A method and structure for low-temperature spray insulation of rural house walls in cold regions
By forming an interface treatment layer on the surface of the walls of farmhouses in cold regions and preheating and layering the spraying material, the problems of insufficient foaming and continuous forming stability of the sprayed insulation main layer under low-temperature construction conditions in cold regions are solved, the uniformity and thickness control of the sprayed layer are achieved, and the bonding stability is improved.
Patent Information
- Application Number
- CN202611516778.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-28
- Publication Date
- 2026-11-17
AI Technical Summary
Under low-temperature construction conditions in cold regions, the state of the sprayed material is affected by the ambient temperature and the surface condition of the base wall, resulting in insufficient foaming and continuous forming stability of the sprayed insulation main layer, and problems such as uneven foaming, local collapse of bubbles, large pores or voids.
An interface treatment layer is formed on the surface of the base wall, and components A and B are preheated. The components are transported and mixed through heated delivery pipelines and heated mixing nozzles. A layered spraying method is adopted, with adjacent sprays using intersecting gun directions. Thickness is measured during construction to form a continuous sprayed insulation main layer.
In a low-temperature environment of 6–15℃, the sprayed insulation base layer is continuously formed, which solves the problems of insufficient foaming and continuous forming stability of the sprayed insulation base layer, improves the bonding stability between the interface treatment layer and the sprayed insulation base layer, and ensures the uniformity and thickness control of the sprayed layer.
Smart Images

Figure CN123109428A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of building energy-saving insulation technology, specifically to a low-temperature spray insulation construction method and structure for rural houses in cold regions. Background Technology
[0002] In cold regions, rural houses typically have walls made of solid red bricks, aerated concrete blocks, concrete, or adobe. Some existing rural houses also retain a layer of lime plaster or other old finishes on the exterior walls. To reduce heat loss through the walls, current technologies usually employ adhesive-bonded insulation boards or on-site spraying of rigid polyurethane foam to form the external wall insulation layer. Among these, sprayed rigid polyurethane foam is mixed and foamed on-site to directly form a continuous insulation layer, reducing the number of seams between boards and making it suitable for construction areas with varying wall surface shapes.
[0003] However, under the low-temperature construction conditions of rural houses in cold regions, the two-component spraying material is easily affected by the ambient temperature, and its conveying state, mixing state and foaming and curing process are prone to change. At the same time, the surface water absorption rate, porosity and residual finish of different rural house base walls vary. If the conventional base treatment is used to directly spray the material, problems such as uneven foaming of the sprayed layer, local collapse of bubbles, large pores or voids and fluctuations in the thickness of the sprayed layer are likely to occur, which will affect the continuous formation of the sprayed insulation main layer. Summary of the Invention
[0004] The purpose of this invention is to provide a method and structure for low-temperature spray insulation construction of rural houses in cold regions, in order to solve the problem that the state of the sprayed material is affected by the ambient temperature and the surface condition of the base wall under low-temperature construction conditions in rural houses in cold regions, resulting in insufficient foaming and continuous forming stability of the main layer of spray insulation.
[0005] To achieve the above objectives, the present invention provides the following technical solution:
[0006] A method for low-temperature spray insulation of rural house walls in cold regions includes the following steps:
[0007] S1. Base treatment: Clean the surface of the base wall, removing dust, oil stains and loose layers; repair cracks and holes in the base wall; and test the moisture content and flatness of the base wall.
[0008] S2. Interface treatment: A special interface treatment agent containing silane coupling agent and nano silica dispersion is applied to the surface of the base wall after the base treatment, and the special interface treatment agent forms an interface treatment layer on the surface of the base wall. After the interface treatment layer reaches the touch dry state, subsequent spraying is carried out.
[0009] S3. Preheating of the spraying material: Component A and Component B of the two-component modified polyurethane rigid foam material are respectively fed into the spraying equipment for preheating. Component A includes a combination of polyether polyol, silane coupling agent modified nano-silica, a low-temperature catalyst system, a physical foaming agent, and an interfacial tackifier. Component B is modified MDI. The conveying pipelines of Component A and Component B are heated, and the mixing nozzle is also heated, so that Component A and Component B are conveyed to the mixing nozzle through the conveying pipelines and mixed. The mixture is then continuously sprayed onto the surface of the base wall to form the main sprayed insulation layer.
[0010] S4. Layered spraying: The A and B components, after being mixed by the mixing gun head, are sprayed onto the surface of the interface treatment layer to form the first spraying layer. After the first spraying layer reaches a non-sticky state, spraying continues to form the subsequent spraying layer. Adjacent spraying layers adopt mutually perpendicular gun directions. Multiple spraying layers are continuously combined to form the sprayed insulation main layer.
[0011] S5. Surface finishing: After the sprayed insulation base layer has cured, the protruding areas on the surface of the sprayed insulation base layer are cut and leveled.
[0012] S6. Construction of the reinforced protective layer: Apply the first layer of polymer-modified crack-resistant mortar to the surface of the sprayed insulation main layer after surface repair, press the alkali-resistant glass fiber mesh into the first layer of polymer-modified crack-resistant mortar, and continue to apply polymer-modified crack-resistant mortar to form a reinforced protective layer.
[0013] S7. Construction of decorative protective layer: After the reinforcement protective layer has been cured, the decorative protective layer shall be constructed on the outer surface of the reinforcement protective layer.
[0014] Further, the special interface treatment agent comprises the following components in parts by weight: 40-50 parts of acrylate emulsion, 3-6 parts of γ-aminopropyltriethoxysilane, 10-15 parts of nano-silica dispersion, 0.3-0.5 parts of defoamer, 2-4 parts of film-forming aid, and 30-40 parts of water; the coating amount of the special interface treatment agent on the substrate wall surface is 150-200 g / m². 2 .
[0015] Further, component A, by weight, comprises 100 parts of a combined polyether polyol, 3-8 parts of silane coupling agent modified nano-silica, 25-40 parts of halogen-free composite flame retardant, 2-4 parts of a foaming agent, 1.5-3.0 parts of a low-temperature catalyst system, 12-20 parts of HFO-type physical foaming agent, 1.0-2.5 parts of water, 0.5-2.0 parts of a nano-toughening modifier, and 2-5 parts of an interfacial tackifier; component B is modified MDI with an isocyanate index of 105-115.
[0016] Furthermore, the combined polyether polyol is formed by compounding polyester polyol and polyether polyol in a mass ratio of 3:7 to 4:6; the low-temperature catalyst system includes an organotin catalyst and a tertiary amine catalyst; the nano-toughening modifier includes organically modified nano-montmorillonite and carbon nanotubes; and the interface thickener is acrylate-modified organosilicon.
[0017] Furthermore, in step S3, component A is preheated to 30-40°C, component B is preheated to 25-35°C, the heating temperature of the heated delivery pipeline is 30-50°C, and the temperature of the mixing nozzle is maintained at 40-50°C.
[0018] Furthermore, in step S4, the spray distance between the mixing gun head and the base wall is 400-600mm, and the gun travel speed is 0.3-0.5m / s; the thickness of the first spray layer formed by the first spray is 30-40mm, the thickness of the spray layer formed by each subsequent spray is 30-50mm, the interval between two adjacent sprays is 5-15min, the number of sprays is 2-3, and the gun travel direction of two adjacent sprays intersects each other.
[0019] Furthermore, in step S1, the moisture content of the base wall is controlled below 10%, and the flatness deviation of the base wall is controlled within 10mm / 2m; in step S5, the flatness deviation of the sprayed insulation main layer is controlled within 5mm / 2m; in step S6, the total thickness of the reinforced protective layer is 3-5mm, and the overlap width between adjacent alkali-resistant glass fiber mesh is not less than 100mm.
[0020] The present invention also provides a low-temperature spray insulation structure for the walls of rural houses in cold regions, comprising, from the inside out, a base wall, an interface treatment layer, a spray insulation main layer, a reinforcing protective layer, and a decorative protective layer.
[0021] The interface treatment layer is disposed on the outer surface of the base wall; the sprayed insulation main layer is disposed on the outer surface of the interface treatment layer and is formed by multiple sprayings of two-component modified polyurethane rigid foam material; the reinforced protective layer is disposed on the outer surface of the sprayed insulation main layer and includes polymer-modified crack-resistant mortar and alkali-resistant glass fiber mesh embedded in the polymer-modified crack-resistant mortar; the decorative protective layer is disposed on the outer surface of the reinforced protective layer.
[0022] Furthermore, the thickness of the interface treatment layer is 0.5–1.0 mm, the thickness of the sprayed insulation main layer is 80–120 mm, the thickness of the reinforcing protective layer is 3–5 mm, and the thickness of the decorative protective layer is 0.3–0.5 mm.
[0023] Furthermore, at the door and window openings of the base wall, the sprayed insulation main layer extends continuously from the main surface of the base wall to the side of the door and window opening; a pre-pressed sealing strip is installed between the window frame and the sprayed insulation main layer, and a sealing layer is installed on the outside of the pre-pressed sealing strip.
[0024] Furthermore, at the corner of the base wall, the sprayed insulation main layer is locally thickened compared to the sprayed insulation main layer on the main surface of the base wall, and a double layer of alkali-resistant glass fiber mesh is set inside the reinforced protective layer, the alkali-resistant glass fiber mesh being continuously set across the corner.
[0025] Furthermore, at the plinth of the base wall, the sprayed insulation main layer extends below the outdoor ground level, a waterproof layer is installed on the outside of the sprayed insulation main layer, a waterproof mortar protective layer is installed on the outside of the waterproof layer, and corner guards are installed in some areas.
[0026] Furthermore, at the eaves of the base wall, the sprayed insulation main layer extends upward and overlaps with the roof insulation layer, and the overlap between the sprayed insulation main layer and the roof insulation layer is filled with polyurethane foam material.
[0027] This invention provides a method and structure for low-temperature spray insulation construction of rural houses in cold regions. It has the following beneficial effects:
[0028] First, this invention forms an interface treatment layer on the surface of the base wall and preheats components A and B separately. The components are then transported and mixed via heated delivery pipelines and heated mixing nozzles. Simultaneously, the previous spray layer reaches a non-sticky state to the touch as a condition for subsequent spraying, and adjacent sprays are applied in intersecting gun directions. This seamlessly integrates base wall condition control, interface treatment, material temperature control, and layered spraying processes. In the 6–15℃ construction environment of this embodiment, no significant bubbles, large holes, or voids were observed in the test sprayed material or the final sprayed material. The three-coat thermal insulation main layer forms a continuous structure, solving the problems of insufficient foaming and continuous forming stability of the thermal insulation main layer under low-temperature construction conditions in cold-region rural housing.
[0029] Secondly, the interface treatment layer is located between the base wall and the sprayed insulation main layer. The acrylic emulsion, γ-aminopropyltriethoxysilane, and nano-silica dispersion in the special interface treatment agent, together with the interface tackifier in the sprayed material, form an interlayer bond. In the example, the minimum tensile bond strength of the sprayed insulation main layer is 0.15 MPa, the average tensile bond strength is 0.172 MPa, and the main failure location after testing is located inside the sprayed insulation main layer. The silane coupling component in the interface treatment layer and the interface tackifier in the sprayed insulation main layer act on the base wall side and the sprayed material side, respectively, improving the bonding stability between the interface treatment layer and the sprayed insulation main layer.
[0030] Third, the main insulation layer is formed by spraying 2-3 layers, with adjacent layers using intersecting spray gun directions. Thickness monitoring is used during construction to control the process and ensure continuous bonding of the multiple layers. In this example, the final core drilling test showed an average thickness of 100.6 mm and a minimum thickness of 97 mm.
[0031] Fourth, an interface treatment layer, a sprayed insulation main layer, a reinforced protective layer, and a decorative protective layer are sequentially installed on the outside of the base wall. The reinforced protective layer is composed of polymer-modified crack-resistant mortar and alkali-resistant glass fiber mesh, thus forming a continuous protective structure on the outside of the sprayed insulation main layer.
[0032] Fifth, the main insulation layer is continuously extended to the sides of the door and window openings, locally thickened at the corners, extended below the outdoor ground at the plinth, and overlapped with the roof insulation layer at the eaves, so that the main wall surface and the door and window openings, corners, plinth and eaves form a continuous insulation structure.
[0033] Sixth, in the embodiment, after a 100mm thick sprayed insulation layer was applied to the 370mm solid red brick base wall, the on-site test showed that the wall's heat transfer coefficient was 0.22W / (m²). 2 K), below 0.25 W / (m 2 ·K) design control value. Attached Figure Description
[0034] Figure 1 This is a process flow diagram of the low-temperature spray insulation construction method for rural houses in cold regions according to the present invention;
[0035] Figure 2 This is a cross-sectional view of the multi-layer composite structure of the wall spray insulation layer of the present invention;
[0036] Figure 3 This is a schematic diagram of the low-temperature spraying material conveying and temperature control of the present invention;
[0037] Figure 4 This is a cross-sectional view of the wall insulation structure in Embodiment 3 of the present invention;
[0038] Figure 5 This is a detailed structural diagram of the key thermal bridge node of the present invention, wherein, Figure 5 (a) shows the construction diagram of the door and window opening nodes. Figure 5 (b) is the construction diagram of the corner node. Figure 5 (c) is the construction diagram of the foot joint. Figure 5 (d) is the construction diagram of the eaves node;
[0039] Figure 6 This is a graph showing the tensile bond strength test results of Embodiment 3 of the present invention;
[0040] Figure 7This is a core drilling test result of the thickness of the sprayed insulation main layer in Embodiment 3 of the present invention.
[0041] The components include: 1. Base wall; 2. Interface treatment layer; 3. Sprayed insulation main layer; 4. Reinforced protective layer; 5. Decorative protective layer; 31. Component A mixing tank; 32. Component B mixing tank; 33. Heating device; 34. Metering pump assembly; 35. Heated delivery pipeline; 36. Mixing nozzle; 37. Control assembly; 41. Polymer modified crack-resistant mortar; 42. Alkali-resistant fiberglass mesh; 51. Window frame; 52. Pre-compressed sealing strip; 53. Sealing layer; 61. Waterproof layer; 62. Waterproof mortar protective layer; 63. Corner guard strip; 71. Roof insulation layer; 72. Polyurethane foam material. Detailed Implementation
[0042] The present invention will be further described below with reference to the accompanying drawings and specific embodiments.
[0043] like Figure 1 As shown, a method for low-temperature spray insulation construction of rural houses in cold regions includes base treatment, interface treatment, preheating of spray materials and equipment preparation, layered spraying, surface finishing, construction of reinforced protective layer and construction of decorative protective layer.
[0044] like Figure 2 As shown, the wall insulation structure formed by the above construction method includes, from the inside out, a base wall 1, an interface treatment layer 2, a sprayed insulation main layer 3, a reinforcing protective layer 4, and a decorative protective layer 5. The reinforcing protective layer 4 includes a polymer-modified crack-resistant mortar 41 and an alkali-resistant glass fiber mesh 42 embedded in the polymer-modified crack-resistant mortar 41.
[0045] The base wall 1 is made of red brick, aerated concrete block, concrete, or adobe. Before construction, the surface of the base wall 1 is cleaned, repaired, and inspected. An interface treatment layer 2 is formed on the surface of the base wall 1. Then, a two-component modified polyurethane rigid foam material is sprayed multiple times on the outside of the interface treatment layer 2. The sprayed layers are sequentially bonded to form a continuous sprayed insulation main layer 3. A reinforcing protective layer 4 and a decorative protective layer 5 are then formed sequentially on the outside of the sprayed insulation main layer 3.
[0046] S1, Base Treatment
[0047] Clean the surface of the base wall 1 of floating dust, oil stains, mortar residue and loose layer, and remove the old decorative layer that is not firmly attached.
[0048] Inspect the surface of the base wall 1 for cracks and holes, and fill and level them with polymer repair mortar. When the crack width is greater than 3mm, remove the loose material in the crack and fill it with polymer repair mortar; when there are local cracks at the corners of door and window openings, embed reinforcing mesh fabric in the repair area.
[0049] When there is oil on the surface of the base wall 1, clean the oily area first, then remove the residue with clean water and dry it. For existing farmhouse walls, if the original plaster layer is hollow, peeling, or loose, remove the loosely attached parts and retain the firmly attached parts after surface cleaning.
[0050] After cleaning and repair, the moisture content of the base wall 1 was tested and controlled below 10%. A 2m straightedge was used to check the flatness of the wall surface, and the flatness deviation was controlled within 10mm / 2m. Protruding areas were ground down, and recessed areas were leveled using polymer repair mortar.
[0051] S2, Interface Processing
[0052] After the base wall 1 is treated, a special interface treatment agent is evenly applied to its outer surface to form an interface treatment layer 2.
[0053] The special interface treatment agent comprises, by weight, 40-50 parts of acrylate emulsion, 3-6 parts of γ-aminopropyltriethoxysilane, 10-15 parts of nano-silica dispersion, 0.3-0.5 parts of defoamer, 2-4 parts of film-forming aid, and 30-40 parts of water.
[0054] Before construction, stir the special interface treatment agent evenly and apply it to the surface of the base wall 1 by brushing or spraying, with a coating amount of 150-200g / m². 2 When using a roller coating method, the coating is applied in a crisscross pattern along different directions to ensure that the special interface treatment agent continuously covers the surface of the base wall 1.
[0055] After the interface treatment agent is applied, curing is required. When the ambient temperature is above 5℃, the curing time should be no less than 2 hours; when the ambient temperature is between 0 and 5℃, the curing time should be no less than 4 hours. Gently touch the surface of interface treatment layer 2 with your finger. Once the surface material does not transfer significantly and the surface is dry to the touch, proceed with the subsequent spraying application.
[0056] The interface treatment layer 2 formed has a thickness of 0.5 to 1.0 mm and is located between the base wall 1 and the sprayed insulation main layer 3.
[0057] In one specific formulation, the special interface treatment agent includes 45 parts by weight of an acrylic emulsion with a solid content of 50%, 4.5 parts by weight of γ-aminopropyltriethoxysilane, 12 parts by weight of a nano-silica dispersion with a solid content of 30%, 0.4 parts by weight of an organosilicon defoamer, 3 parts by weight of a film-forming aid, and 35.1 parts by weight of deionized water.
[0058] S3. Preheating of spraying materials and equipment preparation
[0059] The sprayed insulation main layer 3 is formed using a two-component modified polyurethane rigid foam material, which includes component A and component B.
[0060] Component A, by weight, comprises 100 parts of a composite polyether polyol, 3-8 parts of silane coupling agent modified nano-silica, 25-40 parts of halogen-free composite flame retardant, 2-4 parts of a foam leveler, 1.5-3.0 parts of a low-temperature catalyst system, 12-20 parts of HFO-type physical foaming agent, 1.0-2.5 parts of water, 0.5-2.0 parts of a nano-toughening modifier, and 2-5 parts of an interfacial tackifier.
[0061] The composite polyether polyol is formed by compounding polyester polyol and polyether polyol in a mass ratio of 3:7 to 4:6; the low-temperature catalyst system includes organotin catalyst and tertiary amine catalyst; the HFO-type physical foaming agent is HFO-1233zd(E) or HFO-1336mzz(Z); the nano-toughening modifier includes organic modified nano-montmorillonite and carbon nanotubes, wherein the mass ratio of organic modified nano-montmorillonite to carbon nanotubes is 4:1 to 6:1; the interface tackifier is acrylate-modified organosilicon.
[0062] The halogen-free composite flame retardant includes an intumescent flame retardant and aluminum hydroxide micro powder in a mass ratio of 7:3. The intumescent flame retardant is formed by compounding ammonium polyphosphate, melamine cyanurate and pentaerythritol in a mass ratio of 3:1:1.
[0063] Component B uses modified MDI with an isocyanate index of 105–115.
[0064] like Figure 3 As shown, the spraying equipment includes component A material tank 31, component B material tank 32, heating device 33, metering pump assembly 34, heated delivery pipeline 35, mixing nozzle 36, and control assembly 37.
[0065] Component A is placed in component A container 31, and component B is placed in component B container 32. Component A and component B are preheated separately by heating device 33. Component A is preheated to 30-40°C, and component B is preheated to 25-35°C.
[0066] Components A and B are respectively fed into the corresponding heated delivery lines 35 via the metering pump assembly 34. The heating temperature of the heated delivery lines 35 is set to 30–50°C. The mixing nozzle 36 is independently heated, and its temperature is maintained at 40–50°C.
[0067] After components A and B reach the set temperature, they are circulated and conveyed to make the material temperature in the hopper and heated conveying pipeline 35 tend to be uniform. The control component 37 detects and regulates the material temperature, conveying pressure, and material flow rate.
[0068] A test spray is conducted before the formal coating. Components A and B are mixed according to the preset ratio through mixing nozzle 36 and sprayed onto the surface of the test spray plate. The foaming state of the material is observed, and the sample is cut open to inspect the internal pores after the test spray foam reaches a non-sticky state. The formal coating process begins when no obvious bubble collapse, large pores, or voids are observed in the test spray foam.
[0069] S4, Layered spraying
[0070] The mixing nozzle 36 is directed toward the base wall 1 on which the interface treatment layer 2 is formed. The mixed components A and B are sprayed out by the mixing nozzle 36 and foamed and cured on the surface of the interface treatment layer 2.
[0071] During the spraying process, the distance between the mixing gun head 36 and the wall surface is maintained at 400-600mm, and the gun travel speed is 0.3-0.5m / s.
[0072] The first coat of spraying forms the first coating layer, with a thickness of 30-40 mm. After the first coat of spraying is completed, the first coating layer continues to foam. When the material does not stick to the finger when lightly touched and the free expansion has basically stopped, it is determined that it has reached the state of being non-sticky to the touch.
[0073] After the first coat reaches a non-sticky state to the touch, apply the second coat, with the spray gun direction intersecting the first coat direction. The thickness of each coat, from the second to the subsequent coats, should be 30–50 mm, and the interval between adjacent coats should be 5–15 minutes.
[0074] The total number of spray coats is 2 to 3. When setting up the third spray coat, the spray gun direction is changed again relative to the second coat, so that the spray gun directions of the two adjacent spray coats intersect each other.
[0075] During construction, after each predetermined area is completed, a thickness gauge is used to randomly check the spray thickness, and the coverage of subsequent sprayed areas is adjusted based on the test results. Each spray layer is formed sequentially and combines with each other to ultimately constitute the main sprayed insulation layer 3.
[0076] S5, Surface Finishing
[0077] After spraying, allow the sprayed insulation layer 3 to continue curing. Once the finishing conditions are met, use a 2m straightedge to check the surface flatness of the sprayed insulation layer 3 and mark the overlapping positions of the sprayed strips or other protruding areas.
[0078] The protruding areas are cut and leveled using a hot wire cutter or a long blade. The flatness deviation of the sprayed insulation main layer 3 after the repair is controlled within 5mm / 2m.
[0079] After finishing, remove foam debris and dust to keep the surface of the sprayed insulation layer 3 clean.
[0080] S6. Construction of reinforced protective layer
[0081] Apply the first layer of polymer-modified crack-resistant mortar 41 to the outer surface of the repaired sprayed insulation main layer 3. The thickness of the first layer of polymer-modified crack-resistant mortar 41 is about 2mm.
[0082] While the first layer of polymer-modified crack-resistant mortar 41 remains moist, alkali-resistant glass fiber mesh 42 is laid on the mortar surface and pressed into it. The overlap width between adjacent alkali-resistant glass fiber meshes 42 shall not be less than 100 mm.
[0083] Alkali-resistant fiberglass mesh 42 is continuously installed across the corners, and additional reinforcing mesh is installed at the four corners of door and window openings.
[0084] After the first layer of polymer-modified crack-resistant mortar 41 meets the conditions for subsequent plastering, the second layer of polymer-modified crack-resistant mortar 41 is then applied, so that the alkali-resistant glass fiber mesh 42 is covered by the polymer-modified crack-resistant mortar 41. The two layers of polymer-modified crack-resistant mortar 41 and alkali-resistant glass fiber mesh 42 together form an enhanced protective layer 4.
[0085] The total thickness of the reinforcing protective layer 4 is 3 to 5 mm, and the alkali-resistant glass fiber mesh 42 is located within one-third of the outer surface of the reinforcing protective layer 4 along the thickness direction.
[0086] The alkali-resistant fiberglass mesh 42 has a mesh size of 4mm × 4mm and a unit area mass of 160g / m². 2 The alkali-resistant tensile strength is not less than 750N / 50mm.
[0087] S7. Construction of Decorative Protective Layer
[0088] After the reinforcement protective layer 4 is completed, it shall be cured for no less than 7 days. The moisture content of the reinforcement protective layer 4 shall be tested, and the decorative protective layer 5 shall be constructed when the moisture content drops below 8%.
[0089] Decorative protective layer 5 is made of elastic exterior wall paint or stone paint. When using elastic exterior wall paint, the primer, intermediate coat, and topcoat are applied sequentially, with each coat applied after the previous coat has reached its corresponding dry state. The resulting decorative protective layer 5 has a thickness of 0.3–0.5 mm.
[0090] After the above construction, a multi-layer composite insulation structure consisting of an interface treatment layer 2, a sprayed insulation main layer 3, a reinforced protective layer 4, and a decorative protective layer 5 is formed on the outside of the base wall 1.
[0091] Key node structure
[0092] like Figure 5 As shown, the sprayed insulation main layer 3 is continuously installed at door and window openings, wall corners, plinths, and eaves.
[0093] Figure 5 Image (a) shows the door and window opening details. The sprayed insulation main layer 3 extends continuously from the main surface of the base wall 1 to the side of the door and window opening, and wraps over the reserved position where the window frame 51 is located, with a wrap width of not less than 50mm. A pre-pressed sealing strip 52 is installed between the window frame 51 and the sprayed insulation main layer 3, and a sealing layer 53 is installed on the outside of the pre-pressed sealing strip 52. The sprayed insulation main layer 3 below the window sill is locally thickened.
[0094] Figure 5 Image (b) shows a corner node. The sprayed insulation main layer 3 at the corner is 20-30mm thicker than the sprayed insulation main layer 3 on the main surface of the base wall 1. A double layer of alkali-resistant fiberglass mesh 42 is installed inside the reinforcing protective layer 4 at the corner, and the alkali-resistant fiberglass mesh 42 is laid continuously across the corner.
[0095] Figure 5 The plinth node is shown in (c). The sprayed insulation main layer 3 extends 200mm below the outdoor ground level along the base wall 1. A waterproof layer 61 is installed on the outside of the sprayed insulation main layer 3 at the plinth location, and a 10mm thick waterproof mortar protective layer 62 is installed on the outside of the waterproof layer 61. Corner guards 63 are installed in the local area above the outdoor drainage surface.
[0096] Figure 5 The middle (d) shows the eaves node. The sprayed insulation main layer 3 extends upward along the base wall 1 to the eaves position and overlaps with the roof insulation layer 71, with an overlap width of 250mm; the overlap between the sprayed insulation main layer 3 and the roof insulation layer 71 is filled with polyurethane foam material 72.
[0097] Example 1
[0098] This embodiment uses a newly built brick-concrete structure farmhouse in Harbin as the construction object. The base wall 1 is a solid red brick wall with a thickness of 370mm, and the design control value of the wall heat transfer coefficient is 0.25W / (m²). 2 ·K).
[0099] The thermal conductivity of a 370mm solid red brick wall is taken as 0.81W / (m·K), and its thermal resistance is... for:
[0100] ;
[0101] The combined internal and external surface heat transfer resistance is taken as 0.15m. 2 • K / W. Based on a wall heat transfer coefficient not exceeding 0.25 W / (m²). 2 ·K) is determined, and the total thermal resistance R satisfies:
[0102] ;
[0103] Thermal resistance required for sprayed insulation main layer 3 satisfy:
[0104] ;
[0105] The thermal conductivity of the sprayed insulation material is taken as 0.024 W / (m·K), from which the minimum thickness of the sprayed insulation main layer 3 is obtained. :
[0106] ;
[0107] That is, the minimum thickness is about 81.4mm. In this embodiment, the design thickness of the sprayed insulation main layer 3 is determined to be 100mm.
[0108] Construction shall be carried out according to S1 to S7. The ambient temperature during construction shall be approximately 8°C. Component A shall be preheated to 35°C, and component B shall be preheated to 30°C.
[0109] The thermal insulation base layer is applied in three coats, with target thicknesses of 35mm, 35mm and 30mm respectively. The interval between adjacent coats is approximately 10 minutes.
[0110] The net area of the wall to be sprayed is approximately 220m². 2 Two construction workers worked together to complete the spraying operation. One person operated the spraying equipment, while the other was responsible for supplying materials and assisting with other tasks. The spraying operation took about 6 hours.
[0111] Tensile bond strength tests were conducted at three randomly selected locations after construction, with values of 0.18 MPa, 0.16 MPa, and 0.17 MPa, respectively. Core drilling revealed the actual thickness of the sprayed insulation layer 3 to be 98–103 mm, with a material density of 34–38 kg / m³. On-site testing showed the wall's heat transfer coefficient to be 0.23 W / (m³). 2 ·K).
[0112] Example 2
[0113] This embodiment uses an existing rural house in Changchun as the construction object. The base wall 1 is a red brick wall with a thickness of 490mm, and its outer surface has an original lime plaster layer.
[0114] Before construction, check the bonding condition between the lime plaster layer and the base wall 1. Remove any loose, hollow, or peeling areas, retain the firmly attached areas, and repair any local cracks with polymer repair mortar.
[0115] After the base layer treatment, the moisture content of the base wall 1 was found to be 8.5%.
[0116] Considering the existing wall surface has areas with exposed red bricks and areas with retained plaster, this embodiment adjusts the application rate of the special interface treatment agent to 200g / m². 2 And make the interface treatment agent continuously cover the surface of the base wall 1.
[0117] The designed thickness of the main insulation layer 3 is 90mm. The material is preheated and layered sprayed according to S3 and S4. Each layer continues to form after the previous layer reaches a non-sticky state, until the main insulation layer 3 reaches the designed thickness.
[0118] The main sprayed insulation layer 3 at the door and window opening extends along the main surface of the base wall 1 to the side of the opening; the main sprayed insulation layer 3 at the plinth extends 200mm below the outdoor drainage surface and is equipped with a protective structure.
[0119] Records were taken before and after the renovation under the same heating conditions. Before the renovation, the average indoor temperature in winter was about 12℃, and after the renovation, the average indoor temperature in winter was about 20℃. The heating energy consumption was reduced by about 55% compared with before the renovation.
[0120] Example 3
[0121] This embodiment uses a newly built brick-concrete structure farmhouse in a village in Suihua City, Heilongjiang Province as the construction object. The farmhouse is a single-story house with a pitched roof and a building area of approximately 120 square meters. 2 The floor height is 3.0m, and the exterior wall area is approximately 185m². 2 The net spraying area, excluding door and window openings, is approximately 156m². 2 .
[0122] The base wall 1 is a solid red brick wall with a thickness of 370mm. Without insulation, the heat transfer coefficient of the wall is approximately 1.58W / (m²). 2 ·K).
[0123] The wall insulation structure in this embodiment is as follows: Figure 4 As shown, it consists of a base wall 1, an interface treatment layer 2, a sprayed insulation main layer 3, a reinforced protective layer 4, and a decorative protective layer 5 in sequence.
[0124] The design thickness of the sprayed insulation main layer 3 is determined according to the control value of the wall heat transfer coefficient. The wall heat transfer coefficient is calculated according to the following formula:
[0125] ;
[0126] In the formula, K is the heat transfer coefficient of the wall; The internal surface heat transfer resistance is taken as 0.11m. 2 K / W; The external surface heat transfer resistance is taken as 0.04m. 2 K / W; The thermal resistance of the base wall 1; The thermal resistance of the main insulation layer 3 is determined by spraying; This is to determine the thermal resistance of the surface layer.
[0127] If the thermal conductivity of a 370mm solid red brick wall is taken as 0.81W / (m·K), then:
[0128] ;
[0129] If the thermal conductivity of the sprayed insulation material is taken as 0.024 W / (m·K), and the thickness of the plaster layer is taken as 5 mm with a thermal conductivity of 1.0 W / (m·K), then:
[0130] ;
[0131] according to The total thermal resistance should meet the following requirements:
[0132] ;
[0133] Therefore, we can conclude that:
[0134] ;
[0135] The calculated minimum thickness of the sprayed insulation main layer 3 is:
[0136] ;
[0137] That is, approximately 81.3 mm. Considering the control of the spraying thickness on site, the design thickness of the sprayed insulation main layer 3 is determined to be 100 mm in this embodiment.
[0138] Calculated based on a thickness of 100mm:
[0139] ;
[0140] The corresponding theoretical wall heat transfer coefficient is approximately:
[0141]
[0142] The A component used in this embodiment specifically includes: 100 parts by weight of a combined polyether polyol, wherein the mass ratio of polyester polyol to polyether polyol is 35:65; 5 parts by weight of silane-modified nano-silica; 32 parts by weight of a halogen-free composite flame retardant; 3.2 parts by weight of an organosilicon foam stabilizer; 2.2 parts by weight of a low-temperature catalyst system, wherein 0.3 parts by weight of stannous octoate, 1.2 parts by weight of DMCHA, and 0.7 parts by weight of PMDETA; 16 parts by weight of HFO-1233zd(E); 1.8 parts by weight of deionized water; 1.2 parts by weight of a nano-toughening modifier, wherein the mass ratio of organically modified nano-montmorillonite to carbon nanotubes is 5:1; and 3.5 parts by weight of an interfacial tackifier, wherein the interfacial tackifier is an acrylate-modified organosilicon emulsion.
[0143] Component B uses modified MDI, and the preset ratio of components A and B is 1:1.15, with an isocyanate index of 110.
[0144] The special interface treatment agent includes 45 parts by weight of acrylate emulsion with a solid content of 50%, 4.5 parts by weight of γ-aminopropyltriethoxysilane, 12 parts by weight of nano silica dispersion with a solid content of 30%, 0.4 parts by weight of organosilicon defoamer, 3 parts by weight of film-forming aid, and 35.1 parts by weight of deionized water.
[0145] The reinforcing protective layer 4 uses flexible polymer-modified cement mortar as polymer-modified crack-resistant mortar 41, and the alkali-resistant glass fiber mesh 42 has a mesh size of 4mm×4mm and a unit area mass of 160g / m². 2 .
[0146] The main insulation layer is designed to have a thickness of 100mm, a molding density of 35kg / m³, and a net spraying area of 156m². 2 Calculations show that the total usage of components A and B is approximately 546 kg, with a construction material preparation quantity of approximately 600 kg; the usage of the special interface treatment agent is approximately 28.1 kg, with a preparation quantity of 30 kg; the preparation quantity of polymer-modified crack-resistant mortar 41 is approximately 1050 kg; and the preparation quantity of alkali-resistant glass fiber mesh 42 is approximately 172 m². 2 .
[0147] The daytime ambient temperature during construction is approximately 8–15℃.
[0148] On the morning of the first day of construction, the base layer was prepared. A wire brush and high-pressure air were used to clean the surface of the base wall 1, removing loose dust and mortar residue. Three shrinkage cracks, approximately 2-4 mm wide, were found in the horizontal mortar joints of the wall; these were filled and leveled with polymer repair mortar. One crack, approximately 5 mm wide, was found at the corner of the window opening; after removing loose parts, it was repaired with polymer repair mortar, and a 200 mm × 300 mm reinforcing mesh was embedded.
[0149] After the base treatment, the moisture content of the walls facing different directions was tested. The moisture content was 8.2% for the south wall, 9.1% for the north wall, 7.8% for the east wall, and 8.5% for the west wall. The flatness of the wall was checked using a 2m straightedge. The maximum deviation was 8mm. After grinding the protruding parts, the deviation was controlled within 6mm.
[0150] Interface treatment was carried out on the afternoon of the first day of construction. A special interface treatment agent was applied cross-coated to the surface of the base wall using a short-pile roller, with an actual coating amount of approximately 170 g / m². 2 When the interface treatment is completed, the ambient temperature is about 12℃. After curing for about 3 hours, check the interface treatment layer 2. Its surface is slightly sticky but not sticky to the touch, and then proceed to the subsequent construction.
[0151] On the morning of the second day of construction, the ambient temperature was approximately 6°C. The initial temperature of component A was approximately 8°C, and the initial temperature of component B was approximately 10°C. The target temperature of component A was set to 35°C and the target temperature of component B was set to 28°C using heating device 33; the temperature of the heated delivery pipeline 35 was set to 40°C, and the temperature of the mixing nozzle 36 was set to 45°C.
[0152] After preheating for approximately 50 minutes, the actual temperature of component A reached approximately 34°C, and the actual temperature of component B reached approximately 27°C. The mixture was then circulated for 5 minutes. The spraying pressure was set to 9 MPa, the ratio of component A to component B was set to 1:1.15, and the material flow rate was set to 4 kg / min.
[0153] A test spray was conducted before the formal application. The test spray material foamed evenly, with no obvious bubble collapse on the surface, and reached a non-sticky state to the touch after about 80 seconds. After cutting open the test spray sample, it was observed that the internal pores were evenly distributed, and no obvious large pores or voids were found.
[0154] The ambient temperature was approximately 9°C when the formal spraying began. The first coat started from the south wall, with the mixing nozzle 36 kept approximately 500mm away from the wall and the spray gun speed approximately 0.4m / s. An overlap of approximately 100mm was formed between adjacent sprayed areas, and the target thickness for the first coat was 35mm.
[0155] Approximately 10 minutes after the first coat is applied, when the coating reaches a non-sticky state to the touch, the second coat is applied. The spray gun direction for the second coat is adjusted to a vertical direction intersecting the first coat, with a target thickness of 35mm.
[0156] After the second coat has been applied for approximately 12 minutes and reached a non-sticky state to the touch, the third coat is applied. For the third coat, the spray gun is moved horizontally, with a target thickness of 30mm. These three coats together form a 100mm thick thermal insulation base layer.
[0157] During the construction process, approximately 20m is completed each time. 2The coating area was measured at three random locations using a thickness gauge. The thickness of the first coat was measured to be 33–38 mm; the thickness after three coats was measured to be 96–108 mm, with an average of approximately 102 mm and a standard deviation of 3.2 mm.
[0158] Approximately 16 hours after spraying, surface finishing is performed. A 2m straightedge is used to determine the protruding positions at the overlaps of the sprayed areas, and a hot wire cutter is used for trimming. The maximum flatness deviation after finishing is 4mm / 2m.
[0159] Subsequently, reinforced protective layer 4 is constructed. First, a first layer of polymer-modified crack-resistant mortar 41 with a thickness of approximately 2mm is applied. Alkali-resistant fiberglass mesh 42 is then pressed into the wet mortar, with an overlap width of 100mm between adjacent alkali-resistant fiberglass mesh 42. The overlap width of the alkali-resistant fiberglass mesh 42 at the corners of the walls is not less than 200mm. Reinforcing mesh sheets of 300mm × 400mm are installed at the four corners of door and window openings, arranged in a 45° direction.
[0160] Approximately 2 hours after the first layer of polymer-modified crack-resistant mortar 41 is applied, the second layer of polymer-modified crack-resistant mortar 41 is applied, so that the total thickness of the reinforced protective layer 4 reaches 4-5 mm. The alkali-resistant glass fiber mesh 42 is about 1.5 mm away from the outer surface of the reinforced protective layer 4.
[0161] After curing the protective layer 4 for 7 days, the moisture content was tested and found to be 7.5%. Subsequently, the decorative protective layer 5 was applied, consisting of one coat of sealing primer, one coat of elastic intermediate coat, and two coats of elastic topcoat.
[0162] Door and window openings, wall corners, plinths and eaves according to Figure 5 The structure shown is processed as follows: The sprayed insulation main layer 3 at the window opening is wrapped 50mm over the window frame 51 at the reserved position. A pre-pressed sealing strip 52 is set between the window frame 51 and the sprayed insulation main layer 3, and a sealing layer 53 is set on the outside. The local thickness of the sprayed insulation main layer 3 under the window sill is 130mm.
[0163] The thickness of the sprayed insulation main layer 3 at the corner is 120mm, which is 20mm thicker than the main surface of the wall. The reinforced protective layer 4 is equipped with a double layer of alkali-resistant glass fiber mesh 42.
[0164] The main thermal insulation layer 3 at the plinth extends 200mm below the outdoor ground level, and a waterproof layer 61 with a thickness of about 2mm is set on the outside. A waterproof mortar protective layer 62 with a thickness of 10mm is set on the outside of the waterproof layer 61, and corner guards 63 are set locally above the outdoor drainage surface.
[0165] The sprayed insulation main layer 3 at the eaves extends upward and overlaps with the roof insulation layer 71, which is 200mm thick. The overlap width is 250mm, and the overlap is filled with polyurethane foam material 72.
[0166] After the construction was completed, the tensile bond strength of the sprayed insulation main layer 3 was tested, and the test results are as follows: Figure 6 As shown, the minimum tensile bond strength at each test point was 0.15 MPa, and the average value was 0.172 MPa. The main failure location was inside the sprayed insulation main layer 3.
[0167] The final core drilling thickness of the sprayed insulation main layer 3 was measured, and the results are as follows: Figure 7 As shown, the average thickness of the 8 core drilling test points was 100.6 mm, the lowest tested thickness was 97 mm, and the standard deviation was 3.2 mm. This core drilling test was the final test after the wall insulation structure construction was completed, and was conducted separately from the process test using thickness gauges during the spraying process.
[0168] On-site testing revealed that the heat transfer coefficient of the wall after construction was 0.22 W / (m²). 2 ·K).
[0169] In this embodiment, the ambient temperature during the spraying stage was in the range of approximately 6 to 15°C. Through preheating of components A and B respectively, heat-insulated delivery through heated delivery pipeline 35, and heating of mixing nozzle 36, three-layer spraying and subsequent wall insulation structure construction were completed.
[0170] Although embodiments of the invention have been shown and described, it will be understood by those skilled in the art that various changes, modifications, substitutions and alterations can be made to these embodiments without departing from the principles and spirit of the invention, the scope of which is defined by the appended claims and their equivalents.
Claims
1. A method for low-temperature spray insulation construction of rural house walls in cold regions, characterized in that, Includes the following steps: S1. Base treatment: Clean the surface of the base wall of the farmhouse, removing floating dust, oil stains and loose layers; repair cracks and holes in the base wall; and test the moisture content and flatness of the base wall. S2. Interface treatment: A special interface treatment agent containing silane coupling agent and nano silica dispersion is applied to the surface of the base wall after the base treatment, and the special interface treatment agent forms an interface treatment layer on the surface of the base wall. After the interface treatment layer reaches the touch dry state, subsequent spraying is carried out. S3. Preheating of the spraying material: Component A and Component B of the two-component modified polyurethane rigid foam material are respectively fed into the spraying equipment for preheating. Component A includes a combination of polyether polyol, silane coupling agent modified nano-silica, low-temperature catalyst system, physical foaming agent and interface tackifier. Component B is modified MDI. The delivery pipelines for components A and B are heated, as are the mixing nozzles, so that components A and B are delivered to the mixing nozzles through the delivery pipelines and mixed. The mixture is then sprayed onto the surface of the base wall to form a continuous sprayed insulation layer. S4. Layered spraying: The A and B components, after being mixed by the mixing gun head, are sprayed onto the surface of the interface treatment layer to form the first spraying layer. After the first spraying layer reaches a non-sticky state, spraying continues to form the subsequent spraying layer. Adjacent spraying layers adopt mutually perpendicular gun directions. Multiple spraying layers are continuously combined to form the sprayed insulation main layer. S5. Surface finishing: After the sprayed insulation main layer has cured, the protruding areas on the surface of the sprayed insulation main layer are cut and leveled. S6. Construction of the reinforced protective layer: Apply the first layer of polymer-modified crack-resistant mortar to the surface of the sprayed insulation main layer after surface repair, press the alkali-resistant glass fiber mesh into the first layer of polymer-modified crack-resistant mortar, and continue to apply polymer-modified crack-resistant mortar to form a reinforced protective layer. S7. Construction of decorative protective layer: After the reinforced protective layer has been cured, a decorative protective layer is constructed on the outer surface of the reinforced protective layer.
2. The method for low-temperature spray insulation construction of rural house walls in cold regions according to claim 1, characterized in that: The special interface treatment agent comprises the following components in parts by weight: 40-50 parts of acrylate emulsion, 3-6 parts of γ-aminopropyltriethoxysilane, 10-15 parts of nano silica dispersion, 0.3-0.5 parts of defoamer, 2-4 parts of film-forming aid, and 30-40 parts of water. The application rate of the special interface treatment agent on the surface of the base wall is 150-200 g / m². 2 .
3. The method for low-temperature spray insulation construction of rural house walls in cold regions according to claim 1, characterized in that: Component A comprises the following components in parts by weight: 100 parts of combined polyether polyol, 3-8 parts of silane coupling agent modified nano silica, 25-40 parts of halogen-free composite flame retardant, 2-4 parts of foam leveling agent, 1.5-3.0 parts of low-temperature catalyst system, 12-20 parts of HFO physical foaming agent, 1.0-2.5 parts of water, 0.5-2.0 parts of nano toughening modifier, and 2-5 parts of interface tackifier; The composite polyether polyol is formed by blending polyester polyol and polyether polyol in a mass ratio of 3:7 to 4:
6. The low-temperature catalyst system includes an organotin catalyst and a tertiary amine catalyst; The interface tackifier is an acrylate-modified organosilicon. The isocyanate index of component B is 105 to 115.
4. The method for low-temperature spray insulation construction of rural house walls in cold regions according to claim 1, characterized in that: In step S3, component A is preheated to 30-40°C, and component B is preheated to 25-35°C. The heating temperature of the delivery pipeline is 30-50°C, and the temperature of the mixing nozzle is 40-50°C. After preheating, components A and B are circulated and transported to the mixing nozzle via their respective delivery pipelines.
5. The method for low-temperature spray insulation construction of rural house walls in cold regions according to claim 1, characterized in that: In step S4, the spray distance between the mixing nozzle and the base wall is 400-600mm, and the spray speed is 0.3-0.5m / s; The thickness of the first spray coating layer is 30-40 mm, and the thickness of each subsequent spray coating layer is 30-50 mm. The interval between two adjacent spray coating layers is 5-15 minutes, and the number of spray coating layers is 2-3. The spray gun directions of two adjacent coats are perpendicular to each other.
6. The method for low-temperature spray insulation construction of rural houses in cold regions according to claim 1, characterized in that: In step S1, the moisture content of the base wall is controlled below 10%, and the flatness deviation of the base wall is controlled within 10mm / 2m. In step S2, when the ambient temperature is above 5℃, the curing time of the special interface treatment agent shall not be less than 2 hours, and when the ambient temperature is between 0 and 5℃, the curing time of the special interface treatment agent shall not be less than 4 hours. In step S5, the flatness deviation of the sprayed insulation main layer is controlled within 5mm / 2m; In step S6, the total thickness of the reinforced protective layer is 3-5 mm, and the overlap width between adjacent alkali-resistant glass fiber mesh is not less than 100 mm.
7. A low-temperature spray-coating insulation structure for the walls of rural houses in cold regions, characterized in that: It includes, from the inside out, the base wall, the interface treatment layer, the sprayed insulation main layer, the reinforced protective layer, and the decorative protective layer; The interface treatment layer is directly applied to the outer surface of the base wall. The interface treatment layer is formed by a special interface treatment agent comprising an acrylic emulsion, γ-aminopropyltriethoxysilane, and a nano silica dispersion. The sprayed insulation main layer is directly set on the outer surface of the interface treatment layer and is formed by multiple sprayings of modified polyurethane rigid foam material. The reinforced protective layer is disposed on the outer surface of the sprayed thermal insulation main layer and includes polymer-modified crack-resistant mortar and alkali-resistant glass fiber mesh embedded in the polymer-modified crack-resistant mortar; The decorative protective layer is disposed on the outer surface of the reinforced protective layer; At the door and window openings of the base wall, the sprayed insulation main layer extends continuously from the main surface of the base wall to the side of the door and window opening; at the corners of the base wall, the sprayed insulation main layer is locally thickened relative to the main surface of the base wall; at the plinth of the base wall, the sprayed insulation main layer extends below the outdoor ground level; at the eaves of the base wall, the sprayed insulation main layer extends upward and overlaps with the roof insulation layer.
8. A low-temperature spray-coating insulation structure for the walls of rural houses in cold regions according to claim 7, characterized in that: The thickness of the interface treatment layer is 0.5–1.0 mm; The thickness of the sprayed thermal insulation main layer is 80-120mm; The thickness of the reinforcing protective layer is 3-5 mm, and the alkali-resistant glass fiber mesh is disposed in one-third of the reinforcing protective layer along the thickness direction near the outer surface. The decorative protective layer is an elastic exterior wall coating or a real stone paint layer, with a thickness of 0.3 to 0.5 mm.
9. A low-temperature spray-coating insulation structure for the walls of rural houses in cold regions according to claim 7, characterized in that: The main thermal insulation layer around the door and window openings is folded over to the side of the door and window openings, and the folding width is not less than 50mm. A pre-pressed sealing strip is installed between the door and window frame and the sprayed insulation main layer, and a sealing layer is installed on the outside of the pre-pressed sealing strip; The sprayed insulation main layer at the corner is 20-30mm thicker than the sprayed insulation main layer on the main surface of the base wall. The reinforced protective layer at the corner is provided with a double layer of alkali-resistant glass fiber mesh, and the alkali-resistant glass fiber mesh is continuously installed across the corner.
10. A low-temperature spray-coating insulation structure for the walls of rural houses in cold regions according to claim 7, characterized in that: The sprayed insulation main layer at the plinth extends 200mm below the outdoor ground level. A waterproof layer is installed on the outside of the sprayed insulation main layer at the plinth, and a 10mm thick waterproof mortar protective layer is installed on the outside of the waterproof layer. The sprayed insulation main layer at the eaves extends upward to the eaves and overlaps with the roof insulation layer. The overlap width between the sprayed insulation main layer and the roof insulation layer is 250mm, and the overlap area is filled with polyurethane foam material.