A composite membrane material, its preparation method and application

By using a seven-layer composite structure and a plasticizer compounding system, the problems of flexibility, puncture resistance, and plasticizer leaching in aquaculture seepage prevention materials for shrimp and crab farming have been solved, achieving high-efficiency seepage prevention performance and water quality safety, and meeting the long-term application needs of shrimp and crab farming.

CN123108958APending Publication Date: 2026-11-17ZHEJIANG HAILEDE COMPOSITE NEW MATERIAL CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611273998.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-21
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing aquaculture waterproofing materials suffer from insufficient flexibility, insufficient puncture resistance, and plasticizer migration and leaching issues in shrimp and crab farming scenarios, making it difficult to simultaneously meet the application requirements of high-end aquatic products.

Method used

It adopts a seven-layer composite structure consisting of polyester fiber base fabric, double-sided PVC waterproof functional layer and double-layer water-based acrylic barrier protective surface layer, combined with DOTP and TOTM medical-grade compound plasticizing system, and active zinc oxide and nano silver antibacterial agent to form a double barrier to prevent plasticizer migration and construct a composite anti-ultraviolet system.

Benefits of technology

It achieves high puncture resistance, flexible fit, and low plasticizer leaching, extending service life, meeting the testing standards for high-end aquatic products exports, and reducing water quality safety risks.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123108958A_ABST
    Figure CN123108958A_ABST
Patent Text Reader

Abstract

This application belongs to the technical field of aquaculture seepage prevention materials, specifically relating to a composite membrane material, its preparation method, and its application. This application utilizes a seven-layer composite structure design consisting of a high-strength polyester fiber base fabric, a double-sided PVC seepage prevention functional layer, and a double-layer water-based acrylic barrier protective layer. Combined with a DOTP and TOTM medical-grade compound plasticizing system, it simultaneously achieves three core properties: flexible adhesion, high puncture resistance, and low additive exudation. Performance test results show that the material's permeability coefficient is ≤1.0×10⁻⁶. ‑13 cm / s, CBR burst strength ≥6.5KN, burst strength is more than twice that of conventional HDPE geomembrane and far exceeds the burst strength of ordinary PVC pool cloth which is less than 2KN. It is soft and flexible and does not have the problem of large amount of plasticizer leaching. It perfectly solves the industry pain point that traditional aquatic seepage prevention materials cannot simultaneously take into account flexibility, puncture resistance and low exudation.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application belongs to the technical field of aquaculture seepage prevention materials, specifically relating to a PVC coated composite material for seepage prevention in aquaculture ponds. Background Technology

[0002] Geomembranes are crucial geosynthetic materials for large-scale pond aquaculture, playing a vital role in maintaining water stability, regulating the aquaculture microenvironment, and protecting the soil and water ecosystem. Material selection and product quality directly impact the operational stability, maintenance costs, and production returns of the aquaculture system. Currently, the concentration of materials used in domestic aquaculture geomembranes is high. HDPE geomembranes, with their excellent basic impermeability, weather resistance, and physical properties, have become the dominant material in the industry, accounting for over 90% of market applications. Supplemented by a small amount of PVC flexible pond fabric, this constitutes the mainstream material system for aquaculture geomembranes at present.

[0003] Industry-compliant HDPE geomembranes possess standardized technical parameters. The typical thickness range for aquaculture applications is 0.5-1.5mm, with a tensile strength ≥25MPa, elongation at break ≥700%, and permeability ≤1.0×10⁻⁶. -13 With a strength of cm / s, the material can be given basic UV aging resistance by adding 2%-3% carbon black masterbatch, making it fully adaptable to the working conditions and usage requirements of conventional freshwater fish farming. However, this material has structural compatibility defects in shrimp and crab aquaculture. HDPE geomembrane has a high rigidity modulus and weak flexibility, with a Shore hardness of D60-70. For the complex terrain of shrimp and crab ponds, such as curved slopes and uneven bases, insufficient fit during installation can easily lead to construction defects such as wrinkles, voids, and delamination, damaging the overall airtightness and structural integrity of the impermeable layer and causing the pond's impermeability system to fail. Regarding puncture resistance, the material's overall mechanical parameters meet the standards, but its resistance to concentrated stress in localized areas is insufficient. During shrimp and crab farming, the point-like concentrated loads generated by the shrimp's rostrum and the crab's claws far exceed the local bearing capacity of the membrane, easily forming hidden micro-perforations on the membrane surface. These types of damage points are highly concealed and difficult to inspect and repair, leading to continuous minor leaks in aquaculture ponds and significantly shortening the service life of materials. Under shrimp and crab farming conditions, the effective service life of HDPE geomembranes is only 2-3 years, requiring frequent complete renovation and replacement, resulting in high operation and maintenance costs. While PVC pond fabric has the advantages of flexibility, foldability, and high construction efficiency, the plasticizers such as DOP and DOTP added during the product manufacturing process have fat-soluble migration characteristics. Under long-term immersion in water, they will continue to leach and migrate, failing to meet the testing standards for high-end aquatic products exported. At the same time, the mechanical strength of this material matrix is ​​relatively low, and it has not been specifically reinforced for shrimp and crab biological puncture conditions. After the membrane is damaged, it will further accelerate the dissolution of plasticizers, posing a dual risk to water quality safety and the durability of the aquaculture system.

[0004] In summary, current mainstream aquaculture waterproofing materials have obvious performance limitations, making it difficult to simultaneously achieve the three core properties of flexible bonding, high puncture resistance, and low additive exudation. They also fail to address the industry pain points of rigid membranes being easily damaged and flexible membranes having insufficient safety, making it difficult to meet the standardized application requirements of large-scale, high-quality shrimp and crab farming. Summary of the Invention

[0005] The purpose of this application is to provide a composite membrane material that simultaneously achieves flexible adhesion, high puncture resistance, and low additive exudation, which is specifically achieved through the following technical solution:

[0006] A method for preparing a composite membrane material includes the following steps:

[0007] S1. Apply a base coat to both sides of a polyester fiber base fabric, and perform a pre-plasticization treatment after coating to obtain a modified polyester base fabric intermediate with an adhesive transition layer.

[0008] S2. Apply PVC functional paste to the surface of the tackifying transition layer, and then perform plasticizing treatment to form an intermediate substrate with a PVC anti-seepage functional layer.

[0009] By weight, the PVC functional paste raw material composition includes: 100 parts PVC paste resin, 40-55 parts dioctyl terephthalate, 20-35 parts trioctyl trimellitate, 4-8 parts heat stabilizer, 0.3 parts antioxidant, 2-6 parts ultraviolet stabilizer, 1.5-3 parts active zinc oxide, 0.5-2 parts nano silver antibacterial agent, 0.5-8 parts colorant, and 5-20 parts inorganic filler;

[0010] S3. A water-based acrylic emulsion is coated on the surface of the intermediate substrate, and after drying and curing, a protective surface layer is formed on the surface of the PVC anti-seepage functional layer. After cooling and shaping, a composite membrane material is obtained.

[0011] Preferably, the basis weight of the polyester fiber base fabric is 300~600 g / m². 2 Its longitudinal fracture strength is ≥3000N / 5cm, and its latitudinal fracture strength is ≥2600N / 5cm.

[0012] Preferably, in step S1, the primer contains isocyanate functional groups, and its single-sided coating weight is 5~15 g / m². 2 .

[0013] Preferably, in step S2, the single-sided coating amount of the PVC functional paste is 400~1000 g / m². 2 The thickness of any of the PVC waterproof functional layers is 0.4~0.8mm.

[0014] Preferably, in step S3, the single-sided coating amount of the waterborne acrylic emulsion is 10~30 g / m². 2 The thickness of any of the protective surfaces is 5~20μm.

[0015] Preferably, in step S1, the pre-plasticizing treatment conditions are: temperature 120~150℃, time 30~60s; in step S2, the plasticizing treatment conditions are: temperature 180~220℃, time 60~120s; in step S3, the drying and curing treatment conditions are: temperature 80~120℃, time 30~60s.

[0016] Preferably, the process also includes pretreatment of the polyester fiber base fabric before applying the primer to both sides of the polyester fiber base fabric. The pretreatment includes the following steps: heating the polyester fiber base fabric to 80-120°C using a preheating roller.

[0017] Preferably, the ultraviolet stabilizer is a compound of 2-hydroxy-4-n-octyloxybenzophenone and hindered amine light stabilizer (HALS) in a weight ratio of (1-3):(1-3); the colorant is a compound of titanium dioxide and carbon black in a weight ratio of (2-8):(0.5-2); and the nano-silver antibacterial agent is selected from silver oxide or zirconium phosphate silver-loaded particles with a particle size of 5-20 nm.

[0018] A composite membrane material is prepared using any one of the preparation methods described above.

[0019] The above-mentioned composite membrane material is used in aquaculture.

[0020] Compared with the prior art, this application has the following beneficial effects:

[0021] This application utilizes a seven-layer composite structure design consisting of a high-strength polyester fiber base fabric, a double-sided PVC impermeable functional layer, and a double-layer water-based acrylic barrier protective layer. Combined with a DOTP and TOTM medical-grade compound plasticizing system, it simultaneously achieves three core properties: flexible adhesion, high puncture resistance, and low additive exudation. Performance test results show that the material's permeability coefficient is ≤1.0×10⁻⁶. -13 cm / s, CBR burst strength ≥6.5KN, burst strength is more than twice that of conventional HDPE geomembrane and far exceeds the burst strength of ordinary PVC pool cloth which is less than 2KN. It is soft and flexible and does not have the problem of large amount of plasticizer leaching. It perfectly solves the industry pain point that traditional aquatic seepage prevention materials cannot simultaneously take into account flexibility, puncture resistance and low exudation.

[0022] This application utilizes a high molecular weight TOTM trimer bond structure combined with a low-migration DOTP plasticizer, along with a surface cross-linked dense acrylate barrier membrane to form a double barrier that prevents plasticizer migration and dissolution, significantly reducing the risk of plasticizer leaching during long-term immersion in aquaculture water. Performance test results show that the material exhibits an extremely low plasticizer weight loss and leaching rate after immersion in pure water at 25°C for 30 days, far superior to the leaching levels of plasticizer systems using only TOTM or DOTP. This dual approach, combining internal formulation and external surface structure, ensures the safety of aquaculture water quality and meets the testing standards for high-end aquatic products exported.

[0023] This application uses active zinc oxide combined with nano-silver to replace traditional migratable organic antibacterial and antifungal agents. It relies on the slow-release zinc and silver ions to inhibit the reproduction of algae and pathogenic bacteria in the water for a long time. At the same time, it is combined with UV-531 and hindered amine light stabilizer to construct a composite anti-ultraviolet system. Performance test results show that the strength retention rate of the material is ≥80% after 3000h of accelerated ultraviolet aging. The design service life of the material for open-air aquaculture can reach 5-8 years, which is far superior to the service life of conventional HDPE geomembrane for shrimp and crabs (2-3 years) and ordinary PVC pond cloth for open-air rapid powdering failure. Moreover, zinc oxide and nano-silver do not leach toxic organic additives, so there is no risk of water pollution.

[0024] This application utilizes a seven-layer composite structure design consisting of a high-strength polyester fiber base fabric, a double-sided PVC impermeable functional layer, and a double-layer water-based acrylic barrier protective surface layer. Combined with a DOTP and TOTM medical-grade compound plasticizing system, it simultaneously achieves both long-lasting impermeability and ultra-high puncture resistance. Performance test results show that this material has a permeability coefficient ≤1.0×10⁻¹³cm / s and a CBR puncture strength ≥6.5KN. Its puncture strength is more than twice that of conventional HDPE geomembranes and far exceeds the less than 2KN puncture strength of ordinary PVC pool fabric, perfectly solving the industry pain point where traditional aquaculture impermeable materials cannot simultaneously achieve both impermeability and puncture resistance. Attached Figure Description

[0025] The attached diagram will be briefly described below:

[0026] Figure 1 This is a schematic diagram of the overall membrane structure of the composite membrane material of this application. Detailed Implementation

[0027] The present application will now be further described by way of specific embodiments. Those skilled in the art will be able to implement the present application based on these descriptions. Furthermore, the embodiments of the present application described below are generally only a part of the embodiments of the present application, and not all of the embodiments. Therefore, all other embodiments obtained by those skilled in the art based on the embodiments of the present application without inventive effort should fall within the scope of protection of the present application.

[0028] Example 1

[0029] This embodiment discloses a method for preparing a composite membrane material specifically for aquaculture, which includes the following steps:

[0030] Raw material preparation: By weight, the PVC functional paste raw materials include 100 parts PVC paste resin, 48 parts medical-grade dioctyl terephthalate (DOTP), 28 parts medical-grade trioctyl trimellitate (TOTM), 6 parts calcium-zinc composite heat stabilizer, 0.3 parts antioxidant 1010, 2 parts UV-531 ultraviolet absorber, 2 parts HALS hindered amine light stabilizer, 2 parts active zinc oxide with a particle size of 0.1-5μm, 1 part zirconium phosphate silver-loaded nano-silver antibacterial agent with a particle size of 5-20nm, 5 parts titanium dioxide, 1 part food contact grade carbon black, and 12 parts calcium carbonate inorganic filler; a primer containing isocyanate functional groups and a self-crosslinking waterborne acrylic emulsion are selected; the base fabric is selected with a basis weight of 450g / m². 2 High-strength biaxial polyester warp-knitted fabric with a warp breaking strength ≥3000N / 5cm and a weft breaking strength ≥2600N / 5cm.

[0031] The first step is to perform a pretreatment process on the polyester fiber base fabric. A preheating roller is used to uniformly convey and heat the high-strength biaxially oriented polyester warp-knitted fabric at a controlled temperature of 100℃. The process principle is as follows: During the weaving process, spinning oil adheres to the polyester base fabric, and free moisture is adsorbed on the surface. This moisture and oil prevent the chemical bonding between the isocyanate groups of the undercoat and the hydroxyl groups of the polyester, significantly reducing interlayer adhesion strength. Heating within the range of 80–120℃ allows the moisture to vaporize and the low-molecular-weight oil to decompose and be removed. A clean fiber surface ensures stable anchoring of the subsequent undercoat, providing a reliable interface for the seven-layer composite structure, while also avoiding pinholes and bubbles that may occur during the subsequent coating plasticizing stage.

[0032] After completing the pretreatment of the base fabric, perform step S1, primer coating and preplasticization. Apply a primer containing isocyanate functional groups evenly to both sides of the clean polyester base fabric, with a coating amount of 10 g / m² on each side. 2 The material is then placed in a pre-plasticizing oven and kept at a constant temperature of 135℃ for 45 seconds to obtain a modified polyester base fabric intermediate with a double-sided tackifying transition layer. Process principle: The -NCO groups in the primer adhesive can undergo an addition reaction with the hydroxyl groups on the surface of the polyester fiber to form urethane covalent bonds, achieving permanent anchoring between the adhesive layer and the base fabric. At a pre-plasticizing temperature of 120–150℃, unreacted isocyanate groups undergo dimerization and trimerization crosslinking to form a dense, high-strength tackifying transition layer. This transition layer can build a stress transfer bridge between the polyester base fabric and the subsequent PVC coating, preventing the PVC coating from delaminating from the base fabric during high-temperature plasticizing. (5–15 g / m²) 2 The coating amount ensures both bonding strength and prevents the film from hardening or losing flexibility due to excessive adhesive layer thickness, making it suitable for the construction needs of aquaculture slope bonding.

[0033] Next, the PVC functional paste is prepared, double-sided coated, and plasticized in step S2. First, PVC paste resin, DOTP, TOTM, calcium-zinc stabilizer, calcium carbonate, titanium dioxide, and food-grade carbon black are added to a mixing tank and stirred at low speed for 20 minutes. Then, the zirconium phosphate silver-loaded nano-silver antibacterial agent is pre-mixed with a small amount of DOTP and added to the tank. After the material temperature in the tank cools to below 55℃, UV-531, HALS, antioxidant 1010, and active zinc oxide are added, and stirring at low speed continues for 10 minutes. After stirring, vacuum degassing is performed for 15 minutes. Finally, the PVC paste is evenly coated on both sides of the modified polyester base fabric intermediate using a scraper, with a single-sided coating amount of 700 g / m². 2 The material is then placed in a plasticizing box and kept at a constant temperature of 200℃ for 90 seconds to complete the plasticizing process. After molding, the thickness of the single-layer PVC anti-seepage functional layer is 0.5mm, resulting in an intermediate substrate coated with a double-sided anti-seepage coating.

[0034] Finally, step S3, surface coating, drying, curing, and cooling / setting, is performed. A water-based acrylic emulsion is roller-coated onto the PVC impermeable layers on both sides of the intermediate substrate, with a single-sided coating amount of 12 g / m². 2 The material is placed in an oven and dried at a constant temperature of 95℃ for 45 seconds. After curing, the dry film thickness is 10μm. It is then cooled to room temperature by a cooling roller to set, ultimately producing a food-grade PVC-coated geomembrane material for aquaculture. In the initial drying stage, the water in the emulsion evaporates due to heat, and the acrylate particles fuse together to form a continuous wet film. Heating at 80-120℃ promotes the self-crosslinking reaction of acrylate molecules, generating a dense three-dimensional network barrier protective surface layer on the outer surface of the PVC coating. This surface layer relies on the steric hindrance effect of molecular chains to prevent DOTP and TOTM from migrating to the membrane surface, while simultaneously isolating the aquaculture water from direct contact with the PVC matrix. This creates a dual anti-migration structure of low-migration plasticizers internally and physical barrier on the outer surface, significantly reducing the risk of leaching of plasticizers and functional additives.

[0035] Example 2

[0036] This embodiment discloses a method for preparing a composite membrane material, which specifically includes the following steps:

[0037] Raw material preparation: By weight, the PVC functional paste raw materials include 100 parts PVC paste resin, 50 parts medical-grade dioctyl terephthalate (DOTP), 30 parts medical-grade trioctyl trimellitate (TOTM), 7 parts calcium-zinc composite heat stabilizer, 0.3 parts antioxidant 1010, 2.5 parts UV-531 ultraviolet absorber, 2.5 parts HALS hindered amine light stabilizer, 2.5 parts active zinc oxide with a particle size of 0.1-5μm, 1.2 parts zirconium phosphate silver-loaded nano-silver antibacterial agent with a particle size of 5-20nm, 4 parts titanium dioxide, 1.2 parts food contact grade carbon black, and 15 parts calcium carbonate inorganic filler; a primer containing isocyanate functional groups and a self-crosslinking waterborne acrylic emulsion are selected; the base fabric is selected with a basis weight of 550g / m². 2 High-strength biaxial polyester warp-knitted fabric with a warp breaking strength ≥3000N / 5cm and a weft breaking strength ≥2600N / 5cm.

[0038] First, a pretreatment process for the polyester fiber base fabric is carried out. A preheating roller is used to uniformly convey and heat the high-strength biaxially oriented polyester warp-knitted fabric at a controlled temperature of 110℃. Process principle: During the weaving process of the polyester base fabric, spinning oil adheres to the surface and adsorbs free moisture. Moisture and oil can block the chemical bonding between the isocyanate groups of the undercoat and the hydroxyl groups of the polyester, significantly reducing interlayer bonding strength. Heating within the range of 80-120℃ allows the moisture to vaporize and the low-molecular-weight oil to decompose and be removed. A clean fiber surface ensures stable anchoring of the subsequent undercoat, providing a reliable interface foundation for the seven-layer composite structure. Simultaneously, it avoids pinholes and bubbles that may occur during the subsequent coating plasticizing stage. 550g / m 2 The high-grammage base fabric is specially designed for use in situations where the strong claws of mitten crabs are pierced.

[0039] After completing the pretreatment of the base fabric, perform step S1, primer coating and preplasticization. Apply a primer containing isocyanate functional groups evenly to both sides of the clean polyester base fabric, with a coating amount of 12 g / m² on each side. 2 The material is then placed in a pre-plasticizing oven and kept at a constant temperature of 140℃ for 50 seconds to obtain a modified polyester base fabric intermediate with a double-sided tackifying transition layer. Process principle: The -NCO groups in the primer adhesive can undergo an addition reaction with the hydroxyl groups on the surface of the polyester fiber to form urethane covalent bonds, achieving permanent anchoring between the adhesive layer and the base fabric. At a pre-plasticizing temperature of 120–150℃, unreacted isocyanate groups undergo dimerization and trimerization crosslinking to form a dense, high-strength tackifying transition layer. This transition layer can build a stress transfer bridge between the polyester base fabric and the subsequent PVC coating, preventing the PVC coating from delaminating from the base fabric during high-temperature plasticizing. (5–15 g / m²) 2 The coating amount ensures bonding strength without causing the film to harden or lose flexibility due to excessive adhesive layer thickness, making it suitable for the bonding construction needs of crab pond slopes and irregular soil bases.

[0040] Next, the PVC functional paste is prepared, double-sided coated, and plasticized in step S2. First, PVC paste resin, DOTP, TOTM, calcium-zinc stabilizer, calcium carbonate, titanium dioxide, and food-grade carbon black are added to a mixing tank and stirred at low speed for 20 minutes. Then, the zirconium phosphate silver-loaded nano-silver antibacterial agent is premixed with a small amount of DOTP and added to the tank. After the material temperature in the tank cools to below 55℃, UV-531, HALS, antioxidant 1010, and active zinc oxide are added, and stirring at low speed continues for 10 minutes. After stirring, vacuum degassing is performed for 15 minutes. Finally, the PVC paste is evenly coated on both sides of the modified polyester base fabric intermediate using a scraper, with a single-sided coating amount of 850 g / m². 2 The material is then placed in a plasticizing box and kept at a constant temperature of 210℃ for 100 seconds to complete the plasticizing process. After molding, the thickness of the single-layer PVC anti-seepage functional layer is 0.6mm, resulting in an intermediate substrate covered with a double-sided anti-seepage coating.

[0041] Finally, step S3, surface coating, drying, curing, and cooling / setting, is performed. A water-based acrylic emulsion is roller-coated onto the PVC impermeable layers on both sides of the intermediate substrate, with a single-sided coating amount of 15 g / m². 2 The material is placed in an oven and dried at a constant temperature of 100℃ for 50 seconds. After curing, the dry film thickness is 12μm. It is then cooled to room temperature by a cooling roller to set, finally producing a food-grade PVC-coated impermeable composite membrane material for crab farming. Process principle: In the initial drying stage, the water in the emulsion evaporates due to heat, and the acrylate particles fuse together to form a continuous wet film. Heating at 80-120℃ promotes the self-crosslinking reaction of acrylate molecules, generating a dense three-dimensional network barrier protective surface layer on the outer surface of the PVC coating. This surface layer relies on the steric hindrance effect of molecular chains to prevent the migration of DOTP and TOTM to the membrane surface, while simultaneously isolating the aquaculture water from direct contact with the PVC matrix. This constructs a dual anti-migration structure of low-migration plasticizers internally and physical barrier on the outer surface, significantly reducing the risk of plasticizer and functional additive leaching.

[0042] Example 3

[0043] This embodiment discloses a method for preparing a composite membrane material, which specifically includes the following steps:

[0044] Raw material preparation: By weight, the PVC functional paste raw materials include 100 parts PVC paste resin, 45 parts medical-grade dioctyl terephthalate (DOTP), 25 parts medical-grade trioctyl trimellitate (TOTM), 5 parts calcium-zinc composite heat stabilizer, 0.3 parts antioxidant 1010, 1 part UV-531 ultraviolet absorber, 1 part HALS hindered amine light stabilizer, 1.5 parts active zinc oxide with a particle size of 0.1-5μm, 0.8 parts zirconium phosphate silver-loaded nano-silver antibacterial agent with a particle size of 5-20nm, 6 parts titanium dioxide, 0 parts food contact grade carbon black, and 10 parts calcium carbonate inorganic filler; a primer containing isocyanate functional groups and a self-crosslinking waterborne acrylic emulsion are selected; the base fabric is selected with a basis weight of 300g / m². 2 High-strength biaxial polyester warp-knitted fabric with a warp breaking strength ≥3000N / 5cm and a weft breaking strength ≥2600N / 5cm.

[0045] The first step involves a pretreatment process for the polyester fiber base fabric. A preheating roller is used to uniformly convey and heat the high-strength biaxially oriented polyester warp-knitted fabric at a controlled temperature of 85℃. The process principle is as follows: During the weaving process, spinning oil adheres to the polyester base fabric, and free moisture is adsorbed on the surface. This moisture and oil hinder the chemical bonding between the isocyanate groups of the undercoat and the hydroxyl groups of the polyester, significantly reducing interlayer adhesion strength. Heating within the 80–120℃ range allows the moisture to vaporize and the low-molecular-weight oil to decompose and be removed. A clean fiber surface ensures stable anchoring of the subsequent undercoat, providing a reliable interface foundation for the seven-layer composite structure. The process is carried out indoors without strong sunlight exposure and with a low risk of mechanical puncture. A 300g / m² fiber is selected. 2 Lightweight base fabric reduces raw material costs.

[0046] After completing the pretreatment of the base fabric, perform step S1, primer coating and preplasticization. Apply a primer containing isocyanate functional groups evenly to both sides of the clean polyester base fabric, with a coating amount of 5 g / m² on each side. 2 The material is then placed in a pre-plasticizing oven and kept at a constant temperature of 120℃ for 30 seconds to obtain a modified polyester base fabric intermediate with a double-sided adhesive transition layer. Process principle: The -NCO groups in the primer can undergo an addition reaction with the hydroxyl groups on the surface of the polyester fiber to form urethane covalent bonds, achieving permanent anchoring between the primer layer and the base fabric. At a pre-plasticizing temperature of 120–150℃, unreacted isocyanate groups undergo dimerization and trimerization crosslinking to form a dense, high-strength adhesive transition layer. This transition layer can build a stress transfer bridge between the polyester base fabric and the subsequent PVC coating, preventing the PVC coating from delaminating from the base fabric during high-temperature plasticizing. The low coating amount of primer controls the overall thickness of the film, meeting the lightweight requirements of indoor circulating water tanks.

[0047] Next, the PVC functional paste is prepared, double-sided coated, and plasticized in step S2. First, PVC paste resin, DOTP, TOTM, calcium-zinc stabilizer, calcium carbonate, and titanium dioxide are added to a mixing tank and stirred at low speed for 20 minutes. Then, the zirconium phosphate silver-loaded nano-silver antibacterial agent is pre-mixed with a small amount of DOTP and added to the tank. After the material temperature in the tank cools to below 55℃, UV-531, HALS, antioxidant 1010, and active zinc oxide are added, and stirring at low speed continues for 10 minutes. After stirring, vacuum degassing is performed for 15 minutes. Finally, the PVC paste is evenly coated on both sides of the modified polyester base fabric intermediate using a scraper, with a single-sided coating amount of 400 g / m². 2 The material is then placed in a plasticizing box and kept at a constant temperature of 180℃ for 60 seconds to complete the plasticizing process. After molding, the thickness of the single-layer PVC anti-seepage functional layer is 0.4mm, resulting in an intermediate substrate covered with a double-sided anti-seepage coating.

[0048] Finally, step S3, surface coating, drying, curing, and cooling, is performed. A water-based acrylic emulsion is roller-coated onto the PVC impermeable layers on both sides of the intermediate substrate, with a single-sided coating amount of 8 g / m². 2 The membrane is dried and cured at a constant temperature of 80℃ for 30 seconds in an oven, resulting in a dry film thickness of 8μm. It is then cooled to room temperature using cooling rollers to set its shape, ultimately producing a lightweight, food-grade PVC-coated geomembrane material specifically for factory-scale recirculating aquaculture systems (RAS). Process principle: During the initial drying stage, water in the emulsion evaporates upon heating, and acrylate particles fuse to form a continuous wet film. Heating at 80–120℃ induces a self-crosslinking reaction of acrylate molecules, generating a dense, three-dimensional network barrier protective layer on the outer surface of the PVC coating. This layer, relying on the steric hindrance effect of molecular chains, prevents the migration of DOTP and TOTM to the membrane surface, while simultaneously isolating the aquaculture water from direct contact with the PVC matrix. This creates a dual anti-migration structure of low-migration plasticizers internally and physical barrier on the outer surface, perfectly meeting the stringent requirements of RAS recirculating water systems for zero water leaching. Low-temperature, short-time curing saves energy, and cooling and setting eliminates internal stress, preventing warping and wrinkling issues during indoor installation.

[0049] Comparative Example 1

[0050] This comparative example uses commercially available conventional HDPE geomembrane specifically for aquaculture (compliant with GB / T 17643-2011 "Geosynthetic Materials - Polyethylene Geomembrane" standard, 1.0 mm thick, double-sided smooth structure, density 0.940~0.960 g / cm³). 3 It has a tensile yield strength of 25~30MPa, an elongation at break of 700%~900%, and contains 2%~3% carbon black masterbatch. It does not have a polyester fiber reinforced base fabric, PVC anti-seepage coating, or acrylate barrier surface layer. It does not have a compounded low-exudation plasticizing system or inorganic anti-mildew components. It is a single high-density polyethylene blow-molded / calendered film.

[0051] Comparative Example 2

[0052] This comparative example uses commercially available conventional PVC pond cloth for aquaculture as the control sample (thickness 0.5mm, PVC calendered soft film, containing DOP dioctyl phthalate plasticizer, Shore hardness A80+ / -5, tensile strength 15~20MPa, elongation at break 250%~350%, without UV stabilizer and inorganic antibacterial components).

[0053] Comparative Example 3

[0054] The preparation process, other raw material components, and process parameters of this comparative composite film material are completely consistent with those of Example 1. The only difference is that dioctyl terephthalate (DOTP) is not added when preparing the PVC functional paste, and only trioctyl trimellitate (TOTM) is used as a single plasticizer.

[0055] Comparative Example 4

[0056] The preparation process, other raw material components, and process parameters of this comparative composite film material are completely consistent with those of Example 1. The only difference is that trioctyl trimellitate (TOTM) is not added when preparing the PVC functional paste, and only dioctyl terephthalate (DOTP) is used as a single plasticizer.

[0057] Performance testing

[0058] This performance test included five sets of samples: Example 1, Comparative Example 1 (commercially available HDPE geomembrane), Comparative Example 2 (commercially available conventional PVC pool fabric), Comparative Example 3 (TOTM single plasticized composite membrane only), and Comparative Example 4 (DOTP single plasticized composite membrane). All samples were cut into standard pieces of uniform size and placed in a constant temperature and humidity environment of 23℃ and 50% for 24 hours to complete the pretreatment, eliminate internal stress of the material, and balance the temperature and humidity of the samples. Subsequently, all performance tests were carried out in sequence. This test adopted the national standard standardized testing methods. The testing specifications and test conditions for each item are as follows: the plasticizer water precipitation test adopts the GB / T17688 standard "Geosynthetic Materials Polyvinyl Chloride (PVC) Geomembrane"; the CBR puncture strength is performed according to the GB / T 14800-2010 standard "Geosynthetic Materials Static Puncture Test (CBR Method)"; the permeability coefficient is determined according to GB / T19979.2-2006 "Geosynthetic Materials Impermeable Geomembrane"; the ultraviolet weathering performance is carried out by a 3000h accelerated aging test in a QUV ultraviolet aging chamber, and the tensile strength after aging is tested according to GB / T 1040.1-2025 "Determination of Tensile Properties of Plastics Part 1: General Rules", and the strength retention rate after aging is calculated; the weld strength, flexible bending, and hot air welding compatibility are simultaneously verified using the industry-standard PVC coated fabric testing methods.

[0059] Table 1 Performance Test Results

[0060] Performance indicators Example 1 Comparative Example 1 Comparative Example 2 Comparative Example 3 Comparative Example 4 Plasticizer water extraction rate <0.15% Plasticizer-free 0.85% 0.25% 0.42% Bursting strength (CBR) ≥6.5KN ≥3KN ≥2KN ≥5.5KN ≥6.0KN Permeability coefficient <![CDATA[≤1.0×10 -13 cm / s]]> <![CDATA[≤1.0×10 -13 cm / s]]> <![CDATA[about 10 -12 cm / s]]> <![CDATA[≤1.0×10 -13 cm / s]]> <![CDATA[≤1.0×10 -13 cm / s]]> UV resistance (QUV3000h) Strength retention rate ≥80% Strength retention rate ≥80% (with carbon black added) No UV stabilizer, rapid powdering Strength retention rate ≥80% Strength retention rate ≥80% Flexibility / fit Excellent (bendable and fits well) Poor quality (high rigidity, prone to wrinkling) Excellent (bendable and fits well) Good (can be bent and fits well) Excellent (bendable and fits well) Seam sealing method Hot air welding Double-track hot melt welding Adhesive / High Frequency Welding Hot air welding Hot air welding Difficulty of joint construction Low (handheld welding torch is sufficient) High (requires a professional welding machine) Low but poor durability Low (handheld welding torch is sufficient) Low (handheld welding torch is sufficient) Anti-algae and antibacterial Zinc oxide (non-toxic and non-migrating) + nano silver none MIT / CMIT (Toxic and Migratory) Zinc oxide (non-toxic and non-migrating) + nano silver Zinc oxide (non-toxic and non-migrating) + nano silver

[0061] As can be seen from the table above, the composite membrane of Example 1 of this application is superior to the commercially available HDPE geomembrane of Comparative Example 1 and the ordinary PVC pool fabric of Comparative Example 2 in all five dimensions: burst strength, UV resistance, plasticizer leaching control, ease of construction, and biosafety. Comparing Comparative Examples 3 and 4 with single plasticizing systems, it is evident that the DOTP and TOTM compound plasticizing scheme combined with a water-based acrylic barrier layer can significantly reduce the plasticizer leaching rate, proving that the synergistic structure of compound plasticizing and double-layer barrier is the core key to achieving low leaching safety performance for aquaculture. While HDPE membranes meet the basic parameters of impermeability and weather resistance, they are rigid, lack puncture resistance, and have high construction thresholds. Ordinary PVC pool cloths, although flexible, lack a UV stabilization system and inorganic antibacterial formula, are prone to aging in the open air, and their organic additives pose a risk of water pollution. The seven-layer composite structure synergistic formula system of this application solves all the shortcomings of the two existing mainstream impermeable materials at the same time, taking into account the advantages of high puncture resistance, long-term weather resistance, low additive precipitation, and simple hot air welding construction. It is fully suitable for the long-term open-air immersion conditions of shrimp, crab, fish, and all types of aquaculture in factory-style recirculating water systems. Comparing the data of Comparative Example 3 (single TOTM plasticizer) and Comparative Example 4 (single DOTP plasticizer), it can be seen that the compound plasticizer system exhibits a significant synergistic advantage in terms of plasticizer water leaching rate: the leaching rate of the single TOTM system in Comparative Example 3 is 0.25%, and the leaching rate of the single DOTP system in Comparative Example 4 reaches 0.42%, both significantly higher than the leaching level of less than 0.15% in the compound system of Example 1. This proves that the dual barrier structure of DOTP and TOTM compounded with the water-based acrylate barrier surface is the core key to reducing plasticizer migration and leaching and ensuring the safety of aquaculture water quality.

Claims

1. A method for preparing a composite membrane material, characterized in that, Includes the following steps: S1. Apply a base coat to both sides of a polyester fiber base fabric, and perform a pre-plasticization treatment after coating to obtain a modified polyester base fabric intermediate with an adhesive transition layer. S2. Apply PVC functional paste to the surface of the tackifying transition layer, and then perform plasticizing treatment to form an intermediate substrate with a PVC anti-seepage functional layer. By weight, the PVC functional paste raw material composition includes: 100 parts PVC paste resin, 40-55 parts dioctyl terephthalate, 20-35 parts trioctyl trimellitate, 4-8 parts heat stabilizer, 0.3 parts antioxidant, 2-6 parts ultraviolet stabilizer, 1.5-3 parts active zinc oxide, 0.5-2 parts nano silver antibacterial agent, 0.5-8 parts colorant, and 5-20 parts inorganic filler; S3. A water-based acrylic emulsion is coated on the surface of the intermediate substrate, and after drying and curing, a protective surface layer is formed on the surface of the PVC anti-seepage functional layer. After cooling and shaping, a composite membrane material is obtained.

2. The method for preparing a composite membrane material according to claim 1, characterized in that, The basis weight of the polyester fiber base fabric is 300~600 g / m². 2 Its longitudinal fracture strength is ≥3000N / 5cm, and its latitudinal fracture strength is ≥2600N / 5cm.

3. The method for preparing a composite membrane material according to claim 1, characterized in that, In step S1, the primer contains isocyanate functional groups, and its single-sided coating weight is 5~15 g / m². 2 .

4. The method for preparing a composite membrane material according to claim 1, characterized in that, In step S2, the single-sided coating amount of the PVC functional paste is 400~1000g / m². 2 The thickness of any of the PVC waterproof functional layers is 0.4~0.8mm.

5. The method for preparing a composite membrane material according to claim 1, characterized in that, In step S3, the single-sided coating amount of the waterborne acrylic emulsion is 10~30 g / m². 2 The thickness of any of the protective surfaces is 5~20μm.

6. The method for preparing a composite membrane material according to claim 1, characterized in that, In step S1, the pre-plasticizing treatment conditions are: temperature 120~150℃, time 30~60s; in step S2, the plasticizing treatment conditions are: temperature 180~220℃, time 60~120s; in step S3, the drying and curing treatment conditions are: temperature 80~120℃, time 30~60s.

7. The method for preparing a composite membrane material according to claim 1, characterized in that, It also includes pretreatment of the polyester fiber base fabric before applying the primer to both sides of the polyester fiber base fabric. The pretreatment includes the following steps: heating the polyester fiber base fabric to 80-120℃ using a preheating roller.

8. The method for preparing a composite membrane material according to claim 1, characterized in that, The ultraviolet stabilizer is a compound of 2-hydroxy-4-n-octyloxybenzophenone and hindered amine light stabilizer (HALS) in a weight ratio of (1-3):(1-3); the colorant is a compound of titanium dioxide and carbon black in a weight ratio of (2-8):(0.5-2); the nano-silver antibacterial agent is selected from silver oxide or zirconium phosphate silver-loaded particles with a particle size of 5-20 nm.

9. A composite membrane material, characterized in that, It is prepared by the preparation method described in any one of claims 1 to 8.

10. The application of the composite membrane material according to claim 9 in aquaculture.