A corrosion-resistant submersible pump cable and its preparation method

By combining flexible co-crosslinked coated sheet filler with a high crosslinking density vulcanization system, the problem of insulation blistering and cracking in submersible pump cables during downhole gas decompression was solved, achieving stability and corrosion resistance of the cable under high pressure and improving the overall performance of the cable.

CN123120439APending Publication Date: 2026-11-17陕西西特电缆有限公司
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611627588.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-21
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

During the downhole gas decompression process, the insulation layer of the submersible pump cable is prone to blistering and cracking, leading to the failure of the entire cable. Existing technologies are difficult to effectively resist rapid gas decompression damage while maintaining electrical, mechanical and corrosion resistance properties.

Method used

A corrosion-resistant submersible pump cable is formed by using a flexible co-crosslinked coated sheet filler and a high crosslinking density vulcanization system, combined with a vinyl silane chemical bonding layer and a flexible layer of maleic anhydride-grafted EPDM rubber and liquid EPDM rubber, and an insulation layer is prepared by an extruder and a continuous vulcanization tube. This is then combined with carbon fiber bundle filling and tin-plated steel tape armor.

Benefits of technology

While maintaining corrosion resistance and electrical and mechanical properties, it significantly improves the cable's resistance to rapid gas decompression, reduces the bubbling level and cross-sectional cavity area, decreases the outer diameter change rate, and enhances the stability of the insulation layer.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

This invention belongs to the field of cable manufacturing technology and relates to a corrosion-resistant submersible pump cable and its preparation method. The method includes conductor treatment, applying an adhesive layer, preparing a flexible co-crosslinked coated sheet filler, mixing, extruding an insulation layer, stranding and filling, extruding a sheath layer, applying an anti-corrosion layer, and armoring. The flexible co-crosslinked coated sheet filler consists of sheet filler, a vinyl silane chemically bonded layer on its surface, and a flexible layer. The flexible layer is a composite of maleic anhydride-grafted EPDM rubber and liquid EPDM rubber, retaining unsaturated bonds. The vulcanization system of the insulating compound consists of a peroxide vulcanizing agent, triallyl isocyanurate, and N,N′-m-phenylene bismaleimide. This invention simultaneously reduces the total gas adsorption within the insulation layer, reduces nucleation sites during decompression, and improves cavitation expansion resistance, enabling the cable to exhibit excellent resistance to rapid gas decompression while maintaining corrosion resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of cable manufacturing technology and relates to a corrosion-resistant submersible pump cable and its preparation method. Background Technology

[0002] Submersible pump cables are specialized cables used with submersible electric pump units. They are laid within the confined space of the well casing, with one end connected to the downhole submersible motor and the other end leading to the surface control cabinet via the wellhead. They operate continuously in high-temperature, high-pressure environments and in corrosive media containing oil, water, carbon dioxide, and hydrogen sulfide. Due to the limitations of downhole space and operating conditions, submersible pump cables cannot have joints, and a single section length is typically no less than 2800m. If any part of the cable's insulation is damaged, the entire cable becomes unusable, requiring pump inspection and cable replacement. Therefore, submersible pump cables have high requirements for the integrity of the insulation layer, corrosion resistance, and structural stability.

[0003] To improve the withstand capability of submersible pump cables in downhole media, existing technologies employ various measures. Regarding the insulation layer, nitrile rubber, EPDM rubber, or blends thereof are typically used as the matrix, and their heat resistance, oil resistance, and electrical insulation properties are improved by adjusting the vulcanization and filling systems. Structurally, an adhesive layer is usually placed between the conductor and the insulation layer to prevent downhole gas from seeping into the gap between them. Carbon fiber is filled between the insulation layer and the sheath to balance heat dissipation and structural integrity. An anti-corrosion layer composed of epoxy coal tar pitch, chlorinated polyethylene resin, mica powder, and silica is applied outside the lead alloy sheath, and a double-layer reverse-wrapping armor is provided with tin-plated steel strip.

[0004] The aforementioned measures primarily address chemical corrosion, moisture intrusion, and heat dissipation issues. However, in actual submersible pump tripping operations, cable damage observed during cable retrieval, in addition to deformation, breakage, wear, and corrosion, also includes blistering of the insulation layer. This blistering is often located inside the insulation layer, while no obvious corrosion marks are observed on the outer surface of the insulation layer or the lead alloy sheath corresponding to the blistering site, indicating that its cause differs from corrosion. Analysis reveals that the cable is exposed to high-pressure downhole gas during operation, which dissolves under pressure and diffuses into the insulation layer. During pump inspection and tripping, the pressure inside the wellbore drops to atmospheric pressure in a short time, causing the dissolved gas in the insulation layer to become supersaturated. Unable to diffuse outwards, the gas nucleates and expands inside the insulation layer, resulting in blistering, voids, and even cracking. This damage pattern is similar to the failure pattern of elastic components in oil and gas extraction under rapid decompression conditions. However, unlike elastic components, the insulation layer of the submersible pump cable is encased in a lead alloy sheath. Lead alloy is relatively soft and prone to creep, failing to provide effective mechanical restraint to the insulation layer during decompression.

[0005] Existing technologies for improving gas barrier performance focus on reducing the total amount of gas dissolved and permeated within the insulation layer. For example, mica or other sheet-like fillers are directly added to the rubber matrix, utilizing the tortuous paths formed by the sheets to extend the gas permeation path; another example is using maleic anhydride-grafted EPDM rubber to improve the compatibility between the filler and the matrix, and using it in conjunction with mica or other sheet-like fillers. These methods target the gas permeation process under steady-state conditions, while damage under rapid decompression depends on the nucleation location of bubbles and the expansion resistance of cavities at the moment of decompression, which are not the same physical process. Furthermore, the direct addition of sheet-like fillers introduces a large amount of interface material between the filler and the matrix. The free volume at the interface is higher than that of the matrix, and downhole gas preferentially accumulates at this point under high pressure; during decompression, the edges of the sheets preferentially debond due to stress concentration. Therefore, simply adding sheet-like fillers based on the idea of ​​barrier treatment not only fails to suppress decompression foaming, but may also exacerbate foaming and porosity in systems where cross-linking density is increased to improve cavitation resistance. How to ensure that the insulation layer of submersible pump cables can resist damage from rapid gas decompression while maintaining electrical, mechanical, and corrosion resistance is a technical problem that needs to be solved in this field. Summary of the Invention

[0006] In view of the above-mentioned problems in the existing technology, the purpose of this invention is to provide a corrosion-resistant submersible pump cable and its preparation method, so as to solve the technical problem that the insulation layer of the submersible pump cable will blister and crack due to the decompression of the downhole gas during the tripping operation, which will lead to the failure of the entire cable.

[0007] On one hand, this invention discloses a corrosion-resistant submersible pump cable and its preparation method, the preparation method comprising the following steps: S1. Conductor processing: Select copper wire as the conductor of the cable, tin-plat the surface of the copper wire, and twist the tin-plated copper wire into a bundle to obtain a rough-processed conductor. S2. Applying adhesive layer: Apply the adhesive layer material evenly to the outer periphery of the rough-processed conductor. Heating is required during the application process. The heating temperature range is set to 55-60℃ to obtain the adhesive conductor. S3. Preparation of flexible co-crosslinked coated sheet filler: The sheet filler is dispersed at a solid content of 5% in a mixed solvent of ethanol and deionized water at a volume ratio of 9:1. The pH value is adjusted to 4-5 with acetic acid. Vinyltriethoxysilane at a mass ratio of 2%-4% of the sheet filler is added. The mixture is refluxed at 75-80℃ for 2-4 hours. After filtration, washing, and drying, silanized sheet filler is obtained. Maleic anhydride-grafted EPDM rubber and liquid EPDM rubber are dissolved in xylene at a mass ratio of 1:2-1:4 to prepare a coating solution with a mass fraction of 5%. The silanized sheet filler is added to the coating solution. The mixture is stirred at 60℃ for 2 hours and then heated to 110℃ to remove the solvent. The coating amount is controlled to be 3%-8% of the mass of the sheet filler to obtain flexible co-crosslinked coated sheet filler. S4. Mixing: By weight, 100 parts of EPDM rubber are plasticized for 2 minutes, then 4-6 parts of zinc oxide, 1-2 parts of 2-mercaptobenzimidazole, 0.5-1.5 parts of stearic acid, 1-3 parts of microcrystalline wax, 3-8 parts of paraffin oil, and 20-35 parts of calcined kaolin are added sequentially and mixed. Then, 8-20 parts of the flexible co-crosslinked coated sheet filler are added and mixed for 6-8 minutes. After discharge and cooling, a first-stage rubber is obtained. The first-stage rubber is then mixed with 2.5-3.5 parts of peroxide vulcanizing agent, 1.5-3 parts of triallyl isocyanurate, and 0.5-1.5 parts of N,N′-m-phenylene bismaleimide at a temperature not exceeding 95°C for a second-stage mixing. After thinning and sheeting, the insulating rubber compound is obtained. S5. Extruding the insulation layer: The insulating rubber material is extruded onto the outer periphery of the bonded conductor using an extruder. The extruder head adopts an extended flow channel, which makes the sheet filler oriented along the radial direction of the cable. The extruded wire core enters the continuous vulcanization tube for vulcanization. After vulcanization, the pressure is gradually reduced and the temperature is gradually reduced to obtain the insulated wire core. S6. Stranding and filling: The insulated wire cores are stranded together to obtain the cable core. During the stranding process, carbon fiber bundles are filled into the gaps between the cable cores. After filling, the cable cores are tied tightly with halogen-free water-blocking tape. S7. Extrusion of the sheath layer: Lead alloy material is extruded onto the outer periphery of the cable core using a continuous lead extrusion machine to form a sheath layer. The continuous extrusion temperature range is 290 to 390°C, resulting in a coarse cable. S8. Applying anti-corrosion layer: Applying anti-corrosion material evenly to the outer periphery of the coarse cable to form the anti-corrosion layer, thus obtaining an anti-corrosion cable; S9. Armoring: The anti-corrosion cable is wrapped with tin-plated steel strip in an overlapping manner to obtain the submersible pump cable.

[0008] Further, in S2, the adhesive layer material is composed of 45-55 parts polyacrylate, 35-45 parts polyurethane, 5-12 parts talc, and 0.5-1.5 parts vinyltriethoxysilane by weight.

[0009] Further, in S3, the sheet-like filler is wet-processed mica powder or organo-modified montmorillonite, the aspect ratio of the sheet-like filler is not less than 50, and the particle size distribution D97 is not greater than 30 μm; the grafting rate of the maleic anhydride-grafted EPDM rubber is 0.5%–1.5%; the number-average molecular weight of the liquid EPDM rubber is 2.0 × 10⁻⁶. 3 ~6.0×10 3 The liquid EPDM rubber retains ethylene-bis(norbornene) unsaturated bonds.

[0010] Further, in S4, the EPDM rubber is of the ethylene-ide norbornene type, with a Mooney viscosity ML(1+4) of 40-60 at 100℃ and an ethylene content of 55%-65%; the calcined kaolin is pretreated with 1.5%-2% of its own mass of vinyltriethoxysilane; the peroxide vulcanizing agent is dicumyl peroxide or bis-tert-butylperoxyisopropylbenzene; the discharge temperature of the first stage of mixing is not higher than 120℃, and the rubber is cooled and left to stand for 24 hours after discharge; the Mooney scorch time t5 of the insulating rubber obtained after the second stage of mixing is not less than 15 minutes at 120℃.

[0011] Furthermore, in S5, the barrel temperature of the extruder is controlled in four stages: 40–50°C, 60–70°C, 75–85°C, and 85–95°C, respectively; the die head temperature is 90–95°C; and the extrusion pressure is 15–20 MPa. The convergence half-angle of the extended flow channel is 10°–20°, and the extrusion draw ratio is 1.20–1.30. The nominal thickness of the insulating layer is 1.0–2.0 mm. The steam temperature of the continuous vulcanizing tube is 180–195°C, and the vulcanization time is 2–5 min.

[0012] Further, in S7, the nominal minimum thickness of the sheath layer is 2.5–3.0 mm; in S8, the anti-corrosion material is composed of 60–70 parts by weight of epoxy coal tar pitch, 15–30 parts by weight of chlorinated polyethylene resin, 5–8 parts by weight of mica powder, and 4–8 parts by weight of silica; in S9, the tin-plated steel strip is wrapped and armored twice, the first wrapping being clockwise and the second wrapping being counterclockwise, the nominal thickness of the steel strip being 1.0 mm, and the overlap rate being not less than 30%.

[0013] Further, in S6, the carbon fiber bundle is a polyacrylonitrile-based carbon fiber bundle with a bundle specification of 12K and a linear density of 800tex; the number of insulating wire cores is 3, and the carbon fiber bundles are respectively filled in the three gaps between the 3 insulating wire cores along the axial direction, with each gap filled with 1 bundle.

[0014] On the other hand, the present invention relates to a corrosion-resistant submersible pump cable, which is prepared by the above-mentioned method. The cable, from the inside out, includes at least three bundles of conductors, an adhesive layer, an insulation layer, a filler layer, a sheath layer, an anti-corrosion layer, and an armor layer. The conductors and the insulation layer are bonded together by the adhesive layer. The insulation layer and the sheath layer are filled with carbon fiber bundles. The number of conductors is at least three bundles, and each bundle of conductors is made of at least 26 strands of tin-plated copper wire. The insulation layer is made of insulating rubber, in which flexible co-crosslinked coated sheet filler is dispersed. The flexible co-crosslinked coated sheet filler is composed of sheet filler, a vinyl silane chemical bonding layer covering the surface of the sheet filler, and a flexible layer covering the chemical bonding layer. The flexible layer is made of maleic anhydride-grafted EPDM rubber and liquid EPDM rubber. The flexible layer retains ethylene-methyl-3-norbornene unsaturated bonds and co-crosslinks with the matrix of the insulation layer through the unsaturated bonds.

[0015] Furthermore, the thickness of the flexible layer is 5-20 nm, the coating amount of the flexible layer is 3%-8% of the mass of the sheet filler, and the mass ratio of maleic anhydride-grafted EPDM rubber to liquid EPDM rubber in the flexible layer is 1:2-1:4.

[0016] Furthermore, the cross-sectional area of ​​each bundle of conductors is circular, and the cross-section of the cable is oblong; or the cross-sectional area of ​​each bundle of conductors is sector-shaped, and the cross-section of the cable is circular.

[0017] Compared with the prior art, the technical solution provided by the present invention has at least the following beneficial effects: The insulating compound of this invention simultaneously contains silanized and flexible-layer-coated sheet fillers, as well as a high-crosslinking density vulcanization system composed of peroxide vulcanizing agent, triallyl isocyanurate, and N,N′-m-phenylene bismaleimide. The cable maintains its corrosion resistance, electrical and mechanical properties while exhibiting excellent resistance to rapid gas decompression. Tests were conducted under the conditions of 15 MPa methane pressure, 150°C temperature, saturation for 72 hours, followed by decompression at 3 MPa / min to atmospheric pressure. Examples 1 to 3 showed a foaming grade of 0–1, a cross-sectional void area ratio of 0.6%–1.3%, and an outer diameter change rate of 0.8%–1.6% before and after decompression. The volume resistivity of the insulation layer at 90°C was not less than 3.2 × 10⁻⁶. 13 The dielectric loss factor at 90℃ and 50Hz is no higher than 0.023, and the compression set at 180℃ for 24 hours is no higher than 19.6%. The chemical bonding layer uses vinyl silane, whose vinyl groups can participate in peroxide-initiated free radical reactions, allowing the interface layer to co-crosslink with the matrix and be incorporated into the crosslinking network during vulcanization. This also avoids the ineffective decomposition of peroxide free radicals accelerated by basic groups such as amino groups. The flexible layer is composed of maleic anhydride-grafted EPDM rubber and a number-average molecular weight of 2.0 × 10⁻⁶. 3~6.0×10 3 It is a compound of liquid EPDM rubber, which forms chemical bonds with the surface of the sheets and is homologous with the EPDM rubber matrix. This allows for a smooth transition of modulus from the sheets to the matrix and fills the free volume at the interface, thereby reducing gas accumulation at the interface and preferential debonding during pressure relief. The high cross-linking density vulcanization system improves the resistance of the cross-linking network to cavitation expansion, acting on the nucleation site and cavitation expansion resistance, respectively, along with the flexible coating layer. The amount and aspect ratio of the sheet filler control the total amount of gas adsorption and permeation within the insulation layer. The three elements work together to reduce the foaming level, cross-sectional cavity area ratio, and outer diameter change rate of the insulation layer under pressure relief conditions, without compromising volume resistivity, dielectric loss factor, or compression set. Detailed Implementation

[0018] The technical solution of the present invention will be described below with reference to embodiments. However, the present invention is not limited to the following embodiments. Unless otherwise specified, the experimental and detection methods described in each embodiment are conventional methods; the reagents and materials described are commercially available unless otherwise specified. Unless otherwise specified, all percentages in the following embodiments refer to mass percentages. Unless otherwise specified, all proportions in the following embodiments refer to mass ratios.

[0019] Example 1

[0020] This embodiment provides a process for preparing a corrosion-resistant submersible pump cable.

[0021] S1. Preparation of Flexible Co-crosslinked Coated Sheet Filler. Wet-processed mica powder was selected as the sheet filler, with an aspect ratio of 60, a D97 of 25 μm, and a D50 of 12 μm. Mica powder was dispersed at a solid content of 5% in a mixed solvent of ethanol and deionized water at a volume ratio of 9:1. The pH was adjusted to 4.5 with acetic acid. Vinyltriethoxysilane (3% by weight of mica powder) was added, and the mixture was refluxed at 75°C for 3 hours. After filtration, the mixture was washed three times with anhydrous ethanol and vacuum dried at 90°C for 4 hours to obtain silanized mica powder. Maleic anhydride-grafted EPDM rubber and liquid EPDM rubber were dissolved in xylene at a mass ratio of 1:3 to prepare a 5% (w / w) coating solution. The grafting rate of the maleic anhydride-grafted EPDM rubber was 1.0%, and the number average molecular weight of the liquid EPDM rubber was 2.62 × 10⁻⁶. 3 ; Add silanized mica powder to the coating solution, stir at 60℃ for 2h, heat to 110℃ to remove solvent, vacuum dry, control the coating amount to 5% of the mica powder mass, and obtain flexible co-crosslinked coated sheet filler with a thickness of 8-15nm; thermogravimetric analysis shows that the coating amount is 5.1%.

[0022] S2. Conductor treatment and adhesive coating. Copper wire is selected as the conductor of the cable. The surface of the copper wire is tin-plated and pressed into a circular structure by a forming die. 37 tin-plated copper wires are twisted into a bundle, and 3 bundles are used as conductors. The adhesive material is evenly applied to the outer periphery of the conductor. During the application process, the material is heated at 58°C to obtain an adhesive conductor. By weight, the adhesive layer consists of 50 parts polyacrylate, 40 parts polyurethane, 9 parts talc, and 1 part vinyltriethoxysilane, with a dry film thickness of 35 μm.

[0023] S3. Insulating compound mixing (stage 1). By weight, the insulating compound consists of 100 parts EPDM rubber, 12 parts flexible co-crosslinked coated sheet filler, 28 parts calcined kaolin, 5 parts zinc oxide, 1 part stearic acid, 5 parts paraffin oil, 2 parts microcrystalline wax, 1.5 parts 2-mercaptobenzimidazole, 2 parts triallyl isocyanurate, 1 part N,N′-m-phenylene bismaleimide, and 2.8 parts dicumyl peroxide; wherein the EPDM rubber is ethylene-ide norbornene type, with a Mooney viscosity ML(1+4) of 50 at 100℃, and an ethylene content of 58%. The norbornene content is 4.5%; the calcined kaolin is pretreated with vinyltriethoxysilane at a rate of 1.5% of the calcined kaolin mass; the first stage of mixing is carried out in an internal mixer. First, EPDM rubber is plasticized for 2 minutes, then zinc oxide, 2-mercaptobenzimidazole, stearic acid, microcrystalline wax and paraffin oil are added and mixed for 4 minutes, then calcined kaolin is added and mixed for 6 minutes, then flexible co-crosslinked coated sheet filler is added and mixed for 7 minutes. The discharge temperature is 110℃, and after discharge, it is cooled and left to stand for 24 hours to obtain the first stage of rubber.

[0024] S4. Two-stage mixing of insulating rubber compound. The first stage of rubber compound is put into an internal mixer, and triallyl isocyanurate, N,N′-m-phenylene bismaleimide and dicumyl peroxide are added at a temperature not exceeding 95℃. The mixture is mixed for 6 minutes, passed through a thin sheet 3 times, and left to stand for 8 hours to obtain the insulating rubber compound. The Mooney scorch time t5 of the insulating rubber compound at 120℃ is measured to be 22 minutes.

[0025] S5. Extrusion of the insulation layer. An extruder is used to extrude the insulating compound onto the outer periphery of the bonding conductor. The extruder barrel temperature is controlled in four sections: 45℃ (first section), 65℃ (second section), 80℃ (third section), and 90℃ (fourth section). The die head temperature is 92℃, and the extrusion pressure is controlled at 18MPa. The extruder head uses an extended flow channel with a convergence half-angle of 15° in the convergence section. The extrusion draw ratio is 1.25, ensuring the sheet-like filler is oriented radially along the cable in the convergence section of the flow channel. The nominal thickness of the insulation layer is 1.5mm. The extruded core enters a continuous vulcanizing tube. The steam temperature is controlled at 185℃, and the vulcanization time is 4 minutes. After vulcanization, the pressure and temperature are gradually reduced to obtain the insulated core.

[0026] S6. Stranding and Filling. The three insulated wire cores are stranded together to obtain the cable core. 12K polyacrylonitrile-based carbon fiber bundles with a linear density of 800 tex are used to fill the three gaps between the three insulated wire cores along the axial direction. One bundle is filled in each gap, for a total of three bundles. After filling, the cable core is wrapped tightly with overlapping halogen-free water-blocking tape.

[0027] S7. Extrusion of lead alloy sheath layer. Lead alloy material is extruded onto the outer periphery of the cable core using a continuous extrusion machine to form a lead alloy sheath layer. The continuous extrusion temperature is 310℃, and the nominal minimum thickness of the sheath is 3.0mm.

[0028] S8. Applying the anti-corrosion layer. By weight, the anti-corrosion layer material consists of 62 parts epoxy coal tar pitch, 28 parts chlorinated polyethylene resin, 5 parts mica powder, and 5 parts silica. The above materials are ground and dispersed to a fineness of no more than 60 μm, and then sprayed onto the outer periphery of the lead alloy sheath layer in two coats. Each coat has a dry film thickness of 75 μm, and the dry film thickness of the anti-corrosion layer after curing is 150 μm.

[0029] S9. Armoring. The cable after the anti-corrosion coating is applied is wrapped with tin-plated steel strip in an overlapping manner. The first wrap is clockwise and the second wrap is counterclockwise. The nominal thickness of the steel strip is 1.0mm and the overlap rate is not less than 30%.

[0030] A submersible pump cable, prepared using the above method, comprises, from the inside out, a tin-plated copper conductor, an adhesive layer, an insulation layer, a carbon fiber filler layer, a lead alloy sheath layer, an anti-corrosion layer, and a tin-plated steel tape armor layer. The conductor and insulation layer are bonded together by the adhesive layer. The filler layer consists of three bundles of polyacrylonitrile-based carbon fibers filled in three gaps between three insulated cores. The carbon fiber bundles are 12K with a linear density of 800 tex. The conductor consists of three bundles, each composed of 37 strands of tin-plated copper wire. By weight, the adhesive layer comprises 50 parts polyacrylate, 40 parts polyurethane, 9 parts talc, and 1 part vinyltriethoxysilane. The insulation layer, by weight, comprises 100 parts EPDM rubber, 12 parts flexible co-crosslinked coated sheet filler, 28 parts calcined kaolin, and oxide... The flexible co-crosslinked coated sheet filler consists of 5 parts zinc, 1 part stearic acid, 5 parts paraffin oil, 2 parts microcrystalline wax, 1.5 parts 2-mercaptobenzimidazole, 2 parts triallyl isocyanurate, 1 part N,N′-m-phenylene bismaleimide, and 2.8 parts dicumyl peroxide. It comprises wet-process mica powder, a vinyltriethoxysilane chemically bonded layer coated on the surface of the mica powder, and a flexible layer composed of maleic anhydride-grafted EPDM rubber and liquid EPDM rubber. The aspect ratio of the mica powder is 60, the thickness of the flexible layer is 8–15 nm, and the coating weight of the flexible layer is 5% of the mica powder mass. The mass ratio of maleic anhydride-grafted EPDM rubber to liquid EPDM rubber in the flexible layer is 1:3, and the number average molecular weight of the liquid EPDM rubber is 2.62 × 10⁻⁶.3 The anti-corrosion layer consists of 62 parts by weight of epoxy coal tar pitch, 28 parts of chlorinated polyethylene resin, 5 parts of mica powder, and 5 parts of silica.

[0031] Example 2

[0032] S1. Preparation of Flexible Co-crosslinked Coated Sheet Filler. Wet-process mica powder was selected as the sheet filler, with an aspect ratio of 80, a diameter-to-thickness ratio of 20 μm (D97), and a diameter-to-thickness ratio of 9 μm. Mica powder was dispersed at a solid content of 5% in a mixed solvent of ethanol and deionized water at a volume ratio of 9:1. The pH was adjusted to 5.0 with acetic acid. Vinyltriethoxysilane (4% by weight of mica powder) was added, and the mixture was refluxed at 80°C for 2 hours. After filtration, the mixture was washed three times with anhydrous ethanol and vacuum dried at 100°C for 3 hours to obtain silanized mica powder. Maleic anhydride-grafted EPDM rubber and liquid EPDM rubber were dissolved in xylene at a mass ratio of 1:4 to prepare a 5% (w / w) coating solution. The grafting rate of the maleic anhydride-grafted EPDM rubber was 0.8%, and the number-average molecular weight of the liquid EPDM rubber was 3.58 × 10⁻⁶. 3 ;Silanized mica powder was added to the coating solution and stirred at 60℃ for 2 hours. The solvent was removed by heating to 110℃ and then vacuum dried. The coating amount was controlled to be 8% of the mica powder mass to obtain a flexible co-crosslinked coated sheet filler with a thickness of 12-18 nm. The coating amount was determined to be 8.2% by thermogravimetric analysis.

[0033] S2. Conductor treatment and adhesive coating. Copper wire is selected as the conductor of the cable. The surface of the copper wire is tin-plated and pressed into a circular structure by a forming die. 37 tin-plated copper wires are twisted into a bundle, and 3 bundles are used as conductors. The adhesive material is evenly applied to the outer periphery of the conductor. During the application process, the material is heated at 55°C to obtain an adhesive conductor. By weight, the adhesive layer consists of 52 parts polyacrylate, 40 parts polyurethane, 7 parts talc, and 1 part vinyltriethoxysilane, with a dry film thickness of 25 μm.

[0034] S3. Insulating compound mixing (stage 1). By weight, the insulating compound consists of 100 parts EPDM rubber, 8 parts flexible co-crosslinked coated sheet filler, 35 parts calcined kaolin, 6 parts zinc oxide, 0.5 parts stearic acid, 3 parts paraffin oil, 3 parts microcrystalline wax, 2 parts 2-mercaptobenzimidazole, 3 parts triallyl isocyanurate, 1.5 parts N,N′-m-phenylene bismaleimide, and 3.5 parts dicumyl peroxide; wherein the EPDM rubber is ethylene-ide norbornene type, Mooney viscosity ML(1+4) 100℃ is 60, ethylene content is 62%, and ethylene... The content of norbornene is 5.0%; calcined kaolin is pretreated with vinyltriethoxysilane at a dosage of 2% of the mass of calcined kaolin; the first stage of mixing is carried out in an internal mixer. First, EPDM rubber is plasticized for 2 minutes, then zinc oxide, 2-mercaptobenzimidazole, stearic acid, microcrystalline wax and paraffin oil are added and mixed for 4 minutes. Then, calcined kaolin is added and mixed for 6 minutes. Finally, flexible co-crosslinked coated sheet filler is added and mixed for 8 minutes. The discharge temperature is 115℃. After discharge, the mixture is cooled and left to stand for 24 hours to obtain the first stage of rubber.

[0035] S4. Two-stage mixing of insulating rubber compound. The first stage of rubber compound is put into an internal mixer, and triallyl isocyanurate, N,N′-m-phenylene bismaleimide and dicumyl peroxide are added at a temperature not exceeding 95℃. The mixture is mixed for 6 minutes, passed through a thin sheet 5 times, and left to stand for 24 hours to obtain the insulating rubber compound. The Mooney scorch time t5 of the insulating rubber compound at 120℃ is measured to be 16 minutes.

[0036] S5. Extrusion of the insulation layer. An extruder is used to extrude the insulating compound onto the outer periphery of the bonding conductor. The extruder barrel temperature is controlled in four sections: 40℃ in the first section, 60℃ in the second, 75℃ in the third, and 85℃ in the fourth. The die head temperature is 90℃, and the extrusion pressure is controlled at 20MPa. The extruder head uses an extended flow channel with a convergence half-angle of 12° in the convergence section. The extrusion draw ratio is 1.22, ensuring the sheet-like filler is oriented radially along the cable in the convergence section of the flow channel. The nominal thickness of the insulation layer is 1.5mm. The extruded core enters a continuous vulcanizing tube. The steam temperature is controlled at 195℃, and the vulcanization time is 2.5 minutes. After vulcanization, the pressure and temperature are gradually reduced to obtain the insulated core.

[0037] S6. Stranding and Filling. The three insulated wire cores are stranded together to obtain the cable core. 12K polyacrylonitrile-based carbon fiber bundles with a linear density of 800 tex are used to fill the three gaps between the three insulated wire cores along the axial direction. One bundle is filled in each gap, for a total of three bundles. After filling, the cable core is wrapped tightly with overlapping halogen-free water-blocking tape.

[0038] S7. Extrusion of lead alloy sheath layer. Lead alloy material is extruded onto the outer periphery of the cable core using a continuous extrusion machine to form a lead alloy sheath layer. The continuous extrusion temperature is 290℃, and the nominal minimum thickness of the sheath is 3.0mm.

[0039] S8. Applying the anti-corrosion layer. By weight, the anti-corrosion layer material consists of 60 parts epoxy coal tar pitch, 30 parts chlorinated polyethylene resin, 6 parts mica powder, and 4 parts silica. The above materials are ground and dispersed to a fineness of no more than 60 μm, and then applied to the outer periphery of the lead alloy sheath by spraying in two coats. After curing, the dry film thickness of the anti-corrosion layer is 160 μm.

[0040] S9. Armoring. The cable after the anti-corrosion coating is applied is wrapped with tin-plated steel strip in an overlapping manner. The first wrap is clockwise and the second wrap is counterclockwise. The nominal thickness of the steel strip is 1.0mm and the overlap rate is not less than 30%.

[0041] A submersible pump cable is manufactured using the above-mentioned method. From the inside out, the cable comprises a tin-plated copper conductor, an adhesive layer, an insulation layer, a carbon fiber filler layer, a lead alloy sheath layer, an anti-corrosion layer, and a tin-plated steel tape armor layer. The conductor and insulation layer are bonded together by the adhesive layer. The filler layer consists of three bundles of polyacrylonitrile-based carbon fibers filled in three gaps between three insulated cores. The carbon fiber bundles are 12K with a linear density of 800 tex. The conductor consists of three bundles, each composed of 37 strands of tin-plated copper wire. By weight, the adhesive layer comprises 52 parts polyacrylate, 40 parts polyurethane, 7 parts talc, and 1 part vinyltriethoxysilane. By weight, the insulation layer comprises 100 parts EPDM rubber, 8 parts flexible co-crosslinked coated sheet filler, 35 parts calcined kaolin, and 6 parts zinc oxide. The flexible co-crosslinked coated sheet filler is composed of 0.5 parts stearic acid, 3 parts paraffin oil, 3 parts microcrystalline wax, 2 parts 2-mercaptobenzimidazole, 3 parts triallyl isocyanurate, 1.5 parts N,N′-m-phenylene bismaleimide, and 3.5 parts dicumyl peroxide. The flexible co-crosslinked coated sheet filler consists of wet-process mica powder, a vinyltriethoxysilane chemically bonded layer coated on the surface of the mica powder, and a flexible layer composed of maleic anhydride-grafted EPDM rubber and liquid EPDM rubber coated on the outside. The aspect ratio of the mica powder is 80, the thickness of the flexible layer is 12-18 nm, and the coating amount of the flexible layer is 8% of the mass of the mica powder. The mass ratio of maleic anhydride-grafted EPDM rubber to liquid EPDM rubber in the flexible layer is 1:4, and the number average molecular weight of the liquid EPDM rubber is 3.58 × 10⁻⁶. 3 The anti-corrosion layer consists of 60 parts by weight of epoxy coal tar pitch, 30 parts of chlorinated polyethylene resin, 6 parts of mica powder and 4 parts of silica.

[0042] Example 3

[0043] S1. Preparation of Flexible Co-crosslinked Coated Sheet Filler. Wet-processed mica powder was selected as the sheet filler, with an aspect ratio of 50, a D97 of 30 μm, and a D50 of 15 μm. Mica powder was dispersed at a solid content of 5% in a mixed solvent of ethanol and deionized water at a volume ratio of 9:1. The pH was adjusted to 4.0 with acetic acid. Vinyltriethoxysilane (2% by weight of mica powder) was added, and the mixture was refluxed at 75°C for 4 hours. After filtration, the mixture was washed three times with anhydrous ethanol and vacuum dried at 80°C for 5 hours to obtain silanized mica powder. Maleic anhydride-grafted EPDM rubber and liquid EPDM rubber were dissolved in xylene at a mass ratio of 1:2 to prepare a 5% (w / w) coating solution. The grafting rate of the maleic anhydride-grafted EPDM rubber was 1.5%, and the number average molecular weight of the liquid EPDM rubber was 2.16 × 10⁻⁶. 3 ; Add silanized mica powder to the coating solution, stir at 60℃ for 2h, heat to 110℃ to remove solvent, vacuum dry, control the coating amount to 3% of the mica powder mass, and obtain flexible co-crosslinked coated sheet filler with a thickness of 5-10nm; thermogravimetric analysis shows that the coating amount is 3.2%.

[0044] S2. Conductor treatment and adhesive coating. Copper wire is selected as the conductor of the cable. The surface of the copper wire is tin-plated and pressed into a circular structure by a forming die. 37 tin-plated copper wires are twisted into a bundle, and 3 bundles are used as conductors. The adhesive material is evenly applied to the outer periphery of the conductor. During the application process, the heating temperature is set at 60℃ to obtain an adhesive conductor. By weight, the adhesive layer consists of 45 parts polyacrylate, 44 parts polyurethane, 10 parts talc, and 1 part vinyltriethoxysilane, with a dry film thickness of 50μm.

[0045] S3. Insulating compound mixing (stage 1). By weight, the insulating compound consists of 100 parts EPDM rubber, 20 parts flexible co-crosslinked coated sheet filler, 20 parts calcined kaolin, 4 parts zinc oxide, 1.5 parts stearic acid, 8 parts paraffin oil, 1 part microcrystalline wax, 1 part 2-mercaptobenzimidazole, 1.5 parts triallyl isocyanurate, 0.5 parts N,N′-m-phenylene bismaleimide, and 2.5 parts dicumyl peroxide; wherein the EPDM rubber is ethylene-ide norbornene type, with a Mooney viscosity ML(1+4) of 40 at 100℃ and an ethylene content of 55%. The content of ethylene norbornene is 4.0%; calcined kaolin is pretreated with vinyltriethoxysilane at a dosage of 1.5% of the mass of calcined kaolin; the first stage of mixing is carried out in an internal mixer. First, EPDM rubber is plasticized for 2 minutes, then zinc oxide, 2-mercaptobenzimidazole, stearic acid, microcrystalline wax and paraffin oil are added and mixed for 4 minutes, then calcined kaolin is added and mixed for 6 minutes, then flexible co-crosslinked coated sheet filler is added and mixed for 6 minutes. The discharge temperature is 105℃, and after discharge, it is cooled and left to stand for 24 hours to obtain the first stage of rubber.

[0046] S4. Two-stage mixing of insulating rubber compound. The first stage of rubber compound is put into an internal mixer, and triallyl isocyanurate, N,N′-m-phenylene bismaleimide and dicumyl peroxide are added at a temperature not exceeding 95℃. The mixture is mixed for 6 minutes, passed through a thin sheet 3 times, and left to stand for 4 hours to obtain the insulating rubber compound. The Mooney scorch time t5 of the insulating rubber compound at 120℃ is measured to be 28 minutes.

[0047] S5. Extrusion of the insulation layer. An extruder is used to extrude the insulating compound onto the outer periphery of the bonding conductor. The extruder barrel temperature is controlled in four sections: 50℃ in the first section, 70℃ in the second, 85℃ in the third, and 95℃ in the fourth. The die head temperature is 95℃, and the extrusion pressure is controlled at 15MPa. The extruder head uses an extended flow channel with a convergence half-angle of 18° in the convergence section. The extrusion draw ratio is 1.28, ensuring the sheet-like filler is oriented radially along the cable in the convergence section of the flow channel. The nominal thickness of the insulation layer is 1.0mm. The extruded wire core enters a continuous vulcanizing tube. The steam temperature is controlled at 180℃, and the vulcanization time is 2 minutes. After vulcanization, the pressure and temperature are gradually reduced to obtain the insulated wire core.

[0048] S6. Stranding and Filling. The three insulated wire cores are stranded together to obtain the cable core. 12K polyacrylonitrile-based carbon fiber bundles with a linear density of 800 tex are used to fill the three gaps between the three insulated wire cores along the axial direction. One bundle is filled in each gap, for a total of three bundles. After filling, the cable core is wrapped tightly with overlapping halogen-free water-blocking tape.

[0049] S7. Extruded lead alloy sheath layer. A continuous extrusion mill is used to extrude lead alloy material onto the outer periphery of the cable core to form a lead alloy sheath layer. The continuous extrusion temperature is 390℃, and the nominal minimum thickness of the sheath is 2.5mm.

[0050] S8. Applying the anti-corrosion layer. By weight, the anti-corrosion layer material consists of 70 parts epoxy coal tar pitch, 17 parts chlorinated polyethylene resin, 8 parts mica powder, and 5 parts silica. The above materials are ground and dispersed to a fineness of no more than 60 μm, and then applied to the outer periphery of the lead alloy sheath by spraying in two coats. After curing, the dry film thickness of the anti-corrosion layer is 140 μm.

[0051] S9. Armoring. The cable after the anti-corrosion coating is applied is wrapped with tin-plated steel strip in an overlapping manner. The first wrap is clockwise and the second wrap is counterclockwise. The nominal thickness of the steel strip is 1.0mm and the overlap rate is not less than 35%.

[0052] A submersible pump cable, manufactured using the above-mentioned method, comprises, from the inside out, a tin-plated copper conductor, an adhesive layer, an insulation layer, a carbon fiber filler layer, a lead alloy sheath layer, an anti-corrosion layer, and a tin-plated steel tape armor layer. The conductor and insulation layer are bonded together by the adhesive layer. The filler layer consists of three bundles of polyacrylonitrile-based carbon fibers filled in three gaps between three insulated cores; the carbon fiber bundles are 12K with a linear density of 800 tex. The conductor consists of three bundles, each composed of 37 strands of tin-plated copper wire. By weight, the adhesive layer comprises 45 parts polyacrylate, 44 parts polyurethane, 10 parts talc, and 1 part vinyltriethoxysilane. The insulation layer, by weight, comprises 100 parts EPDM rubber, 20 parts flexible co-crosslinked coated sheet filler, 20 parts calcined kaolin, and 4 parts zinc oxide. The flexible co-crosslinked coated sheet filler consists of wet-process mica powder, a vinyltriethoxysilane chemically bonded layer coated on the surface of the mica powder, and a flexible layer composed of maleic anhydride-grafted EPDM rubber and liquid EPDM rubber coated on the outside. The mica powder has an aspect ratio of 50, the flexible layer has a thickness of 5-10 nm, and the coating amount of the flexible layer is 3% of the mass of the mica powder. The mass ratio of maleic anhydride-grafted EPDM rubber to liquid EPDM rubber in the flexible layer is 1:2, and the number average molecular weight of the liquid EPDM rubber is 2.16 × 10⁻⁶. 3 The anti-corrosion layer consists of 70 parts by weight of epoxy coal tar pitch, 17 parts of chlorinated polyethylene resin, 8 parts of mica powder and 5 parts of silica.

[0053] Comparative Example 1 Insulation layer samples were prepared according to a formula of a high- and low-temperature resistant modified EPDM composite cable material using a simple blend of maleic anhydride-grafted EPDM rubber and mica. The raw materials, by weight, included: 55 parts maleic anhydride-grafted EPDM rubber, 45 parts methyl vinyl phenyl silicone rubber, 6.2 parts ethylene-octene copolymer, 13 parts silica, 22 parts mica, 32 parts calcined clay, 40 parts hydrotalcite, and 3.5 parts stearic acid. The ingredients are: 1 part zinc oxide, 5.2 parts sulfur, 1.6 parts di(2,4-dichlorobenzoyl) peroxide, 1.45 parts ethylene glycol, 1 part polyethylene glycol, 1.6 parts 3-aminopropyltrimethoxysilane, 2 parts accelerator, 5.3 parts plasticizer, and 2.6 parts antioxidant. The accelerator is a combination of accelerator TMTD and accelerator DM in a 1:1 mass ratio, and the antioxidant is a combination of antioxidant OD and antioxidant AW in a 1:1 mass ratio.

[0054] The plasticizer was prepared according to the following process: 0.0058 parts by weight of lead oxide were added to 42 parts by weight of glycerol and stirred evenly. 25 parts by weight of soybean oil were added, stirred, and heated to 215°C for 4.3 hours. The mixture was then cooled in ice water to obtain soybean oil monoglyceride. 40 parts by weight of the obtained soybean oil monoglyceride were mixed with 36 parts by weight of maleic anhydride and stirred evenly. 0.018 parts by weight of tetrabutyl titanate and 12 parts by weight of isooctanol were added. The mixture was stirred and heated to 200°C under nitrogen protection for 12.6 hours. After the reaction was completed, the mixture was evacuated for 4.2 hours, then cooled, washed, and dried to obtain the plasticizer.

[0055] The above raw materials were mixed in an internal mixer according to the specified ratio, sheeted on an open mill, and vulcanized in a flat vulcanizing machine at a vulcanization temperature of 160°C for 20 minutes to obtain an insulation layer sample. Except for the insulating rubber compound, which is the same as in this comparative example, the other structural layers of the cable and the preparation conditions are the same as in Example 1.

[0056] Comparative Example 2 Based on Example 1, 12 parts of wet mica powder without any surface treatment were replaced with flexible co-crosslinked coated sheet filler, and 3 parts of maleic anhydride-grafted EPDM rubber were added separately. That is, the rubber compound was added by directly blending maleic anhydride-grafted EPDM rubber with mica. The aspect ratio of mica and the grade of maleic anhydride-grafted EPDM rubber were the same as in Example 1. The mica was not silanized and did not form a flexible coating layer. Everything else was the same as in Example 1.

[0057] Comparative Example 3 Based on Example 1, the vinyltriethoxysilane in S1 was replaced with an equal amount of 3-aminopropyltrimethoxysilane, and the remaining silanization conditions and flexible layer coating conditions were the same as in Example 1.

[0058] Comparative Example 4 Based on Example 1, S1 only involves silanization without flexible layer coating. That is, mica powder is directly added as a filler after being treated with vinyltriethoxysilane. The rest is the same as in Example 1.

[0059] Comparative Example 5 Based on Example 1, the original 2.8 parts of dicumyl peroxide, 2 parts of triallyl isocyanurate, and 1 part of N,N′-m-phenylene bismaleimide were replaced with 1.8 parts of dicumyl peroxide and 1 part of triallyl isocyanurate in the insulating compound, and the rest were the same as in Example 1.

[0060] Comparative Example 6 The insulating compound consists of 100 parts of EPDM rubber, 30 parts of calcined kaolin, 5 parts of zinc oxide, 1 part of stearic acid, 5 parts of paraffin oil, 1.5 parts of 2-mercaptobenzimidazole, 2.0 parts of dicumyl peroxide, and 1 part of triallyl isocyanurate, which is the conventional insulating compound for submersible pump cables. The rest is the same as in Example 1.

[0061] (1) Rapid gas decompression test: Place the insulation layer sample in an autoclave, introduce methane to a pressure of 15 MPa, raise the temperature to 150 °C, and maintain it for 72 h to fully saturate the sample with gas; determine the amount of methane absorbed in the saturated sample by water displacement method; then reduce the pressure to atmospheric pressure at a rate of 3 MPa / min, take out the sample, and adjust it at 23 °C for 24 h according to GB / T2941-2006 "General Procedure for Sample Preparation and Conditioning of Rubber Physical Test Methods"; observe the bubbling on the sample surface, and observe the cross section along the transverse direction. The bubbling level is evaluated according to the following levels: Level 0: No visible bubbling on the surface and no holes or cracks on the cross section; Level 1: No visible bubbling on the surface but sporadic holes and no cracks on the cross section; Level 2: Individual small protrusions are visible on the surface and obvious holes on the cross section but no cracks; Level 3: Bubbling is visible on the surface and cracks are present on the cross section; Level 4: Dense bubbling on the surface and local cracking; Level 5: Surface cracking or delamination.

[0062] (2) Percentage of cross-sectional hole area: Take the above-mentioned cut sample and use microscopic image analysis to determine the proportion of the total cross-sectional hole area to the total cross-sectional area.

[0063] (3) Change rate of outer diameter before and after decompression: The diameter of the sample was measured at 23℃ within 1 hour after the decompression was completed and compared with the diameter at the same position before the test to calculate its change rate.

[0064] (4) Volume resistivity at 90℃: determined according to GB / T1692-2008 "Determination of Insulation Resistivity of Vulcanized Rubber".

[0065] (5) Dielectric loss factor at 90℃ and 50Hz: Determined according to GB / T1409-2006 "Recommended method for measuring the permittivity and dielectric loss factor of electrical insulation materials at power frequency, audio frequency and high frequency (including meter wavelength)".

[0066] (6) Tensile strength and elongation at break: determined according to GB / T528-2009 "Determination of tensile stress-strain properties of vulcanized rubber or thermoplastic rubber".

[0067] (7) Compression set at 180℃ for 24 hours: determined according to GB / T7759.1-2015 "Determination of compression set of vulcanized rubber or thermoplastic rubber - Part 1: Under normal and high temperature conditions".

[0068] (8) Neutral salt spray test: The neutral salt spray test shall be carried out in accordance with GB / T10125-2021 “Artificial atmosphere corrosion test salt spray test”. The test solution is a sodium chloride solution with a mass concentration of 50 g / L. The temperature inside the chamber is 35℃ and the spraying is continuous for 1000 h. After the test, the sample shall be taken out, rinsed with clean water and dried at room temperature. The corrosion of the tin-plated steel strip armor layer shall be checked. The percentage of the corrosion area to the outer surface area of ​​the armor layer shall be determined by image analysis. Then the armor layer shall be peeled off and the anti-corrosion layer shall be observed for blistering, cracking and peeling.

[0069] (9) Simulated well fluid high temperature and high pressure immersion test: Take a cable sample with a length of 500 mm, seal both ends with sealing joints, place it in a high temperature and high pressure reactor, inject simulated well fluid into the reactor, the simulated well fluid is an aqueous solution containing 50 g / L sodium chloride, 5 g / L calcium chloride and 3 g / L magnesium chloride; introduce carbon dioxide into the reactor until the partial pressure is 2.0 MPa, introduce hydrogen sulfide until the partial pressure is 0.1 MPa, raise the temperature to 150℃, and immerse at constant temperature and pressure for 30 days; after the test, take out the sample, rinse and dry it, peel off the armor layer to observe the blistering and peeling of the anti-corrosion layer, and determine the adhesion of the anti-corrosion layer after immersion according to the method described in (10); then remove the anti-corrosion layer, observe the surface condition of the lead alloy sheath, measure the maximum depth of the corrosion pit, and calculate the corrosion rate of the lead alloy sheath based on the pit depth and immersion time.

[0070] (10) Adhesion test of anti-corrosion layer: The adhesion between the anti-corrosion layer and the lead alloy sheath was determined according to GB / T5210-2006 "Adhesion test of paint and varnish by pull-out method". The test was conducted once before the simulated well fluid immersion test and once after the immersion test. The ratio of the adhesion after immersion to the adhesion before immersion was taken as the adhesion retention rate.

[0071] Table 1: Resistance to rapid gas decompression

[0072] Table 2: Electrical and Mechanical Properties

[0073] Table 3: Corrosion Resistance

[0074] As shown in Tables 1 and 2, the insulation layers of Examples 1 to 3 are significantly superior to their counterparts in terms of blistering level, cross-sectional cavity area ratio, and outer diameter change rate after rapid gas decompression. They also maintain high volume resistivity, low dielectric loss factor, and good compression set. This indicates that by simultaneously employing flexible co-crosslinked sheet fillers and a high-crosslink density peroxide vulcanization system in the insulating compound, the insulation layer is less prone to blistering and cracking under high-pressure gas intrusion and rapid decompression, and its electrical and mechanical properties remain undamaged. Blistering damage to the insulation layer has been recorded on-site as an independent form of corrosion damage during submersible pump jacking operations. Cable damage that needs to be checked during cable jacking includes deformation, breakage, wear, blistering, and corrosion. When the steel tape armor is missing, the sheath will swell and rupture due to sudden pressure changes. This example specifically addresses this type of damage.

[0075] Comparative Example 1 is a cable material formulation using maleic anhydride-grafted EPDM rubber as the base rubber and directly blended with mica. In this formulation, the amount of maleic anhydride-grafted EPDM rubber is 40-60 parts by weight, and mica is a directly added filler, used in amounts of 10-35 parts by weight. Mica is used in combination with silica, calcined clay, and hydrotalcite to improve physical properties, electrical insulation properties, and gas barrier properties. The results of this comparative example are: a foaming grade of 4, a cross-sectional cavity area ratio of 11.2%, and a change in outer diameter before and after pressure reduction of 7.8%, where the cross-sectional cavity area ratio is 14 times that of Example 1. Its saturated gas adsorption capacity is 46.5 mg / g. -1 It is 2.5 times that of Example 1. The tensile strength and elongation at break of this formulation are 16.5 MPa and 452.0%, respectively; however, its compression set at 180°C for 24 hours reaches 38.6%.

[0076] Comparative Example 2 involved simply blending maleic anhydride-grafted EPDM rubber with mica in the rubber compound of Example 1 without silanization or flexible layer coating. In other words, these two raw materials were introduced separately into the insulation system of this invention. The results showed a foaming grade of 3, a cross-sectional cavity area ratio of 5.6%, and an outer diameter change rate of 4.1% before and after decompression, all significantly worse than Example 1; while its saturated gas adsorption was 19.2 mg / g. -1 Compared with 18.6 mg / g in Example 1 -1 The results are essentially the same. This set of data shows that the total amount of gas adsorbed did not increase after simple blending, but foaming damage was significantly aggravated. This comparison also shows that simply introducing the raw materials in this type of formulation in their own way not only fails to achieve the effects of this invention, but also makes the resistance to rapid gas decompression lower than that of conventional rubber compounds without flake fillers.

[0077] Comparative Example 3, which replaced vinyltriethoxysilane with 3-aminopropyltrimethoxysilane, showed a foaming grade of 2, a void area ratio of 3.4%, and a compression set of 21.2% at 180°C for 24 hours, all inferior to Example 1. The amino group in aminosilane is a basic group, which accelerates the ineffective decomposition of peroxide free radicals and forms localized undersulfurization near the sheet, resulting in a low crosslinking density in the interface region and reduced anti-cavitation ability during pressure relief. Simultaneously, the amino group does not participate in peroxide crosslinking, resulting in a lack of covalent bonding between the interface layer and the matrix. The coupling agent used in the existing formulation is 3-aminopropyltrimethoxysilane, whose vulcanization system is a composite of sulfur and di(2,4-dichlorobenzoyl) peroxide, which works in conjunction with this silane. The vulcanization system of this invention is a high crosslinking density system mainly composed of dicumyl peroxide and combined with triallyl isocyanurate and N,N′-m-phenylene bismaleimide, which is incompatible with this system. Therefore, the practice of treating sheet fillers with aminosilane cannot be followed. The vinyl groups in vinylsilanes can co-crosslink with the matrix during vulcanization, incorporating the interface layer into the crosslinking network. This is the premise for this scheme to simultaneously improve crosslinking density and improve interfacial bonding.

[0078] Comparative Example 4, which only silanized without coating the flexible layer, resulted in a foaming grade of 2 and a cross-sectional void area ratio of 3.7%, which was an improvement over Comparative Example 2 but still significantly worse than Example 1. Silanization sealed the acidic sites on the sheet surface and solved the interference of filler on peroxide crosslinking, but it did not solve the abrupt change in modulus between the inorganic sheet and the rubber matrix; the interface would still preferentially debond during decompression expansion. The only difference between Comparative Example 4 and Example 1 was the presence or absence of a flexible layer with a thickness of 5–20 nm, indicating that this flexible layer is a key structural element determining whether the interface can withstand decompression expansion.

[0079] Comparative Example 5 maintained flexible coating while reducing crosslinking density, achieving a foaming grade of 1 and a cross-sectional cavity area ratio of 1.9%. It outperformed Comparative Examples 2 to 4 in terms of resistance to decompression damage, but its compression set at 180°C for 24 hours was 26.5%, significantly higher than the 16.8% of Example 1, and its volume resistivity was 2.6 × 10⁻⁶. 13 The Ω·m value is also lower than that of Example 1. This result indicates that flexible coating can prevent the interface of the sheet filler from becoming a nucleation site. However, when the cross-linked network is not strong enough to resist cavitation expansion, pores will still appear during the decompression process, and low cross-linking density will cause the insulation layer to deform and degrade its electrical properties at high temperatures.

[0080] Comparative Example 6 is a conventional submersible pump cable insulation compound. Its foaming rating is 3, the cross-sectional cavity area ratio is 5.8%, and the outer diameter change rate before and after decompression is 4.2%, all three indicators being poor. The calcined kaolin in the conventional compound is also a flaky filler, but its aspect ratio is much lower than the mica powder used in this solution, resulting in limited barrier effect. Furthermore, its interface can also become a nucleation site for gas, consistent with its poor resistance to decompression damage.

[0081] The saturated gas adsorption capacities of Examples 1, 2, and 3 were 18.6, 20.4, and 16.8 mg·g, respectively. -1 The amount of gas absorbed decreases with increasing amount of sheet filler, but the resistance to decompression damage is not directly proportional to the amount of gas absorbed. Example 3 showed a lower amount of gas absorbed than Example 1, but a slightly higher foaming level and pore size ratio, indicating that the total amount of gas entering the insulation layer and the degree of damage after decompression are two separately controllable quantities. This scheme uses different control paths for both: the amount of sheet filler and its aspect ratio control the total amount of gas absorbed and permeated, while the flexible co-crosslinking coating layer and the high-crosslinking density vulcanization system control the nucleation site and pore expansion resistance. Comparative Example 1 loses control over both paths simultaneously. Its methyl vinyl phenyl silicone rubber phase has a much larger free volume than EPDM rubber, so the gas preferentially dissolves and accumulates in this phase. The phase interface between the two elastomers also provides numerous nucleation sites, thus the amount of gas absorbed and the foaming damage reach their maximum simultaneously. In this invention, a chemically bonded layer composed of vinyl silane and EPDM rubber grafted with maleic anhydride are sequentially set on the surface of the sheet filler. 3 ~6.0×10 3 A flexible layer composed of liquid EPDM rubber is used. A chemically bonded layer seals acidic sites on the sheet surface and introduces vinyl groups that can participate in free radical reactions. The flexible layer fills the free volume at the interface and allows for a smooth transition of modulus from the sheet to the matrix. The ethylene-bis(norbornene) unsaturated bonds retained in the flexible layer allow it to co-crosslink with the matrix during vulcanization, becoming part of the crosslinked network. A high-crosslink density vulcanization system is then constructed using triallyl isocyanurate and N,N′-m-phenylene bismaleimide in combination with dicumyl peroxide, improving the network's resistance to hole expansion. The insulating layer thus achieves lower total adsorption, fewer nucleation sites, and higher resistance to hole expansion. The bubbling grade and the percentage of void area at the fracture surface are reduced from level 4 to level 0 and from 11.2% to 0.8%, respectively, compared to this technical solution.

[0082] As shown in Table 3, after 1000 hours of neutral salt spray testing, the corrosion area of ​​the armor layer of the cables in Examples 1 to 3 was 0.8%–1.0%; after 30 days of immersion in simulated well fluid at high temperature and high pressure, the corrosion rate of the lead alloy sheath was 0.0058–0.0069 mm·a. -1The adhesion retention rate of the anti-corrosion layer was 91.7%–94.1%, with no blistering or peeling. No visible pitting was observed on the lead alloy sheath surface. This indicates that the cable of the present invention exhibits excellent corrosion resistance in high-temperature, high-pressure well fluid environments containing chloride ions, carbon dioxide, and hydrogen sulfide, meeting the requirements for long-term operation of submersible pump cables in wells. Comparative Examples 1 to 6 have different insulation materials than the examples, but the structure and preparation conditions of the lead alloy sheath, anti-corrosion layer, and armor layer are the same as in Example 1. The test results of the three corrosion resistance indicators are at the same level as in Example 1, with the numerical differences being experimental dispersion. This result demonstrates that the improvements made to the insulation material and insulation preparation process in this invention have not adversely affected the corrosion resistance of the cable, and the outer protective system of the cable remains intact.

[0083] The embodiments described above are only some, not all, of the embodiments of the present invention. The detailed description of the embodiments of the present invention is not intended to limit the scope of the claimed invention, but merely to illustrate preferred embodiments. All other embodiments obtained by those skilled in the art through related deductions and substitutions based on the inventive concept, without inventive effort, are within the scope of protection of the present invention.

Claims

1. A method for preparing a corrosion-resistant submersible pump cable, characterized in that, Includes the following steps: S1. Conductor processing: Select copper wire as the conductor of the cable, tin-plat the surface of the copper wire, and twist the tin-plated copper wire into a bundle to obtain a rough-processed conductor. S2. Applying adhesive layer: Apply the adhesive layer material evenly to the outer periphery of the rough-processed conductor. Heating is required during the application process. The heating temperature range is set to 55-60℃ to obtain the adhesive conductor. S3. Preparation of flexible co-crosslinked coated sheet filler: The sheet filler is dispersed at a solid content of 5% in a mixed solvent of ethanol and deionized water at a volume ratio of 9:

1. The pH value is adjusted to 4-5 with acetic acid. Vinyltriethoxysilane at a mass ratio of 2%-4% of the sheet filler is added. The mixture is refluxed at 75-80℃ for 2-4 hours. After filtration, washing, and drying, silanized sheet filler is obtained. Maleic anhydride-grafted EPDM rubber and liquid EPDM rubber are dissolved in xylene at a mass ratio of 1:2-1:4 to prepare a coating solution with a mass fraction of 5%. The silanized sheet filler is added to the coating solution. The mixture is stirred at 60℃ for 2 hours and then heated to 110℃ to remove the solvent. The coating amount is controlled to be 3%-8% of the mass of the sheet filler to obtain flexible co-crosslinked coated sheet filler. S4. Mixing: By weight, 100 parts of EPDM rubber are plasticized for 2 minutes, then 4-6 parts of zinc oxide, 1-2 parts of 2-mercaptobenzimidazole, 0.5-1.5 parts of stearic acid, 1-3 parts of microcrystalline wax, 3-8 parts of paraffin oil, and 20-35 parts of calcined kaolin are added sequentially and mixed. Then, 8-20 parts of the flexible co-crosslinked coated sheet filler are added and mixed for 6-8 minutes. After discharge and cooling, a first-stage rubber is obtained. The first-stage rubber is then mixed with 2.5-3.5 parts of peroxide vulcanizing agent, 1.5-3 parts of triallyl isocyanurate, and 0.5-1.5 parts of N,N′-m-phenylene bismaleimide at a temperature not exceeding 95°C for a second-stage mixing. After thinning and sheeting, the insulating rubber compound is obtained. S5. Extruding the insulation layer: The insulating rubber material is extruded onto the outer periphery of the bonded conductor using an extruder. The extruder head adopts an extended flow channel, which makes the sheet filler oriented along the radial direction of the cable. The extruded wire core enters the continuous vulcanization tube for vulcanization. After vulcanization, the pressure is gradually reduced and the temperature is gradually reduced to obtain the insulated wire core. S6. Stranding and filling: The insulated wire cores are stranded together to obtain the cable core. During the stranding process, carbon fiber bundles are filled into the gaps between the cable cores. After filling, the cable cores are tied tightly with halogen-free water-blocking tape. S7. Extrusion of the sheath layer: Lead alloy material is extruded onto the outer periphery of the cable core using a continuous lead extrusion machine to form a sheath layer. The continuous extrusion temperature range is 290 to 390°C, resulting in a coarse cable. S8. Applying anti-corrosion layer: Applying anti-corrosion material evenly to the outer periphery of the coarse cable to form the anti-corrosion layer, thus obtaining an anti-corrosion cable; S9. Armoring: The anti-corrosion cable is wrapped with tin-plated steel strip in an overlapping manner to obtain the submersible pump cable.

2. The method for preparing the corrosion-resistant submersible pump cable according to claim 1, characterized in that, In S2, the adhesive layer material is composed of 45-55 parts polyacrylate, 35-45 parts polyurethane, 5-12 parts talc, and 0.5-1.5 parts vinyltriethoxysilane by weight.

3. The method for preparing the corrosion-resistant submersible pump cable according to claim 1, characterized in that, In S3, the sheet-like filler is wet-processed mica powder or organo-modified montmorillonite, the aspect ratio of the sheet-like filler is not less than 50, and the particle size distribution D97 is not greater than 30 μm; the grafting rate of the maleic anhydride-grafted EPDM rubber is 0.5%–1.5%; the number-average molecular weight of the liquid EPDM rubber is 2.0 × 10⁻⁶. 3 ~6.0×10 3 The liquid EPDM rubber retains ethylene-bis(norbornene) unsaturated bonds.

4. The method for preparing the corrosion-resistant submersible pump cable according to claim 1, characterized in that, In S4, the EPDM rubber is of the ethylene-ide norbornene type, with a Mooney viscosity ML(1+4) of 40-60 at 100°C and an ethylene content of 55%-65%. The calcined kaolin is pretreated with 1.5% to 2% of its own mass of vinyltriethoxysilane for surface pretreatment; The peroxide sulfiding agent is dicumyl peroxide or bis-tert-butylperoxide-isopropylbenzene; The discharge temperature of the first stage of compounding should not exceed 120℃, and the mixture should be cooled and left to stand for 24 hours after discharge. The Mooney scorch time t5 of the insulating compound obtained after two-stage mixing is not less than 15 min at 120℃.

5. The method for preparing the corrosion-resistant submersible pump cable according to claim 1, characterized in that, In S5, the barrel temperature of the extruder is controlled in four sections: 40-50℃, 60-70℃, 75-85℃, and 85-95℃, respectively; the die head temperature is 90-95℃; and the extrusion pressure is 15-20MPa. The convergence half-angle of the extended flow channel is 10° to 20°, and the extrusion draw ratio is 1.20 to 1.

30. The nominal thickness of the insulating layer is 1.0 to 2.0 mm; The steam temperature of the continuous vulcanizing tube is 180–195°C, and the vulcanization time is 2–5 min.

6. The method for preparing the corrosion-resistant submersible pump cable according to claim 1, characterized in that, In S7, the nominal minimum thickness of the sheath layer is 2.5 to 3.0 mm; In S8, the anti-corrosion material is composed of 60-70 parts of epoxy coal tar pitch, 15-30 parts of chlorinated polyethylene resin, 5-8 parts of mica powder and 4-8 parts of silicon dioxide by weight. In S9, the tin-plated steel strip is wrapped and armored twice. The first wrap is clockwise and the second wrap is counterclockwise. The nominal thickness of the steel strip is 1.0 mm and the overlap rate is not less than 30%.

7. The method for preparing the corrosion-resistant submersible pump cable according to claim 1, characterized in that, In S6, the carbon fiber bundle is a polyacrylonitrile-based carbon fiber bundle with a bundle specification of 12K and a linear density of 800 tex; The number of insulating wire cores is 3, and the carbon fiber bundles are respectively filled in the three gaps between the 3 insulating wire cores along the axial direction, with each gap filled with 1 bundle.

8. A corrosion-resistant submersible pump cable, characterized in that, The submersible pump cable is manufactured using the method for preparing a corrosion-resistant submersible pump cable according to any one of claims 1 to 7. The cable comprises, from the inside out, a conductor, an adhesive layer, an insulation layer, a filler layer, a sheath layer, an anti-corrosion layer, and an armor layer in no fewer than three bundles. The conductor and the insulating layer are bonded together by the adhesive layer; The space between the insulating layer and the sheath layer is filled with carbon fiber bundles; The number of conductors is not less than 3 bundles and each bundle of conductors is made of not less than 26 strands of tin-plated copper wires twisted together; The insulating layer is made of insulating adhesive, in which flexible co-crosslinked coated sheet filler is dispersed. The flexible co-crosslinked coated sheet filler consists of sheet filler, a vinyl silane chemically bonded layer coated on the surface of the sheet filler, and a flexible layer coated outside the chemically bonded layer. The flexible layer is made of maleic anhydride-grafted EPDM rubber and liquid EPDM rubber. The flexible layer retains ethylene-methyl-3-norbornene unsaturated bonds and co-crosslinks with the matrix of the insulating layer through the unsaturated bonds.

9. The corrosion-resistant submersible pump cable according to claim 8, characterized in that, The thickness of the flexible layer is 5-20 nm, the coating amount of the flexible layer is 3%-8% of the mass of the sheet filler, and the mass ratio of maleic anhydride-grafted EPDM rubber to liquid EPDM rubber in the flexible layer is 1:2-1:

4.

10. The corrosion-resistant submersible pump cable according to claim 8, characterized in that, Each bundle of the conductors has a circular cross-sectional area, and the cable has an oblong cross-section. Alternatively, the cross-section of each bundle of conductors may be fan-shaped, and the cross-section of the cable may be circular.