained by hydrolyzing and coating with tetraethyl orthosilicate and then calcining to remove the template. S2, tetrabutyl titanate, after being complexed with acetylacetone, reacts with strontium nitrate in an aqueous potassium hydroxide solution via hydrothermal reaction to obtain strontium titanate nanocrystals; S3. Mix the molten sliced paraffin wax with the hollow silica microspheres obtained in S1, impregnate under vacuum, centrifuge, and cool to obtain wax-loaded hollow silica microspheres. S4. Add the wax-loaded hollow silica microspheres obtained in S3 and the strontium titanate nanocrystals obtained in S2 to deionized water, disperse them evenly by ultrasonication, add barium chloride solution and sodium sulfate solution dropwise, react at 40-50℃, wash and dry to obtain core-shell particles that reflect radiation. S5. The sucrose aqueous solution was hydrothermally carbonized, then carbonized again under nitrogen protection and activated by mixing with potassium hydroxide. After washing, drying, grinding and dispersing, it was sieved to obtain porous carbon microspheres. S6. Mix the reflective core-shell particles obtained in S4 with water-based acrylic resin and sodium polyacrylate, add deionized water to make a slurry, and apply the reflective slurry to the outer surface of polyester base fabric. After pre-baking at 40-50℃, dry at 80-110℃ to form a reflective layer. S7. Mix the porous carbon microspheres obtained in S5 with water-based acrylic resin, add deionized water to adjust the slurry, and obtain a dark-colored absorbent slurry. Apply the slurry to the inner surface of the polyester base fabric, dry it, and form a dark-colored absorbent layer to obtain a heat-insulating and cooling umbrella fabric.
8. The method for preparing a heat-insulating and cooling umbrella fabric according to claim 7, characterized in that, In S4, the power of the ultrasonic dispersion is 200-400 W, and the time is 10-30 min.
9. The method for preparing a heat-insulating and cooling umbrella fabric according to claim 7, characterized in that, In S6, the wet film thickness of the reflective radiation slurry is 30-60 μm, the pre-baking time is 10-20 min, and the drying time is 5-15 min.