Composition for forming negative electrode, secondary battery negative electrode, and secondary battery

By combining resins with specific functional groups, carbon-silicon composite particles, and monolayer carbon nanotubes, the problem of insufficient dispersion of monolayer carbon nanotubes was solved, improving the dispersion and adhesion of the negative electrode material and enhancing the battery performance of the secondary battery.

CN123120660APending Publication Date: 2026-11-17DIC CORP
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202610461076.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2025-05-14
Filing Date
2026-04-09
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

In existing technologies, the dispersibility and adhesion of single-layer carbon nanotubes to the current collector are insufficient, which leads to a decrease in the battery performance of the anode material. In particular, when silicon-containing anode active materials and single-layer carbon nanotubes are mixed, it is difficult to disperse them stably, which affects the high capacity and lifespan of the battery.

Method used

A composition for forming a negative electrode is formed by combining resins with specific functional groups (urethane, urea, amide, and imide groups) with composite particles containing carbon and silicon, single-layer carbon nanotubes, and carboxymethyl cellulose, using an aqueous solvent. This improves dispersibility and adhesion, and inhibits SEI rupture.

Benefits of technology

Excellent dispersion of silicon-containing anode active material and single-layer carbon nanotubes was achieved, which improved the durability of the electrolyte and the tightness of the current collector, improved the charge and discharge efficiency and capacity retention, and enhanced the battery characteristics of the secondary battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

This invention provides a negative electrode forming composition, a secondary battery negative electrode formed from the negative electrode forming composition, and a secondary battery having the negative electrode. The negative electrode forming composition can form a secondary battery with excellent dispersion of the negative electrode active material and monolayer carbon nanotubes, and excellent battery characteristics such as electrolyte durability, adhesion to the current collector, charge / discharge efficiency, and capacity retention. A negative electrode forming composition comprises: a resin (A) having one or more functional groups selected from urethane, urea, amide, and imide groups; a negative electrode active material (B) containing composite particles of carbon and silicon; monolayer carbon nanotubes; carboxymethyl cellulose or a salt thereof; and an aqueous solvent.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to a composition for forming a negative electrode, a negative electrode for a secondary battery, and a secondary battery. More specifically, this invention relates to a composition for forming a negative electrode for a non-aqueous secondary battery, a negative electrode for a non-aqueous secondary battery, and a non-aqueous secondary battery. Background Technology

[0002] Non-aqueous secondary batteries, such as lithium-ion batteries (non-aqueous electrolyte secondary batteries), are rapidly being developed for hybrid vehicles, electric vehicles, and household batteries due to their high energy density and rechargeability, and their application scope is expanding. Furthermore, in recent years, with the development of high performance and miniaturization in various portable electronic and communication devices, the demand for secondary batteries with further improvements in capacity, cycle characteristics, discharge rate, and other battery properties is also increasing. To further enhance the performance of non-aqueous secondary batteries, research is underway to improve various battery components, such as electrodes.

[0003] The negative electrode for non-aqueous secondary batteries typically comprises a current collector and an electrode layer (negative electrode material layer) formed on the current collector. This negative electrode material layer is formed, for example, from a slurry-like composition for forming a negative electrode by dispersing a composition containing a negative electrode active material and a binder (adhesive) in a dispersion medium.

[0004] In previous lithium-ion rechargeable batteries, graphite was mainly used as the anode material. However, due to the low theoretical capacity density of graphite (372 mAh / g), there are limitations to the development of lithium-ion batteries with higher energy densities. To compensate for the theoretical capacity density of graphite, anode materials using elements capable of absorbing and releasing lithium ions, such as metals like silicon and tin, or alloys and oxides of other elements, are being researched. Among these, silicon has a theoretical capacity more than 10 times that of graphite (4200 mAh / g), therefore silicon and silicon-containing anode active materials are attracting much attention as next-generation anode materials capable of achieving high capacity.

[0005] For example, Patent Document 1 discloses a particulate material composed of composite particles, wherein the composite particles contain micropores and mesopores at a predetermined volume ratio, and the total pore volume, as measured by gas adsorption, is 0.4 to 0.75 cm³. 3 / g of porous carbon skeleton and multiple nanoscale silicon regions located within the pores of the porous carbon skeleton, wherein the mass ratio of silicon to the porous carbon skeleton is in the range of 0.9 to 1.9 times the total pore volume.

[0006] Furthermore, to extend the lifespan of secondary batteries, research has been conducted on using carbon nanotubes, which exhibit excellent conductivity, as conductive additives in the electrode composition. Patent Document 2 discloses a monolayer carbon nanotube dispersion containing specific carboxymethyl cellulose and water, with the monolayer carbon nanotube content ranging from 0.47% to 1.00% by mass. This dispersion exhibits excellent dispersion stability of the monolayer carbon nanotubes and can be applied to electrode coatings for non-aqueous electrolyte secondary batteries containing silicon-based active materials.

[0007] In addition, studies were conducted on using copolymers containing structural units based on nitrile monomers and structural units based on acrylic acid as adhesives.

[0008] For example, Patent Document 3 discloses an adhesive resin composition containing a copolymer and an alkaline compound; the copolymer contains structural units from a nitrile-containing monomer, structural units from a monomer containing an acidic functional group, and structural units from a specific monomer in a predetermined ratio; the alkaline compound can neutralize the aforementioned acidic functional groups. This adhesive resin composition exhibits excellent electrolyte resistance, high adhesion between active materials and between the active materials and the current collector, prevents electrode peeling, and achieves high capacity and excellent charge-discharge cycle characteristics. Patent Document 4 discloses an acrylonitrile copolymer adhesive containing predetermined amounts of acrylonitrile units, acrylate units, acrylamide units, and acrylate units, which can adapt to the periodic volume changes that occur with the absorption and release of lithium ions by the electrode active materials during charge and discharge, thereby improving battery characteristics such as capacity and cycle characteristics.

[0009] Existing technical documents

[0010] Patent documents

[0011] Patent Document 1: International Publication No. 2020 / 234586

[0012] Patent Document 2: Japanese Patent No. 7194860

[0013] Patent Document 3: Japanese Patent Application Publication No. 2012-051999

[0014] Patent Document 4: International Publication No. 2018 / 032665 Summary of the Invention

[0015] The problem that the invention aims to solve

[0016] Monolayer carbon nanotubes have a small average fiber diameter, ranging from 0.5 to 10 nm, and due to their strong cohesion caused by van der Waals forces, they are difficult to disperse stably and uniformly at high concentrations. Although commercially available aqueous dispersions of monolayer carbon nanotubes contain carboxymethyl cellulose as a dispersant, the actual content of monolayer carbon nanotubes is less than 0.4% by mass. The concentration of monolayer carbon nanotubes in the dispersion disclosed in Patent Document 2 is also 0.77% to 0.97% by mass. Furthermore, when preparing compositions for negative electrode formation, the dispersant effect of carboxymethyl cellulose tends to decrease due to adsorption by components such as binders. As a result, it can easily lead to reduced adhesion to the current collector and affect battery performance, such as cycle characteristics.

[0017] The adhesives in Patent Documents 3 and 4 do not adequately follow the volume expansion and contraction caused by the insertion and removal of lithium ions in silicon-based anode active materials, nor do they provide sufficient durability. Furthermore, their compatibility with monolayer carbon nanotubes cannot be considered sufficient.

[0018] Therefore, there is a desired anode forming material that can improve battery characteristics such as high capacity based on silicon-containing anode active materials and long lifespan achieved by using monolayer carbon nanotubes as conductive additives, improve the dispersion of silicon-containing anode active materials and monolayer carbon nanotubes, have excellent adhesion between anode active materials or between anode active materials and current collectors, effectively suppress the rupture of SEI (Solid Electrolyte Interphase), and exhibit balanced durability to electrolytes.

[0019] The inventors have studied aqueous anode-forming compositions that can suppress aggregation and improve dispersion stability even when combined with silicon-containing anode active materials as anode active materials and monolayer carbon nanotubes as conductive additives at high concentrations. The results showed that if a resin with specific functional groups is included, the resulting anode material layer exhibits excellent durability to the electrolyte and excellent adhesion to the current collector. Furthermore, it effectively improves battery characteristics such as charge / discharge efficiency and capacity retention, thus completing the present invention.

[0020] The purpose of this invention is to provide a negative electrode forming composition for a secondary battery that can form a silicon-containing negative electrode active material and a single layer of carbon nanotubes with excellent dispersibility and excellent battery characteristics such as durability with electrolyte, adhesion to current collector, charge and discharge efficiency and capacity retention, a negative electrode for a secondary battery formed from the negative electrode forming composition, and a secondary battery having the negative electrode.

[0021] Methods for solving problems

[0022] The present invention has the following aspects.

[0023] [1] A composition for forming a negative electrode comprises: a resin (A) having one or more functional groups selected from urethane, urea, amide and imide; a negative electrode active material (B) comprising composite particles containing carbon and silicon; a single-layer carbon nanotube; carboxymethyl cellulose or a salt thereof; and an aqueous solvent.

[0024] [2] The negative electrode forming composition according to [1], wherein the resin (A) is in the form of particles with an average particle size of 50 to 500 nm.

[0025] [3] The negative electrode forming composition according to [1] or [2], wherein the total functional group concentration of urethane group, urea group, amide group and imide group in the above resin (A) is 10 to 2000 mmol / kg.

[0026] [4] The negative electrode forming composition according to any one of [1] to [3], wherein, relative to the total amount of units constituting the above-mentioned resin (A), the content of structural units based on aromatic vinyl monomers (a1) is 15% by mass or more and 80% by mass or less, the content of structural units based on (meth)acrylates (a2) is 15% by mass or more and 80% by mass or less, the content of structural units based on vinyl monomers (a3) ​​having acid groups is 0.1% by mass or more and 10% by mass or less, and the content of structural units based on vinyl monomers (a4) having one or more functional groups selected from urethane groups, urea groups, amide groups and imide groups is 0.1% by mass or more and 10% by mass or less.

[0027] [5] The negative electrode forming composition according to any one of [1] to [4], wherein the composite particles contained in the negative electrode active material (B) are composite carbon particles having a porous carbon material and a silicon component, and having a silicon component in at least a portion of the pores of the porous carbon material.

[0028] [6] The negative electrode forming composition according to any one of [1] to [5], wherein, relative to the total mass of the negative electrode forming composition, the content of the resin (A) is 0.1% by mass or more and 5% by mass or less, the content of the negative electrode active material (B) is 30% by mass or more and 60% by mass or less, the content of the monolayer carbon nanotube is 0.005% by mass or more and 0.3% by mass or less, the content of the carboxymethyl cellulose is 0.01% by mass or more and 3% by mass or less, and the content of the aqueous solvent is 35% by mass or more and 65% by mass or less.

[0029] [7] The negative electrode forming composition according to any one of [1] to [6] has a viscosity of 200 mPa·s or more and 20000 mPa·s or less.

[0030] [8] The negative electrode forming composition according to any one of [1] to [7], wherein when the mixture obtained by mixing the above resin (A) in a manner of 1.85% by mass, the above monolayer carbon nanotubes in a manner of 0.03% by mass, the above carboxymethyl cellulose in a manner of 0.04% by mass and the above aqueous solvent in a manner of 98.08% by mass is filtered using a 200-mesh filter, the amount of the above monolayer carbon nanotubes remaining on the filter is less than 1% of the above monolayer carbon nanotubes contained in the mixture.

[0031] [9] The negative electrode forming composition according to any one of [1] to [8], wherein the viscosity of the mixture formed by mixing the above-mentioned resin (A) in the manner of 1.2% by mass, the above-mentioned negative electrode active material (B) in the manner of 56.4% by mass, the above-mentioned carboxymethyl cellulose in the manner of 0.6% by mass and the above-mentioned aqueous solvent in the manner of 41.8% by mass is 200 mPa·s or more and 20000 mPa·s or less.

[0032]

[10] A secondary battery negative electrode comprising a negative electrode material layer formed using any one of the negative electrode forming compositions described in [1] to [9].

[0033]

[11] A secondary battery comprising the secondary battery negative electrode, positive electrode, electrolyte and separator described in

[10] .

[0034] Invention Effects

[0035] According to the present invention, a negative electrode forming composition for a secondary battery that can form a silicon-containing negative electrode active material and a single layer of carbon nanotubes with excellent dispersibility and excellent battery characteristics such as durability to electrolyte, adhesion to current collector, charge-discharge efficiency and capacity retention, a secondary battery negative electrode formed by the negative electrode forming composition, and a secondary battery having the negative electrode are provided. Detailed Implementation

[0036] The present invention is a composition for forming a negative electrode, comprising: a resin (A) having one or more functional groups selected from urethane, urea, amide and imide groups (hereinafter also referred to as "resin (A)"); a negative electrode active material (B) containing composite particles containing carbon and silicon (hereinafter also referred to as "negative electrode active material (B)"); a single-layer carbon nanotube; carboxymethyl cellulose or a salt thereof; and an aqueous solvent.

[0037] The embodiments of the present invention will now be described in detail. It should be noted that, in this specification, the numerical range represented by "~" indicates the range in which the values ​​before and after the "~" are respectively the minimum and maximum values.

[0038] Resin (A) has one or more functional groups selected from urethane, urea, amide, and imide groups. Resin (A) can be linear or branched, and can be random, block, graded, or grafted, or can have a cross-linked structure.

[0039] One or more functional groups selected from urethane, urea, amide and imide can be present in the main chain of resin (A), or in the side chain or at the end.

[0040] The resin (A) is preferably in particulate form with an average particle size of 50 to 500 nm. If the resin (A) is in particulate form within the above-mentioned particle size range, it is easier to improve the dispersibility of the negative electrode active material (B) and the monolayer carbon nanotubes in the negative electrode forming composition of the present invention. Furthermore, the adhesion between the negative electrode active materials (B) and each other, or between the negative electrode active material (B) and the current collector, is easily excellent. Consequently, the secondary battery having a negative electrode obtained from the negative electrode forming composition of the present invention tends to have excellent battery characteristics such as charge / discharge efficiency and capacity retention. It should be noted that the average particle size of the resin (A) refers to the cumulative 50% diameter (D50) of the volume reference in the particle size distribution obtained by laser diffraction.

[0041] Resin (A) with an average particle size of 50-500 nm can be appropriately manufactured by emulsion polymerization as described later.

[0042] Furthermore, the total functional group concentration of urethane groups, urea groups, amide groups, and imide groups in resin (A) is preferably 10 to 2000 mmol / kg, more preferably 15 to 1500 mmol / kg. If the functional group concentration is within the above range, the dispersibility of the negative electrode active material (B) and the monolayer carbon nanotubes in the negative electrode forming composition of the present invention is easily improved, and the adhesion between the negative electrode active materials (B) and each other or between the negative electrode active material (B) and the current collector is also easily excellent.

[0043] It should be noted that the details of the method for calculating the total functional group concentration of urethane, urea, amide and imide groups in resin (A) are described later in Example 1.

[0044] The weight-average molecular weight (Mw) of resin (A) is preferably in the range of 10,000 to 5,000,000, more preferably in the range of 50,000 to 1,000,000. It should be noted that the weight-average molecular weight (Mw) of resin (A) can be determined using gel permeation chromatography (GPC) as a conversion of the weight-average molecular weight of standard polystyrene.

[0045] The resin (A) has one or more functional groups selected from urethane, urea, amide and imide groups, preferably derived from structural units based on polymerizable monomers having these functional groups.

[0046] The resin (A) preferably has a structural unit based on an aromatic vinyl monomer (a1), a structural unit based on a (meth)acrylate (a2), a structural unit based on a vinyl monomer with an acid group (a3), or a structural unit of a vinyl monomer (a4) having one or more functional groups selected from urethane, urea, amide and imide (hereinafter also referred to as "functionalized vinyl monomer (a4)").

[0047] Examples of aromatic vinyl monomers (a1) include styrene, α-methylstyrene, 2-methylstyrene, 3-methylstyrene, 4-methylstyrene, 4-propylstyrene, 4-tert-butylstyrene, 4-cyclohexylstyrene, 4-dodecylstyrene, 2,4-dimethylstyrene, 2,4-diisopropylstyrene, 2,4,6-trimethylstyrene, 2-ethyl-4-benzylstyrene, 4-(phenylbutyl)styrene, 1-vinylnaphthalene, 2-vinylnaphthalene, vinylanthracene, N,N-diethyl-4-aminoethylstyrene, vinylpyridine, 4-methoxystyrene, monochlorostyrene, dichlorostyrene, divinylbenzene, etc. They can be used alone or in combination of two or more. Among these, styrene, α-methylstyrene, and 4-methylstyrene are preferred, with styrene being more preferred.

[0048] (Meth)acrylate (a2) is preferably CH2=CR 1 -COOR 2 (where R is in the formula) 1 R represents a hydrogen atom or a methyl group. 2 Indicates alkyl, cycloalkyl, aryl, or aralkyl. R 2 The alkyl, cycloalkyl, aryl, or aralkyl groups represented may have substituents. Here, R 2 The alkyl group preferably has 1 to 20 carbon atoms, the cycloalkyl group preferably has 3 to 20 carbon atoms, the aryl group preferably has 6 to 20 carbon atoms, and the aralkyl group preferably has 7 to 20 carbon atoms. As R 2 The alkyl, cycloalkyl, aryl, or aralkyl groups may have substituents, such as halogen atoms, hydroxyl groups, alkoxy groups, amino groups, etc.

[0049] Examples of (meth)acrylates (a2) include, for example, methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, butyl (meth)acrylate, pentyl (meth)acrylate, hexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, lauryl (meth)acrylate, stearyl (meth)acrylate, phenyl (meth)acrylate, benzyl (meth)acrylate, 2-hydroxyethyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 4-hydroxy-n-butyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 2-hydroxy-n-butyl (meth)acrylate, 3-hydroxy-n-butyl (meth)acrylate, 1,4-cyclohexanediethanol mono(meth)acrylate, N-(2-hydroxyethyl)(meth)acrylamide, and glycerol mono(meth)acrylate. Acrylates, polyethylene glycol mono(meth)acrylates, polypropylene glycol mono(meth)acrylates, 2-hydroxy-3-phenoxypropyl(meth)acrylates, 2-(meth)acryloyloxyethyl-2-hydroxyethyl phthalate, N,N-dimethylaminoethyl(meth)acrylates, N,N-diethylaminoethyl(meth)acrylates, N,N-dimethylaminopropyl(meth)acrylates, N,N-diethylaminopropyl(meth)acrylates, polyethylene glycol (meth)acrylates, methoxy polyethylene glycol (meth)acrylates, polypropylene glycol (meth)acrylates, methoxy polypropylene glycol (meth)acrylates, polybutylene glycol (meth)acrylates, methoxy polybutylene glycol (meth)acrylates, ethylene glycol di(meth)acrylates, propylene glycol di(meth)acrylates, etc. They can be used alone or in combination of two or more types.

[0050] Vinyl monomers with acid groups (a3) ​​are compounds possessing acidic functional groups such as carboxyl, sulfonyl, and phosphine groups, as well as olefinic unsaturated double bonds. Examples include acrylic acid, methacrylic acid, crotonic acid, maleic acid or its anhydride, itaconic acid or its anhydride, citraconic acid, vinylbenzoic acid, fumaric acid, vinylbenzenesulfonic acid, and phosphonoethyl methacrylate. They can be used alone or in combination with two or more.

[0051] The functional group-containing vinyl monomer (a4) is a compound having one or more functional groups selected from urethane, urea, amide and imide groups, as well as an alkene unsaturated double bond.

[0052] Examples of vinyl monomers having urethane or urea groups include butyl urethane acrylate as shown in formula (a4-1) and alkyl urethane acrylates such as the compound shown in formula (a4-2). In formula (a4-2), R and R' each independently represent an alkylene group. It should be noted that the compound shown in formula (a4-2) can be a commercially available product, such as "EBECRYL (registered trademark) 8402" manufactured by Daicel-Allnex.

[0053] [Chemistry 1]

[0054]

[0055] Furthermore, examples of vinyl monomers having urethane or urea groups include reaction products having urethane and urea groups obtained by reacting a compound having an isocyanate group with the hydroxyl group of a compound having a hydroxyl group and an olefinic unsaturated double bond, and reaction products having urea and olefinic unsaturated double bonds obtained by reacting a compound having an isocyanate group with the hydroxyl group of a compound having an amino and olefinic unsaturated double bond. Moreover, reaction products obtained by reacting an alcohol or amine with the isocyanate group of a compound having an isocyanate group and an olefinic unsaturated double bond can also be used as functionalized vinyl monomers (a4). Examples include the reaction product of ethyl 2-isocyanate methacrylate with ethanol, the reaction product of ethyl 2-isocyanate methacrylate with diethylamine, and the reaction product of hydroxyl-containing acrylates such as hydroxyethyl acrylate with diisocyanate compounds, i.e., urethane acrylates.

[0056] Examples of vinyl monomers having amide groups include (meth)acrylamide monomers.

[0057] (methyl)acrylamide monomers are preferably CH2=CR 3 -CONHR 4 (where R is in the formula) 3 R represents a hydrogen atom or a methyl group. 4 R represents a hydrogen atom, alkyl, cycloalkyl, or aryl group. 4 The alkyl, cycloalkyl, or aryl groups represented may have substituents. Here, R... 4 The alkyl group preferably has 1 to 20 carbon atoms, the cycloalkyl group preferably has 3 to 20 carbon atoms, and the aryl group preferably has 6 to 20 carbon atoms. As R 4 The alkyl, cycloalkyl, or aryl groups represented may have substituents, such as halogen atoms, hydroxyl groups, alkoxy groups, etc.

[0058] Examples of (meth)acrylamide monomers include (meth)acrylamide, N-methyl (meth)acrylamide, N-ethyl (meth)acrylamide, N-propyl (meth)acrylamide, N-butyl (meth)acrylamide, N-hydroxymethyl (meth)acrylamide, N-hydroxymethyl (meth)acrylamide, and N-butoxymethyl (meth)acrylamide.

[0059] Examples of vinyl monomers having an imide group include maleimide and phenylmaleimide.

[0060] These functional group-containing vinyl monomers (a4) can be used alone or in combination with two or more.

[0061] The resin (A) may have structural units based on other monomers that are different from the above-mentioned aromatic vinyl monomers (a1), (meth)acrylates (a2), vinyl monomers with acid groups (a3), and vinyl monomers containing functional groups (a4) without impairing the effects of the present invention.

[0062] Other monomers mentioned above include, for example, vinyl chloride, vinyl bromide, vinylidene chloride and other halogenated vinylides, vinyl acetate, (meth)acrylonitrile, sodium (meth)allyl sulfonate, sodium (meth)allyloxybenzene sulfonate, sodium styrene sulfonate, 2-acrylamido-2-methylpropanesulfonic acid and its salts, lithium (meth)acrylate, sodium (meth)acrylate and other (meth)acrylate salts, tetrahydrofurfuryl (meth)acrylate, glycidyl (meth)acrylate, vinyltrimethoxysilane, vinyltriethoxysilane, vinylmethyldimethoxysilane, 3-(meth)acryloyloxypropyltrimethoxysilane, 3-(meth)acryloyloxypropyltriethoxysilane, 3-(meth)acryloyloxypropylmethyldimethoxysilane, etc.

[0063] It should be noted that in this specification, "(meth)acrylic acid" is a term that refers to acrylic acid, methacrylic acid, and both. "(meth)acrylate" is a term that refers to acrylate, methacrylate, and both.

[0064] In resin (A), relative to the total amount of units constituting resin (A), it is preferable that the content of structural units based on aromatic vinyl monomers (a1) is 15% by mass or more and 80% by mass or less, the content of structural units based on (meth)acrylates (a2) is 15% by mass or more and 80% by mass or less, the content of structural units based on vinyl monomers having acid groups (a3) ​​is 0.1% by mass or more and 10% by mass or less, and the content of structural units based on functional group-containing vinyl monomers (a4) is 0.1% by mass or more and 10% by mass or less.

[0065] If the content of structural units based on each monomer is set within the above-mentioned range, it is easy to impart softness to the resin (A), and one or more functional groups selected from urethane groups, urea groups, amide groups, and imide groups based on functional group-containing vinyl monomers (a4) interact with the functional groups present on the surface of the negative electrode active material (B) and the monolayer carbon nanotubes, making it easy to increase the concentration of the negative electrode active material (B) and SWCNTs in the negative electrode forming composition of the present invention, and easily improving their dispersibility and dispersion stability. In addition, the adhesion to the current collector and the durability to the electrolyte are easily improved. Furthermore, the charge-discharge characteristics and discharge capacity retention rate of the secondary battery having the negative electrode formed by the negative electrode forming composition of the present invention are easily improved.

[0066] It should be noted that the content of each of the above-mentioned structural units in resin (A) can usually be adjusted in the following way: in the polymerization described later, the mass ratio of each monomer component is set to the above range so that the polymerization of each monomer component is substantially completed.

[0067] Resin (A) can be manufactured by known polymerization methods such as solution polymerization, bulk polymerization, suspension polymerization, and emulsion polymerization. Among these methods, emulsion polymerization is preferred from the viewpoint of easily and readily manufacturing particulate resin (A) with an average particle size within the aforementioned range.

[0068] As a method for obtaining particulate resin (A) by emulsion polymerization, an example method is as follows: In an aqueous medium, in the presence of an emulsifier and a polymerization initiator, aromatic vinyl monomers (a1), (meth)acrylates (a2), vinyl monomers having acid groups (a3), and functionalized vinyl monomers (a4) are mixed in the above-mentioned mass ratio range, and further free radical polymerization is carried out by coexisting other monomers as needed. The polymerization temperature is preferably in the range of 0 to 100°C, more preferably in the range of 30 to 90°C. The polymerization time is generally preferably in the range of 0.5 to 50 hours, more preferably in the range of 1 to 24 hours.

[0069] The emulsion of the obtained resin (A) can be used directly to prepare the negative electrode forming composition of the present invention, or it can be diluted with water or an aqueous solvent as needed to prepare the negative electrode forming composition of the present invention.

[0070] Examples of aqueous media include water, water, and mixtures of water and organic solvents mixed with water. Examples of organic solvents mixed with water include alcohols such as methanol, ethanol, n-propanol, and isopropanol; ketones such as acetone and methyl ethyl ketone; polyalkylene glycols such as ethylene glycol, diethylene glycol, and propylene glycol; alkyl ethers of polyalkylene glycols; amides such as N-methyl-2-pyrrolidone, N,N-dimethylacetamide, N,N-dimethylformamide, and N,N-diethylformamide; ureas such as N,N-dimethylethylurea, N,N-dimethylpropyleneurea, and tetramethylurea; and dimethyl sulfoxide, sulfolane, 1,3-dimethyl-2-imidazolinone, and hexamethylphosphoric triamine.

[0071] From the perspective of safety and reducing environmental impact, it is preferable to use water alone as the aqueous medium.

[0072] The aqueous medium is preferably of the same type as the aqueous solvent contained in the negative electrode forming composition of the present invention. In this case, the aqueous medium used when manufacturing particulate resin (A) by emulsion polymerization can be directly used as the aqueous solvent constituting the negative electrode forming composition of the present invention, which is convenient.

[0073] In other words, resin (A) is preferably used in the preparation of the negative electrode forming composition of the present invention by dispersing particulate resin (A) obtained by emulsion polymerization in an aqueous medium.

[0074] Examples of polymerization initiators include azo compounds such as 2,2'-azobis(isobutyronitrile), 2,2'-azobis(2-methylbutyronitrile), and azobiscyanopentanoic acid; organic peroxides such as tert-butyl peroxypentanoate, tert-butyl peroxybenzoate, tert-butyl peroxy-2-ethylhexanoate, di-tert-butyl peroxide, cumene hydroperoxide, benzoyl peroxide, and tert-butyl hydroperoxide; hydrogen peroxide; persulfates such as ammonium persulfate, potassium persulfate, and sodium persulfate; water-soluble azo compounds such as 2,2'-azobis(2-methylpropanediamine hydrochloride); and redox-type compounds that combine oxidants such as persulfates with reducing agents such as sodium bisulfite, ammonium bisulfite, sodium thiosulfate, and bisulfite, as well as polymerization promoters such as sulfuric acid, ferric sulfate, and copper sulfate. From the viewpoint of facilitating polymerization reactions in aqueous media, water-soluble polymerization initiators are preferred. The amount of polymerization initiator relative to the total amount of monomers used in the manufacture of resin (A) is preferably in the range of 0.001 to 5 mol%, more preferably in the range of 0.01 to 2 mol%.

[0075] In addition, for purposes such as adjusting molecular weight, chain transfer agents such as thiols, thioglycol, carbon tetrachloride, and α-methylstyrene dimers can coexist.

[0076] Examples of emulsifiers include alkylbenzene sulfonates such as sodium dodecylbenzene sulfonate, polyoxyethylene alkylphenyl sulfonates, polyoxyethylene alkyl diphenyl ether sulfonates, alkyl diphenyl ether disulfonates, sodium lauryl sulfate, sodium dodecyl sulfate, and other alkyl sulfate salts; polyoxyethylene alkyl ether sulfates such as sodium polyoxyethylene lauryl ether sulfate; anionic emulsifiers such as dialkyl succinate sulfonate, sodium stearate, and sodium lauryl ether; and polyoxyethylene alkyl ethers such as polyoxyethylene lauryl ether. Nonionic emulsifiers include polyoxyethylene derivatives such as alkyl ethers of oxyene oxide, polyoxyethylene alkylphenyl ethers, and polyoxyethylene diphenyl ether; sorbitan fatty acid esters such as sorbitan monolaurate; glycerol fatty acid esters such as glycerol monostearate; and polyoxyethylene fatty acid esters such as polyethylene glycol monolaurate. Cationic emulsifiers include alkylamine salts such as stearylamine acetate and quaternary ammonium salts such as lauryltrimethylammonium chloride. Biionic emulsifiers include alkyl (amide) betaine and alkyl dimethylamine oxide.

[0077] These emulsifiers can be used alone or in combination of two or more.

[0078] The amount of emulsifier used is preferably in the range of 0.01 to 5% by mass relative to the total amount of monomers used in the manufacture of resin (A).

[0079] Furthermore, from the viewpoint of easily improving the dispersion stability of the obtained particulate resin (A) in an aqueous medium, the pH can be adjusted by using alkaline and / or acidic compounds.

[0080] Examples of basic compounds include amines such as methylamine, dimethylamine, trimethylamine, ethylamine, diethylamine, triethylamine, 2-aminoethanol, and 2-dimethylaminoethanol; inorganic bases such as ammonia, sodium hydroxide, and potassium hydroxide; and quaternary ammonium hydroxides such as tetramethylammonium hydroxide, tetra-n-butylammonium hydroxide, and trimethylbenzylammonium hydroxide. They can be used individually or in combination of two or more. Amines and ammonia are preferred.

[0081] Examples of acidic compounds include carboxylic acids such as formic acid, acetic acid, propionic acid, and lactic acid; monomethyl phosphate and dimethyl phosphate monoesters or diesters of phosphoric acid; organic sulfonic acids such as methanesulfonic acid, benzenesulfonic acid, and dodecylbenzenesulfonic acid; and inorganic acids such as hydrochloric acid, sulfuric acid, nitric acid, and phosphoric acid. One type may be used alone, or two or more may be used in combination. Carboxylic acids are preferred.

[0082] The negative electrode forming composition of the present invention may, as needed, contain other organic binders besides resin (A) without impairing the effects of the present invention. Examples of such other organic binders include styrene-butadiene rubber copolymers; unsaturated carboxylic acid copolymers such as (meth)acrylate copolymers composed of the above-mentioned (meth)acrylate (a2) and vinyl monomers having acid groups (a3); and polymers such as polyvinylidene fluoride, polyethylene oxide, polyepoxychlorohydrin, polyphosphazene, polyacrylonitrile, polyimide, and polyamide-imide.

[0083] The negative electrode forming composition of the present invention contains a negative electrode active material (B), which comprises composite particles containing carbon and silicon. It has been known that negative electrode active materials are obtained by pulverizing silicon substrates such as silicon ingots to the 50-100 nm level, adding carbon, mixing, and then calcining. However, there is room for improvement in battery characteristics such as battery capacity when used in lithium-ion secondary batteries. In recent years, as a negative electrode active material that improves battery characteristics and can suppress the effects of silicon expansion and contraction, for example, the development of composite particles containing carbon and silicon is being promoted: (i) using a porous material composed of carbon-based materials as a base (matrix), and depositing or vaporizing silicon in the fine pores of the porous material using silane gas or the like to form composite particles containing carbon and silicon; (ii) coating the surface of nanoscale silicon crystals with graphene by CVD, thereby forming a porous flexible carbon phase around it, thus forming composite particles containing carbon and silicon.

[0084] The composite particles contained in the negative electrode active material (B) of the negative electrode forming composition of the present invention can be applied in either of the methods described in (i) or (ii). Preferably, the composite particles contained in the negative electrode active material (B) are composite carbon particles having a porous carbon material and a silicon component, with at least a portion of the porous carbon material containing silicon. Here, the porous carbon material preferably has a porous carbon framework comprising micropores and mesopores, with a total pore volume of 0.4 to 0.75 cm³ as measured by gas adsorption. 3 / g. The silicon component is preferably composed of multiple nanoscale silicon regions located within the pores of the aforementioned porous carbon framework.

[0085] In composite carbon particles, the preferred mass ratio of silicon to the porous carbon framework is 0.9 to 1.9 times the total micropore volume. This mass ratio can be determined through elemental analysis.

[0086] In the composite carbon particles, preferably more than 90% by mass of the silicon content is located in the internal pore volume of the porous carbon framework, more preferably more than 95% by mass is located in the internal pore volume of the porous carbon framework.

[0087] The D50 of the composite carbon particles is preferably in the range of 1 μm to 30 μm.

[0088] The D10 of the composite carbon particles is preferably 0.5 μm or more, more preferably 1 μm or more. The D90 of the composite carbon particles is preferably 50 μm or less, more preferably 25 μm or less. In addition, the particle size distribution span of the composite carbon particles specified as (D90-D10) / D50 is preferably 5 or less, more preferably 3 or less.

[0089] The D10, D50, and D90 of the composite carbon particles were determined by conventional laser ablation methods according to ISO 13320:2009.

[0090] The preferred BET surface area of ​​the composite carbon particles is 0.1~100 m². 2 / g, more preferably 1~25m 2 / g. The BET surface area is determined according to ISO 9277 by measuring the physical adsorption of gas molecules on a solid surface.

[0091] The shape of the composite carbon particles can be, for example, spherical or elliptical.

[0092] The composite carbon particles are preferably obtained by chemical vapor infiltration (CVI) of silicon-containing precursors into the porous structure of a porous carbon framework. Here, CVI refers to a process in which a gaseous silicon-containing precursor is thermally decomposed on its surface to form elemental silicon and gaseous byproducts. Examples of gaseous silicon-containing precursors include silanes (SiH4), silane derivatives (disilazane, trisilane, tetrasilane, etc.), and trichlorosilanes (SiHCl3). These silicon-containing precursors can be used alone or as a mixture diluted to 0.5–20% by volume using inert gases such as nitrogen or argon.

[0093] The CVI process can be carried out using known devices such as fixed-bed reactors, rotary kilns, and fluidized-bed reactors at temperatures ranging from 400°C to 700°C.

[0094] Examples of such composite carbon particles include, for instance, the composite particles disclosed in Patent Document 1 mentioned above.

[0095] The negative electrode forming composition of the present invention contains monolayer carbon nanotubes. Carbon nanotubes are formed by winding planar graphite (graphene sheets) consisting of a six-membered ring network of carbon into a cylindrical shape. Monolayer carbon nanotubes (SWCNTs) have a structure with one layer of graphite wound around them, while multilayer carbon nanotubes (MWCNTs) have a structure with two or more layers of graphite wound around them.

[0096] The sidewalls of CNTs can be graphite structures, or at least a portion of them can have an amorphous structure.

[0097] Examples of CNT shapes include needle-like, cylindrical, fishbone-like, playing card-like (sheet-like), and coil-like. These shapes can be used individually or in combination of two or more. Needle-like or cylindrical shapes are preferred.

[0098] Examples of CNT forms include graphite whiskers, filamentous carbon, graphite fibers, ultrafine carbon nanotubes, carbon nanotubes, carbon protofibrils, carbon microtubes, and carbon nanofibers. CNTs can possess one of these forms individually or in combination with two or more forms.

[0099] If SWCNT is used as a conductive additive for the negative electrode, it is softer than MWCNT. Therefore, when silicon-based active materials with large volume changes due to expansion and contraction during charging and discharging are used as negative electrode active materials, it is easier to follow the volume change, which can improve battery performance such as cycle characteristics.

[0100] The diameter (fiber diameter) of SWCNTs is not particularly limited; the average diameter can be, for example, 0.4~100nm, 0.5~10nm, or 1.0~5.0nm. The length of SWCNTs is not particularly limited; the average length can be, for example, 50nm~1mm, or 0.5~100μm. The aspect ratio (the ratio of average length to average diameter) of SWCNTs is not particularly limited; for example, it can be greater than 10 or greater than 100.

[0101] The average diameter and average length of SWCNTs were determined by measuring the diameter and length of 50 randomly selected SWCNTs from images measured using atomic force microscopy, and then calculated by their arithmetic mean.

[0102] SWCNTs may contain MWCNTs without compromising their effectiveness. The SWCNT content relative to the overall carbon nanotube is preferably 80% by mass or more, more preferably 95% by mass or more, and may also be 100% by mass.

[0103] Furthermore, in the particle size distribution of SWCNTs obtained by laser diffraction, the cumulative 10% diameter (D10) based on volume is in the range of 0.01 to 0.1 μm, the cumulative 50% diameter (D50) based on volume is in the range of 0.01 to 30 μm, and the cumulative 90% diameter (D90) based on volume is preferably in the range of 0.05 to 100 μm. Additionally, it is preferable that the ratio of D10 to D50 of the SWCNTs is 0.20 or more, and D90 is less than 200 μm. More preferably, the ratio of D10 to D50 of the SWCNTs is 0.20 or more and 1.0 or less.

[0104] If the D10, D50 and D90 of SWCNT satisfy the above-mentioned numerical range and the above-mentioned relationship, the dispersibility and dispersion stability of the negative electrode forming composition of the present invention are easily excellent, and the uniformity of the formed negative electrode material layer is excellent, thereby easily resulting in excellent battery characteristics of a secondary battery having a negative electrode with the negative electrode material layer and the current collector.

[0105] In this specification, the D10, D50, and D90 values ​​of SWCNT are measured using a laser diffraction particle size distribution measuring device "MASTERSIZER LMS-3000" manufactured by MALVERN PANALITICAL. Under the measurement conditions of "particle type: non-spherical, refractive index 1.75, absorptivity 0.01, dispersion solvent: water, refractive index 1.33", the total volume of the SWCNT particle group dispersed in water was set to 100% to obtain a cumulative curve. The particle sizes at the points where the cumulative volume on the cumulative curve is 10%, 50%, and 90% were set as D10, D50, and D90, respectively.

[0106] The negative electrode forming composition of the present invention may, as needed, further contain conductive additives other than SWCNT without impairing the effects of the present invention. Examples of such other conductive additives include carbon black, graphite, acetylene black, conductive oxides, nitrides, etc. When the negative electrode forming composition of the present invention further contains other conductive additives, their amount is preferably in the range of 1 to 10% by mass relative to the negative electrode active material (B).

[0107] The carboxymethyl cellulose (hereinafter also referred to as "CMC") constituting the negative electrode forming composition of the present invention has a structure in which the hydroxyl groups in the glucose residues constituting cellulose are replaced with carboxymethyl ether groups. CMC may have a carboxyl group (-COOH), may have a carboxyl salt form, or may have both.

[0108] Examples of salts that can be used as salts of carboxymethyl cellulose include alkali metal salts such as sodium, lithium, and potassium salts; alkaline earth metal salts such as calcium and magnesium salts; ammonium salts; alkylamine salts; and organic salts such as alkanolamine salts. These salts may contain one or more types. Alkali metal salts are preferred, and sodium salts are more preferred.

[0109] It should be noted that in this specification, "carboxymethyl cellulose" refers to carboxymethyl cellulose and / or its salts.

[0110] The degree of etherification of CMC is not particularly limited, but is generally preferred to be in the range of 0.65 to 0.85, and more preferably in the range of 0.70 to 0.80. If the degree of etherification of CMC is within the above range, the aggregation of negative electrode active material (B) and SWCNT in the negative electrode forming composition of the present invention can be easily suppressed by balancing the hydrophilicity of CMC with its adhesion to negative electrode active material (B) and SWCNT, thereby easily improving dispersibility and dispersion stability.

[0111] The weight-average molecular weight (Mw) of the CMC is not particularly limited, but is generally preferred to be in the range of 120,000 to 250,000, and more preferably in the range of 130,000 to 200,000. If the Mw of the CMC is within the above range, it is easy to suppress the increase in viscosity of the negative electrode forming composition of the present invention, and the adhesion of the negative electrode active material (B) and SWCNT is easily improved. Therefore, it is easy to achieve a high concentration of the negative electrode active material (B) and SWCNT, suppress their aggregation, achieve excellent dispersibility and dispersion stability, and easily improve battery performance.

[0112] It should be noted that the degree of etherification of CMC and Mw can be determined, for example, by the method described in the aforementioned Patent Document 2.

[0113] The negative electrode forming composition of the present invention may, as needed, contain other water-soluble polymeric dispersants besides CMC, within a range that does not impair the effects of the present invention. Examples of such other water-soluble polymeric dispersants include gelatin, polyvinylpyrrolidone, sodium polyacrylate, and polyvinyl alcohol. When the negative electrode forming composition of the present invention further contains other water-soluble polymeric dispersants, their amount is preferably in the range of 1 to 5% by mass relative to the negative electrode active material (B).

[0114] Examples of aqueous solvents constituting the negative electrode forming composition of the present invention include water, water, and mixtures of water and organic solvents mixed with water. Examples of organic solvents mixed with water include organic solvents that can be used as aqueous media when obtaining particulate resin (A) by emulsion polymerization, and are the same as the organic solvents described above.

[0115] From the perspective of safety and reducing environmental impact, it is preferable to use water alone as an aqueous solvent.

[0116] Aqueous solvents can be directly applied to the aqueous medium used when manufacturing particulate resin (A) via emulsion polymerization. In other words, in the preparation of the negative electrode forming composition of the present invention, resin (A) is used in such a way that particulate resin (A) obtained by emulsion polymerization is dispersed in an aqueous medium, and an aqueous solvent (preferably water) is added as needed. The method for preparing the negative electrode forming composition of the present invention is simple and therefore preferred.

[0117] In the negative electrode forming composition of the present invention, relative to the total mass of the negative electrode forming composition, the content of resin (A) is preferably 0.1% by mass or more and 5% by mass or less, the content of negative electrode active material (B) is 30% by mass or more and 60% by mass or less, the content of SWCNT is 0.005% by mass or more and 0.3% by mass or less, the content of CMC is 0.01% by mass or more and 3% by mass or less, and the content of aqueous solvent is 35% by mass or more and 65% by mass or less.

[0118] The content of resin (A) is more preferably 0.5% by mass or more and 3.0% by mass or less relative to the total mass of the composition for forming the negative electrode.

[0119] The content of negative electrode active material (B) is more preferably 35% by mass or more and 58% by mass or less, relative to the total mass of the composition for forming the negative electrode.

[0120] The content of SWCNT is more preferably 0.01% by mass or more and 0.2% by mass or less relative to the total mass of the composition for forming the negative electrode.

[0121] The CMC content is more preferably 0.05% by mass or more and 2% by mass or less relative to the total mass of the composition for forming the negative electrode.

[0122] The content of aqueous solvent is more preferably 40% by mass or more and 60% by mass or less relative to the total mass of the composition for forming the negative electrode.

[0123] Furthermore, in the negative electrode forming composition of the present invention, the ratio of negative electrode active material (B) to resin (A) is preferably in the range of 15 to 200, more preferably in the range of 40 to 80.

[0124] The total proportion of SWCNT to resin (A) is preferably in the range of 0.005 to 0.2, and more preferably in the range of 0.01 to 0.1.

[0125] The ratio of CMC to the negative electrode active material (B) is preferably in the range of 0.0005 to 0.06, and more preferably in the range of 0.001 to 0.03.

[0126] The preferred ratio of CMC to SWCNT is in the range of 1 to 105, and more preferably in the range of 30 to 60.

[0127] The negative electrode forming composition of the present invention may, as needed, contain other resins besides resin (A), surfactants, antioxidants, light stabilizers, plasticizers, viscosity modifiers, organic or inorganic fillers, and other additives, within a range that does not impair the effects of the present invention.

[0128] The viscosity of the negative electrode forming composition of the present invention is preferably 200 mPa·s or more and 20,000 mPa·s or less, more preferably 1,000 mPa·s or more and 15,000 mPa·s or less. When the viscosity is within the above range, it is easy to coat with a stable thickness.

[0129] For the negative electrode forming composition of the present invention, it is preferable that when filtering a mixture obtained by mixing 1.85% by mass of resin (A), 0.03% by mass of SWCNT, 0.04% by mass of CMC, and 98.08% by mass of aqueous solvent, which are components thereof, through a 200-mesh filter, the amount of SWCNT remaining on the filter is less than 1% of the SWCNT contained in the mixture. If the amount of SWCNT remaining on the filter is less than 1% through the above operation, the aggregation of SWCNT in the negative electrode forming composition of the present invention is suppressed, which is an indicator of good dispersibility.

[0130] In this case, as resin (A), it is preferable that, relative to the total amount of structural units, the content of structural units based on the above-mentioned aromatic vinyl monomer (a1) is 15% or more and 80% or less by mass, the content of structural units based on the above-mentioned (meth)acrylate (a2) is 15% or more and 80% or less by mass, the content of structural units based on the above-mentioned vinyl monomer (a3) ​​having an acid group is 0.1% or more and 10% or less by mass, and the content of structural units based on the above-mentioned functional group-containing vinyl monomer (a4) is 0.1% or more and 10% or less by mass.

[0131] As a SWCNT, it is preferred to have an average diameter of 0.4 to 100 nm, an average length of 50 nm to 1 mm, an aspect ratio of 10 or higher, and a D50 of 0.01 to 30 μm.

[0132] Sodium carboxymethyl cellulose is preferred as the CMC.

[0133] Examples of aqueous solvents include water alone, water and mixtures of solvents mixed with water, with water alone being preferred.

[0134] Furthermore, for the negative electrode forming composition of the present invention, it is preferable that the viscosity of the mixture formed by mixing 1.2% by mass of resin (A), 56.4% by mass of negative electrode active material (B), 0.6% by mass of CMC, and 41.8% by mass of aqueous solvent is 200 mPa·s or more and 20,000 mPa·s or less. If the viscosity of the mixture is within the above range, the negative electrode active material (B) in the negative electrode forming composition of the present invention has good dispersibility, the negative electrode forming composition of the present invention has excellent operability, and the obtained negative electrode has excellent electrical properties.

[0135] In this case, as resin (A), it is preferable that, relative to the total amount of structural units, the content of structural units based on the above-mentioned aromatic vinyl monomer (a1) is 15% or more and 80% or less by mass, the content of structural units based on the above-mentioned (meth)acrylate (a2) is 15% or more and 80% or less by mass, the content of structural units based on the above-mentioned vinyl monomer (a3) ​​having an acid group is 0.1% or more and 10% or less by mass, and the content of structural units based on the above-mentioned functional group-containing vinyl monomer (a4) is 0.1% or more and 10% or less by mass.

[0136] As the negative electrode active material (B), composite carbon particles having a porous carbon material and a silicon component, wherein at least a portion of the pores of the porous carbon material has a silicon component and a D50 in the range of 1 μm to 30 μm are preferred.

[0137] Sodium carboxymethyl cellulose is preferred as the CMC.

[0138] Examples of aqueous solvents include water alone, water and mixtures of solvents mixed with water, with water alone being preferred.

[0139] It is speculated that in the negative electrode forming composition of the present invention, one or more functional groups selected from urethane, urea, amide, and imide groups present in the resin (A) readily exhibit interaction with functional groups present on the surface of the negative electrode active material (B) and the surface of SWCNTs. Furthermore, the appropriate flexibility of the molecular chain of the resin (A) inhibits the aggregation of the negative electrode active material (B) and SWCNTs. This effect is also believed to be further enhanced by the presence of CMC in the negative electrode forming composition of the present invention.

[0140] As a result, it is believed that the concentration of negative electrode active material (B) and SWCNT in the negative electrode forming composition of the present invention can be increased, and their dispersibility and dispersion stability in aqueous solvents can be improved. In addition, the adhesion between negative electrode active materials (B), between SWCNTs, between negative electrode active materials (B) and SWCNTs and the current collector, as well as their durability in electrolytes, are improved. Consequently, the charge-discharge characteristics, discharge capacity retention rate, and other battery performance of the secondary battery having a negative electrode formed by the negative electrode forming composition of the present invention are improved.

[0141] Secondary batteries

[0142] The present invention also provides a secondary battery negative electrode having a negative electrode material layer formed using the negative electrode forming composition of the present invention described above.

[0143] The present invention also provides a secondary battery comprising a negative electrode, a positive electrode, an electrolyte, and a separator.

[0144] As the non-aqueous secondary battery of the present invention, a non-aqueous electrolyte secondary battery and a solid electrolyte secondary battery are preferred, especially a non-aqueous electrolyte secondary battery having a negative electrode material layer formed using the negative electrode forming composition of the present invention, which easily exhibits excellent performance. For example, in the case of a wet electrolyte secondary battery of the present invention, it can be constructed by arranging the negative electrode and positive electrode of the present invention opposite each other with a separator in between and injecting electrolyte.

[0145] The negative electrode of the secondary battery of the present invention is obtained, for example, by coating the negative electrode forming composition of the present invention onto a current collector to form a thin film, thereby forming a negative electrode material layer. Examples of materials for the current collector include copper, nickel, titanium, and stainless steel. The current collector is preferably formed into a foil, perforated foil, mesh, or other strip-like shape. Additionally, porous materials such as porous metals (foamed metals) and carbon paper can also be used as current collectors.

[0146] Methods for coating the negative electrode forming composition of the present invention onto the current collector include, for example, metal mask printing, electrostatic coating, dip coating, spraying, roll coating, doctor blade coating, gravure coating, and screen printing. After coating, it is preferable to perform rolling processing using a flatbed press, calendering rolls, or the like as needed.

[0147] Alternatively, the paste-like negative electrode forming composition can be molded into sheets or granules and then integrated with the current collector by means of rollers, presses or combinations thereof, thereby obtaining a negative electrode material layer.

[0148] The negative electrode material layer formed on the current collector or the negative electrode material layer integrated with the current collector is preferably subjected to heat treatment. Through this heat treatment, the solvent from the negative electrode forming composition of the present invention can be removed, and the high strength brought about by the curing of the resin (A) can be achieved, thereby improving the adhesion between the negative electrode active materials (B) and between the negative electrode active materials (B) and the current collector.

[0149] The heat treatment temperature is preferably in the range of 50~220℃, more preferably in the range of 100~200℃. The heat treatment time is not particularly limited, and is typically in the range of 1 minute to 20 hours.

[0150] It should be noted that, from the viewpoint of preventing oxidation of the current collector during heat treatment, it is preferable to carry out heat treatment in a non-oxidizing gas atmosphere such as helium, argon, or nitrogen, or in a vacuum atmosphere.

[0151] Furthermore, after heat treatment, the negative electrode, consisting of a negative electrode material layer formed on the current collector or a negative electrode material layer integrated with the current collector, is preferably subjected to pre-pressurization treatment from the viewpoint of adjusting the electrode density. The electrode density of the negative electrode is typically preferably 1~1.8 g / cm³. 3More preferably, it is 1.1~1.7 g / cm³. 3 More preferably, it is 1.2~1.6 g / cm³. 3 .

[0152] Higher electrode density tends to improve sealing and volumetric capacity density. However, excessively high density reduces porosity in the electrode, weakens the suppression of volume expansion of silicon and other materials, makes it difficult to control negative electrode expansion, and sometimes reduces capacity retention. Therefore, it is important to select the optimal range for electrode density.

[0153] The positive electrode, like the negative electrode, is obtained by forming a positive electrode material layer on the surface of the current collector. For example, a positive electrode material (positive electrode active material), a conductive material, and an organic binder (adhesive) are mixed with a solvent and kneaded using a dispersion device such as a mixer, ball mill, super mill, or pressure kneader to prepare a positive electrode material slurry. This positive electrode material slurry can then be coated onto the current collector to form the positive electrode layer. The current collector can then be made of metals or alloys such as aluminum, titanium, or stainless steel, and can be formed into foil, perforated foil, mesh, or other strip shapes.

[0154] There are no particular restrictions on the positive electrode material (positive electrode active material) used in the positive electrode material layer. In non-aqueous electrolyte secondary batteries, such as in the case of making lithium-ion secondary batteries, examples include metal compounds, metal oxides, metal sulfides, and conductive polymers that can be doped or intercalated with lithium ions.

[0155] Specifically, examples include lithium cobalt oxide (LiCoO2) and other lithium cobalt composite oxides (LCO), lithium nickel oxide (LiNiO2), lithium manganese oxide (LiMnO2) and their composite oxides (LiCoxNiyMnzO2, x+y+z=1; lithium nickel manganese cobalt composite oxide (NMC)); lithium manganese spinel (LiMn2O4), lithium vanadium compounds, V2O5, V6O 13 VO2, MnO2, TiO2, MoV2O8, TiS2, V2S5, VS2, MoS2, MoS3, Cr3O8, Cr2O5, olivine-type LiMPO4 (where M is Co, Ni, Mn, or Fe); conductive polymers such as polyacetylene, polyaniline, polypyrrole, polythiophene, and polybenzoxene; and porous carbon. They can be used individually or in combination of two or more.

[0156] From the perspectives of operating voltage, volumetric density, theoretical capacity, high-temperature stability, and economy, lithium iron phosphate compounds such as olivine-type LiFePO4 are preferred.

[0157] The average particle size of the positive electrode active material is not particularly limited. For example, when lithium cobalt oxide (LCO) or lithium nickel manganese cobalt oxide (NMC) is used as the positive electrode active material, its average particle size is generally preferably 1 μm or more and 100 μm or less, more preferably 5 μm or more and 50 μm or less. In addition, when lithium iron phosphate (LFP) is used as the positive electrode active material, its average particle size is generally preferably 0.01 μm or more and 5 μm or less, more preferably 0.1 μm or more and 1 μm or less.

[0158] If the average particle size of the positive electrode active material is within the above-mentioned range, then when manufacturing a secondary battery, the positive electrode expansion rate during charging and discharging is small, and it is easy to prevent the decrease in reversible charge-discharge capacity per unit volume. Furthermore, it is easier to suppress the peeling of the electrode film (positive electrode material layer) from the current collector during electrode film fabrication.

[0159] The average particle size of the positive electrode active material is the particle size (D50) that accumulates to 50% when the volume cumulative distribution curve is plotted from the small diameter side in the particle size distribution measured by dynamic light scattering method using a laser diffraction particle size analyzer or similar device.

[0160] The positive electrode active material can be coated with a coating material to cover at least a portion of its surface. As the coating material, materials that are expected to improve electronic conductivity, lithium-ion conductivity, and inhibit electrolyte decomposition are preferred; examples include electronically conductive materials such as carbon, titanium, and nickel. From the viewpoint of improving the chemical and thermal stability of the positive electrode active material and suppressing the tendency for the charge-discharge performance of the resulting secondary battery to decrease, carbon is preferred, and low-crystallinity carbon is more preferred.

[0161] When at least a portion of the surface of the positive electrode active material is coated with a coating material, the average thickness of the coating layer is preferably 10 nm or more and 300 nm or less, more preferably 20 nm or more and 200 nm or less. Furthermore, the content of the coating material is preferably 1 to 30% by mass relative to the total amount of the constituent components of the positive electrode active material and the coating material.

[0162] Examples of conductive materials used in the positive electrode layer include conductive polymers such as polyacetylene, polyaniline, polypyrrole, polythiophene, and polybenzoxene, as well as porous carbon. One type can be used alone, or two or more can be used in combination.

[0163] Organic binders used in the cathode material layer include, for example, styrene-butadiene rubber copolymers; olefinic unsaturated carboxylic acid esters such as methyl methacrylate, ethyl methacrylate, butyl methacrylate, methacrylonitrile, and hydroxyethyl methacrylate, as well as unsaturated carboxylic acid copolymers such as (meth)acrylic acid copolymers formed from olefinic unsaturated carboxylic acids such as acrylic acid, methacrylic acid, itaconic acid, fumaric acid, and maleic acid; and polymers such as polyvinylidene fluoride, polyethylene oxide, polyepoxychlorohydrin, polyphosphazene, polyacrylonitrile, polyimide, polyamide-imide, and carboxymethyl cellulose.

[0164] As a separator, nonwoven fabrics, cloths, microporous membranes, or combinations thereof, mainly composed of polyolefins such as polyethylene and polypropylene, can be used. It should be noted that a separator is not required in non-aqueous electrolyte secondary batteries where the positive and negative electrodes do not directly contact each other.

[0165] As an electrolyte, for example, an organic electrolyte can be used, which is prepared by dissolving lithium salts such as LiClO4, LiPF6, LiAsF6, LiBF4, and LiSO3CF3 in one or more of non-aqueous solvents such as ethylene carbonate, propylene carbonate, butyl carbonate, vinylene carbonate, fluoroethylene carbonate, cyclopentanone, sulfolane, 3-methylsulfolane, 2,4-dimethylsulfolane, 3-methyl-1,3-oxazolidin-2-one, γ-butyrolactone, dimethyl carbonate, diethyl carbonate, methyl ethyl carbonate, methyl propyl carbonate, butyl methyl carbonate, ethyl propyl carbonate, butyl ethyl carbonate, dipropyl carbonate, 1,2-dimethoxyethane, tetrahydrofuran, 2-methyltetrahydrofuran, 1,3-dioxolane, methyl acetate, and ethyl acetate.

[0166] The structure of the secondary battery using the negative electrode forming composition of the present invention is not particularly limited. Generally, it is a structure obtained by winding the positive electrode, the negative electrode and the separator provided as needed into a flat spiral shape to form a wound electrode assembly, or by making them into a flat plate shape and stacking them to form a stacked electrode assembly, and then sealing these electrode assemblies into an outer casing.

[0167] Secondary batteries using the negative electrode forming composition of the present invention can be used as, for example, paper-type batteries, button-type batteries, coin-type batteries, stacked batteries, cylindrical batteries, prismatic batteries, etc.

[0168] The negative electrode forming composition of the present invention is also applicable to all electrochemical devices that use lithium ion insertion and de-entry as a charging and discharging mechanism, such as hybrid capacitors, solid lithium secondary batteries, etc.

[0169] The negative electrode forming composition, negative electrode, and secondary battery having the negative electrode of the present invention have been described above, but the present invention is not limited to the configuration of the above embodiments. For example, the negative electrode forming composition, negative electrode, and secondary battery having the negative electrode of the present invention may be modified by adding other arbitrary configurations to the configuration of the above embodiments, or may be replaced with any configuration that performs the same function.

[0170] Example

[0171] The present invention will now be specifically described through examples. However, the present invention is not limited to the examples described below. The raw materials used in the examples and comparative examples are described below.

[0172] <Monomers constituting resin (A)>

[0173] Aromatic vinyl monomers (a1)

[0174] ST: Styrene

[0175] DVB: Divinylbenzene

[0176] (Meth)acrylates (a2)

[0177] MMA: Methyl methacrylate

[0178] BA: n-Butyl acrylate

[0179] 2EHA: 2-Ethylhexyl acrylate

[0180] Vinyl monomers with acid groups (a3)

[0181] MAA: Methacrylic acid

[0182] AA: Acrylic acid

[0183] IA: itaconic acid

[0184] Vinyl monomers containing functional groups (a4)

[0185] AM: Acrylamide

[0186] NMAM: N-hydroxymethylacrylamide

[0187] PMI: N-Phenylonmaleimide

[0188] MOI-A: The product obtained by reacting 155.15 parts by mass of ethyl 2-isocyanate methacrylate with 46.07 parts by mass of ethanol.

[0189] MOI-B: The product obtained by reacting 155.15 parts by mass of ethyl 2-isocyanate methacrylate with 73.14 parts by mass of diethylamine.

[0190] <Negative Electrode Active Material>

[0191] Composite particles (B1): Produced by Liyang Tianmu Pilot Battery Materials Technology Co., Ltd., silicon-carbon composite anode material.

[0192] Artificial graphite: Zichen, "NT-5H"

[0193] Natural graphite: "P-15B-ZG" manufactured by Nippon Carbon Co., Ltd.

[0194] <Conductive additives>

[0195] SWCNT: Single-layer carbon nanotubes, OCSiAl fabricated as "TUBALL BATT H2O"

[0196] AB: Acetylene Black, Denka "Li-400"

[0197] Carboxymethyl cellulose

[0198] CMC: "Sunrose (registered trademark) MAC 350 HC" (trade name, manufactured by Nippon Paper Corporation)

[0199] <Aqueous Solvents>

[0200] Water: Ion-exchanged water

[0201] NMP: N-methylpyrrolidone

[0202] Synthesis example 1

[0203] (1) Mix 50 parts by mass of water and 0.5 parts by mass of “ADEKA REASOAP SR-10” (trade name, ether sulfate type ammonium salt, manufactured by ADEKA, hereinafter referred to as “SR-10”) at 25°C, then add 50 parts by mass of ST and 1 part by mass of DVB as aromatic vinyl monomers (a1), 47 parts by mass of EHA as (meth)acrylate (a2), 1 part by mass of MAA as vinyl monomers with acid groups (a3), and 1 part by mass of AM as vinyl monomers with functional groups (a4), and mix at 25°C to prepare an emulsion (hereinafter referred to as “raw material emulsion”). (2) Separately prepare a solution by dissolving 0.2 parts by mass of ammonium persulfate in 10 parts by mass of water (hereinafter referred to as “initiator solution”). (3) Add 220 parts by mass of water and 0.5 parts by mass of SR-10 to a reaction vessel equipped with a stirrer, thermometer, and cooler and dissolve them, then heat to 80°C. The raw material emulsion obtained in (1) and the initiator solution obtained in (2) were simultaneously added dropwise to the solution over 3 hours. After the addition was completed, polymerization was carried out at 80°C for 2 hours. The reaction mixture was cooled to 25°C, the pH was adjusted to 7 with 25% ammonia, water was added, and the concentration of non-volatile components (solid components) was adjusted to 40.0% by mass, thereby obtaining resin (A1) as an emulsion aqueous solution.

[0204] The average particle size (D50) of the obtained resin (A1) was determined using a NANOTRAC WAVER II manufactured by Microtrac BEL, and the result was 220 nm.

[0205] In addition, the total functional group concentration of urethane, urea, amide and imide groups in resin (A1) was calculated to be 141 mmol / kg.

[0206] <Methods for Calculating Functional Group Concentration>

[0207] The functional group concentration of resin (A1) refers to the number of moles of functional groups contained in 1 kg of resin (A1). If the total number of structural units contained in resin (A) is set as i, then the functional group concentration can be expressed using the content W1~W of each of the i structural units. i Molecular weight Mw1~Mw i and the number of functional groups F1~F i It can be calculated from the following formula (α).

[0208] [Number 1]

[0209]

[0210] For example, in the case of Synthesis Example 1, if ST is set as structural unit 1, DVB as structural unit 2, EHA as structural unit 3, MAA as structural unit 4, and AM as structural unit 5, then the following calculation formula can be used to calculate it.

[0211] [Number 2]

[0212]

[0213] Synthesis Example 2~Synthesis Example 13

[0214] In Synthesis Example 1(1), the types and amounts of the aromatic vinyl monomer (a1), (meth)acrylate (a2), acid-group-containing vinyl monomer (a3), and functional group-containing vinyl monomer (a4) used in the preparation of the raw material emulsion were changed as shown in Table 1. Otherwise, the same operation as in Synthesis Example 1 was performed to obtain resins (A2)~(A11) and (CA1)~(CA2) as emulsion aqueous solutions. The D50 and functional group concentrations of the obtained resins (A2)~(A11) and (CA1)~(CA2) are shown in Table 1.

[0215] [Table 1]

[0216]

[0217] Example 1

[0218] (1) Preparation of the composition for negative electrode formation

[0219] In a planetary mixer (PRIMIX "2P-03"), 193.94 parts by mass of the composite particles (B1) as the negative electrode active material and 2.0 parts by mass of CMC were weighed and stirred for 10 minutes. Hereinafter, unless otherwise specified, stirring using a planetary mixer will be performed using the same apparatus.

[0220] Next, 105.51 parts by mass of ion-exchanged water were added and mixed at 80 rpm for 60 minutes. Then, 4.29 parts by mass of ion-exchanged water were added and stirred at 50 rpm for 15 minutes. The above operation was repeated 4 times to obtain a paste-like slurry with a solid component concentration of 61.5% by mass.

[0221] Next, 15.0 parts by weight of SWCNT were added to the slurry and stirred at 50 rpm for 15 minutes. Then, 10.0 parts by weight of an emulsified aqueous solution of resin (A1) was added and stirred at 50 rpm for 15 minutes to prepare a slurry-like composition 1 for forming a negative electrode.

[0222] The mass percentages of resin (A1), composite particles (B1), SWCNT, CMC, and water in the obtained negative electrode forming composition 1 are shown in Table 3.

[0223] (2) Fabrication of the negative electrode

[0224] The coating amount (areal density) of the dried negative electrode forming composition 1 is 8.8 mg / cm³. 2 The gap of the bar coater is adjusted in a certain way, and the negative electrode forming composition 1 is coated onto the copper foil, which serves as the current collector, using the bar coater. The foil is then dried for 8 minutes using a blower dryer set to 80°C.

[0225] The dried electrodes were cut into 40mm wide pieces and then rolled using a TESTER Industrial Co., Ltd. "Small Benchtop Roller Press SA-602" to achieve a layer density of 1.65g / cm³. 3 After being pressed in a certain way, it was vacuum dried at 110℃ for 10 hours to obtain negative electrode 1.

[0226] (3) Preparation of positive electrode composition

[0227] Weigh 94.0 parts by mass of olivine-type lithium iron phosphate (LiFePO4) as the positive electrode active material and 3.0 parts by mass of AB as the conductive material, and stir for 30 seconds using a rotary mixer.

[0228] Next, add 27.0 parts by weight of polyvinylidene fluoride (PVDF, manufactured by KUREHA, W#9700) (equivalent to 2.16 parts by weight on a solids basis) and 19.0 parts by weight of NMP, mix until a paste is formed, and then stir with a rotary mixer for 2 minutes. Since the mixture generates heat during stirring, cool it to room temperature with ice water, stir again with a rotary mixer for 2 minutes, and then cool to room temperature with ice water.

[0229] Next, 10.5 parts by mass of PVDF (equivalent to 0.84 parts by mass of solids) and 5 parts by mass of NMP were added to the mixture, and it was mixed until the mixture became homogeneous.

[0230] The viscosity of the obtained slurry was measured using a type B viscometer at 25°C and 30 rpm, and NMP was added in a manner that resulted in a viscosity range of 2000–4000 mPa·s. Finally, the mixture was stirred for 30 seconds using a rotary mixer to prepare a slurry-like positive electrode composition.

[0231] (4) Production of the positive electrode

[0232] The coating weight (area density) of the dried positive electrode composition was 25.0 mg / cm³. 2The gap of the rod coater was adjusted, and the obtained positive electrode composition was coated onto a carbon-coated aluminum foil serving as the current collector using the rod coater. The foil was then dried in a blower-type dryer set to 80°C for 10 minutes. The dried electrode was cut into 40mm wide pieces and pressed using a roller press (TESTER Industrial Co., Ltd.'s "Small Benchtop Roller Press SA-602") to achieve a layer density of 2.5 g / cm³. 3 After being pressed in a certain way, the cathode was obtained by vacuum drying at 110°C for 10 hours.

[0233] (5) Making a secondary battery

[0234] Using a Thomson scalpel, the negative electrode 1 prepared in (2) above was cut into a 24mm × 24mm square with tabs, and the positive electrode prepared in (4) above was cut into a 22mm × 22mm square with tabs. For the tabs of the cut electrodes, nickel tab leads were welded to the negative electrode 1 and aluminum tab leads were welded to the positive electrode. On the other hand, as a diaphragm, a 25μm thick polyethylene microporous membrane was cut into a 28mm × 3.8cm rectangle using a Thomson scalpel. The positive and negative electrodes 1 were placed face to face through the diaphragm, packaged with a laminated film, and the tabs were fixed by heat pressing. Then, LiPF6 was dissolved at a concentration of 1 mol / L in a mixed solution of ethylene carbonate / dimethyl carbonate / ethyl methyl carbonate = 30 / 30 / 40 (volume ratio), and 1 vol% ethylene carbonate and 5 vol% fluoroethylene carbonate were added to obtain a non-aqueous electrolyte solution. 300 μL of this non-aqueous electrolyte solution was added, and the battery was completely sealed by vacuum lamination to prepare a laminated secondary battery 1.

[0235] Examples 2-11, Comparative Examples 1-2

[0236] In Example 1(1), instead of the emulsified aqueous solution of resin (A1) obtained in Synthesis Example 1, emulsified aqueous solutions of resins (A2)~(A11) and (CA1)~(CA2) obtained in Synthesis Examples 2~13 were used. Otherwise, the same procedure as in Example 1 was followed to prepare slurry-like negative electrode forming compositions 2~11 and C1~C2. Then, the same procedure as in Example 1(2)~(5) was performed to obtain negative electrodes 2~11 and C1~C2 using the respective negative electrode forming compositions, as well as laminated secondary batteries 2~11 and C1~C2.

[0237] Examples 12-23

[0238] In Example 1(1), the mass percentages of resin (A1), composite particles (B1) as negative electrode active material, artificial or natural graphite, SWCNT or AB as conductive additives, CMC, and water in the obtained negative electrode forming composition were varied as shown in Table 3. Otherwise, the same procedure as in Example 1 was followed to prepare slurry-like negative electrode forming compositions 12-23. Next, the same procedures as in Example 1(2)-(5) were performed to obtain negative electrodes 12-23 and laminated secondary batteries 12-23 using each of the negative electrode forming compositions.

[0239] 2. Evaluation

[0240] 2-1. Dispersion stability

[0241] (1) Miscibility of SWCNT with emulsions of various resins

[0242] 33.8 g of water was added to 3.75 g of a 0.4% by mass SWCNT dispersion, and the mixture was stirred at 2000 rpm for 30 seconds using a rotary mixer (Thinky Corporation "ARE-310 (trade name)"). Next, 2.5 g of each resin obtained in Synthesis Examples 1-13 (40% by mass of solids) was added, and the mixture was again stirred at 2000 rpm for 30 seconds using a rotary mixer. The resulting mixture (a mixture of 1.85% by mass of resin (A), 0.03% by mass of SWCNT, 0.04% by mass of CMC, and 98.08% by mass of aqueous solvent) was filtered through a 200-mesh filter. The amount of residue remaining in the filter was measured, and the mass ratio of the residue to the amount of SWCNT present in the mixture was calculated. The miscibility was evaluated according to the following criteria: A higher mass ratio of residue indicates greater SWCNT aggregation.

[0243] <Evaluation Criteria>

[0244] ◎: The mass percentage of residue is less than 0.2%.

[0245] ○: The mass percentage of residue is 0.2% or more but less than 0.6%.

[0246] △: The mass percentage of residue is 0.6% or more but less than 1.0%.

[0247] ×: The mass ratio of residue is 1.0% or more.

[0248] (2) Viscosity of the composition for forming the negative electrode

[0249] The viscosity (mPa·s, initial viscosity) of the negative electrode forming compositions prepared in each example and comparative example was measured using a type B viscometer at 25°C and 30 rpm.

[0250] In addition, in a planetary mixer, 194.0 parts by mass of the composite particles (B1) as the negative electrode active material and 2.0 parts by mass of CMC were weighed and stirred for 10 minutes. Then, 100.97 parts by mass of ion-exchanged water were added and mixed at 80 rpm for 60 minutes, followed by 4.29 parts by mass of ion-exchanged water and stirred at 50 rpm for 15 minutes. This operation was repeated 4 times to obtain a paste-like slurry with a solid component concentration of 61.5% by mass. Next, 10.0 parts by mass of an emulsified aqueous solution of resin (A1) with a non-volatile component concentration of 40.0% by mass obtained in Synthesis Example 1 was added, and the viscosity of the mixture prepared by stirring at 50 rpm for 15 minutes (a mixture in which resin (A) is 1.2% by mass, negative electrode active material (B) is 56.4% by mass, carboxymethyl cellulose is 0.6% by mass, and aqueous solvent is 41.8% by mass) was measured, and the result was 550 mPa·s.

[0251] 2-2. Peel strength of the negative electrode

[0252] Test pieces measuring 25 mm wide and 100 mm long were cut from the negative electrodes prepared in the various embodiments and comparative examples. The negative electrode active material side of the test piece was used as the adhesive side and was attached to a stainless steel plate using double-sided adhesive tape (Nitto Denko Corporation "No5015"). On the other hand, about 10 mm of copper foil was peeled off from the end, and polyimide tape was attached thereon. This served as the mounting part for a peel test device (Shimadzu Corporation "Autograph AG-XPlus"), and a 180° peel test was performed using a peel tester to determine the peel strength.

[0253] 2-3. Battery characteristics (initial charge / discharge efficiency and capacity retention)

[0254] The secondary batteries prepared in each embodiment and comparative example were installed in a charge-discharge device, placed at 25°C for 3 hours, and then charged and discharged once at 0.1C to determine the initial charge-discharge efficiency.

[0255] Next, the charge-discharge cycle at 60°C and 0.2C was repeated 50 times, and the discharge capacity retention rate after 50 cycles at 60°C (after 50 cycles) was determined by the following formula relative to the first discharge capacity at 0.2C (initial discharge capacity).

[0256] Capacity retention rate (%) = 100 × Discharge capacity at the 50th discharge (mAh / g) / Initial discharge capacity (mAh / g)

[0257] The results are shown in Tables 2 and 3.

[0258] [Table 2]

[0259]

[0260] [Table 3]

[0261]

[0262] As shown in Tables 2 and 3, the composite particles and SWCNTs in the negative electrode forming composition of the present invention exhibit excellent dispersion. Furthermore, the negative electrode formed from the negative electrode forming composition of the present invention exhibits excellent adhesion to the electrode, and the secondary battery equipped with this negative electrode achieves an initial charge-discharge efficiency of over 90%, a capacity retention rate of over 90%, and excellent balance of battery characteristics.

[0263] Industrial availability

[0264] The negative electrode forming composition of the present invention can form a secondary battery negative electrode and a secondary battery with excellent battery characteristics such as durability against electrolyte, excellent adhesion to current collector, excellent dispersion of specific composite particles containing carbon and silicon and monolayer carbon nanotubes, and excellent charge / discharge efficiency and capacity retention. The secondary battery having this negative electrode exhibits excellent battery characteristics such as charge / discharge performance, and can be effectively used in portable electronic devices, for example, as a paper battery, button battery, coin battery, stacked battery, cylindrical battery, or prismatic battery.

Claims

1. A composition for forming a negative electrode, comprising: Resin (A) having one or more functional groups selected from urethane, urea, amide and imide groups; The negative electrode active material (B) contains composite particles containing carbon and silicon; Single-layer carbon nanotubes; Carboxymethyl cellulose or its salts; as well as Aqueous solvents.

2. The composition for forming a negative electrode according to claim 1, wherein, The resin (A) is in the form of particles with an average particle size of 50~500nm.

3. The composition for forming a negative electrode according to claim 1, wherein, The total functional group concentration of the resin (A) consisting of urethane, urea, amide, and imide groups is 10-2000 mmol / kg.

4. The composition for forming a negative electrode according to claim 1, wherein, Relative to the total amount of units constituting the resin (A), the content of structural units based on aromatic vinyl monomers (a1) is 15% by mass or more and 80% by mass or less, the content of structural units based on (meth)acrylates (a2) is 15% by mass or more and 80% by mass or less, the content of structural units based on vinyl monomers having acid groups (a3) ​​is 0.1% by mass or more and 10% by mass or less, and the content of structural units based on vinyl monomers (a4) having one or more functional groups selected from urethane groups, urea groups, amide groups, and imide groups is 0.1% by mass or more and 10% by mass or less.

5. The composition for forming a negative electrode according to claim 1, wherein, The composite particles contained in the negative electrode active material (B) are composite carbon particles having porous carbon material and silicon components, and at least a portion of the porous carbon material contains silicon components.

6. The composition for forming a negative electrode according to claim 1, wherein, Relative to the total mass of the negative electrode forming composition, the content of the resin (A) is 0.1% by mass or more and 5% by mass or less, the content of the negative electrode active material (B) is 30% by mass or more and 60% by mass or less, the content of the monolayer carbon nanotube is 0.005% by mass or more and 0.3% by mass or less, the content of the carboxymethyl cellulose is 0.01% by mass or more and 3% by mass or less, and the content of the aqueous solvent is 35% by mass or more and 65% by mass or less.

7. The composition for forming a negative electrode according to claim 1, wherein the viscosity is 200 mPa·s or more and 20000 mPa·s or less.

8. The composition for forming a negative electrode according to claim 1, wherein, When a mixture obtained by mixing the resin (A) in the manner of 1.85% by mass, the monolayer carbon nanotubes in the manner of 0.03% by mass, the carboxymethyl cellulose in the manner of 0.04% by mass, and the aqueous solvent in the manner of 98.08% by mass is filtered using a 200-mesh filter, the amount of monolayer carbon nanotubes remaining on the filter is less than 1% of the monolayer carbon nanotubes contained in the mixture.

9. The composition for forming a negative electrode according to claim 1, wherein, The viscosity of the mixture obtained by mixing the resin (A) at 1.2% by mass, the negative electrode active material (B) at 56.4% by mass, the carboxymethyl cellulose at 0.6% by mass, and the aqueous solvent at 41.8% by mass is 200 mPa·s or more and 20000 mPa·s or less.

10. A secondary battery negative electrode comprising a negative electrode material layer formed using the negative electrode forming composition according to any one of claims 1 to 9.

11. A secondary battery comprising the negative electrode, positive electrode, electrolyte, and separator as described in claim 10.

Citation Information

Patent Citations

  • Binder resin composition, electrode for energy device, and energy device

    JP2012051999A

  • Acrylonitrile copolymer adhesive and use of same in lithium ion battery

    WO2018032665A1

  • Electroactive materials for metal-ion batteries

    WO2020234586A1