A high-nickel NCM811 / LLZO all-solid-state composite electrode with an in-situ constructed interface transition layer and its preparation method

By constructing a lithium-containing inorganic transition layer in situ in the NCM811/LLZO composite cathode, the problems of limited solid-solid contact area and interface debonding are solved, realizing a high-stability and low-impedance all-solid-state composite electrode suitable for high-energy-density all-solid-state lithium batteries.

CN123120635APending Publication Date: 2026-11-17ZHENGZHOU UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611313136.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-27
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

In NCM811/LLZO composite cathodes, the solid-solid contact area is limited and there are many interfacial pores. During cycling, the interface debonding and contact loss are severe. Traditional pre-coating methods are difficult to improve internal contact, and high-temperature co-firing can easily damage the cathode structure.

Method used

By constructing a lithium-containing inorganic transition layer in situ in the actual contact area of ​​NCM811/LLZO, the contact gap is filled by liquid precursor wetting and capillary action to form a continuous lithium-ion conductive bridge, which isolates side reactions and buffers chemical-mechanical mismatch. Low-temperature heat treatment is used to avoid structural damage.

Benefits of technology

It increases the solid-solid contact area, reduces interfacial impedance, improves interfacial structural stability, reduces contact loss during cycling, and avoids the negative effects of high-temperature co-firing.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure FT_1
    Figure FT_1
  • Figure FT_2
    Figure FT_2
  • Figure FT_3
    Figure FT_3
Patent Text Reader

Abstract

This invention belongs to the field of all-solid-state lithium battery electrode materials and solid-solid interface engineering technology, specifically relating to a high-nickel NCM811 / LLZO all-solid-state composite electrode with an in-situ constructed interface transition layer and its preparation method. The composite electrode of this invention includes a positive electrode active material, a solid electrolyte, and an in-situ interface transition layer located at the contact region between the two; depending on electron transport requirements, it may further include a conductive carbon material. The solid electrolyte is Li7La3Zr2O. 12 Or a cubic phase derivative doped with elements such as Ta, Nb, Al, and Ga. The positive electrode active material is NCM811, or a layered oxide of NCM or NCMA with a Ni content of not less than 80%; wherein NCM811 is LiNi. 0.8 Co 0.1 Mn 0.1 O2 layered oxide. This invention preferably uses a Li3PO4-based interfacial transition layer. Phosphates exhibit good high-voltage chemical stability and can serve as an electronically insulating and lithium-ion-conducting interfacial phase. Furthermore, the glass transition, interfacial wettability, and mechanical compliance of the transition layer can be adjusted by adding small amounts of elements such as B, Si, and Al.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of all-solid-state lithium battery electrode materials and solid-solid interface engineering technology, specifically relating to a high-nickel layered oxide LiNi 0.8 Co 0.1 Mn 0.1 O2 (NCM811) is used as the positive electrode active material, and garnet-type oxide solid electrolyte Li7La3Zr2O is used. 12 Using LLZO as an ion conductor, this paper describes a method for constructing an all-solid-state composite electrode with a continuous lithium-ion conductive transition layer through in-situ reaction of an interfacial precursor at the contact region between NCM811 and LLZO. This technology is applicable to high-energy-density all-solid-state lithium batteries, power batteries, and energy storage batteries. Background Technology

[0002] High-nickel cathode material NCM811 possesses high reversible specific capacity and operating voltage, making it an important cathode candidate material for high-energy-density all-solid-state batteries. LLZO exhibits high lithium-ion conductivity, good thermal stability, and a wide electrochemical stability window, making it a typical oxide solid-state electrolyte.

[0003] However, in NCM811 / LLZO composite cathodes, the direct mechanical mixing of the two rigid inorganic particles typically results in discrete point contacts or localized surface contacts, leaving pores at the interface. During charge and discharge, NCM811 undergoes anisotropic lattice contraction / expansion, further leading to contact degradation, localized debonding, and increased tortuosity of the ion transport path between NCM811 and LLZO. Simultaneously, at high potentials, interdiffusion or side reactions may occur at the interface between the cathode active material and the solid electrolyte, generating an interface phase with low lithium-ion conductivity, causing a continuous increase in interface impedance.

[0004] Existing methods often employ pre-fabricated coating layers followed by mechanical mixing with solid electrolytes, or rely on high-temperature co-firing to improve contact. The former is prone to secondary interfaces between the coating layer and LLZO, making it difficult to fill the randomly formed nano / micron-level contact gaps within the composite electrode; the latter may induce lithium loss in the high-nickel cathode, surface halogenation, cation mixing, and high-temperature side reactions between NCM and LLZO. Therefore, a method is needed to construct a transition layer that can be generated in situ in the actual NCM811 / LLZO contact area during the composite electrode forming process, possessing both lithium-ion conductivity and interface buffering capabilities.

[0005] This invention primarily addresses the following issues: limited solid-solid contact area and numerous interfacial pores between NCM811 and LLZO rigid particles; volume changes in NCM811 during cycling leading to interfacial debonding and contact loss; high-resistance interfacial side reactions that may occur when NCM811 / LLZO are in direct contact; the existence of a secondary interface between the coating layer and the solid electrolyte in traditional pre-coating methods, making it difficult to adaptively repair the actual contact points inside the composite electrode; and the risk of damage to the high-nickel cathode structure during high-temperature co-firing. Therefore, this invention provides an interface engineering scheme of "first composite contact, then in-situ layering," which preferentially enriches the lithium-containing interface precursor in the NCM811 / LLZO particle contact area and transforms it into a continuous or semi-continuous lithium-ion conductive transition layer through low-temperature heat treatment, thereby reducing solid-solid interface impedance and improving the stability of the interface structure during cycling. Summary of the Invention

[0006] To address the problems existing in the prior art, this invention provides a high-nickel NCM811 / LLZO all-solid-state composite electrode with an in-situ constructed interface transition layer and its preparation method, mainly to achieve the following technical objectives: 1. Increase the effective solid-solid contact area: By utilizing the wetting and capillary action of the liquid precursor to fill the contact gap of NCM811 / LLZO, in-situ layering is formed in the actual contact area, reducing the local ion flow density concentration caused by point contact.

[0007] 2. Constructing a continuous lithium-ion transport bridge: A lithium-containing inorganic transition phase is formed, establishing a low-torsional-degree Li-type phase between NCM811 and LLZO. + Migration channels reduce cross-interface transmission barriers.

[0008] 3. Isolate interface side reactions: The transition layer nanoscale isolates the NCM811 surface from the LLZO host, suppressing direct chemical reactions under high potential conditions and the continuous growth of high-resistivity interfacial phases.

[0009] 4. Buffer chemical-mechanical mismatch: By absorbing some of the interfacial stress through a nanoscale, non-fully rigid transition layer, particle debonding, pore formation, and contact loss during cycling are reduced.

[0010] 5. Reduce heat treatment strength: An in-situ conversion process with a temperature lower than that of traditional oxide co-firing is adopted to minimize lithium loss, cation mixing, and surface structure degradation in high-nickel NCM811.

[0011] 6. The process is expandable: This method can be integrated with composite cathode preparation processes such as dry mixing, wet slurry preparation, roll forming, or cold pressing, and can be extended to LLZO with different particle sizes and its doped systems.

[0012] To achieve the above-mentioned technical objectives, the present invention adopts the following technical solution: The present invention first provides a high-nickel NCM811 / LLZO all-solid-state composite electrode with an in-situ constructed interface transition layer.

[0013] The composite electrode includes a positive electrode active material, a solid electrolyte, and an in-situ interface transition layer located at the contact area between the two; depending on the electron transport requirements, it may further include conductive carbon materials (such as conductive carbon black (Super-P), conductive carbon nanotubes, or other conductive carbon materials).

[0014] Furthermore, the positive electrode active material is NCM811, or a layered oxide of NCM or NCMA with a Ni content of not less than 80%; the NCM811 is LiNi. 0.8 Co 0.1 Mn 0.1 O2 layered oxide.

[0015] Furthermore, the solid electrolyte is Li7La3Zr2O 12 (LLZO) or its stable cubic phase derivatives doped with elements such as Ta, Nb, Al, and Ga.

[0016] Furthermore, the solid electrolyte can also be a cubic phase stabilized garnet electrolyte such as Ta-LLZO, Nb-LLZO, Al-LLZO, or Ga-LLZO.

[0017] Specifically, the interface transition layer is a lithium- and oxygen-containing ion-conducting inorganic phase, formed by the in-situ reaction of one or more of the lithium source and phosphorus, boron, and silicon sources inside the composite electrode. Preferably, it includes Li3PO4, lithium boron oxide (Li3BO3 (lithium borate)), lithium silicon oxide (Li2SiO3 (lithium metasilicate)), or a composite phase thereof. During low-temperature conversion, Li3BO3 and Li2SiO3 may also be in the form of amorphous / glassy lithium borate or lithium silicate phases with the corresponding stoichiometric composition as the main component. The interface transition layer is mainly distributed in the contact neck of NCM811 / LLZO particles, the interparticle gaps, and the side of the NCM811 surface adjacent to LLZO, rather than being formed only on the surface of a single powder pre-coated particle.

[0018] Specifically, the equivalent thickness of the interface transition layer is about 2-50 nm, preferably 5-20 nm; based on the total mass of the all-solid composite electrode, the content of the interface precursor conversion product is 0.1-5 wt% of the total mass of the positive electrode active material and the solid electrolyte, preferably 0.3-2 wt%.

[0019] In the composite electrode, the mass ratio of the positive electrode active material to the solid electrolyte is (4~9):(1~4), preferably 60:40-90:10, and more preferably 70:30-85:15.

[0020] This invention further provides a method for preparing a high-nickel NCM811 / LLZO all-solid-state composite electrode with an in-situ constructed interface transition layer, comprising the following steps: 1) Raw material pretreatment Weigh out NCM811 positive electrode active material and vacuum dry or dry at normal pressure for a certain period of time, and set aside for later use; weigh out cubic phase LLZO solid electrolyte (hereinafter referred to as LLZO) and vacuum dry or dry at normal pressure for a certain period of time, and set aside for later use, in order to reduce the adverse effects of surface adsorbed water and carbonate on interface construction. 2) NCM811 / LLZO composite and solid-state contact network backbone construction The dried NCM811 positive electrode active material and LLZO are weighed according to a certain mass ratio and mixed under certain conditions. Then, they are pre-pressed by cold pressing, rolling pressing or molding to obtain composite powder or pre-pressed sheet that forms the NCM811 / LLZO contact skeleton, so that NCM811 and LLZO establish an initial solid-solid contact network. 3) Preparation of lithium phosphate interfacial precursor solution The lithium source and the film-forming anionic precursor are dissolved or dispersed in a first solvent to obtain a low-viscosity interface precursor solution; by adjusting the concentration of the precursor solution, the final interface phase does not excessively cover the electron transport path. 4) Selective wetting of the contact area The interface precursor solution is introduced into the composite powder or pre-compressed sheet that forms the NCM811 / LLZO contact framework by means of spray wetting, drop addition, vacuum wetting, atomization deposition, or small amount of liquid phase assisted mixing. The interface precursor solution is preferentially introduced into the NCM811 / LLZO contact neck and interparticle micropores by capillary action. The drop addition-vacuuming-restoration of normal pressure process is repeated until all the precursor solution is introduced into the composite powder. Then, the solvent is removed by drying at 30-80℃, so that the precursor is retained near the real solid-solid interface to obtain the composite material. 5) Low-temperature in-situ reaction generates Li3PO4-based interfacial transition layer The dried composite material is placed in a tube furnace and heated to 200-500℃ at a rate of 1-5℃ / min under an atmosphere of air, pure oxygen, or a mixture of oxygen and an inert protective gas (such as argon, nitrogen, helium, carbon dioxide, etc.). The temperature is held for 0.5-6h to perform heat treatment, which causes the precursor to decompose and generate a lithium-ion-containing conductive interface transition layer in situ in the NCM811 / LLZO contact area. 6) Conductive agent composite and composite cathode forming Step 5) After the heat treatment is completed, cool to room temperature to obtain NCM811 / Li3PO4 / LLZO in-situ interface composite powder. Then crush and sieve it. Add a conductive agent to the in-situ treated composite powder and perform low-shear mixing to make the conductive agent evenly distributed between the NCM811 particles. Then prepare the composite positive electrode layer by cold pressing, molding or rolling, and bond it with a dense LLZO solid electrolyte sheet to prepare a high-nickel NCM811 / LLZO all-solid-state composite electrode.

[0021] Specifically, in step 1), the NCM811 positive electrode active material is LiNi. 0.8 Co 0.1 Mn 0.1 O2 layered oxide; the LLZO is Li7La3Zr2O 12 Or its stable cubic phase derivatives doped with elements such as Ta, Nb, Al, and Ga.

[0022] Specifically, in step 1), the drying conditions for the NCM811 positive electrode active material are vacuum drying or atmospheric pressure drying at 80-150℃ for 2-12 hours.

[0023] Specifically, in step 1), the drying conditions for the cubic LLZO solid electrolyte are vacuum drying or atmospheric pressure drying at 100-300℃ for 2-12 h.

[0024] Specifically, in step 1), the LLZO powder is selected from submicron to several micron-sized particles so that it can fill the gaps between the secondary NCM811 particles.

[0025] Specifically, in step 2), the mass ratio of NCM811 positive electrode active material to LLZO is (4~9):(1~4), preferably 60:40-90:10, and more preferably 70:30-85:15.

[0026] Specifically, in step 2), the dried NCM811 positive electrode active material is mixed with LLZO by low-energy ball milling, three-dimensional mixing or dry mechanical mixing; the mixing time is 20~80min.

[0027] Specifically, in step 3), the film-forming anion precursor is one or more of phosphorus source, boron source, and silicon source.

[0028] Specifically, the lithium source is anhydrous lithium acetate, lithium nitrate, lithium lactate, or other lithium that can decompose at lower temperatures to provide Li. + The sources of phosphorus are lithium salts; phosphorus sources are phosphoric acid, ammonium dihydrogen phosphate or organic phosphate esters; boron sources are boric acid or borate esters; and silicon sources are tetraethyl orthosilicate, etc.

[0029] Specifically, in step 3), the first solvent is anhydrous ethanol or an ethanol-based low-aqueous solvent.

[0030] Specifically, in step 3), when preparing the interface precursor solution, the obtained interface phase is Li3PO4, lithium boron oxide (Li3BO3 (lithium borate)), lithium silicon oxide (Li2SiO3 (lithium metasilicate)) or a composite phase thereof. The total concentration of lithium source, phosphorus source, boron source and / or silicon source in the precursor solution is controlled so that the theoretical mass of the interface phase formed after complete conversion accounts for 0.3-2.0 wt% of the total mass of NCM811 and LLZO.

[0031] Specifically, in step 5), the heat treatment temperature is preferably 250-400 ℃ to balance the full conversion of the precursor and the structural stability of NCM811.

[0032] Specifically, in step 5), the equivalent thickness of the interface transition layer is about 2-50 nm, preferably 5-20 nm; based on the total mass of the all-solid composite electrode, the content of the interface precursor conversion product is 0.1-5 wt% of the total mass of NCM811 and LLZO, preferably 0.3-2 wt%, and more preferably 0.5-1.5 wt%.

[0033] Specifically, in step 6), the conductive agent is conductive carbon black (Super-P), conductive carbon nanotubes or other conductive carbon materials; the amount of conductive agent added is 0-10 wt% of the total mass of the composite powder, preferably 1-5 wt%, and more preferably 2-3 wt%.

[0034] Specifically, in step 6), the dense LLZO solid electrolyte sheet can be made of cubic phase LLZO or its Ta, Nb, Al, Ga doped derivative powder, pressed at 50-200 MPa and sintered at 1100-1250℃ for 1-12 h; during sintering, it is preferable to cover with masterbatch of the same composition to reduce lithium loss, and after sintering, it is prepared by double-sided grinding, polishing and drying, preferably with a relative density of not less than 90%.

[0035] Specifically, in step 6), an electrode blank can be prepared first, and then the wetting and in-situ transformation in steps 4) and 5) can be completed.

[0036] Furthermore, the present invention also provides a high-nickel NCM811 / LLZO all-solid-state composite electrode with an in-situ constructed interface transition layer prepared by the above method.

[0037] Furthermore, based on a general inventive concept, the present invention also provides the application of the high-nickel NCM811 / LLZO all-solid-state composite electrode with the in-situ constructed interface transition layer in the preparation of all-solid-state lithium-ion batteries.

[0038] This invention preferably employs a Li3PO4-based interfacial transition layer. Phosphates exhibit good high-voltage chemical stability and can serve as an electronically insulating and lithium-ion-conducting interfacial phase. Furthermore, the glass transition, interfacial wettability, and mechanical compliance of the transition layer can be adjusted by adding small amounts of elements such as B, Si, and Al.

[0039] The main innovative aspects of this invention include the following: 1. Unlike the approach of “first fully coating NCM811 and then mechanically adding LLZO”, this invention emphasizes in-situ layering after establishing real contact between the two particles, so that the interface material is preferentially located in the NCM811 / LLZO contact area that most needs improvement.

[0040] 2. The in-situ transition layer simultaneously serves as an "ion transport bridge, chemical isolation layer, and stress buffer layer," which helps reduce interfacial impedance and maintain contact integrity after cycling.

[0041] 3. Low-temperature in-situ conversion avoids prolonged high-temperature co-firing of NCM811 and LLZO, reducing the risk of lithium loss, surface reconstruction, and element interdiffusion in high-nickel cathodes.

[0042] 4. The precursor solution is used in small quantities, and the transition layer is at the nanoscale, which can improve Li+ transport while minimizing significant blockage to the electron transport network.

[0043] 5. The process has low equipment requirements and is compatible with existing powder mixing, vacuum impregnation, roll pressing / cold pressing and low temperature heat treatment equipment, and has the potential for further scale-up and verification.

[0044] Compared with the prior art, the advantages of the present invention are: 1. The in-situ interface construction mechanism of "contact first, then layer": Instead of conventional pre-coating of NCM811 or LLZO, after the NCM811 / LLZO composite contact network is formed, the precursor is directionally transported to the real solid-solid interface and transformed in situ using capillary wetting.

[0045] 2. Contact neck enrichment type transition layer structure: The transition phase is mainly enriched in the contact neck of the two phases and adjacent pores, forming a locally continuous Li. + Transmission bridges reduce transmission losses caused by ineffective full-surface thick cladding.

[0046] 3. Chemical stability and chemomechanical synergy: The interface layer reduces the direct reaction between NCM811 and LLZO, and also utilizes the characteristics of nanoscale / composite glass ceramics to buffer volume mismatch and contact loss during cycling.

[0047] 4. Low-temperature interface reaction window: By using lithium salts and phosphorus / boron / silicon precursors that can be decomposed at low temperatures, the interface layer formation temperature is controlled within a range that does not require high-temperature co-firing of NCM811 / LLZO.

[0048] 5. Tunable interface layer system: Through Li3PO4-based, lithium boron oxide-based, lithium silicon oxide-based or composite systems, the synergistic regulation of interface ionic conductivity, mechanical compliance and high voltage stability can be achieved. Attached Figure Description

[0049] Figure 1 Comparison of the microstructures of composite cathodes with liquid electrolytes and solid electrolytes; Figure 1 In the figure, a represents a liquid electrolyte composite cathode, where the liquid can wet the pores between particles; b represents a solid electrolyte composite cathode, which contains pores, grain boundaries, and high ion transport curvature. This figure illustrates how the present invention constructs a continuous interface transition layer in the actual contact region of NCM811 / LLZO, reduces porosity, and improves Li... + The necessity of cross-interface transmission; Figure 2 A schematic diagram of the chemical-mechanical and CAM-SE interface effects resulting from replacing the liquid electrolyte with a solid electrolyte; Figure 2 In the figure, 'a' indicates that after CAM cyclic cracking, liquid electrolyte can enter new cracks, while rigid solid electrolyte is difficult to refill; 'b' indicates that CAM volume change leads to CAM-SE contact loss; 'c' indicates that CAM and SE in solid composite cathodes easily form point contacts and are affected by pores and grain boundaries. This figure is used to illustrate the stress buffering and interface stabilizing effect of the in-situ interface transition layer of the present invention. Figure 3 Mechanism / design diagram showing the relationship between maximum particle size and chemical diffusion coefficient at different magnification ratios; Figure 3 The figure shows the relationship between particle size and chemical diffusion coefficient under 0.1C, 1C and 5C conditions, and indicates the typical range of NCM and lithium iron phosphate (LFP). This figure is used to illustrate the coupling relationship between NCM particle size, diffusion distance and rate performance, and provides a basis for particle size distribution design of NCM811 and fine-particle LLZO. Figure 4 Figures showing the variation in spherical CAM particle size and the variation in axial dimensions of the NCM811 lattice. Figure 4 In the text, 'a' represents the evolution of the maximum radius of different CAMs with the initial particle radius; 'b' represents the overall size change of NCM811, which can be decomposed into changes in the a-axis and c-axis directions; the anisotropic size change of NCM811 is prone to stress concentration and debonding at its contact interface with rigid LLZO. This invention buffers this chemical-mechanical mismatch through an in-situ nano-transition layer. Figure 4This diagram illustrates the mechanism of maximum particle radius variation and NCM811 lattice a-axis and c-axis anisotropy variation for different cathode active materials during cycling, used to explain the relationship between chemical-mechanical mismatch, particle size, and interfacial contact maintenance in high-nickel layered cathodes. Detailed Implementation

[0050] The present invention will be further described in detail below with reference to specific embodiments, but the scope of protection of the present invention is not limited to the following embodiments. The following embodiments are only used to clearly illustrate the technical solutions of the present invention. Any technical solutions obtained by conventional adjustments or equivalent substitutions to the ratio of positive electrode active material to solid electrolyte, type of interfacial precursor, concentration of precursor solution, wetting method, heat treatment conditions and electrode forming process based on the technical concept of the present invention should fall within the scope of protection of the present invention.

[0051] Unless otherwise specified, the experimental methods used in the following examples are conventional methods; unless otherwise specified, the instruments and equipment used in the following examples are commercially available conventional instruments and equipment; unless otherwise specified, the reagents, raw materials, etc. used in the following examples are conventional commercial products and can be obtained through commercial channels.

[0052] In the following examples and comparative examples, room temperature or normal temperature refers to 25±5℃.

[0053] The comparative examples and embodiments all used commercially produced primary sintered products, Li(Ni), provided by Henan Xinxiang Tianli Lithium Energy Group Co., Ltd. 0.8 Co 0.1 Mn 0.1 The initial raw material is O2 ternary positive electrode active material, which is commercially known as 1-calcined NCM811. Its preparation method can be achieved by conventional means in the existing technology, and it is not the inventive point of this invention, so it will not be described in detail.

[0054] The garnet-type oxide solid electrolyte used in the following examples is preferably a Ta / Al stable cubic phase LLZO solid electrolyte (hereinafter referred to as LLZO), and its preparation method is referenced in the literature (Shin DO, Oh K, Kim KM, Park KY, Lee B, Lee YG, Kang K. Synergistic multi-doping effects on the Li7La3Zr2O12 solid electrolyte for fast lithium ion conduction). Scientific Reports , 2015 , 5:18053.).

[0055] Specifically, Li2CO3, La2O3, ZrO2, and the corresponding Ta2O5 and / or Al2O3 are used as raw materials, weighed according to the target stoichiometric ratio, and mixed in a planetary ball mill at approximately 200 r / min for 10 h using isopropanol as the medium. After drying, the mixture is calcined at approximately 1000℃ for 2-4 h to obtain cubic phase LLZO-based powder. When used for composite cathodes, the calcined powder can be low-energy ground and sieved to submicron to several micron levels, preferably with a D50 of approximately 0.5-3 μm. When used to prepare dense electrolyte sheets, the powder is ground again, pressed into sheets at approximately 50 MPa, and sintered at approximately 1200℃ under a cover of the same composition masterbatch, preferably for about 6 h. Subsequently, the sheets are double-sided ground and polished to a thickness of approximately 0.4-0.8 mm and dried for later use.

[0056] In the all-solid-state composite electrode of the following embodiments, the positive electrode active material is a layered oxide LiNi. 0.8 Co 0.1 Mn 0.1 O2 (NCM811), solid electrolyte is garnet-type Li7La3Zr2O 12 (LLZO).

[0057] In the all-solid-state composite electrode, both materials are granular. NCM811 particles and LLZO particles contact each other to form a composite ion transport network. Simultaneously, a lithium-ion-containing conductive interface transition layer is generated in situ in the actual contact area of ​​the NCM811 / LLZO particles, the contact neck, and the gaps between adjacent particles. This interface transition layer is preferably a Li3PO4-based phosphate transition layer with an equivalent thickness of 2-50 nm, preferably 5-20 nm. The interface transition layer fills the local solid-solid contact gaps between NCM811 and LLZO and is tightly bonded to the surfaces of the particles on both sides, forming a continuous or semi-continuous Li3PO4-based conductive interface between NCM811 and LLZO. + The transmission channel simultaneously isolates NCM811 from the LLZO body at the nanoscale to reduce interfacial side reactions caused by direct contact and buffer the interfacial stress and contact loss caused by the cyclic volume change of NCM811.

[0058] For high-nickel NCMs (such as NCM811), there are also significant anisotropic size changes during charging and discharging, which can easily cause CAM particle cracking and CAM / SE interface contact loss, resulting in increased interface impedance.

[0059] Therefore, the present invention does not simply form a complete coating layer on the surface of NCM811 particles in advance, but first constructs a real solid-solid contact network of NCM811 / LLZO, and then uses a low-viscosity interface precursor liquid to wet the contact network, so that the precursor preferentially enters the contact neck and particle gap, and forms an interface transition layer through low-temperature in-situ reaction.

[0060] The preparation method of this invention mainly includes the following steps: pretreatment of NCM811 and LLZO raw materials, NCM811 / LLZO composite and solid contact network skeleton construction, preparation of lithium phosphate interface precursor solution, wetting of NCM811 / LLZO real contact area with interface precursor solution, low-temperature in-situ reaction to generate lithium ion conductive interface transition layer, conductive agent composite and cold pressing or roll forming, etc.

[0061] Example 1: Li3PO4-based in-situ interfacial transition layer NCM811 / LLZO composite cathode Example 1 provides a method for preparing a high-nickel NCM811 / LLZO all-solid-state composite electrode with an in-situ constructed interface transition layer. The specific steps are as follows: 1) Pretreatment of NCM811 and LLZO raw materials Weigh out NCM811 positive electrode active material and vacuum dry it at 120℃ for 6 hours for later use; weigh out cubic phase LLZO solid electrolyte (hereinafter referred to as LLZO) and dry it at 200℃ under normal pressure for 4 hours for later use, in order to reduce the adverse effects of surface adsorbed water and carbonate on interface construction.

[0062] The NCM811 positive electrode active material is preferably made of spherical or near-spherical secondary particle powder, and the LLZO is preferably made of fine particle powder with a particle size smaller than that of the NCM811 secondary particles, so that the LLZO can enter the gaps between the NCM811 particles. This invention points out that the combination of small-sized solid electrolyte particles and spherical CAM particles is beneficial for obtaining higher packing density and reducing residual porosity inside the composite positive electrode.

[0063] 2) NCM811 / LLZO composite and solid-state contact network backbone construction Weigh the dried NCM811 powder and LLZO powder according to the mass ratio of NCM811:LLZO=80:20, and place them in a three-dimensional motion mixer or other low-shear three-dimensional mixing equipment. Mix them at about 20-30 r / min for 60 min to make the fine-sized LLZO evenly distributed among the NCM811 particles. In order to avoid secondary particle breakage of NCM811 caused by high-energy ball milling, high-speed ball milling is not used in this embodiment.

[0064] During the mixing process, mechanical energy is controlled to avoid high-energy collisions and significant breakage of the secondary NCM811 particles. After mixing, pre-forming is then performed using cold pressing, rolling, or molding to obtain a composite powder, forming a stable pre-compressed composite framework between the NCM811 and LLZO particles. The purpose of this pre-compression is not to obtain a final high-density electrode, but rather to pre-form actual contact points, contact necks, and interparticle micropores of NCM811 / LLZO, providing a spatial structural basis for the subsequent directional wetting of the interface precursor solution.

[0065] By adjusting the mass ratio of NCM811 to LLZO, a high loading of NCM811 is ensured while allowing LLZO to form Li throughout the composite cathode. + Transmission network.

[0066] 3) Preparation of lithium phosphate interfacial precursor solution Lithium and phosphorus sources were selected to prepare interfacial precursor solutions.

[0067] In this embodiment, the lithium source is anhydrous lithium acetate, and the phosphorus source is phosphoric acid with a mass fraction of approximately 85%; both should use battery-grade or analytical-grade reagents or higher.

[0068] Taking 10.0 g of the NCM811 / LLZO composite framework obtained in step 2 (i.e., the composite powder in step 2) as an example, 0.171 g of anhydrous lithium acetate and 0.100 g of phosphoric acid with a mass fraction of approximately 85% were added to 10.0 mL of anhydrous ethanol, and the mixture was continuously stirred to form a homogeneous, low-viscosity interfacial precursor solution. The Li:P molar ratio was approximately 3:1, and approximately 0.10 g of Li3PO4 was theoretically generated upon complete conversion, accounting for approximately 1.0 wt% of the total mass of NCM811 and LLZO. The interfacial phase obtained during the preparation of the interfacial precursor solution was Li3PO4.

[0069] By employing a lower interfacial phase content, the formation of an excessively thick electronic insulating layer can be avoided. This invention utilizes Li3PO4 primarily for interfacial Li... + Conductive and chemical isolation are provided, while electron transport is still mainly undertaken by NCM811 particles and an external conductive phase.

[0070] 4) The interface precursor solution wets the actual contact area of ​​NCM811 / LLZO. The composite powder forming the NCM811 / LLZO contact framework obtained in step 2) is placed in a vacuum impregnation tank or vacuum drying oven equipped with a vacuum gauge and a slow pressure relief valve. The interface precursor liquid prepared in step 3) is slowly added dropwise to the surface of the composite powder. A vacuum is drawn to a gauge pressure of approximately -0.09 to -0.095 MPa (corresponding to an absolute pressure of approximately 5-10 kPa) and maintained for 10 minutes to allow sufficient air to be expelled from the composite powder. Then, the pressure is slowly restored to normal, utilizing the pressure difference and capillary action to allow the precursor liquid to enter the NCM811 / LLZO contact area along the open channels between the particles. In this embodiment, the interface precursor liquid is added at a ratio of approximately 1.0 mL / g to the mass of the NCM811 / LLZO composite framework; that is, approximately 10.0 mL of precursor liquid is used for 10.0 g of composite framework. Repeat the process of adding, vacuuming, and restoring atmospheric pressure until the designed amount of precursor liquid is completely incorporated into the composite powder (this can be repeated 2-3 times). Then, slowly dry the powder at 50-70℃ to allow the solvent to gradually evaporate, thus obtaining the composite material. During this process, the lithium and phosphorus source precursors are retained and enriched in the contact necks of NCM811 and LLZO particles, adjacent micropores, and the surface areas where they contact each other.

[0071] This step is the key difference between this invention and conventional pre-coating technology. Conventional coating first forms a protective layer on the entire surface of individual NCM811 particles before adding a solid electrolyte, thus still resulting in a new solid-solid interface of "coating layer / LLZO". This invention, however, first forms an actual NCM811 / LLZO contact network, then uses a precursor solution to wet the actual contact area, allowing the transition layer to form directly on the actual Li-bearing surface. + Location of cross-interface transmission (e.g.) Figure 1 (As shown).

[0072] 5) Low-temperature in-situ reaction generates Li3PO4-based interfacial transition layer The dried composite material was placed in a tube furnace. In this embodiment, a pure oxygen atmosphere (preferably O2 purity ≥ 99.9%) was used, and the temperature was increased to 325°C at a heating rate of 2°C / min and held for 2 hours. During the heat treatment, the lithium- and phosphorus-containing precursors adsorbed and enriched in the NCM811 / LLZO contact area underwent decomposition and in-situ reaction, forming a Li3PO4-based lithium-ion conductive interface transition layer in the NCM811 / LLZO contact neck and interparticle gaps. Subsequently, the furnace was cooled to room temperature under the same atmosphere.

[0073] The resulting transition layer is mainly located in the actual contact area between NCM811 and LLZO, rather than uniformly covering all free surfaces of NCM811; its equivalent thickness is preferably controlled between 5-20 nm.

[0074] This nanoscale Li3PO4-based lithium-ion conductive interfacial transition layer isolates the direct contact between NCM811 and LLZO, reducing unfavorable interfacial reactions; and forms Li between the two phases. + The transmission bridge also provides a certain interface buffer space for the minute size changes that occur during the charging and discharging of NCM811.

[0075] This invention points out that volume changes in high-nickel NCM cause porosity and contact loss between CAM and SE, and since the oxide SE itself is harder, maintaining a tight solid-solid contact is particularly difficult. Simultaneously, NCM811 exhibits significant anisotropic dimensional changes in the a-axis and c-axis directions (e.g., Figure 2 (As shown).

[0076] 6) Conductive agent composite and composite cathode forming Step 5) After heat treatment, the powder is cooled to room temperature in the furnace to obtain NCM811 / Li3PO4 / LLZO in-situ interface composite powder. Then, it is lightly crushed and sieved. Then, SUPER-P® Li conductive carbon black (Imerys Graphite & Carbon, typical BET specific surface area of ​​about 62 m2 / g) is added as a conductive agent, accounting for 2.5 wt% of the total mass of the composite powder. The powder is then mixed in a three-dimensional motion mixer at a low shear rate of about 20 r / min for 20 min to make the conductive agent evenly distributed among the NCM811 particles.

[0077] Subsequently, a composite cathode layer was prepared by unidirectional cold pressing: the composite powder was placed in a mold and bonded to a dense LLZO solid electrolyte sheet, and held under pressure of about 100 MPa for 3 min to obtain a high-nickel NCM811 / LLZO all-solid-state composite electrode with a thickness of about 100-200 μm.

[0078] The dense LLZO solid electrolyte sheet used can be found in the reference (Shin DO, Oh K, Kim KM, Park KY, Lee B, Lee YG, Kang K. Synergistic multi-doping effects on the Li7La3Zr2O12 solid electrolyte for fast lithium ion conduction). Scientific Reports , 2015 The method described in 5:18053. is as follows: the garnet-type cubic phase LLZO powder is ground again, pressed into tablets at about 50 MPa, covered with masterbatch of the same composition, sintered at about 1200℃ for about 6 h, polished on both sides to about 0.4-0.8 mm and vacuum dried at 200℃ for 4 h for later use.

[0079] The composite powder is bonded to a dense LLZO solid electrolyte sheet to assemble an all-solid-state battery, and a constant external stacking pressure of about 2-5 MPa is maintained during testing.

[0080] For systems with a sufficiently strong electronic conductivity network, the amount of conductive agent added can be appropriately reduced. This invention points out that when the electronic conductivity of CAM is sufficient, a high CAM volume fraction may even be possible for constructing a carbon-free composite cathode; at the same time, polymer binders may clog the active surface and transport channels, therefore reducing the binder content or using a dry process has advantages for preparing all-solid-state composite electrodes.

[0081] Example 2: Low-content Li3PO4 in-situ interface transition layer composite cathode Example 2 provides a method for preparing a high-nickel NCM811 / LLZO all-solid-state composite electrode with an in-situ constructed interface transition layer. Example 2 is basically the same as Example 1 and is carried out strictly according to the steps of "raw material pretreatment - composite contact network skeleton construction - precursor solution preparation - interface precursor solution wetting - low temperature in-situ conversion - conductive agent composite and composite cathode forming".

[0082] The difference between Example 2 and Example 1 is as follows: In step 3), reduce the amount of interfacial precursor solution added so that the theoretical mass of Li3PO4 after complete conversion accounts for approximately 0.3-0.5 wt% of the total mass of NCM811 / LLZO. The remaining NCM811 / LLZO ratio, impregnation method, drying method, and heat treatment process are the same as in Example 1.

[0083] This embodiment is mainly used to investigate whether in-situ Li3PO4 can form an effective ion transport bridge in the NCM811 / LLZO contact region at a low interface phase content, while minimizing the influence of the electronic insulation interface on electron transport.

[0084] Compared to Example 1, the transition layer formed in Example 2 is theoretically thinner and has a lower interface coverage, which can be used to determine the minimum amount of interface phase to be added to meet the interface stability requirements.

[0085] Example 3: High-content Li3PO4 in-situ interface transition layer composite cathode Example 3 provides a method for preparing a high-nickel NCM811 / LLZO all-solid-state composite electrode with an in-situ constructed interface transition layer. Example 3 is basically the same as Example 1, except that: In step 3), increase the amount of interfacial precursor solution added so that the theoretical mass of Li3PO4 after complete conversion accounts for about 1.5-2.0 wt% of the total mass of NCM811 / LLZO.

[0086] All other steps are consistent with those in Example 1.

[0087] A higher content of the interfacial phase can increase the filling degree of the NCM811 / LLZO contact region and improve the continuity of the interfacial layer, but if Li3PO4 is excessive, it may increase the resistance of the electron transport path. Therefore, by gradient adjustment of the amount of interfacial layer added in Examples 1-3, the improvement of interfacial contact and the Li3PO4 content can be determined. + The optimal balance between interfacial transport and electronic conduction.

[0088] Example 4: Li3PO4-Lithium Boron Oxide Composite In-situ Transition Layer Example 4 provides a method for preparing a high-nickel NCM811 / LLZO all-solid-state composite electrode with an in-situ constructed interface transition layer. Example 4 is basically the same as Example 1, with the main difference being in steps 3) and 5).

[0089] In step 3), in addition to lithium and phosphorus sources, a certain amount of boron source is added to the interface precursor solution, preferably boric acid.

[0090] The amounts of phosphorus and boron sources were controlled so that the final interface phase was a composite lithium-containing transition layer composed of Li3PO4 and Li3BO3 (lithium borate), and the total content of the interface phase was controlled at 0.5-2.0 wt% of the total mass of NCM811 / LLZO.

[0091] Li3BO3 has been reported in publications as a lithium-ion conductive / binder phase in garnet-type oxide solid electrolyte composite cathodes, see the literature (Ohta S, Komagata S, Seki J, Saeki T, Morishita S, Asaoka T. All-solid-state lithium ion battery using garnet-type oxide and Li3BO3 solid electrolytes fabricated by screen-printing). Journal of Power Sources , 2013 , 238: 53-56.).

[0092] Step 4) The method of drop addition combined with vacuum impregnation is still used to preferentially enrich lithium, phosphorus and boron precursors in the NCM811 / LLZO contact area.

[0093] Step 5) Perform heat treatment at a temperature of 250-350℃ to transform the precursor into a Li3PO4-lithium boron oxide composite interface layer in situ in the contact area.

[0094] The purpose of introducing lithium boron oxide is to improve the amorphous or glassy characteristics and mechanical compliance of the interface layer, so that it can more fully fill the tiny contact gaps of NCM811 / LLZO and adapt to the size changes of NCM811 during cycling.

[0095] Example 5: In-situ wetting construction of interface layer after composite cathode forming Example 5 was used to verify the feasibility of in-situ interface construction under different process sequences.

[0096] 1) Raw material pretreatment NCM811 and LLZO were dried according to the method in Example 1.

[0097] 2) Preparation of composite cathode preform Weigh the dried powder according to the mass ratio of NCM811:LLZO=80:20, place it in a three-dimensional motion mixer and mix at about 20-30 r / min for 60 min. Add about 2 wt% of SUPER-P® Li conductive carbon black (Imerys Graphite & Carbon) as a conductive agent, and the mixed powder is prepared.

[0098] The mixed powder is pre-formed into a porous composite cathode blank by unidirectional cold pressing. The pre-pressing pressure is about 50 MPa and the pressure is held for 1 min, so that the blank has transferable mechanical strength, while retaining open channels for the precursor liquid to wet.

[0099] 3) Preparation of interfacial precursor solution The Li3PO4 interface precursor solution was prepared using the same lithium and phosphorus sources as in Example 1.

[0100] 4) Vacuum impregnation of electrode sheets The porous composite cathode preform is placed in a vacuum impregnation tank or vacuum drying oven equipped with a vacuum gauge, and the vacuum is evacuated to a gauge pressure of approximately -0.09 to -0.095 MPa (absolute pressure of approximately 5-10 kPa) and maintained for 10 min. Then, an interfacial precursor liquid is introduced, allowing the precursor liquid to penetrate into the interior along the open channels in the composite cathode and enter the NCM811 / LLZO contact area.

[0101] After restoring to normal pressure, the impregnation continues to allow the precursor solution to fully penetrate the electrode interior. In this embodiment, the precursor solution is added at a ratio of approximately 1.0 mL / g of the porous composite cathode preform volume, and fine-tuned according to the actual porosity of the preform until there is no obvious free liquid on the surface.

[0102] 5) Drying and low-temperature in-situ transformation After slow drying at 50-70℃, the precursor is heat-treated at 250-400℃ (held for 1-3 hours) and then cooled to room temperature, so that the precursor is converted in situ into a Li3PO4-based interface layer in the actual contact area of ​​NCM811 / LLZO inside the formed composite cathode.

[0103] 6) Secondary densification After heat treatment, the composite cathode is densified by secondary unidirectional cold pressing: it is held at a pressure of about 150 MPa for 3 minutes to further enhance the contact between particles; for continuous sheet electrodes, the equivalent linear pressure rolling method can also be used, with the electrode thickness being stable and no through cracks appearing as the endpoint, to obtain an in-situ interface modified all-solid-state composite cathode.

[0104] This implementation method can further improve the positioning accuracy of the precursor to the effective contact interface inside the actual electrode, and is especially suitable for thick electrodes or high-load composite cathodes.

[0105] Comparative Example 1: NCM811 / LLZO Direct Mechanical Hybrid Composite Cathode Comparative Example 1 and Example 1 used the same NCM811, LLZO main materials and mass ratio.

[0106] The specific method is as follows: NCM811 and LLZO were dried according to the method in Example 1; Using the method in step 2) of Example 1, low-energy mixing was performed at a mass ratio of NCM811:LLZO=80:20; Do not prepare an interface precursor solution; No precursor solution vacuum impregnation is performed; No in-situ generation of the Li3PO4 interface layer is performed; The same amount of conductive agent as in Example 1 was directly added and pressed into a composite positive electrode.

[0107] The core difference between Comparative Example 1 and Example 1 lies only in the absence of the in-situ interface transition layer of the actual contact area of ​​NCM811 / LLZO.

[0108] By comparing with Example 1, the effects of the in-situ Li3PO4 interface transition layer on solid-solid contact, interface impedance, post-cycle contact retention, and electrode polarization can be evaluated.

[0109] Comparative Example 2: NCM811 pre-coated with Li3PO4 and mechanically mixed with LLZO The amounts of NCM811, LLZO, and Li3PO4 used in Comparative Example 2 were basically the same as those in Example 1.

[0110] The difference lies in the order in which the interface layers are formed. Specifically: First, NCM811 was pretreated, and lithium- and phosphorus-containing precursor solutions were prepared using the method in Example 1. Then, NCM811 was dispersed separately in the lithium- and phosphorus-containing precursor solutions, so that the precursors were adsorbed onto the entire surface of the NCM811 particles. After drying, the same heat treatment conditions as in Example 1 were used to pre-form a Li3PO4 coating layer on the surface of the NCM811 particles.

[0111] Then, NCM811 pre-coated with Li3PO4 and LLZO are mechanically mixed at a mass ratio of 80:20, and the same amount of conductive agent is added and pressed into a composite positive electrode.

[0112] In Comparative Example 2, Li3PO4 was formed before NCM811 and LLZO established a real contact relationship. Therefore, the obtained Li3PO4 mainly exhibited as a pre-coating layer on the entire surface of NCM811. After NCM811 and LLZO were combined, a new "Li3PO4 / LLZO" solid-solid interface was still formed.

[0113] By comparing Comparative Example 2 with Example 1, the differences and technical effects of the present invention's "first constructing an NCM811 / LLZO contact network, and then forming layers in situ in the actual contact area" compared to the traditional "first coating NCM811, and then adding LLZO" process can be evaluated.

[0114] Comparative Example 3: High-Temperature Co-fired NCM811 / LLZO Composite Cathode NCM811 and LLZO were mixed in the same proportion as in Example 1, without adding an interfacial precursor solution. The resulting NCM811 / LLZO composite powder was then co-fired at 800°C for 2 hours at a heating rate of 2°C / min. The atmosphere used was pure oxygen or an oxygen-containing atmosphere consistent with that in Example 1, to promote direct sintering contact between the two inorganic particles. This temperature is significantly higher than the preferred low-temperature in-situ lamination window of 250-400°C in this invention, and was used to compare the potential for high-nickel cathode structural degradation, interfacial side reactions, and elemental interdiffusion caused by high-temperature co-firing.

[0115] Subsequently, the same amount of conductive agent as in Example 1 was added to form a composite positive electrode.

[0116] Comparative Example 3 is used to compare the differences between the traditional process of improving oxide solid-solid contact by increasing sintering strength and the low-temperature in-situ interface construction process of the present invention.

[0117] Performance testing and characterization methods To verify the function of the in-situ interface transition layer of the present invention, the following tests can be carried out on Examples 1-5 and Comparative Examples 1-3 respectively.

[0118] 1. Microstructure and interfacial contact characterization The distribution of NCM811 and LLZO in the composite cathode and the interparticle contact were observed using SEM and cross-sectional SEM. The three-dimensional pores and solid-solid contact area inside the composite cathode were analyzed using FIB-SEM. The interparticle porosity and effective contact area of ​​the embodiment and the comparative example were compared.

[0119] The key comparison is whether significant porosity and debonding occur in the NCM811 / LLZO contact area before and after the cycle.

[0120] 2. Characterization of the interface transition layer structure The NCM811 / LLZO contact area was observed using TEM or HRTEM, and the interface layer thickness was measured. Elemental surface and line scans of the NCM811 / transition layer / LLZO region were performed using STEM-EDS or EELS to confirm that the P and Li related interface components are mainly enriched in the real NCM811 / LLZO contact area, rather than simply uniformly distributed on all NCM811 free surfaces.

[0121] The characterization results are also important structural evidence proving that the present invention differs from conventional pre-coating methods.

[0122] 3. Interfacial chemical characterization The chemical state and elemental distribution of the NCM811 / LLZO composite interface were analyzed using XPS, depth XPS, or TOF-SIMS, and the content of interfacial by-reaction products in the examples and comparative examples were compared.

[0123] By analyzing the changes in the chemical state of the interface before and after cycling, the inhibitory effect of the Li3PO4-based in-situ interface layer on the direct reaction between NCM811 and LLZO was determined.

[0124] 4. Electrochemical impedance spectroscopy The examples and comparative examples were assembled into all-solid-state batteries with the same structure. After being left to stand at 25°C and under the same stacking pressure until the open-circuit voltage stabilized, AC impedance spectroscopy (EIS) was performed. A Bio-Logic VSP-3e or equivalent electrochemical workstation could be used, with an AC perturbation amplitude of 5 mV and a frequency range of 100 kHz–1 mHz. Tests were performed at the initial state and after the 10th, 50th, and 100th cycles at the same state of charge. A unified equivalent circuit was used to fit the bulk / grain boundary impedance and the interface / charge transfer impedance, and the interface impedance and its growth rate were compared. For the high-nickel cathode study, the EIS test used a 5 mV perturbation and a frequency range of 1 mHz–100 kHz, as detailed in the reference (Wang W, Shi Y, Li P, Wang R, Ye F, Zhang X, Li W, Wang Z, Xu C, Xu D, Xu Q, Cui X. Rational rock-salt phase engineering of a nickel-richlayered cathode interface for enhanced rate and cycling stability). Energy& Environmental Science , 2024, 17: 4283-4294.); For the analytical method of the evolution of interfacial impedance of solid high-nickel cathodes with cycling, please refer to the following literature (Koerver R, Aygün I, Leichtweiß T, Dietrich C, Zhang W, Binder JO, Hartmann P, Zeier WG, Janek J. Capacity Fade in Solid-State Batteries: Interphase Formation and Chemomechanical Processes in Nickel-RichLayered Oxide Cathodes and Lithium Thiophosphate Solid Electrolytes). Chemistry of Materials , 2017 , 29: 5574-5582.).

[0125] Record the initial interface impedance, the interface impedance after different number of cycles, and the impedance growth rate; to ensure comparability, the electrode area, positive electrode active material loading, LLZO sheet thickness, test temperature, and external pressure of each group of batteries are kept consistent.

[0126] It is expected that after the formation of a Li3PO4-based ion-conducting transition layer in the actual contact region of NCM811 / LLZO in Example 1, the Li3PO4-based transition layer will have a more continuous Li3PO4-based transition layer compared to the directly mechanically mixed sample. + Transmission path and more stable interface contact.

[0127] 5. Constant current charge / discharge and rate performance testing The Xinwei CT-4008Q or equivalent multi-channel battery testing system was used for testing at 25°C under the same external stacking pressure. When Li metal was used as the counter / reference electrode, the voltage window could be set to 3.0-4.3 V (vs. Li / Li+). First, activation was performed at 0.1C for 3 cycles, followed by sequential testing at 0.1C, 0.2C, 0.5C, and 1C rates, maintaining each rate for 5 cycles, then returning to 0.1C to evaluate capacity recovery. For long-term cycling, at least 100 cycles at 0.5C were performed. The initial charge / discharge specific capacity, first-cycle coulombic efficiency, discharge specific capacity at each rate, rate recovery capacity, capacity retention, and average coulombic efficiency were recorded.

[0128] The voltage window and test equipment / temperature mentioned above can be found in the literature (Wang W, Shi Y, Li P, Wang R, YeF, Zhang X, Li W, Wang Z, Xu C, Xu D, Xu Q, Cui X. Rational rock-salt phase engineering of a nickel-rich layered cathode interface for enhanced rate and cycling stability). Energy & Environmental Science , 2024 According to the test method in (17: 4283-4294.), the solid-state system should additionally maintain a constant stacking pressure and uniform LLZO thickness and area.

[0129] 6. Characterization of post-cycle chemical-mechanical stability After completing the specified cycles, the test was stopped under the same state of charge, and the all-solid-state battery was disassembled in an inert atmosphere or a low dew point dry environment. The composite cathode was observed using cross-sectional SEM, FIB-SEM, and, if necessary, TEM / HRTEM to compare the cracking of NCM811 particles, the porosity / debonding of the NCM811 / LLZO interface, the breakage of the LLZO network, and the continuity of the interface layer before and after cycling. The design basis for the particle size and volume changes of the solid-state cathode and the chemical-mechanical failure can be found in the reference (Minnmann P, Strauss F, Bielefeld A, Ruess R, Adelhelm P, Burkhardt S, Dreyer SL, Trevisanello E, Ehrenberg H, Brezesinski T, Richter FH, Janek J. Designing Cathodes and Cathode Active Materials for Solid-State Batteries). Advanced Energy Materials , 2022For characterization of interface / contact loss in high-nickel solid cathode cycling, please refer to the following reference (Koerver R, Aygün I, Leichtweiß T, Dietrich C, Zhang W, Binder JO, Hartmann P, Zeier WG, Janek J. Capacity Fade in Solid-State Batteries: Interphase Formation and Chemomechanical Processes in Nickel-Rich LayeredOxide Cathodes and Lithium Thiophosphate Solid Electrolytes). Chemistry of Materials , 2017 , 29: 5574-5582. / Koerver R, Zhang W, de Biasi L, SchweidlerS, Kondrakov AO, Kolling S, Brezesinski T, Hartmann P, Zeier WG, Janek J. Chemo-mechanical expansion of lithium electrode materials - on the route tomechanically optimized all-solid-state batteries. Energy & Environmental Science , 2018 , 11: 2142-2158.).

[0130] Key comparisons: Whether the NCM811 particles have undergone obvious cracking; Does an interfacial porosity occur between NCM811 and LLZO? Has the LLZO solid electrolyte network broken? Does the Li3PO4-based interface transition layer remain in the NCM811 / LLZO contact region?

[0131] Figure 3Mechanism / design diagram of the relationship between maximum particle size and chemical diffusion coefficient at different magnification ratios (Reference: Minnmann P, Strauss F, Bielefeld A, Ruess R, Adelhelm P, Burkhardt S, Dreyer S L, Trevisanello E, Ehrenberg H, Brezesinski T, Richter FH, Janek J. Designing Cathodes and Cathode Active Materials for Solid-State Batteries). Advanced Energy Materials , 2022 , 12: 2201425.); Figure 3 The figure shows the relationship between particle size and chemical diffusion coefficient under 0.1C, 1C and 5C conditions, and indicates the typical range of NCM and lithium iron phosphate (LFP). This figure is used to illustrate the coupling relationship between NCM particle size, diffusion distance and rate performance, and provides a basis for particle size distribution design of NCM811 and fine-particle LLZO. Figure 4 Figures showing the variation in spherical CAM particle size and the variation in axial dimensions of the NCM811 lattice. Figure 4 In the text, 'a' represents the evolution of the maximum radius of different CAMs with the initial particle radius; 'b' represents the overall size change of NCM811, which can be decomposed into changes in the a-axis and c-axis directions; the anisotropic size change of NCM811 is prone to stress concentration and debonding at its contact interface with rigid LLZO. This invention buffers this chemical-mechanical mismatch through an in-situ nano-transition layer. Figure 4 This diagram illustrates the mechanism of maximum particle radius variation and NCM811 lattice a-axis and c-axis anisotropy changes during cycling for different cathode active materials (Reference: Minnmann P, Strauss F, Bielefeld A, Ruess R, Adelhelm P, Burkhardt S, Dreyer SL, Trevisanello E, Ehrenberg H, Brezesinski T, Richter FH, Janek J. Designing Cathodes and Cathode Active Materials for Solid-State Batteries). Advanced Energy Materials , 2022 (12: 2201425.), used to explain the relationship between the chemomechanical mismatch, particle size and interfacial contact maintenance of high-nickel layered cathodes.

[0132] The foregoing has shown and described the basic principles and main features of the present invention, as well as its advantages. Those skilled in the art should understand that the present invention is not limited to the above embodiments. The embodiments and descriptions in the specification are merely illustrative of the principles of the invention. Various changes and modifications can be made to the invention without departing from its spirit and scope, and all such changes and modifications fall within the scope of the present invention as claimed. The scope of protection of this invention is defined by the appended claims and their equivalents.

Claims

1. A high-nickel NCM811 / LLZO all-solid-state composite electrode with an in-situ constructed interface transition layer, characterized in that, The composite electrode includes a positive electrode active material, a solid electrolyte, and an in-situ interface transition layer located at the contact area between the two; depending on the electron transport requirements, it may further include a conductive carbon material. The positive electrode active material is NCM811, or a layered oxide of NCM or NCMA with a Ni content of not less than 80%; the NCM811 is LiNi. 0.8 Co 0.1 Mn 0.1 O2 layered oxides; The solid electrolyte is Li7La3Zr2O 12 Or its stable cubic phase derivatives doped with elements such as Ta, Nb, Al, and Ga; Alternatively, the solid electrolyte may be a cubic phase stabilized garnet electrolyte such as Ta-LLZO, Nb-LLZO, Al-LLZO, or Ga-LLZO.

2. The high-nickel NCM811 / LLZO all-solid-state composite electrode as described in claim 1, characterized in that, The interface transition layer is a lithium- and oxygen-containing ion-conducting inorganic phase, formed by the in-situ reaction of one or more of the lithium source and phosphorus, boron, and silicon sources inside the composite electrode. It preferably includes Li3PO4, lithium boron oxide (Li3BO3), lithium silicon oxide (Li2SiO3), or a composite phase thereof. The interface transition layer is mainly distributed in the contact neck of NCM811 / LLZO particles, the interparticle gaps, and the side of the NCM811 surface adjacent to LLZO, rather than being formed only on the surface of a single powder pre-coated particle. The equivalent thickness of the interface transition layer is approximately 2-50 nm; the content of the interface precursor conversion product, based on the total mass of the all-solid-state composite electrode, is 0.1-5 wt% of the total mass of the positive electrode active material and the solid electrolyte. In the composite electrode, the mass ratio of the positive electrode active material to the solid electrolyte is (4~9):(1~4).

3. A method for preparing a high-nickel NCM811 / LLZO all-solid-state composite electrode with an in-situ constructed interface transition layer, characterized in that, Includes the following steps: 1) Raw material pretreatment Weigh out NCM811 positive electrode active material and vacuum dry or dry at normal pressure for a certain period of time, and set aside for later use; weigh out cubic phase LLZO solid electrolyte and vacuum dry or dry at normal pressure for a certain period of time, and set aside for later use, in order to reduce the adverse effects of surface adsorbed water and carbonate on interface construction. 2) NCM811 / LLZO composite and solid-state contact network backbone construction The dried NCM811 positive electrode active material and LLZO are weighed according to a certain mass ratio and mixed under certain conditions. Then, they are pre-pressed by cold pressing, rolling pressing or molding to obtain composite powder or pre-pressed sheet that forms the NCM811 / LLZO contact skeleton, so that NCM811 and LLZO establish an initial solid-solid contact network. 3) Preparation of lithium phosphate interfacial precursor solution The lithium source and the film-forming anionic precursor are dissolved or dispersed in a first solvent to obtain a low-viscosity interface precursor solution; by adjusting the concentration of the precursor solution, the final interface phase does not excessively cover the electron transport path. 4) Selective wetting of the contact area The interface precursor solution is introduced into the composite powder or pre-compressed sheet that forms the NCM811 / LLZO contact framework by means of spray wetting, drop addition, vacuum wetting, atomization deposition, or small amount of liquid phase assisted mixing. The interface precursor solution is preferentially introduced into the NCM811 / LLZO contact neck and interparticle micropores by capillary action. The drop addition-vacuuming-restoration of normal pressure process is repeated until all the precursor solution is introduced into the composite powder. Then, the solvent is removed by drying at 30-80℃, so that the precursor is retained near the real solid-solid interface to obtain the composite material. 5) Low-temperature in-situ reaction generates Li3PO4-based interfacial transition layer The dried composite material is placed in a tube furnace and heated to 200-500℃ at a rate of 1-5℃ / min under air, pure oxygen or a mixture of oxygen and inert protective gas, and held for 0.5-6 h to perform heat treatment, so that the precursor decomposes and a lithium-ion conductive interface transition layer is generated in situ in the NCM811 / LLZO contact area. 6) Conductive agent composite and composite cathode forming Step 5) After the heat treatment is completed, cool to room temperature to obtain NCM811 / Li3PO4 / LLZO in-situ interface composite powder. Then crush and sieve it. Add a conductive agent to the in-situ treated composite powder and perform low-shear mixing to make the conductive agent evenly distributed between the NCM811 particles. Then prepare the composite positive electrode layer by cold pressing, molding or rolling, and bond it with a dense LLZO solid electrolyte sheet to prepare a high-nickel NCM811 / LLZO all-solid-state composite electrode.

4. The preparation method according to claim 3, characterized in that, In step 1), the NCM811 positive electrode active material is LiNi. 0.8 Co 0.1 Mn 0.1 O2 layered oxide; the LLZO is Li7La3Zr2O 12 Or its stable cubic phase derivatives doped with elements such as Ta, Nb, Al, and Ga; In step 1), the drying conditions for the NCM811 positive electrode active material are vacuum drying or atmospheric pressure drying at 80-150℃ for 2-12 hours. In step 1), the drying conditions for the cubic LLZO solid electrolyte are vacuum drying or atmospheric pressure drying at 100-300℃ for 2-12 h.

5. The preparation method according to claim 3, characterized in that, In step 2), the mass ratio of NCM811 positive electrode active material to LLZO is (4~9):(1~4). In step 2), the dried NCM811 positive electrode active material is mixed with LLZO by low-energy ball milling, three-dimensional mixing or dry mechanical mixing; the mixing time is 20~80min.

6. The preparation method according to claim 3, characterized in that, In step 3), the film-forming anion precursor is one or more of phosphorus source, boron source, and silicon source; The lithium source is anhydrous lithium acetate, lithium nitrate, lithium lactate, or other materials that can decompose at lower temperatures to provide lithium. + Lithium salts; phosphorus sources include phosphoric acid, ammonium dihydrogen phosphate, or organic phosphate esters; boron sources include boric acid or borate esters; and silicon sources include tetraethyl orthosilicate, etc. In step 3), the first solvent is anhydrous ethanol or an ethanol-based low-aqueous solvent.

7. The preparation method according to claim 3, characterized in that, In step 3), when preparing the interface precursor solution, the obtained interface phase is Li3PO4, Li3BO3 (lithium borate), Li2SiO3 (lithium metasilicate) or a composite phase thereof. The total concentration of lithium source, phosphorus source, boron source and / or silicon source in the precursor solution is controlled so that the theoretical mass of the interface phase formed after complete conversion accounts for 0.3-2.0 wt% of the total mass of NCM811 and LLZO.

8. The preparation method according to claim 3, characterized in that, In step 5), the heat treatment temperature is 250-400℃ to ensure both the full conversion of the precursor and the structural stability of NCM811. In step 5), the equivalent thickness of the interface transition layer is about 2-50 nm; the content of the interface precursor conversion product is 0.1-5 wt% of the total mass of NCM811 and LLZO based on the total mass of the all-solid composite electrode.

9. The preparation method according to claim 3, characterized in that, In step 6), the conductive agent is conductive carbon black, conductive carbon nanotubes, or other conductive carbon materials; the amount of conductive agent added is 0-10 wt% of the total mass of the composite powder. The dense LLZO solid electrolyte sheet can be obtained by pressing cubic phase LLZO or its Ta, Nb, Al, Ga doped derivative powders at 50-200 MPa and sintering at 1100-1250℃ for 1-12 h. After sintering, it is subjected to double-sided grinding, polishing and drying. The preferred relative density is not less than 90%.

10. The application of the high-nickel NCM811 / LLZO all-solid-state composite electrode with an in-situ constructed interface transition layer as described in claim 1 or 2 in the preparation of all-solid-state lithium-ion batteries.