A high-strength, bend-resistant copper alloy stranded wire and its preparation method
By controlling the entire process and strengthening the elements of copper alloy wire, the problem of synergistic improvement of high strength, high conductivity and bending fatigue resistance of copper alloy wire was solved, and high-strength and bending-resistant copper alloy stranded wire suitable for electronic information communication wire harnesses was prepared, meeting the requirements of fine diameter and high frequency bending.
Patent Information
- Application Number
- CN202611536253.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-30
- Publication Date
- 2026-11-17
AI Technical Summary
Existing copper alloy wires struggle to achieve a good balance between high strength, high conductivity, and high resistance to bending fatigue, especially under conditions of reduced diameter and high-frequency reciprocating bending, where it is difficult to synergistically improve these properties.
By controlling the grain size and microstructure at different processing stages throughout the entire process and in stages, combined with intermediate aging and finished product drawing, a uniform and fine microcrystalline structure is formed. Cr, Mg, Ag and B elements are added for strengthening, controlling the uniform distribution of alloying elements and the uniformity of the microstructure, and reducing stress concentration.
This technology achieves a comprehensive improvement in the high strength, high conductivity, and excellent bending fatigue resistance of copper alloy stranded wires, making them suitable for electronic information communication harnesses, especially for extending service life under high-frequency bending conditions in folding equipment and robot joints.
Smart Images

Figure 6ABCB64C6F1D9 
Figure 6ABCB64C6F4CF 
Figure 6ABCB64C6F6FC
Abstract
Description
Technical Field
[0001] This invention belongs to the field of electronic information communication cable manufacturing, specifically relating to a high-strength, bend-resistant copper alloy stranded wire and its preparation method. Background Technology
[0002] With the development of foldable electronic devices and intelligent equipment such as robots, cables need to withstand high-frequency reciprocating bending and torsion for extended periods during use. Therefore, cables for electronic information communication not only need to have high conductivity, but also high strength and excellent bending fatigue performance to meet the requirements of smaller diameter, lighter weight, and longer service life.
[0003] Currently, the conductors of such cables mainly use pure copper and solid solution strengthened copper alloys, represented by copper-tin alloys. Pure copper has the advantages of high conductivity and good plasticity, but its strength is relatively low, and it is prone to local plastic deformation and fatigue damage during long-term high-frequency reciprocating bending. Copper-tin alloys can improve material strength through solid solution strengthening of Sn atoms, but Sn atoms dissolved in the copper matrix will enhance electron scattering, thus reducing conductivity. In addition, coarse or uneven grains and uneven distribution of microstructure and composition can easily cause uneven cyclic deformation and local strain concentration, promoting the initiation of fatigue cracks.
[0004] Therefore, existing copper alloy wires still fall short in terms of synergistic improvement of high strength, high conductivity and high bending fatigue resistance, especially under conditions of miniaturized wire diameter and high-frequency reciprocating bending, it is difficult to achieve a good match between the above properties. Summary of the Invention
[0005] To address the shortcomings of existing technologies, this invention provides a high-strength, bend-resistant copper alloy stranded wire and its preparation method. By controlling the grain size and microstructure at different processing stages throughout the entire process, a uniform and fine microcrystalline structure is ultimately formed. Combined with intermediate aging and finished product drawing, precipitates are formed, grains are refined, and deformation structures are created. This results in copper alloy single wires and copper alloy stranded wires that possess high strength, high conductivity, and excellent bending fatigue resistance, thus meeting the application requirements of electronic information communication wire harnesses.
[0006] To achieve the above objectives, the technical solution adopted by this invention is: a method for preparing high-strength, bend-resistant copper alloy stranded wire, the steps of which include smelting, casting, solution treatment, hot rolling, intermediate drawing, aging treatment, finished product drawing, and stranding; wherein the copper alloy single wire obtained after finished product drawing for stranding comprises the following components by mass percentage: Cr 0.15~0.32%, Mg 0.08~0.16%, Ag 0.08~0.14%, B 0.003~0.007%, with the balance being Cu; During the casting process, continuous casting is carried out by the downward continuous casting method. The casting temperature is 1250±10℃, the downward speed is 2~5mm / s, the ingot is pulled out in the same direction as the gravity direction, and an alloy rod with a diameter of 20~40mm is obtained. The average grain size in the as-cast state is 200~420μm. In the solution treatment, the cast alloy rod is held at 900±10℃ for 1~4h under a protective atmosphere, followed by water quenching, and the average grain size after solution treatment is controlled to be 230~450μm. During the hot rolling process, the heating temperature is 790±10℃, the rolling passes are 6~13, the section shrinkage rate per pass is 15~35%, the final rolling temperature is controlled not lower than 650℃, the average grain size of the alloy rod after hot rolling is 20~80 μm, and the diameter of the alloy rod is 6~10mm. During the intermediate drawing process, the alloy rod is drawn in multiple passes at room temperature, with a single pass deformation of 10-20%, and the alloy rod is drawn to the preset diameter. The average grain size of the alloy rod is 2-10 μm. In the aging treatment, the alloy rod with a preset diameter is placed at 450±10℃ for 1~4h and the average grain size of the alloy rod after treatment is 4~20μm; In the finished product drawing process, the alloy rod is drawn in multiple passes at room temperature until the target diameter is reached. The deformation amount per pass is 10~20%, resulting in a copper alloy single wire with an average grain size of 0.4~2μm and an internal stress of 200~300MPa. During the stranding process, multiple copper alloy single wires of the target diameter are stranded into copper alloy stranded wire on a stranding machine. The stranding rate is controlled at 100~300m / min, the pitch ratio is controlled at 35~50, and the single wire tension is controlled at 0.2~1.5N.
[0007] In some embodiments, during the smelting process, cathode copper is added to a vacuum induction furnace and heated until it melts; then copper-chromium alloy, copper-magnesium alloy, metallic silver and copper-boron alloy are added in sequence and melted into a copper alloy liquid; after the alloy is completely melted, it is refined under vacuum at 1100-1300°C for 10-25 minutes, and low-frequency electromagnetic stirring is applied during the refining process.
[0008] In some embodiments, the copper-chromium alloy is Cu-10Cr, the copper-magnesium alloy is Cu-20Mg, and the copper-boron alloy is Cu-5B.
[0009] In some embodiments, during the casting process, the drawdown rate is 4±0.01 mm / s, the diameter of the cast alloy rod is 30±0.1 mm, and the average grain size in the as-cast state is 260±10 μm.
[0010] In some embodiments, the protective atmosphere during the solution treatment is high-purity argon, the holding time is 2±0.1h, and the average grain size after solution treatment is 290±15μm.
[0011] In some embodiments, during the hot rolling process, the final rolling temperature is 670±10℃, and the average grain size of the alloy rod after hot rolling is 50±10μm.
[0012] In some embodiments, the alloy rod obtained after intermediate drawing has a diameter of 0.6 mm and an average grain size of 8 ± 1 μm.
[0013] In some embodiments, the holding time for aging treatment is 2±0.1h, and the average grain size after aging is 14±1.5μm.
[0014] In some embodiments, the copper alloy single wire obtained after drawing has a diameter of 0.1 mm, an average grain size of 0.6 ± 0.1 μm, and an internal stress of 241 ± 13 MPa.
[0015] This invention also proposes a high-strength, bend-resistant copper alloy stranded wire, prepared by the method described above, wherein the tensile strength of the copper alloy single wire is 610–640 MPa, the conductivity is 81–82% IACS, and the torsion count is 30–40 revolutions; the tensile strength of the copper alloy stranded wire is 585–625 MPa, the breaking force is 170–200 N, and the bend resistance under normal temperature and 9.8 N load conditions is 290,000–350,000 cycles.
[0016] The beneficial effects of this invention are as follows: 1. This invention achieves multi-element synergistic strengthening by adding Mg, Ag, and B to the Cu-Cr binary alloy. Cr primarily enhances the alloy's strength through precipitation strengthening; Mg and Cr synergistically form a Mg core-Cr shell structure, promoting Cr precipitation from the copper matrix while reducing the content of Cr and Mg solid-solubilized elements in the matrix, thus balancing strengthening and electrical conductivity; Ag plays an auxiliary strengthening and precipitation regulation role; trace amounts of B improve grain boundary conditions, enhancing processing and fatigue performance. The synergistic effect of these elements comprehensively improves the alloy's strength, electrical conductivity, and bending fatigue resistance.
[0017] 2. This invention utilizes processes such as continuous casting, solution treatment, hot rolling, multi-pass drawing, intermediate aging, and finished product drawing to control the grain size and microstructure at different stages throughout the entire process and in stages. This promotes the uniform distribution of alloying elements, improves the uniformity of microstructure and composition, and reduces stress concentration caused by local component segregation and microstructure differences. At the same time, by rationally controlling the grain size, it enhances the hindering effect of grain boundaries on dislocation movement, improves material strength, and inhibits the accumulation of local damage and the initiation and propagation of fatigue cracks during repeated bending, thereby improving the bending fatigue resistance of single wires and strands.
[0018] 3. This invention regulates the residual stress generated during the drawing process by rationally matching intermediate aging and final drawing processes, thereby reducing local stress concentration while maintaining material strength. Furthermore, by controlling the stranding process, it reduces the additional deformation and damage generated by individual wires during stranding, making the stress on each individual wire more uniform, reducing the adverse effects of stranding on the original structure and properties of the individual wires, thereby reducing local strain concentration and fatigue damage accumulation during reciprocating bending, delaying the initiation and propagation of fatigue cracks, and improving the overall bending fatigue resistance of the stranded wire.
[0019] Therefore, the copper alloy wire harness prepared by this invention is suitable for electronic information communication wire harnesses that are frequently bent back and forth during use. It can be applied to folding parts of mobile phones, laptops, and other devices, as well as joint parts of industrial robots, collaborative robots, and humanoid robots. It can meet the high requirements of these parts for wire harness bending fatigue performance, strength, and conductivity. Detailed Implementation
[0020] The present invention will be further described in detail below with reference to the embodiments, but this should not be construed as limiting the invention in any way.
[0021] A method for preparing high-strength, bend-resistant copper alloy stranded wire includes the following steps: smelting, casting, solution treatment, hot rolling, intermediate drawing, aging treatment, finished product drawing, and stranding. The finished product drawing yields copper alloy single wires for stranding, and multiple copper alloy single wires are stranded into copper alloy stranded wire on a stranding machine. The copper alloy single wire comprises the following components by mass percentage: Cr 0.15~0.32%, Mg 0.08~0.16%, Ag 0.08~0.14%, B 0.003~0.007%, with the balance being Cu. Specific steps are as follows: S1. According to the composition of the copper alloy single wire, add cathode copper to the vacuum induction furnace and heat it until it melts; then add copper-chromium alloy, copper-magnesium alloy, metallic silver and copper-boron alloy in sequence and melt them into copper alloy liquid. S2, after the alloy is completely melted, it is refined under vacuum at 1100-1300℃ for 10-25 min, and low-frequency electromagnetic stirring is applied during the refining process; S3, after refining, protective gas is introduced to a slightly positive pressure for casting. During casting, continuous casting is carried out by downward continuous casting. The casting temperature is 1250±10℃, the downward speed is 2~5 mm / s, and the ingot is pulled out in the same direction as the direction of gravity, resulting in an alloy rod with a diameter of 20~40mm and an average grain size of 200~420 μm in the as-cast state. S4. The alloy rod is solution treated at 900±10℃ for 1~4h under a protective atmosphere, followed by water quenching. The average grain size of the alloy rod after solution treatment is 230~450 μm. S5, after solution treatment, the alloy rod is heated to 790±10℃ and hot rolled, and rolled into an alloy rod with a diameter of 6~10mm in 6-13 passes. The single-pass section reduction rate is 15~35%, and the final rolling temperature is controlled not to be lower than 650℃. The average grain size of the hot-rolled alloy rod is 20~80μm. S6, the hot-rolled alloy rod is drawn in multiple passes at room temperature to obtain an alloy rod with a preset diameter, wherein the deformation amount per pass is 10~20%, and the average grain size of the obtained alloy rod is 2~10μm; S7. The alloy rod of the preset diameter is kept at 450±10℃ for 1~4h for intermediate aging. After intermediate aging, the average grain size of the alloy rod is 4-20μm. S8, the aged alloy rod is drawn at room temperature until a copper alloy single wire of the target diameter is obtained; the drawing process includes multiple passes, with a deformation of 10-20% per pass, and the average grain size of the obtained copper alloy single wire is 0.4-2 μm, and the internal stress is 200-300 MPa. S9 involves stranding multiple copper alloy single wires into copper alloy stranded wire on a stranding machine. The stranding rate is controlled at 100~300m / min, the pitch ratio is controlled at 35~50, and the single wire tension is controlled at 0.2~1.5 N. No additional annealing is performed after stranding.
[0022] The strength and bending fatigue resistance of copper alloys are determined by their microstructure, which is the result of the synergistic effect of composition and thermomechanical processing. Cr relies on high-temperature solid solution and room-temperature microsolubility differences to achieve aging precipitation strengthening, but the size and distribution of the precipitates are highly dependent on the precise control of the solution, quenching, and aging processes. Mg segregates at the precipitate interface to inhibit Cr phase coarsening, Ag provides solid solution strengthening with minimal impact on conductivity, and trace amounts of B improve hot workability through grain boundary segregation. The effectiveness of these alloying effects is also constrained by the matching of melt homogeneity, hot rolling recrystallization behavior, and cold deformation. For thin-diameter conductors, fatigue cracks often initiate in areas of coarse grains, intergranular continuous precipitation, or residual stress concentration introduced by drawing / stranding. Therefore, by systematically coordinating the composition formulation with parameters across all processes—melting, casting, solution treatment, hot rolling, cold drawing, intermediate aging, finished product drawing, and stranding—and implementing gradient control of grain size and internal stress at each stage, high strength and long fatigue life can be achieved simultaneously while ensuring conductivity.
[0023] To characterize the comprehensive performance of copper alloy single wires and their stranded wire bundles obtained within the alloy composition and process parameters defined in this application, the present invention tests their tensile properties, electrical conductivity, and torsional properties according to GB / T4909.3-2009, GB / T3048.4-2025, and GB / T239.1-2023, respectively. Simultaneously, a reciprocating bending test is performed on the stranded wire bundles. Under normal temperature conditions, one end of the sample is fixed, a constant load of 9.8 N is applied to the free end, and the bundles are bent 90° in both the forward and reverse directions along a cylindrical surface of a specified radius, repeated until the bundle breaks. The number of bending cycles is recorded. Test results show that, within the range of alloy composition and preparation process parameters specified in this application, the tensile strength of the obtained copper alloy single wire is 610–640 MPa, the electrical conductivity is 81–82% IACS, and the torsion cycles are 30–40 revolutions; after the copper alloy single wire is stranded to form a wire bundle, its tensile strength is 585–625 MPa, the breaking force is 170–200 N, and the bending resistance under normal temperature and 9.8 N load conditions is 290,000–350,000 cycles.
[0024] Example 1
[0025] In this embodiment, the copper alloy single wire composition includes the following preferred components by mass percentage: Cr 0.22%, Mg 0.14%, Ag 0.10%, B 0.005%, with the balance being copper.
[0026] A method for preparing a high-strength, bend-resistant copper alloy stranded wire, the specific steps of which are as follows: S1. According to the preferred composition of the copper alloy single wire, cathode copper is added to the vacuum induction furnace and heated until it melts; Cu-10Cr master alloy, Cu-20Mg master alloy, metallic silver and Cu-5B master alloy are added in sequence and melted into copper alloy liquid. S2, after the alloy is completely melted, it is refined under vacuum at 1200±10℃ for 15±5min, and low-frequency electromagnetic stirring is applied during the refining process. The stirring frequency is 20±2Hz, the current is 200±10A, the stirring time is 15±2min, and the direction is changed once every 30±1s. S3, after refining, is filled with high-purity argon gas (purity ≥99.999%) to a slight positive pressure of 0.03~0.05 MPa for casting. The casting is carried out by continuous casting using a downward drawing method. The casting temperature is 1250±10℃, the downward drawing speed is 4±0.01 mm / s, and the ingot is pulled out in the same direction as the direction of gravity, resulting in an alloy rod with a diameter of 30±0.1mm and an average grain size of 260±10 μm in the as-cast state. S4. The alloy rod was solution treated at 900±10℃ for 2±0.1h under a high-purity argon protective atmosphere, followed by water quenching. The average grain size of the alloy rod after solution treatment was 290±15 μm. S5, the solution-treated alloy rod is heated to 790±10℃ and hot-rolled in 9 passes to an alloy rod with a diameter of 8mm. The section reduction rates of each pass are 24%, 25%, 26%, 27%, 27%, 27%, 27%, 27% and about 18.7% respectively. The final rolling temperature is not lower than 670±10℃. The average grain size of the hot-rolled alloy rod is 50±10μm. S6, the hot-rolled alloy rod is drawn in 32 passes at room temperature to obtain an alloy rod with a preset diameter of 0.6 mm, wherein the deformation amount per pass is 15%, and the average grain size of the resulting alloy rod is 8±1 μm; S7, an alloy rod with a diameter of 0.6 mm was held at 450±10℃ for 2±0.1 h for intermediate aging. After intermediate aging, the average grain size of the alloy rod was 14±1.5 μm. S8, the aged alloy rod is drawn at room temperature until a copper alloy single wire with a target diameter of 0.1 mm is obtained; the drawing process includes 22 passes, with a deformation of 15% per pass, and the average grain size of the obtained copper alloy single wire is 0.6±0.1 μm, and the internal stress is 241±13 MPa. S9 involves stranding 40 copper alloy single wires into a copper alloy stranded wire on a stranding machine. The stranding rate is controlled at 180±10m / min, the pitch ratio is controlled at 40, and the single wire tension is controlled at 1.2±0.05 N. No additional annealing is performed after stranding.
[0027] The main technical specifications of the copper alloy single wire and stranded wire prepared in this embodiment are shown in Table 1 and Table 2, respectively.
[0028]
[0029]
[0030] Comparative Example 1: This comparative example uses conventional pure copper 0.1mm single wire as the comparison material. 40 / 0.1mm pure copper stranded wire was prepared using the same single wire diameter, number of single wires and stranding method as in Example 1. The main technical indicators of the pure copper single wire and stranded wire obtained in this comparative example are shown in Table 3 and Table 4, respectively.
[0031]
[0032]
[0033] As shown in Tables 1 and 3, under the same single-wire diameter, the tensile strength of the copper alloy single wire obtained in Example 1 is 625 MPa, which is about 83.8% higher than that of the pure copper single wire (340 MPa); the bending and torsion cycles increased from 21 revolutions to 35 revolutions, an increase of about 66.7%. Meanwhile, the conductivity of the single wire in Example 1 reached 81.5% IACS, indicating that the present invention maintains high conductivity while improving strength and deformation resistance.
[0034] As shown in Tables 2 and 4, under the same 40 / 0.1mm stranded wire structure and 9.8 N room temperature load conditions, the tensile strength of the stranded wire in Example 1 is 602 MPa, the breaking force is 187 N, and the number of bending cycles reaches 323,000. Compared with pure copper stranded wire, the tensile strength of the stranded wire in Example 1 is increased by about 91.1%, the breaking force is increased by about 82.6%, and the number of bending cycles is increased by about 127.5%, indicating that the copper alloy stranded wire prepared by this invention has good strength and bending fatigue resistance.
[0035] Comparative Example 2: This comparative example uses a conventional binary copper-tin alloy (Cu-0.35Sn) 0.1mm single wire as the comparison material, and prepares 40 / 0.1 mm copper-tin alloy stranded wire using the same single wire diameter, number of single wires and stranding method as in Example 1. The main technical indicators of the copper-tin alloy single wire and stranded wire obtained in this comparative example are shown in Table 5 and Table 6, respectively.
[0036]
[0037]
[0038] As shown in Tables 1 and 5, under the same single-wire diameter, the tensile strength of the copper alloy obtained in Example 1 is 625 MPa, which is lower than the 730 MPa of the Cu-0.35Sn alloy in Comparative Example 2. However, its conductivity increased from 76.8% IACS to 81.5% IACS, an increase of approximately 6.1%, and the number of bending and torsion cycles increased from 24 to 35, an increase of approximately 45.8%. This indicates that the present invention, through precipitation strengthening and microstructure control, further balances conductivity and deformation resistance while maintaining a high strength level.
[0039] As shown in Tables 2 and 6, under the same 40 / 0.1mm stranded wire structure and a room temperature load of 9.8 N, the copper alloy stranded wire obtained in Example 1 achieved a bending resistance of 323,000 cycles, which is approximately 81.5% higher than the 178,000 cycles of the Cu-0.35Sn alloy stranded wire in Comparative Example 2. The tensile strength of the stranded wire in Example 1 was 602 MPa, and the breaking force was 187 N, lower than the 702 MPa and 218 N of Comparative Example 2, but still maintaining a high strength level. In summary, the copper alloy stranded wire obtained in this invention exhibits a good overall balance between electrical conductivity and bending fatigue resistance.
[0040] The above embodiments are only used to illustrate the technical solutions of the present invention and are not intended to limit it. Those skilled in the art should understand that modifications or equivalent substitutions can be made to the specific implementation of the present invention with reference to the above embodiments. Any modifications or equivalent substitutions that do not depart from the spirit and scope of the present invention are within the protection scope of the pending claims.
Claims
1. A method for preparing a high-strength, bend-resistant copper alloy stranded wire, characterized in that, The process includes smelting, casting, solution treatment, hot rolling, intermediate drawing, aging treatment, finished product drawing, and stranding; wherein the copper alloy single wire obtained after finished product drawing for stranding comprises the following components by mass percentage: Cr 0.15~0.32%, Mg 0.08~0.16%, Ag 0.08~0.14%, B 0.003~0.007%, with the balance being Cu; During the casting process, continuous casting is carried out by the downward continuous casting method. The casting temperature is 1250±10℃, the downward speed is 2~5mm / s, the ingot is pulled out in the same direction as the gravity direction, and an alloy rod with a diameter of 20~40mm is obtained. The average grain size in the as-cast state is 200~420μm. In the solution treatment, the cast alloy rod is held at 900±10℃ for 1~4h under a protective atmosphere, followed by water quenching, and the average grain size after solution treatment is controlled to be 230~450μm. During the hot rolling process, the heating temperature is 790±10℃, the rolling passes are 6~13, the section shrinkage rate per pass is 15~35%, the final rolling temperature is controlled not lower than 650℃, the average grain size of the alloy rod after hot rolling is 20~80 μm, and the diameter of the alloy rod is 6~10mm. During the intermediate drawing process, the alloy rod is drawn in multiple passes at room temperature, with a single pass deformation of 10-20%, and the alloy rod is drawn to the preset diameter. The average grain size of the alloy rod is 2-10 μm. In the aging treatment, the alloy rod with a preset diameter is placed at 450±10℃ for 1~4h and the average grain size of the alloy rod after treatment is 4~20μm; In the finished product drawing process, the alloy rod is drawn in multiple passes at room temperature until the target diameter is reached. The deformation amount per pass is 10~20%, resulting in a copper alloy single wire with an average grain size of 0.4~2μm and an internal stress of 200~300MPa. During the stranding process, multiple copper alloy single wires of the target diameter are stranded into copper alloy stranded wire on a stranding machine. The stranding rate is controlled at 100~300m / min, the pitch ratio is controlled at 35~50, and the single wire tension is controlled at 0.2~1.5N.
2. The method for preparing high-strength, bend-resistant copper alloy stranded wire according to claim 1, characterized in that, During the smelting process, cathode copper is added to the vacuum induction furnace and heated until it melts; then copper-chromium alloy, copper-magnesium alloy, metallic silver and copper-boron alloy are added in sequence and melted into a copper alloy liquid; after the alloy is completely melted, it is refined at 1100-1300℃ under vacuum for 10-25 minutes, and low-frequency electromagnetic stirring is applied during the refining process.
3. The method for preparing high-strength, bend-resistant copper alloy stranded wire according to claim 2, characterized in that, The copper-chromium alloy is Cu-10Cr, the copper-magnesium alloy is Cu-20Mg, and the copper-boron alloy is Cu-5B.
4. The method for preparing high-strength, bend-resistant copper alloy stranded wire according to claim 1, characterized in that, During the casting process, the downward drawing rate is 4±0.01mm / s, the diameter of the cast alloy rod is 30±0.1mm, and the average grain size in the as-cast state is 260±10μm.
5. The method for preparing high-strength, bend-resistant copper alloy stranded wire according to claim 1, characterized in that, In the solution treatment, the protective atmosphere is high-purity argon, the holding time is 2±0.1h, and the average grain size after solution treatment is 290±15μm.
6. The method for preparing high-strength, bend-resistant copper alloy stranded wire according to claim 1, characterized in that, During the hot rolling process, the final rolling temperature is 670±10℃, and the average grain size of the alloy rod after hot rolling is 50±10μm.
7. The method for preparing high-strength, bend-resistant copper alloy stranded wire according to claim 1, characterized in that, The diameter of the alloy rod obtained after intermediate drawing is 0.6 mm, and the average grain size is 8 ± 1 μm.
8. The method for preparing high-strength, bend-resistant copper alloy stranded wire according to claim 7, characterized in that, The aging treatment time was 2±0.1h, and the average grain size after aging was 14±1.5μm.
9. The method for preparing high-strength, bend-resistant copper alloy stranded wire according to claim 8, characterized in that, The diameter of the copper alloy single wire obtained after drawing is 0.1 mm, the average grain size is 0.6 ± 0.1 μm, and the internal stress is 241 ± 13 MPa.
10. A high-strength, bend-resistant copper alloy stranded wire, characterized in that, The product is prepared by the preparation method according to any one of claims 1-9, wherein the tensile strength of the copper alloy single wire is 610-640 MPa, the electrical conductivity is 81-82% IACS, and the number of torsion cycles is 30-40 revolutions; the tensile strength of the copper alloy stranded wire is 585-625 MPa, the breaking force is 170-200 N, and the number of bending cycles under normal temperature and 9.8 N load conditions is 290,000-350,000.