A method for preparing a fire-resistant three-core 10kV steel tape armored cross-linked cable
By combining epoxy-functionalized phenylsiloxane and sulfonated graphene anchored zirconium amine carboxylic acid skeleton, the problems of insufficient fire resistance, flame retardancy and insulation performance of cables are solved, forming a multi-layer protection system and improving the overall fire protection capability and mechanical properties of cables.
Patent Information
- Application Number
- CN202611585973.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-10-14
- Publication Date
- 2026-11-17
AI Technical Summary
The fire resistance, flame retardancy, insulation, and mechanical properties of existing 10kV power cables need further improvement. Traditional flame retardants have poor compatibility with polyolefin matrices, graphene fillers are prone to agglomeration leading to material embrittlement and reduced insulation strength, and the synergistic effect between the outer sheath and the internal fire-resistant structure is insufficient.
The system employs a combination of epoxy-functionalized phenylsiloxane and sulfonated graphene anchored zirconium amine carboxylic acid skeleton. Through chemical bonding, it improves interfacial compatibility, inhibits graphene sheet stacking, and forms a continuous and dense carbon layer. Combined with a multi-layered refractory structure, it enhances overall fire resistance and protection. The outer sheath material is composed of polyethylene material, multi-element functional flame retardant, epoxy-functionalized phenylsiloxane, sulfonated graphene anchored zirconium amine carboxylic acid skeleton, and auxiliary additives, forming a multi-layered buffer protection system.
It significantly improves the halogen-free, low-smoke flame retardant rating of the cable, enhances its insulation and mechanical properties, ensures stable operation of the cable at a voltage level of 10kV, resists flame erosion and mechanical damage, and improves the cable's crack resistance.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] This invention relates to the field of power cable technology, specifically to a method for preparing a fire-resistant three-core 10kV steel tape armored cross-linked cable. Background Technology
[0002] As a key power transmission and distribution equipment in the power distribution network, the outer sheath of 10kV power cables plays an important role in protecting the internal structure of the cable from external environmental corrosion, providing flame retardancy and fire resistance, and insulation protection. Currently, polyethylene or polyvinyl chloride is often used as the matrix, and the performance is improved by adding functional fillers such as inorganic hydroxides, organophosphorus flame retardants, or graphene. Flame retardant modification mainly utilizes the thermal decomposition of fillers to release non-combustible gases or form a surface carbon layer to isolate oxygen and heat. Graphene, with its two-dimensional sheet structure, blocks heat conduction and smoke diffusion. In the overall cable structure, steel tape armor layer combined with fire-resistant materials such as mica tape is often used to construct a multi-layer protection system to enhance mechanical protection and fire resistance.
[0003] However, the above technologies still have certain limitations. Traditional flame retardants have poor compatibility with polyolefin matrices, and excessive incorporation can easily disrupt the continuity of the matrix, creating micropore defects at the interface. This weakens the mechanical properties of the sheath, such as tensile strength, elongation at break, and other properties, and also has an adverse effect on insulation performance. Graphene fillers are prone to stacking and agglomeration in the matrix due to the van der Waals forces between the layers, which can form stress concentration points that lead to material embrittlement and may also create local conductive paths that reduce insulation strength. In addition, relying solely on flame retardant modification of the outer sheath lacks effective synergy with the internal fire-resistant structure of the cable, and there is still room for improvement in the overall fire protection effect.
[0004] To address this technical deficiency, a solution is proposed. Summary of the Invention
[0005] The purpose of this invention is to provide a method for preparing a fire-resistant three-core 10kV steel tape armored cross-linked cable, which solves the technical problem that the fire resistance, flame retardancy, insulation performance and mechanical properties of cross-linked cables in the prior art need to be further improved.
[0006] The objective of this invention can be achieved through the following technical solution: a method for preparing a fire-resistant three-core 10kV steel-tape armored cross-linked cable, comprising the following steps:
[0007] S1. After the three cable cores are bundled together, filler material is placed between the conductor gaps, and then wrapping tape is used to wrap the cable to form a wrapping layer.
[0008] S2. After extruding and coating polyolefin on the outside of the wrapping layer to form an isolation layer, galvanized steel strip is used for armoring to form an armor layer. Then, composite mica tape is used to wrap the outside of the armor layer to form a protective layer.
[0009] S3. After the outer sheath material is extruded and wrapped around the outside of the protective layer, it is vulcanized and cross-linked to form an outer sheath layer, thus obtaining a fire-resistant three-core 10kV steel tape armored cross-linked cable. The outer sheath material is composed of polyethylene material, multi-element functional flame retardant, epoxy functionalized phenylsiloxane, sulfonated graphene anchored zirconium amine carboxylic acid skeleton and auxiliary additives.
[0010] Furthermore, in step S3, the multi-element functional flame retardant is prepared by the following steps:
[0011] A1. Under a nitrogen atmosphere, boron amino acid active ester is added to a reaction vessel containing anhydrous toluene. After stirring at 20-30℃ for 15-30 min, an anhydrous toluene solution of vanillin octyl silyl ether is added dropwise. After the addition is complete, stirring is continued at 20-30℃ for 1-2 h. Then, the temperature is first raised to 60-70℃ and reacted for 2-3 h, and then the temperature is further raised to 105-110℃ and reacted for 10-12 h. After the reaction is completed, the mixture is cooled to room temperature, filtered, and the filter cake is washed 2-3 times with anhydrous petroleum ether and then transferred to a vacuum drying oven and dried at 35-45℃ to constant weight to obtain a boron-silicon bifunctional Schiff base.
[0012] The reaction formula for preparing borosilicate bifunctional Schiff bases:
[0013]
[0014] In the formula:
[0015]
[0016] A2. Under a nitrogen atmosphere, a borosilicate bifunctional Schiff base is added to a reactor containing tetrahydrofuran and swelled at 20-30°C for 1-2 hours. Then, DOPO is added, and the mixture is stirred at 20-30°C for 40-60 minutes. The temperature is then raised to 60-65°C and refluxed for 10-12 hours. After the reaction is complete, the mixture is cooled to room temperature, filtered, and the filter cake is washed 2-3 times with anhydrous tetrahydrofuran. The cake is then transferred to a vacuum drying oven and dried to constant weight at 40-45°C and -0.09 MPa vacuum to obtain a multi-element functional flame retardant.
[0017] The reaction formula for preparing multi-element functional flame retardants:
[0018]
[0019] In the formula:
[0020]
[0021] Further, in step A1, the ratio of the amount of boron amino active ester, anhydrous toluene, and vanillin octyl silyl ether in anhydrous toluene solution is 1g:10-12mL:12.5-13.5mL, and the mass fraction of the vanillin octyl silyl ether in anhydrous toluene solution is 25%; in step A2, the ratio of the amount of borosilicate bifunctional Schiff base, tetrahydrofuran, and DOPO is 1g:10-15mL:0.78g.
[0022] Further, in step A1, the preparation method of the vanillin octyl silyl ether is as follows: Under a nitrogen atmosphere, vanillin and triethylamine are added to a reaction vessel containing anhydrous tetrahydrofuran. After stirring at 0-5°C for 15-20 min, a dichloromethyloctylsilane tetrahydrofuran solution is added dropwise. After the addition is complete, stirring continues at 0-5°C for 20-30 min. Then, the temperature is first raised to 20-30°C and reacted for 2-4 h, followed by further heating to 45-55°C and reacting for 2-3 h. After the reaction is complete, the mixture is cooled to room temperature, filtered, and the filtrate is... After removing the solvent by vacuum distillation at 0-40℃, the product is transferred to petroleum ether for static chromatography and filtration. The product is washed 2-3 times with petroleum ether and then transferred to a vacuum drying oven and dried to constant weight at 35-45℃ and -0.09MPa vacuum to obtain vanillin octyl silane. The ratio of vanillin, triethylamine, anhydrous tetrahydrofuran, and dichloromethyloctylsilane tetrahydrofuran solution is 1g:0.96mL:8-10mL:2.6-2.8mL, and the mass fraction of dichloromethyloctylsilane tetrahydrofuran solution is 30%.
[0023] The reaction formula for preparing vanillin octyl silyl ether:
[0024]
[0025] The mass spectrometry data for vanillin octylsilyl ether are as follows: m / z: 472.23 (100.0%), 473.23 (33.8%), 474.23 (6.5%), 474.22 (3.4%), 475.23 (1.2%).
[0026] The HNMR data for vanillin octyl silyl ether are as follows: 1 H NMR (400 MHz, CDCl3) δ: 9.82 (s, 2H), 7.44 (d, 2H), 7.34 (dd, 2H), 6.92 (d, 2H), 3.91 (s, 6H), 1.20-1.40 (m, 14H), 0.88 (t, 3H), 0.62 (m, 2H), 0.12 (s, 3H).
[0027] Furthermore, the preparation method of the boron-ammonia active ester is as follows: under a nitrogen atmosphere, boric acid and 3-amino-1-propanol are added to a reaction vessel containing anhydrous toluene. After stirring at 20-30℃ for 10-20 min, the temperature is first raised to 70-80℃ and stirring is continued for 20-30 min. Then, the temperature is raised to 105-110℃ and refluxed for 10-12 h. After the reaction is completed, the mixture is cooled to room temperature and filtered. The filtrate is distilled under reduced pressure at 70-80℃ and 1-5 kPa for 3-4 h, and then transferred to a vacuum drying oven and vacuum dried at 50-60℃ for 12-15 h to obtain the boron-ammonia active ester. The ratio of boric acid, 3-amino-1-propanol and anhydrous toluene is 1 g: 3.6-3.7 g: 10-15 mL.
[0028] The reaction formula for preparing boron amino esters:
[0029]
[0030] The mass spectrometry data of the boron amino active ester are as follows: m / z: 233.19 (100.0%), 232.19 (24.8%), 234.19 (10.8%), 233.20 (2.5%), 235.20 (1.1%).
[0031] The HNMR data of the boron amino acid active ester are as follows: 1 H NMR (400 MHz, DMSO-d6) δ: 3.62 (t, J≈6.0 Hz, 6H, BO-CH2), 2.63 (t, J≈6.8 Hz, 6H, CH2-NH2), 1.64 (m, 6H, -OCH2-CH2-CH2NH2), 1.20~1.80 (br, 6H, -NH2).
[0032] Further, in step S3, the preparation method of the epoxy-functionalized phenylsiloxane is as follows: under a nitrogen atmosphere, 3-glycidyl etheroxypropyltrimethoxysilane, diphenylsilanediol and barium hydroxide are added to a reaction vessel, stirred for 10-15 min, and then heated to 70-80℃ at a rate of 2-3℃ / min, and kept at this temperature for 5-6 h. After the reaction is completed, the temperature is lowered to 50-60℃, filtered, and the filtrate is transferred to a vacuum drying oven and dried under a vacuum environment of 50-60℃ for 4-5 h to obtain the epoxy-functionalized phenylsiloxane; the ratio of the amount of 3-glycidyl etheroxypropyltrimethoxysilane, diphenylsilanediol and barium hydroxide is 18-19 mL: 27.5 g: 0.09 g.
[0033] The reaction formula for preparing epoxy-functionalized phenylsiloxanes:
[0034]
[0035] In the formula:
[0036]
[0037] Furthermore, in step S3, the sulfonated graphene-anchored zirconium amine carboxylic acid skeleton is prepared by the following steps:
[0038] B1. Graphene oxide is added to a reaction vessel containing anhydrous dimethyl sulfoxide and ultrasonically dispersed for 1-2 hours. Then, 1,4-butanesulfonate lactone is added and stirred for 20-30 minutes. Sodium hydroxide is then added and the temperature is increased to 100-105℃ at a rate of 2-3℃ / min. The reaction is carried out for 20-24 hours. After the reaction is completed, the mixture is cooled to room temperature and centrifuged. The product is washed 3-4 times with deionized water and anhydrous ethanol, respectively, and then transferred to a drying oven and dried at 70-80℃ to constant weight to obtain sulfonated graphene oxide.
[0039] B2. Diaminoterephthalic acid and zirconium tetrachloride were added to a reaction vessel containing N,N-dimethylformamide and ultrasonically dispersed for 40-60 min. Deionized water was then added and stirred for 10-20 min. Sulfonated graphene oxide was then added and stirred for 20-30 min. Glacial acetic acid was then added and stirred for another 10-20 min. The temperature was raised to 110-120℃ and the reaction was carried out for 20-24 h. After the reaction was completed, the product was centrifuged and washed 3-4 times with N,N-dimethylformamide and anhydrous methanol, respectively. The product was then transferred to a drying oven and dried at 60-70℃ to constant weight to obtain the sulfonated graphene-anchored zirconium amine carboxylic acid skeleton.
[0040] Further, in step B1, the ratio of graphene oxide, anhydrous dimethyl sulfoxide, 1,4-butanesulfonate lactone, and sodium hydroxide is 1g:700-800mL:9-11mL:1.8g; in step B2, the ratio of diaminoterephthalic acid, zirconium tetrachloride, N,N-dimethylformamide, deionized water, sulfonated graphene oxide, and glacial acetic acid is 1g:1.15-1.35g:100-150mL:0.8-1.2mL:0.2g:10mL.
[0041] Further, in step S3, the polyethylene material is obtained by uniformly mixing 60-68 parts of polyethylene, 20-26 parts of ethylene-vinyl acetate copolymer, and 6-10 parts of maleic anhydride-grafted polyethylene by weight; the auxiliary additive is obtained by uniformly mixing 1.0-1.6 parts of dicumyl peroxide, 0.3-0.5 parts of antioxidant 1010, 0.2-0.4 parts of zinc stearate, and 0.6-1.0 parts of polyethylene wax by weight.
[0042] Furthermore, in step S3, the ratio of polyethylene material, multi-element functional flame retardant, epoxy functionalized phenylsiloxane, sulfonated graphene anchored zirconium amine carboxylic acid skeleton and auxiliary additives is 86-104 parts by weight: 30-38 parts: 4-6 parts: 2-4 parts: 2.1-3.5 parts.
[0043] The present invention has the following beneficial effects:
[0044] 1. The epoxy-functionalized phenylsiloxane of this invention relies on epoxy active groups to construct an organic-inorganic interface link, promoting the uniform dispersion of flame-retardant functional components in the polyolefin matrix; the sulfonated graphene anchored zirconium amine carboxylic acid skeleton binds the graphene sheets with the zirconium amine carboxylic acid skeleton, inhibiting the stacking and aggregation of the sheets, and the zirconium metal sites inside the skeleton further catalyze the formation of the carbon layer. Each functional component achieves synergistic effect through elemental complementarity and special microstructure. During combustion, a continuous and dense barrier carbon layer can be rapidly generated to inhibit heat conduction diffusion and smoke release. At the same time, in conjunction with the multi-layer fire-resistant structure composed of the alkali-free glass fiber filling wrapping layer and the mica composite ceramicized silicone tape protective layer of the cable body, the outer sheath carbon layer and the inner fire-resistant protection structure of the cable work together to block the flame from eroding inward, effectively improving the halogen-free low-smoke flame-retardant rating of the cable and significantly enhancing the overall fire protection capability of the cable.
[0045] 2. The epoxy-functionalized phenylsiloxane of this invention improves the interfacial compatibility between the functional fillers and the polyolefin matrix through chemical bonding, reducing microscopic gaps at the interface between the two phases; the sulfonated graphene anchored zirconium amine carboxylic acid skeleton uses the zirconium amine carboxylic acid skeleton to anchor the graphene sheets, eliminating local conductive pathways induced by graphene agglomeration, reducing the number of insulation defect points inside the sheath, and the components work together to retain the inherent insulation properties of the polymer matrix to the greatest extent. In addition, relying on the inner insulation barrier formed by the peelable cross-linked polyethylene insulation layer and the water-blocking layer inside the cable, and with the galvanized steel tape armor layer to resist external mechanical damage, the insulation risks caused by sheath cracking due to external forces are reduced, and the breakdown voltage of the cable sheath is protected in a coordinated manner, so that the finished cable can stably adapt to the insulation operation conditions of the 10kV voltage level.
[0046] 3. In this invention, the epoxy groups of epoxy-functionalized phenylsiloxane can chemically bond with the matrix and various fillers, respectively, strengthening the interfacial bonding force between the two phases and alleviating the material embrittlement problem caused by the introduction of fillers; the porous zirconium amine carboxylic acid skeleton anchored by sulfonated graphene can transfer and disperse external loads, eliminate stress concentration points inside the material, and the substances work together to achieve flame retardant modification while retaining the mobility of polymer chain segments. Combined with the multi-layer buffer protection system composed of cable cabling filler, polyolefin isolation layer and steel tape armor layer, it weakens the direct impact of external loads on the sheath, optimizes the tensile stress, tensile strength and elongation at break of the sheath, improves the overall mechanical toughness of the cable outer sheath, and enhances the crack resistance of the cable during laying and service. Detailed Implementation
[0047] The technical solution of the present invention will be clearly and completely described below with reference to the embodiments. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.
[0048] In this application, the peelable crosslinked polyethylene is a commercially available material, model LLDPE 7120B;
[0049] In this application, the water-blocking tape is a commercially available material with a resistance of 1500Ω and the product number TF-BD138;
[0050] In this application, the steel strip is a commercially available material, model ZR-DJVP3VP3;
[0051] In this application, the alkali-free glass fiber filament is a commercially available material with a grade of 9-13 μm, a tensile strength of 1700 MPa, and an elastic modulus of 80 MPa.
[0052] In this application, the thickness of the alkali-free fiberglass tape is 0.20 mm, and its long-term temperature resistance is 300℃;
[0053] In this application, the polyolefin is a commercially available material with the grade NF358;
[0054] In this application, the galvanized steel strip is made of Q235B and has a thickness of 0.3mm;
[0055] In this application, the mica composite ceramicized silicone tape is a commercially available material with a flame retardant rating of UL94 and a breakdown voltage of 30kv / mm.
[0056] In this application, the polyethylene is a commercially available material, of type HDPE, and batch number 431-8;
[0057] In this application, the commercially available ethylene-vinyl acetate copolymer material is designated as UE630.
[0058] In this application, the maleic anhydride-grafted polyethylene is a commercially available material with the grade TY 1355 and the product number HH9160HYFXJ7.
[0059] In this application, the graphene oxide is a commercially available material with a specification of 1000 mesh and a model number of LG-1401.
[0060] Example 1
[0061] This embodiment provides a method for preparing a multi-element functional flame retardant, including the following steps:
[0062] Step I: Preparation of boron amino acid active ester
[0063] Under a nitrogen atmosphere, 200 g of boric acid and 720 g of 3-amino-1-propanol were weighed and added to a reaction vessel containing 2000 mL of anhydrous toluene. After stirring at 20 °C for 10 min, the temperature was first raised to 70 °C and stirring was continued for 20 min. Then, the temperature was raised to 105 °C and refluxed for 10 h. After the reaction was completed, the mixture was cooled to room temperature and filtered. The filtrate was distilled under reduced pressure at 70 °C and 1 kPa for 3 h and then transferred to a vacuum drying oven and dried under vacuum at 50 °C for 12 h to obtain boron-amino acid active ester.
[0064] Reaction mechanism for the preparation of boron amino active esters:
[0065] During the reaction, boric acid and 3-amino-1-propanol undergo a stepwise dehydration esterification reaction under reflux heating. The hydroxyl oxygen atom in 3-amino-1-propanol attacks the electron-deficient boron atom in boric acid to form a tetracoordinate borate ester intermediate. Subsequently, through proton transfer and dehydration, the hydroxyl groups on the boric acid molecule are successively replaced by 3-aminopropoxy groups, finally generating a boron amino active ester containing three 3-aminopropoxy substituents.
[0066] Step II: Preparation of vanillin octylsilyl ether
[0067] Under a nitrogen atmosphere, 100 g of vanillin and 96 mL of triethylamine were weighed and added to a reaction vessel containing 800 mL of anhydrous tetrahydrofuran. After stirring at 0 °C for 15 min, 260 mL of 30 wt% dichloromethyloctylsilane tetrahydrofuran solution was added dropwise. After the addition was complete, stirring was continued at 0 °C for 20 min. Then, the temperature was raised to 20 °C and reacted for 2 h, and then the temperature was raised to 45 °C and reacted for 2 h. After the reaction was completed, the mixture was cooled to room temperature and filtered. The filtrate was distilled under reduced pressure at 30 °C to remove the solvent, and then transferred to petroleum ether for static chromatography and filtration. The product was washed twice with petroleum ether and then transferred to a vacuum drying oven and dried to constant weight at 35 °C and -0.09 MPa vacuum to obtain vanillin octylsilyl ether.
[0068] Reaction mechanism for the preparation of vanillin octyl silyl ether:
[0069] During the reaction, vanillin and dichloromethyloctylsilane undergo a silylation reaction in the presence of triethylamine. The phenolic hydroxyl group in the vanillin molecule forms a more nucleophilic phenolic oxygen group under the basic action of triethylamine. Subsequently, the phenolic oxygen group attacks the silicon atom in dichloromethyloctylsilane, breaking the silicon-chlorine bond and forming a silicon-oxygen bond. The hydrogen chloride released during the reaction is captured by triethylamine to form a triethylamine salt, allowing two vanillin molecules to successively attach to the same methyloctylsilane center through the phenolic oxygen group, ultimately yielding vanillin octylsilane.
[0070] Step III: Preparation of borosilicate bifunctional Schiff bases
[0071] Under a nitrogen atmosphere, 100g of boron-ammonia active ester was weighed and added to a reaction vessel containing 1000mL of anhydrous toluene. After stirring at 20°C for 15min, 1250mL of anhydrous toluene solution of 25wt% vanillin octyl silyl ether was added dropwise. After the addition was complete, stirring was continued at 20°C for 1h. Then, the temperature was raised to 60°C and reacted for 2h, and then raised to 105°C and reacted for 10h. After the reaction was completed, the mixture was cooled to room temperature, filtered, and the filter cake was washed twice with anhydrous petroleum ether and then transferred to a vacuum drying oven and dried at 35°C to constant weight to obtain a boron-silicon bifunctional Schiff base.
[0072] Reaction mechanism for the preparation of borosilicate bifunctional Schiff bases:
[0073] During the reaction, boron amino ester and vanillin octyl silyl ether undergo a Schiff base condensation reaction through dropwise mixing and gradual heating. The amino group in the boron amino ester attacks the carbonyl carbon of the aldehyde group in vanillin octyl silyl ether to form an alkanolamine intermediate. Subsequently, carbon-nitrogen double bonds are generated through proton transfer and dehydration. Since the boron amino ester contains multiple amino groups and the vanillin octyl silyl ether contains multiple aldehyde groups, the condensation process proceeds continuously between molecules, allowing the boron-containing structural units and the silicon-containing structural units to be connected through imine bonds, ultimately yielding a boron-silicon bifunctional Schiff base.
[0074] Step IV: Preparation of multi-element functional flame retardants
[0075] Under a nitrogen atmosphere, 100g of borosilicate bifunctional Schiff base was weighed and added to a reactor containing 1000mL of tetrahydrofuran. The mixture swelled at 20°C for 1 hour. Then, 78g of DOPO was added. The mixture was stirred at 20°C for 40 minutes, then heated to 60°C and refluxed for 10 hours. After the reaction was completed, the mixture was cooled to room temperature, filtered, and the filter cake was washed twice with anhydrous tetrahydrofuran. The cake was then transferred to a vacuum drying oven and dried to constant weight at 40°C and -0.09MPa vacuum to obtain a multi-element functional flame retardant.
[0076] Reaction mechanism for preparing multi-element functional flame retardants:
[0077] During the reaction, the borosilicate bifunctional Schiff base, after swelling, undergoes an imine addition reaction with 9,10-dihydro-9-oxa-10-phosphenanthrene-10-oxide under stirring and reflux conditions. In this reaction, the phosphorus atom in the phosphine hydrogen bond attacks the imine carbon atom in the Schiff base structure, causing the imine carbon-nitrogen double bond to open and undergo proton transfer. This transforms the original imine bond into a phosphorus-substituted carbon-nitrogen single bond, thereby grafting the phosphenanthrene oxide structure onto the boron- and silicon-containing molecular framework, ultimately yielding a multi-element functional flame retardant.
[0078] Example 2
[0079] This embodiment provides a method for preparing a multi-element functional flame retardant, including the following steps:
[0080] Step I: Preparation of boron amino acid active ester
[0081] Under a nitrogen atmosphere, 200 g of boric acid and 740 g of 3-amino-1-propanol were weighed and added to a reaction vessel containing 3000 mL of anhydrous toluene. After stirring at 30 °C for 20 min, the temperature was first raised to 80 °C and stirred for another 30 min, then raised to 110 °C and refluxed for 12 h. After the reaction was completed, the mixture was cooled to room temperature and filtered. The filtrate was then distilled under reduced pressure at 80 °C and 5 kPa for 4 h, and then transferred to a vacuum drying oven and dried under vacuum at 60 °C for 15 h to obtain boron-amino acid active ester.
[0082] Step II: Preparation of vanillin octylsilyl ether
[0083] Under a nitrogen atmosphere, 100 g of vanillin and 96 mL of triethylamine were weighed and added to a reaction vessel containing 1000 mL of anhydrous tetrahydrofuran. After stirring at 5 °C for 20 min, 280 mL of 30 wt% dichloromethyloctylsilane tetrahydrofuran solution was added dropwise. After the addition was complete, stirring was continued at 5 °C for 30 min. Then, the temperature was raised to 30 °C and reacted for 4 h, followed by further heating to 55 °C and reacting for 3 h. After the reaction was completed, the mixture was cooled to room temperature and filtered. The filtrate was then distilled under reduced pressure at 40 °C to remove the solvent, transferred to petroleum ether, and allowed to stand for chromatography and filtration. The product was washed three times with petroleum ether and then transferred to a vacuum drying oven and dried to constant weight at 45 °C and -0.09 MPa vacuum to obtain vanillin octylsilyl ether.
[0084] Step III: Preparation of borosilicate bifunctional Schiff bases
[0085] Under a nitrogen atmosphere, 100g of boron-ammonia active ester was weighed and added to a reaction vessel containing 1200mL of anhydrous toluene. After stirring at 30℃ for 30min, 1350mL of anhydrous toluene solution of 25wt% vanillin octyl silyl ether was added dropwise. After the addition was complete, stirring was continued at 30℃ for 2h. Then, the temperature was raised to 70℃ and reacted for 3h, and then the temperature was raised to 110℃ and reacted for 12h. After the reaction was completed, the mixture was cooled to room temperature, filtered, and the filter cake was washed three times with anhydrous petroleum ether and then transferred to a vacuum drying oven and dried at 45℃ to constant weight to obtain a boron-silicon bifunctional Schiff base.
[0086] Step IV: Preparation of multi-element functional flame retardants
[0087] Under a nitrogen atmosphere, 100g of borosilicate bifunctional Schiff base was weighed and added to a reactor containing 1500mL of tetrahydrofuran. The mixture swelled at 30℃ for 2h, followed by the addition of 78g of DOPO. The mixture was first stirred at 30℃ for 60min, then heated to 65℃ and refluxed for 12h. After the reaction was completed, the mixture was cooled to room temperature, filtered, and the filter cake was washed three times with anhydrous tetrahydrofuran. The cake was then transferred to a vacuum drying oven and dried to constant weight at 45℃ and -0.09MPa vacuum to obtain a multi-element functional flame retardant.
[0088] Example 3
[0089] This embodiment provides a method for preparing a multi-element functional flame retardant, including the following steps:
[0090] Step I: Preparation of boron amino acid active ester
[0091] Under a nitrogen atmosphere, 200 g of boric acid and 730 g of 3-amino-1-propanol were weighed and added to a reaction vessel containing 2500 mL of anhydrous toluene. After stirring at 25 °C for 15 min, the temperature was first raised to 75 °C and stirred for another 25 min, then raised to 105 °C and refluxed for 11 h. After the reaction was completed, the mixture was cooled to room temperature and filtered. The filtrate was then distilled under reduced pressure at 75 °C and 3 kPa for 3.5 h, and then transferred to a vacuum drying oven and dried under vacuum at 55 °C for 14 h to obtain boron-amino acid active ester.
[0092] Step II: Preparation of vanillin octylsilyl ether
[0093] Under a nitrogen atmosphere, 100 g of vanillin and 96 mL of triethylamine were weighed and added to a reaction vessel containing 900 mL of anhydrous tetrahydrofuran. After stirring at 3 °C for 18 min, 270 mL of 30 wt% dichloromethyloctylsilane tetrahydrofuran solution was added dropwise. After the addition was complete, stirring was continued at 3 °C for 25 min. Then, the temperature was raised to 25 °C and reacted for 3 h, followed by further heating to 50 °C and reacting for 2.5 h. After the reaction was completed, the mixture was cooled to room temperature, filtered, and the filtrate was distilled under reduced pressure at 35 °C to remove the solvent. The filtrate was then transferred to petroleum ether for static chromatography and filtration. The product was washed three times with petroleum ether and then transferred to a vacuum drying oven and dried to constant weight at 40 °C and -0.09 MPa vacuum to obtain vanillin octylsilyl ether.
[0094] Step III: Preparation of borosilicate bifunctional Schiff bases
[0095] Under a nitrogen atmosphere, 100g of boron-ammonia active ester was weighed and added to a reaction vessel containing 1100mL of anhydrous toluene. After stirring at 25°C for 25min, 1300mL of anhydrous toluene solution of 25wt% vanillin octyl silyl ether was added dropwise. After the addition was complete, stirring was continued at 25°C for 1.5h. Then, the temperature was raised to 65°C and reacted for 2.5h, and then raised to 105°C and reacted for 11h. After the reaction was completed, the mixture was cooled to room temperature, filtered, and the filter cake was washed three times with anhydrous petroleum ether and then transferred to a vacuum drying oven and dried at 40°C to constant weight to obtain a boron-silicon bifunctional Schiff base.
[0096] Step IV: Preparation of multi-element functional flame retardants
[0097] Under a nitrogen atmosphere, 100g of borosilicate bifunctional Schiff base was weighed and added to a reactor containing 1250mL of tetrahydrofuran. The mixture swelled at 25°C for 1.5h. Then, 78g of DOPO was added. The mixture was stirred at 25°C for 50min, then heated to 60°C and refluxed for 11h. After the reaction was completed, the mixture was cooled to room temperature, filtered, and the filter cake was washed three times with anhydrous tetrahydrofuran. The cake was then transferred to a vacuum drying oven and dried to constant weight at 40°C and -0.09MPa vacuum to obtain a multi-element functional flame retardant.
[0098] Example 4
[0099] This embodiment provides a method for preparing a sulfonated graphene-anchored zirconium amine carboxylic acid skeleton, comprising the following steps:
[0100] Step i: Preparation of sulfonated graphene oxide
[0101] Weigh 10g of graphene oxide and add it to a reaction vessel containing 7000mL of anhydrous dimethyl sulfoxide. After ultrasonic dispersion for 1h, add 90mL of 1,4-butanesulfonate lactone and stir for 20min. Then add 18g of sodium hydroxide and heat to 100℃ at a rate of 2℃ / min for 20h. After the reaction is completed, cool to room temperature and centrifuge. Wash the product three times with deionized water and anhydrous ethanol, respectively, and then transfer it to a drying oven and dry it at 70℃ to constant weight to obtain sulfonated graphene oxide.
[0102] Reaction mechanism for the preparation of sulfonated graphene oxide:
[0103] During the reaction, oxygen-containing active groups such as hydroxyl groups on the surface of graphene oxide are activated in the alkaline environment formed by sodium hydroxide, forming nucleophilic oxygen anion sites. These oxygen anion sites attack the cyclic sulfonate structure of 1,4-butanesulfonate lactone, causing 1,4-butanesulfonate lactone to undergo a nucleophilic ring-opening reaction. The butyl sulfonate segments are then grafted onto the surface of the graphene oxide sheets via ether bonds, thereby obtaining sulfonated graphene oxide with butyl sulfonate structures on its surface.
[0104] Step ii: Preparation of sulfonated graphene-anchored zirconium amine carboxylic acid skeleton
[0105] Weigh 20g of diaminoterephthalic acid and 23g of zirconium tetrachloride and add them to a reactor containing 2000mL of N,N-dimethylformamide. After ultrasonic dispersion for 40min, add 16mL of deionized water and stir for 10min. Then add 4g of sulfonated graphene oxide and stir for 20min. Add 200mL of glacial acetic acid and continue stirring for 10min. Heat to 110℃ and react for 20h. After the reaction is complete, centrifuge and wash the product three times with N,N-dimethylformamide and anhydrous methanol, respectively. Transfer to a drying oven and dry at 60℃ to constant weight to obtain the sulfonated graphene anchored zirconium amine carboxylic acid skeleton.
[0106] Reaction mechanism for preparing sulfonated graphene anchored zirconium amine carboxylic acid skeleton:
[0107] During the reaction, zirconium tetrachloride undergoes hydrolysis and hydroxylation in deionized water to form a zirconium oxide cluster precursor containing zirconium hydroxyl groups and zirconium oxide bonds. Subsequently, the zirconium oxide cluster precursor undergoes a carboxylate coordination assembly reaction with the carboxyl group in diaminoterephthalic acid to form an amino-substituted zirconium carboxylic acid skeleton. At the same time, the sulfonate groups, hydroxyl groups, and carboxyl groups on the surface of sulfonated graphene oxide undergo a coordination anchoring reaction with the zirconium sites in the zirconium oxide cluster precursor or the zirconium carboxylic acid skeleton, causing the zirconium carboxylic acid skeleton to be generated in situ on the surface of sulfonated graphene oxide, resulting in a sulfonated graphene-anchored zirconium amine carboxylic acid skeleton.
[0108] Example 5
[0109] This embodiment provides a method for preparing a sulfonated graphene-anchored zirconium amine carboxylic acid skeleton, comprising the following steps:
[0110] Step i: Preparation of sulfonated graphene oxide
[0111] Weigh 10g of graphene oxide and add it to a reaction vessel containing 8000mL of anhydrous dimethyl sulfoxide. After ultrasonic dispersion for 2h, add 110mL of 1,4-butanesulfonate lactone and stir for 30min. Then add 18g of sodium hydroxide and heat to 105℃ at a rate of 3℃ / min for 24h. After the reaction is completed, cool to room temperature and centrifuge. Wash the product four times with deionized water and anhydrous ethanol, respectively, and then transfer it to a drying oven and dry it at 80℃ to constant weight to obtain sulfonated graphene oxide.
[0112] Step ii: Preparation of sulfonated graphene-anchored zirconium amine carboxylic acid skeleton
[0113] Weigh 20g of diaminoterephthalic acid and 27g of zirconium tetrachloride and add them to a reaction vessel containing 3000mL of N,N-dimethylformamide. After ultrasonic dispersion for 60min, add 24mL of deionized water and stir for 20min. Then add 4g of sulfonated graphene oxide and stir for 30min. Add 200mL of glacial acetic acid and continue stirring for 20min. Heat to 120℃ and react for 24h. After the reaction is complete, centrifuge and wash the product four times with N,N-dimethylformamide and anhydrous methanol. Transfer to a drying oven and dry at 70℃ to constant weight to obtain the sulfonated graphene anchored zirconium amine carboxylic acid skeleton.
[0114] Example 6
[0115] This embodiment provides a method for preparing a sulfonated graphene-anchored zirconium amine carboxylic acid skeleton, comprising the following steps:
[0116] Step i: Preparation of sulfonated graphene oxide
[0117] Weigh 10g of graphene oxide and add it to a reaction vessel containing 7500mL of anhydrous dimethyl sulfoxide. After ultrasonic dispersion for 1.5h, add 100mL of 1,4-butanesulfonate lactone and stir for 25min. Then add 18g of sodium hydroxide and heat to 100℃ at a rate of 2℃ / min for 22h. After the reaction is completed, cool to room temperature and centrifuge. Wash the product four times with deionized water and anhydrous ethanol, respectively, and then transfer it to a drying oven and dry it at 75℃ to constant weight to obtain sulfonated graphene oxide.
[0118] Step ii: Preparation of sulfonated graphene-anchored zirconium amine carboxylic acid skeleton
[0119] Weigh 20g of diaminoterephthalic acid and 25g of zirconium tetrachloride and add them to a reactor containing 2500mL of N,N-dimethylformamide. After ultrasonic dispersion for 50min, add 20mL of deionized water and stir for 15min. Then add 4g of sulfonated graphene oxide and stir for 25min. Add 200mL of glacial acetic acid and continue stirring for 15min. Heat to 115℃ and react for 22h. After the reaction is complete, centrifuge and wash the product four times with N,N-dimethylformamide and anhydrous methanol. Transfer to a drying oven and dry at 65℃ to constant weight to obtain the sulfonated graphene anchored zirconium amine carboxylic acid skeleton.
[0120] Example 7
[0121] This embodiment provides a method for preparing a fire-resistant three-core 10kV steel tape armored cross-linked cable, including the following steps:
[0122] Step 1: Conductor Forming
[0123] 36 copper wires are twisted together by a stranding machine to obtain copper stranded wire. The outside of the copper stranded wire is covered with peelable cross-linked polyethylene to form an insulation layer with a thickness of 5.0 mm. Then, water-blocking tape is continuously and evenly wrapped around the outside of the shielding layer to form a water-blocking layer. Then, steel tape is continuously and evenly wrapped around the outside of the water-blocking layer to form a steel tape shielding layer.
[0124] Three groups of conductors covered by steel strip shielding layers are cabled in a right-hand direction. Alkali-free glass fiber filaments are filled into the gaps between the conductors, and alkali-free glass fiber tape is used to continuously and evenly wrap the filling material and conductors to form a wrapping layer on the outside of the filling material.
[0125] Polyolefin is melted, extruded, and continuously and evenly coated onto the outside of the wrapping layer to form an isolation layer with a thickness of 4.5 mm. Galvanized steel strip is continuously and evenly coated onto the outside of the isolation layer to form an armor layer. Finally, mica composite ceramicized silicone tape is wrapped onto the outside of the armor layer to form a protective layer.
[0126] Step 2: Preparation of epoxy-functionalized phenylsiloxanes
[0127] Under a nitrogen atmosphere, 180 mL of 3-glycidyl etheroxypropyltrimethoxysilane, 275 g of diphenylsilanediol, and 0.9 g of barium hydroxide were weighed and added to a reaction vessel. After stirring for 10 min, the temperature was increased to 70 °C at a rate of 2 °C / min and maintained at this temperature for 5 h. After the reaction was completed, the temperature was lowered to 50 °C, filtered, and the filtrate was transferred to a vacuum drying oven and dried under vacuum at 50 °C for 4 h to obtain epoxy-functionalized phenylsiloxane.
[0128] Reaction mechanism for the preparation of epoxy-functionalized phenylsiloxanes:
[0129] During the reaction, the siloxy group in 3-glycidyl etheroxypropyltrimethoxysilane undergoes a methanol removal condensation reaction with the silanol in diphenylsilanediol to generate a siloxane bond. With the continuous condensation between the siloxy group and the silanol, the glycidyl etheroxypropylsiloxane unit and the diphenylsiloxane unit are connected by siloxane bonds and gradually form a branched siloxane structure, in which the epoxy group is retained on the organic side chain, and finally an epoxy-functionalized phenylsiloxane containing epoxy side groups and phenyl substituents is obtained.
[0130] Step 3: Preparation of premix
[0131] 60 parts of polyethylene, 20 parts of ethylene-vinyl acetate copolymer, and 6 parts of maleic anhydride-grafted polyethylene were mixed evenly to obtain a polyethylene material.
[0132] 1.0 part of dicumyl peroxide, 0.3 part of antioxidant 1010, 0.2 part of zinc stearate and 0.6 part of polyethylene wax were mixed evenly to obtain the auxiliary additive;
[0133] Weigh out the following by weight: 86 parts of polyethylene material, 30 parts of the multi-element functional flame retardant prepared in Example 1, 4 parts of epoxy functionalized phenylsiloxane, 2 parts of the sulfonated graphene anchored zirconium amine carboxylic acid skeleton prepared in Example 4, and 2.1 parts of auxiliary additives. Add them to a high-speed mixer and premix for 10 minutes at 80°C and 600 r / min to obtain a premix.
[0134] Step 4: Preparation of fire-resistant three-core 10kV steel tape armored cross-linked cable
[0135] The premixed material is fed into a twin-screw extruder. The twin-screw extruder has six temperature zones set from the feed end towards the die head, with temperatures of 145℃, 150℃, 155℃, 155℃, 150℃, and 150℃ respectively. The screw speed is 60 r / min. After melting and plasticizing, the material is extruded and coated onto the outside of the protective layer, forming an outer sheath layer with a thickness of 3.0 mm. Then, the coated cable is sent into a closed hot air vulcanizing furnace at 180℃ for 10 minutes of heat preservation and vulcanization. After that, it is cooled and shaped by passing through a 70℃ hot water section and a 25℃ cold water section. Finally, it is pulled and wound to obtain a fire-resistant three-core 10kV steel tape armored cross-linked cable.
[0136] Example 8
[0137] This embodiment provides a method for preparing a fire-resistant three-core 10kV steel tape armored cross-linked cable, including the following steps:
[0138] Step 1: Conductor Forming
[0139] 36 copper wires are twisted together by a stranding machine to obtain copper stranded wire. The outside of the copper stranded wire is covered with peelable cross-linked polyethylene to form an insulation layer with a thickness of 5.0 mm. Then, water-blocking tape is continuously and evenly wrapped around the outside of the shielding layer to form a water-blocking layer. Then, steel tape is continuously and evenly wrapped around the outside of the water-blocking layer to form a steel tape shielding layer.
[0140] Three groups of conductors covered by steel strip shielding layers are cabled in a right-hand direction. Alkali-free glass fiber filaments are filled into the gaps between the conductors, and alkali-free glass fiber tape is used to continuously and evenly wrap the filling material and conductors to form a wrapping layer on the outside of the filling material.
[0141] Polyolefin is melted, extruded, and continuously and evenly coated onto the outside of the wrapping layer to form an isolation layer with a thickness of 4.5 mm. Galvanized steel strip is continuously and evenly coated onto the outside of the isolation layer to form an armor layer. Finally, mica composite ceramicized silicone tape is wrapped onto the outside of the armor layer to form a protective layer.
[0142] Step 2: Preparation of epoxy-functionalized phenylsiloxanes
[0143] Under a nitrogen atmosphere, 190 mL of 3-glycidyl etheroxypropyltrimethoxysilane, 275 g of diphenylsilanediol, and 0.9 g of barium hydroxide were weighed and added to a reaction vessel. After stirring for 15 min, the temperature was increased to 80 °C at a rate of 3 °C / min and maintained for 6 h. After the reaction was completed, the temperature was lowered to 60 °C, filtered, and the filtrate was transferred to a vacuum drying oven and dried under vacuum at 60 °C for 5 h to obtain epoxy-functionalized phenylsiloxane.
[0144] Step 3: Preparation of premix
[0145] 68 parts of polyethylene, 26 parts of ethylene-vinyl acetate copolymer, and 10 parts of maleic anhydride-grafted polyethylene were mixed evenly to obtain a polyethylene material.
[0146] 1.6 parts of dicumyl peroxide, 0.5 parts of antioxidant 1010, 0.4 parts of zinc stearate and 1.0 part of polyethylene wax were mixed evenly to obtain the auxiliary additive;
[0147] Weigh out the following by weight: 104 parts of polyethylene material, 38 parts of the multi-element functional flame retardant prepared in Example 2, 6 parts of epoxy functionalized phenylsiloxane, 4 parts of the sulfonated graphene anchored zirconium amine carboxylic acid skeleton prepared in Example 5, and 3.5 parts of auxiliary additives. Add them to a high-speed mixer and premix for 15 minutes at 100°C and 800 r / min to obtain a premix.
[0148] Step 4: Preparation of fire-resistant three-core 10kV steel tape armored cross-linked cable
[0149] The premixed material is fed into a twin-screw extruder. The twin-screw extruder has six temperature zones set from the feed end toward the die head, with temperatures of 145℃, 150℃, 155℃, 155℃, 150℃, and 150℃ respectively. The screw speed is 80 r / min. After melting and plasticizing, the material is extruded and coated onto the outside of the protective layer, forming an outer sheath layer with a thickness of 3.4 mm. Then, the coated cable is sent into a closed hot air vulcanizing furnace at 185℃ for 15 minutes of heat preservation and vulcanization. After that, it is cooled and shaped by passing through an 80℃ hot water section and a 35℃ cold water section. Finally, it is pulled and wound to obtain a fire-resistant three-core 10kV steel tape armored cross-linked cable.
[0150] Example 9
[0151] This embodiment provides a method for preparing a fire-resistant three-core 10kV steel tape armored cross-linked cable, including the following steps:
[0152] Step 1: Conductor Forming
[0153] 36 copper wires are twisted together by a stranding machine to obtain copper stranded wire. The outside of the copper stranded wire is covered with peelable cross-linked polyethylene to form an insulation layer with a thickness of 5.0 mm. Then, water-blocking tape is continuously and evenly wrapped around the outside of the shielding layer to form a water-blocking layer. Then, steel tape is continuously and evenly wrapped around the outside of the water-blocking layer to form a steel tape shielding layer.
[0154] Three groups of conductors covered by steel strip shielding layers are cabled in a right-hand direction. Alkali-free glass fiber filaments are filled into the gaps between the conductors, and alkali-free glass fiber tape is used to continuously and evenly wrap the filling material and conductors to form a wrapping layer on the outside of the filling material.
[0155] Polyolefin is melted, extruded, and continuously and evenly coated onto the outside of the wrapping layer to form an isolation layer with a thickness of 4.5 mm. Galvanized steel strip is continuously and evenly coated onto the outside of the isolation layer to form an armor layer. Finally, mica composite ceramicized silicone tape is wrapped onto the outside of the armor layer to form a protective layer.
[0156] Step 2: Preparation of epoxy-functionalized phenylsiloxanes
[0157] Under a nitrogen atmosphere, 185 mL of 3-glycidyl etheroxypropyltrimethoxysilane, 275 g of diphenylsilanediol, and 0.9 g of barium hydroxide were weighed and added to a reaction vessel. After stirring for 12 min, the temperature was increased to 75 °C at a rate of 2 °C / min and maintained at this temperature for 5.5 h. After the reaction was completed, the temperature was lowered to 55 °C, filtered, and the filtrate was transferred to a vacuum drying oven and dried under vacuum at 55 °C for 4.5 h to obtain epoxy-functionalized phenylsiloxane.
[0158] Step 3: Preparation of premix
[0159] 64 parts of polyethylene, 23 parts of ethylene-vinyl acetate copolymer, and 8 parts of maleic anhydride-grafted polyethylene were mixed evenly to obtain polyethylene material.
[0160] 1.3 parts of dicumyl peroxide, 0.4 parts of antioxidant 1010, 0.3 parts of zinc stearate and 0.8 parts of polyethylene wax were mixed evenly to obtain the auxiliary additive;
[0161] Weigh out the following by weight: 95 parts polyethylene material, 34 parts multi-element functional flame retardant prepared in Example 3, 5 parts epoxy functionalized phenylsiloxane, 3 parts sulfonated graphene anchored zirconium amine carboxylic acid skeleton prepared in Example 6, and 2.3 parts auxiliary additives. Add them to a high-speed mixer and premix for 12 minutes at 90°C and 700 r / min to obtain a premix.
[0162] Step 4: Preparation of fire-resistant three-core 10kV steel tape armored cross-linked cable
[0163] The premixed material is fed into a twin-screw extruder. The twin-screw extruder has six temperature zones set from the feed end toward the die head, with temperatures of 145℃, 150℃, 155℃, 155℃, 150℃, and 150℃ respectively. The screw speed is 70 r / min. After melting and plasticizing, the material is extruded and coated onto the outside of the protective layer, forming an outer sheath layer with a thickness of 3.2 mm. Then, the coated cable is sent into a closed hot air vulcanizing furnace at 180℃ for 12 minutes of heat preservation and vulcanization. After that, it is cooled and shaped by passing through a 75℃ hot water section and a 30℃ cold water section. Finally, it is drawn and wound to obtain a fire-resistant three-core 10kV steel tape armored cross-linked cable.
[0164] Comparative Example 1
[0165] The difference between this comparative example and Example 9 is that step IV in Example 3 is omitted, and the borosilicate bifunctional Schiff base prepared in step III is used to replace the multi-element functional flame retardant in step three of Example 9.
[0166] Comparative Example 2
[0167] The difference between this comparative example and Example 9 is that Example 3 is omitted, and a commercially available flame retardant is used instead of the multi-element functional flame retardant in step three of Example 9.
[0168] Comparative Example 3
[0169] The difference between this comparative example and Example 9 is that step ii in Example 6 is omitted, and the sulfonated graphene oxide prepared in step i is used to replace the sulfonated graphene anchored zirconium amine carboxylic acid skeleton in step three of Example 9.
[0170] Comparative Example 4
[0171] The difference between this comparative example and Example 9 is that Example 6 is omitted, and the sulfonated graphene anchored zirconium amine carboxylic acid skeleton in step 3 of Example 9 is replaced with graphene oxide used in step i.
[0172] Comparative Example 5
[0173] The difference between this comparative example and Example 9 is that step two in Example 9 is omitted, and epoxy-functionalized phenylsiloxane is not added in step three of Example 9.
[0174] Performance testing:
[0175] Referring to the standard GB / T 19666-2019 "General Rules for Flame Retardant and Fire-Resistant Wires, Cables or Optical Cables", the fire-resistant three-core 10kV steel tape armored cross-linked cable outer sheath samples prepared in Examples 7-9 and Comparative Examples 1-5 were kept in an environment with a temperature of (23±2)℃ and a relative humidity of 35%±5% for 24h. They were then subjected to a combustion test in a 1m³ standard smoke box under the specified conditions. The halogen content, smoke density, light transmittance and carbonization spread height of the combustion products were measured simultaneously. The halogen-free low-smoke flame retardant rating of the outer sheath layer of the fire-resistant three-core 10kV steel tape armored cross-linked cables prepared in Examples 7-9 and Comparative Examples 1-5 were determined respectively.
[0176] Referring to standard GB / T 1408.1-2016 "Electrical Strength Test Methods for Insulating Materials - Part 1: Power Frequency Test", the fire-resistant three-core 10kV steel tape armored cross-linked cable outer sheath samples prepared in Examples 7-9 and Comparative Examples 1-5 were kept in an environment with a temperature of (23±5)℃ and a relative humidity of 50%±5% for at least 24h. Under the AC voltage conditions of power frequency 48Hz-62Hz, a constant voltage increase rate of 1kV / s-3kV / s was applied to the samples until breakdown occurred. The highest voltage value at the moment of breakdown was recorded. The power frequency breakdown voltage of the outer sheath of the fire-resistant three-core 10kV steel tape armored cross-linked cable prepared in Examples 7-9 and Comparative Examples 1-5 was measured respectively.
[0177] Referring to standard GB / T 2951.11-2008 "General Test Methods for Insulation and Sheath Materials of Cables and Optical Fibers - Part 11: General Test Methods - Thickness and Dimensional Measurements - Mechanical Properties Tests", the outer sheath samples of fire-resistant three-core 10kV steel-tape armored cross-linked cables prepared in Examples 7-9 and Comparative Examples 1-5 were kept at a temperature of (23±5)℃ for at least 3 hours. Dumbbell-shaped specimens were cut from the sheath layer, and the specimens were stretched to fracture at a tensile speed of (250±50) mm / min under the condition of (23±5)℃. The maximum tensile force, maximum tensile stress, and elongation at break were recorded. The tensile stress, tensile strength, and elongation at break of the outer sheath layer of the fire-resistant three-core 10kV steel-tape armored cross-linked cables prepared in Examples 7-9 and Comparative Examples 1-5 were measured respectively. The specific test results are shown in Table 1 below:
[0178] Table 1 - Performance Test Data of Samples
[0179]
[0180] Data Analysis:
[0181] Comparative analysis of the data in Table 1 above shows that the fire-resistant three-core 10kV steel-tape armored cross-linked cable prepared by this invention has the following characteristics: halogen-free low-smoke flame retardant rating of its outer sheath (WDZA), breakdown voltage of 25.5kV, tensile stress of 13.7MPa, tensile strength of 16.1MPa, and elongation at break of 372%.
[0182] Compared with Example 1, the DOPO addition step was eliminated, and a borosilicate bifunctional Schiff base was used to replace the multi-element functional flame retardant. The role of phosphorus in gas-phase quenching free radicals was lost, and solid-phase charring was achieved solely by boron-silicon. At the same time, the borosilicate bifunctional Schiff base had poor compatibility with the polyolefin matrix, and the number of interface defects inside the sheath increased. As a result, the halogen-free low-smoke flame retardant rating dropped to WDZB, the breakdown voltage dropped to 20.2kV, the tensile stress dropped to 10.5MPa, the tensile strength dropped to 11.2MPa, and the elongation at break dropped to 245%.
[0183] Comparative Example 2, which uses commercially available ordinary flame retardants instead of self-made multi-element functional flame retardants, lacks the synergistic flame-retardant structure of boron, silicon, and phosphorus molecules. Conventional flame-retardant components require higher filler amounts to exert their flame-retardant effect, disrupting the continuity of the polyolefin matrix, resulting in poor filler-matrix interface bonding, increased internal porosity and defects in the sheath, and causing the halogen-free low-smoke flame retardant rating to drop to WDZB. The breakdown voltage drops significantly to 17.3kV, tensile stress drops to 9.2MPa, tensile strength drops to 9.6MPa, and elongation at break drops significantly to 183%.
[0184] Comparative Example 3: The in-situ growth process of the zirconium amine carboxylic acid framework was eliminated, and sulfonated graphene oxide was used directly as a filler. Without the anchoring and constraint of the zirconium amine carboxylic acid framework on the graphene sheets, the graphene sheets were prone to stacking and agglomeration. At the same time, the catalytic carbonization effect of zirconium metal sites was missing. The agglomeration sites formed stress concentration points and potential local conductive paths, resulting in a reduction of the halogen-free low-smoke flame retardant rating to WDZB, a breakdown voltage of 19.4kV, a tensile stress of 10.3MPa, a tensile strength of 10.5MPa, and an elongation at break of 228%.
[0185] Comparative Example 4 directly replaced sulfonated graphene with original graphene oxide to anchor the zirconium amine carboxylic acid skeleton. The graphene oxide was not sulfonated or anchored by the MOF skeleton, resulting in poor compatibility with the polyolefin matrix and further exacerbating the sheet aggregation phenomenon. This not only weakened the char-forming and smoke-suppressing ability, but also generated a large number of insulation defects and stress concentration points, causing the halogen-free low-smoke flame retardant rating to drop to WDZC, the breakdown voltage to drop to 16.2kV, the tensile stress to drop to 9.4MPa, the tensile strength to drop to 8.8MPa, and the elongation at break to drop to 156%.
[0186] Comparative Example 5: When preparing the premix, no epoxy-functionalized phenylsiloxane was added. The lack of an organic-inorganic interface bridge constructed by epoxy groups weakened the interfacial bonding force between the multi-element flame retardant, graphene-based filler and polyethylene matrix. A large number of micro-crack defects were generated at the two-phase interface, which reduced the halogen-free low-smoke flame retardant rating to WDZB, the breakdown voltage to 20.5kV, the tensile stress to 10.9MPa, the tensile strength to 11.5MPa, and the elongation at break to 139%.
[0187] The above are merely examples and descriptions of the structure of the present invention. Those skilled in the art can make various modifications or additions to the specific embodiments described, or use similar methods to replace them, as long as they do not deviate from the structure of the invention or exceed the scope defined in the claims, all of which should fall within the protection scope of the present invention.
Claims
1. A method for preparing a fire-resistant three-core 10kV steel-tape armored cross-linked cable, characterized in that, Includes the following steps: S1. After the three cable cores are bundled together, filler material is placed between the conductor gaps, and then wrapping tape is used to wrap the cable to form a wrapping layer. S2. After extruding and coating polyolefin on the outside of the wrapping layer to form an isolation layer, galvanized steel strip is used for armoring to form an armor layer. Then, composite mica tape is used to wrap the outside of the armor layer to form a protective layer. S3. After the outer sheath material is extruded and wrapped around the outside of the protective layer, it is vulcanized and cross-linked to form an outer sheath layer, thus obtaining a fire-resistant three-core 10kV steel tape armored cross-linked cable. The outer sheath material is composed of polyethylene material, multi-element functional flame retardant, epoxy functionalized phenylsiloxane, sulfonated graphene anchored zirconium amine carboxylic acid skeleton and auxiliary additives.
2. The method for preparing a fire-resistant three-core 10kV steel-tape armored cross-linked cable according to claim 1, characterized in that, In step S3, the multi-element functional flame retardant is prepared by the following steps: A1. Under a nitrogen atmosphere, boron amino acid active ester is added to a reaction vessel containing anhydrous toluene. After stirring at 20-30℃ for 15-30 min, an anhydrous toluene solution of vanillin octyl silyl ether is added dropwise. After the addition is complete, stirring is continued at 20-30℃ for 1-2 h. Then, the temperature is first raised to 60-70℃ and reacted for 2-3 h, and then the temperature is further raised to 105-110℃ and reacted for 10-12 h. After the reaction is completed, post-processing is performed to obtain a boron-silicon bifunctional Schiff base. A2. Under a nitrogen atmosphere, a borosilicate bifunctional Schiff base is added to a reactor containing tetrahydrofuran and swelled at 20-30°C for 1-2 hours. Then, DOPO is added, and the mixture is stirred at 20-30°C for 40-60 minutes. The temperature is then raised to 60-65°C and refluxed for 10-12 hours. After the reaction is completed, post-treatment is performed to obtain a multi-element functional flame retardant.
3. The method for preparing a fire-resistant three-core 10kV steel-tape armored cross-linked cable according to claim 2, characterized in that, In step A1, the ratio of the amount of boron amino active ester, anhydrous toluene, and vanillin octyl silyl ether in anhydrous toluene solution is 1g:10-12mL:12.5-13.5mL, and the mass fraction of the vanillin octyl silyl ether in anhydrous toluene solution is 25%; in step A2, the ratio of the amount of borosilicate bifunctional Schiff base, tetrahydrofuran, and DOPO is 1g:10-15mL:0.78g.
4. The method for preparing a fire-resistant three-core 10kV steel-tape armored cross-linked cable according to claim 3, characterized in that, In step A1, the preparation method of vanillin-octyl silane is as follows: under a nitrogen atmosphere, vanillin and triethylamine are added to a reaction vessel containing anhydrous tetrahydrofuran. After stirring at 0-5℃ for 15-20 min, a dichloromethyloctylsilane tetrahydrofuran solution is added dropwise. After the addition is complete, stirring is continued at 0-5℃ for 20-30 min. Then, the temperature is first raised to 20-30℃ and reacted for 2-4 h, and then the temperature is further raised to 45-55℃ and reacted for 2-3 h. After the reaction is completed, post-processing is performed to obtain vanillin-octyl silane. The ratio of vanillin, triethylamine, anhydrous tetrahydrofuran, and dichloromethyloctylsilane tetrahydrofuran solution is 1 g: 0.96 mL: 8-10 mL: 2.6-2.8 mL, and the mass fraction of the dichloromethyloctylsilane tetrahydrofuran solution is 30%.
5. The method for preparing a fire-resistant three-core 10kV steel-tape armored cross-linked cable according to claim 4, characterized in that, The preparation method of the boron-ammonia active ester is as follows: under a nitrogen atmosphere, boric acid and 3-amino-1-propanol are added to a reaction vessel containing anhydrous toluene. After stirring at 20-30℃ for 10-20 min, the temperature is first raised to 70-80℃ and stirring is continued for 20-30 min. Then, the temperature is raised to 105-110℃ and refluxed for 10-12 h. After the reaction is completed, post-treatment is performed to obtain the boron-ammonia active ester. The ratio of boric acid, 3-amino-1-propanol and anhydrous toluene is 1 g: 3.6-3.7 g: 10-15 mL.
6. The method for preparing a fire-resistant three-core 10kV steel-tape armored cross-linked cable according to claim 1, characterized in that, In step S3, the preparation method of the epoxy-functionalized phenylsiloxane is as follows: under a nitrogen atmosphere, 3-glycidyl etheroxypropyltrimethoxysilane, diphenylsilanediol and barium hydroxide are added to a reaction vessel, stirred for 10-15 min, and then heated to 70-80℃ at a rate of 2-3℃ / min, and kept at this temperature for 5-6 h. After the reaction is completed, post-processing is performed to obtain the epoxy-functionalized phenylsiloxane; the ratio of the amount of 3-glycidyl etheroxypropyltrimethoxysilane, diphenylsilanediol and barium hydroxide is 18-19 mL: 27.5 g: 0.09 g.
7. The method for preparing a fire-resistant three-core 10kV steel-tape armored cross-linked cable according to claim 1, characterized in that, In step S3, the sulfonated graphene-anchored zirconium amine carboxylic acid skeleton is prepared by the following steps: B1. Graphene oxide is added to a reaction vessel containing anhydrous dimethyl sulfoxide and ultrasonically dispersed for 1-2 hours. Then, 1,4-butanesulfonate lactone is added and stirred for 20-30 minutes. Sodium hydroxide is then added and the temperature is increased to 100-105℃ at a rate of 2-3℃ / min. The reaction is carried out for 20-24 hours. After the reaction is completed, post-treatment is performed to obtain sulfonated graphene oxide. B2. Diaminoterephthalic acid and zirconium tetrachloride were added to a reaction vessel containing N,N-dimethylformamide and ultrasonically dispersed for 40-60 min. Then, deionized water was added and stirred for 10-20 min. Sulfonated graphene oxide was then added and stirred for 20-30 min. Glacial acetic acid was then added and stirred for another 10-20 min. The temperature was then raised to 110-120℃ and the reaction was carried out for 20-24 h. After the reaction was completed, post-processing was performed to obtain the sulfonated graphene-anchored zirconium amine carboxylic acid skeleton.
8. The method for preparing a fire-resistant three-core 10kV steel-tape armored cross-linked cable according to claim 7, characterized in that, In step B1, the ratio of graphene oxide, anhydrous dimethyl sulfoxide, 1,4-butanesulfonate lactone, and sodium hydroxide is 1g:700-800mL:9-11mL:1.8g; in step B2, the ratio of diaminoterephthalic acid, zirconium tetrachloride, N,N-dimethylformamide, deionized water, sulfonated graphene oxide, and glacial acetic acid is 1g:1.15-1.35g:100-150mL:0.8-1.2mL:0.2g:10mL.
9. The method for preparing a fire-resistant three-core 10kV steel-tape armored cross-linked cable according to claim 1, characterized in that, In step S3, the polyethylene material is obtained by uniformly mixing 60-68 parts of polyethylene, 20-26 parts of ethylene-vinyl acetate copolymer, and 6-10 parts of maleic anhydride-grafted polyethylene by weight; the auxiliary additive is obtained by uniformly mixing 1.0-1.6 parts of dicumyl peroxide, 0.3-0.5 parts of antioxidant 1010, 0.2-0.4 parts of zinc stearate, and 0.6-1.0 parts of polyethylene wax by weight.
10. The method for preparing a fire-resistant three-core 10kV steel-tape armored cross-linked cable according to claim 1, characterized in that, In step S3, the ratio of polyethylene material, multi-element functional flame retardant, epoxy functionalized phenylsiloxane, sulfonated graphene anchored zirconium amine carboxylic acid skeleton and auxiliary additives is 86-104 parts by weight: 30-38 parts: 4-6 parts: 2-4 parts: 2.1-3.5 parts.