A borate-doped LMFP-BO cathode material and its preparation method
By using LMFP-BO cathode material doped with borate, the problems of structural instability and low conductivity of LMFP material during charge and discharge processes have been solved, achieving electrochemical performance with high capacity, long life and low polarization, which is suitable for power batteries.
Patent Information
- Application Number
- CN202611382066.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-08
- Publication Date
- 2026-11-17
AI Technical Summary
Lithium manganese iron phosphate (LMFP) materials suffer from structural instability and low electronic conductivity due to problems such as Jahn-Teller distortion and slow lithium-ion diffusion during charge and discharge, making it difficult to meet the requirements of high power output. At the same time, uneven mixing of carbon sources leads to interface instability, affecting its application in power batteries.
By using LMFP-BO cathode material doped with borate, precise control of raw material ratio and precursor pretreatment is employed to achieve in-situ substitution of borate in the crystal lattice and synergistic effect of transition metal vacancies. Combined with molecular-level dispersion and microwave gelation, a continuous carbon network is formed, ensuring the material's structural stability and conductivity.
It significantly improves the structural stability and conductivity of the material, increases the discharge capacity and cycle life at high rates, reduces interfacial impedance, and achieves highly efficient electrochemical performance.
Abstract
Description
Technical Field
[0001] This invention belongs to the field of battery cathode material technology, and relates to an LMFP-BO cathode material doped with borate and its preparation method. Background Technology
[0002] Lithium manganese iron phosphate (LMFP), as an upgraded alternative to lithium iron phosphate (LFP), has attracted much attention in recent years. By introducing manganese into LFP, LMFP increases the charge-discharge platform from 3.4V to 4.1V, and theoretically improves the energy density by about 20% compared to LFP, while retaining the inherent thermal stability and long cycle life of the olivine structure. However, LMFP has revealed many insurmountable bottlenecks in its industrial application, such as:
[0003] First, during the charging and discharging process, Mn 3+ Jahn-Teller distortion caused by electronic configuration induces asymmetric stretching of the octahedral lattice. This distortion gradually accumulates during repeated lithium insertion / extraction, leading to microcracks and lattice dislocations within the particles, ultimately causing particle pulverization and increased internal resistance. Simultaneously, the tetrahedral framework of PO4 lacks rigidity, resulting in non-uniform expansion and contraction of the unit cell during lithium insertion / extraction. The accumulated stress during long-term cycling reduces capacity retention.
[0004] Secondly, LMFP has a one-dimensional lithium-ion migration channel, and its lithium-ion diffusion coefficient is much lower than that of layered oxide cathode materials. At the same time, the transition metal octahedrons in the olivine structure are separated by PO4 tetrahedra, which cannot form a continuous electronic conduction network and have low electronic conductivity. This "double low" defect makes the material's capacity underperform at conventional rates and its polarization is severe at high power output, making it difficult to meet the high-rate performance requirements of power batteries.
[0005] Third, during the high-temperature sintering stage, the protons generated by the dissociation of water molecules adsorbed in the precursor or raw material react with the Li groups on the lithium sites. + An exchange occurs, forming an electrochemically inert rock salt phase layer on the particle surface. This blocks the migration pathway of lithium ions from the electrolyte to the crystal lattice, leading to a decrease in specific capacity and an increase in interfacial impedance. Furthermore, improper control of the raw material ratio can easily lead to the precipitation of inactive impurities such as pyrophosphate and lithium phosphate, further diluting the content of active materials.
[0006] Fourth, existing technologies mostly adopt a simple physical mixing of carbon source and raw material followed by carbonization. It is difficult to achieve uniform distribution of carbon source at the molecular level in precursor. The carbon coating layer formed after carbonization is often uneven in thickness and is prone to falling off from the substrate surface during cycling. Summary of the Invention
[0007] To address the above problems, this invention provides a borate-doped LMFP-BO cathode material and its preparation method, wherein the proportions of the raw materials for the LMFP-BO cathode material are as follows:
[0008] The lithium source, calculated as elemental lithium, is added in an amount of 0.98-1.06 mol. When the amount added is less than 1.00 mol, it can suppress the Li content during sintering. + / H + The surface rock salt phase generated by the exchange is enriched in the form of Li3PO4 at the grain boundaries in the high-temperature stage when the amount added is higher than 1.03 mol, which plays an in-situ surface modification role and can further improve the interface stability. However, when it exceeds 1.06 mol, it is easy to induce the formation of impurity phases, so the upper limit is set to 1.06 mol.
[0009] The iron source, calculated as elemental iron, is added in an amount of 0.46-0.52 mol. When the iron content is below 0.46 mol, the excessively high Mn content will exacerbate the Jahn-Teller distortion effect; when the iron content is above 0.52 mol, the Fe... 3+ Increased impurities reduce the average operating voltage of the material.
[0010] The amount of manganese source added is 0.44-0.5 mol based on manganese element. The total amount of iron and manganese elements is 0.96-0.99 mol. The reserved 0.01-0.04 mol transition metal vacancies help reduce the lattice expansion stress during the lithium-ion insertion / extraction process. When the total amount of substances is less than 0.96 mol, too many cation vacancies will destroy the connection rigidity of MO6 octahedra. When it is greater than 0.99 mol, it is difficult to accommodate the local structural distortion caused by subsequent borate substitution.
[0011] The boron source, calculated as elemental boron, was added in the range of 0.018-0.032 mol. When the boron addition was below 0.018 mol, the lattice prestressing strengthening effect was not significant; when it was above 0.032 mol, the excess BO3... 3- Planar elements will excessively compress adjacent MO6 octahedra, causing Li + The passageway partially collapsed.
[0012] The phosphorus source, calculated as elemental phosphorus, is added in an amount of 0.95-0.99 mol. The combined amount of phosphorus and boron sources must satisfy the requirement that the total occupancy of anion sites (P+B) is 0.98-1.01 mol. That is, the precise amount of phosphorus source added is determined by reverse calculation based on the actual weighed value of the boron source (e.g., when boron is 0.025 mol, phosphorus is 0.955-0.985 mol). When P+B is below 0.98 mol, excessive anion vacancies will reduce the chemical stability of the olivine framework; when it is above 1.01 mol, excess phosphate ions cannot enter the crystal lattice and will form pyrophosphate impurities at the grain boundaries.
[0013] The amount of complexing agent added is 1.1-1.6 times the sum of the total amount of metal ions (i.e., 1.1-1.6 times the sum of the amounts of lithium, iron, and manganese ions). When the amount of lithium source added is >1.03 mol, the amount of complexing agent should be 1.5-1.6 times to fully complex excess lithium ions and prevent them from precipitating in the form of acetate crystals during the gelation stage. When the amount of lithium source added is <1.00 mol, the ratio of complexing agent should be 1.1-1.3 times to avoid excessive organic residue leading to excessive carbon content and dilution of active materials.
[0014] The amount of carbon source added, calculated as carbon element, is 0.85-1.6 mol.
[0015] Preferably, the lithium source is one or more of lithium acetate, lithium carbonate, lithium hydroxide, and lithium nitrate, with 1 mol of lithium acetate being the most preferred.
[0016] Preferably, the iron source is one or more of ferrous sulfate, ferrous oxalate, ferrous nitrate and ferrous chloride, and most preferably 0.5 mol of ferrous sulfate.
[0017] Preferably, the manganese source is one or more of manganese acetate, manganese sulfate, manganese nitrate and manganese chloride, and most preferably 0.47 mol of manganese acetate.
[0018] Preferably, the boron source is one or more of boric acid, trimethyl borate, triethyl borate, and lithium metaborate, and most preferably 0.025 mol of boric acid.
[0019] Preferably, the phosphorus source is one or more of phosphoric acid, ammonium dihydrogen phosphate, and diammonium hydrogen phosphate, with the most preferred being 0.0965 mol of phosphoric acid.
[0020] Preferably, the complexing agent is one or more of citric acid, tartaric acid, EDTA and gluconic acid, and most preferably 2.56 mol of citric acid.
[0021] Preferably, the carbon source is one or more of sucrose, glucose, soluble starch and polyvinyl alcohol, with 1.2 mol of sucrose being the most preferred.
[0022] The specific preparation method of the LMFP-BO cathode material is as follows:
[0023] Step 1: Mix manganese, D-gluconic acid, and water at a ratio of 1 mol:(0.5-0.8) mol:(1.5-2.5) L, and evaporate the mixture in a water bath at 60-90℃ and 100-200 rpm until the volume is reduced to 1 / 4-1 / 3 of the original volume. Allow the mixture to stand for 2-4 hours to cool and crystallize. Filter the mixture, remove the filtrate, and dry the precipitate at 35-45℃ for 3-5 hours to obtain the pretreated manganese source. This pretreatment step can improve the manganese content of Mn. 2+By complexing with organic ligands at the molecular level, it effectively inhibits Mn during the subsequent sol-gel process. 2+ Hydrolysis and segregation lay the foundation for achieving atomically uniform doping.
[0024] Preferably, when manganese acetate is used, the water bath temperature is 60-80℃, and when manganese sulfate, manganese nitrate or manganese chloride is used, the water bath temperature is 70-90℃.
[0025] Step two: Boron, mannitol, and anhydrous ethanol are mixed at a ratio of 1 mol:(1.5-2.0) mol:(0.8-1.2) L, refluxed at 50-100℃ for 2-5 h, and the ethanol is removed by vacuum distillation to obtain a pretreated boron source. This pretreatment alters the molecular configuration of the boron source, making it easier to disperse uniformly in the sol system and release BO3 in situ during subsequent heat treatment. 3- This enables precise replacement of lattice sites.
[0026] Preferably, when boric acid or lithium metaborate is used, reflux at 50-70°C for 2-4 hours; when borate esters are used, no ethanol needs to be added, and reflux at 80-100°C for 3-5 hours.
[0027] Step 3: Dissolve the pretreated manganese source in deionized water to prepare a solution with a manganese concentration of 0.3-0.5 mol / L. Then add 30-40% of the total amount of complexing agent and stir at 45-55℃ and 100-200 rpm for 1-2 hours to form a stable manganese-citric acid-gluconic acid ternary complex system, denoted as solution A.
[0028] Step 4: Mix the pretreated boron source, phosphorus source and anhydrous ethanol. The amount of anhydrous ethanol used is 1.2-2 L / mol boron. Stir at 40-50℃ and 100-200 rpm for 1-2 hours. Then add the lithium source and the remaining complexing agent, and continue stirring until completely dissolved. Adjust the pH to 3.5-4.5 and label it as solution B.
[0029] Preferably, when using ammonium phosphate, deionized water is used as the solvent.
[0030] Step 5: Dissolve the iron source in deionized water to prepare a solution with a ferrous ion concentration of 0.4-0.6 mol / L. Add an antioxidant at a concentration of 0.5-1.0% of the iron source. Stir at 60-90 rpm for 20-40 minutes under inert gas protection to obtain stable Fe. 2+ The solution is denoted as solution C.
[0031] Preferably, the antioxidant is ascorbic acid.
[0032] Step 6: Under inert gas protection, add solution C dropwise to solution A while stirring continuously at a rate of 2-3% of total volume / min. After the addition is complete, continue stirring at 60-90 rpm for 40-50 min. Then, add solution B dropwise to the above solution at a rate of 1.5-2.5% of total volume / min, maintaining the pH value at 4-4.5 during the addition process. After all the addition is complete, add a carbon source and microwave irradiate at 400-600W and 60-70℃ for 15-25 min to promote the rapid formation of a gel with a three-dimensional interpenetrating network structure in the sol system. Microwave treatment shortens the gelation time and improves the uniformity and cross-linking density of the gel network structure.
[0033] Step 7: Dry the above gel at 110-120℃ for 10-14 hours, then heat it to 300-350℃ at a heating rate of 1.5-2.5℃ / min under inert gas protection, and hold it at this temperature for 2-3 hours. This pre-carbonization step partially carbonizes citric acid and sucrose to form a conductive carbon framework, while mannitol borate decomposes and releases BO3 in situ. 3- By pre-anchoring it to the phosphate framework through BOP bonding, boron volatilization loss during high-temperature sintering is avoided.
[0034] Step 8: Grind the pre-carbonized product at 100-200 rpm for 15-20 min, then heat it to 700-750℃ at a rate of 1-2℃ / min under a nitrogen-hydrogen mixed atmosphere, hold it at that temperature for 6-10 h, and then allow it to cool naturally to room temperature. During the sintering process, the pre-embedded BO3... 3- Groups and PO4 3- In-situ substitution reactions occur at the sites, triggering precise shrinkage of the lattice parameters, while the carbothermic reducing atmosphere effectively suppresses Mn. 3+ The formation of borate-doped LMFP-BO cathode material yields the product.
[0035] Preferably, the volume ratio of nitrogen to hydrogen in the nitrogen-hydrogen mixed atmosphere is 95:5.
[0036] The present invention has the following advantages:
[0037] (1) This invention utilizes BO3 3- The synergistic effect of lattice site substitution and transition metal vacancies significantly enhances structural stability, alters the local coordination field symmetry of transition metal sites, and fundamentally weakens the Mn content. 3+ The Jahn-Teller distortion driving force, and BO3 3- With PO4 3- The geometrical differences effectively offset the tensile stress concentration during the charging and discharging process, and the reserved transition metal vacancies further provide stress buffering, so that the material always maintains an intact lattice framework during repeated cycles, solving the problems of particle pulverization and internal resistance increase.
[0038] (2) This invention significantly improves ionic and electronic conductivity through the synergistic effect of boron lattice substitution and precursor molecular-level dispersion. Manganese and D-gluconic acid undergo pre-molecular-level complexation crystallization, and boron reacts with mannitol to generate ester derivatives. This achieves atomic-level uniform dispersion of transition metals and boron sources in the sol, ensuring the uniform dispersion of BO3. 3- The electrons truly enter the lattice sites rather than merely enriching at grain boundaries. The three-dimensional interpenetrating network gel structure, rapidly formed by wave irradiation, transforms into a continuous, interconnected conductive carbon framework after carbonization, enabling rapid electron transport within the electrode and effectively suppressing electrochemical polarization.
[0039] (3) This invention improves the purity of the particle interface by adjusting the ratio of lithium source to complexing agent and the ratio of phosphorus source to boron source. When the lithium source ratio is too high, the complexing agent ratio is increased to prevent lithium salt precipitation; when the lithium source ratio is too low, the complexing agent ratio is decreased to avoid excessive organic residue, thus preventing Li... + / H + The exchange reaction reduces the formation of an inert rock salt phase layer on the particle surface. Simultaneously, the precise binding ratio of the phosphorus / boron source is calculated in reverse based on the measured boron source value, ensuring that no excess phosphate ions remain at the grain boundaries to form pyrophosphate impurities. This maintains a clean olivine phase interface on the particle surface, significantly reducing interfacial charge transfer resistance.
[0040] (4) This invention enables the carbon source to solidify simultaneously with the inorganic framework during the gelation stage, achieving molecular-level anchoring of the carbon coating layer. The carbon source is not simply mixed physically later, but is simultaneously dispersed and solidified with metal ions and boron sources throughout the entire gel network. Microwave irradiation further accelerates the gelation process and avoids component sedimentation and phase separation. The carbonized coating layer has no local exposed areas, and the carbon layer is not easily peeled off during long-term cycling, always providing stable electrical contact and conductive support between particles. Detailed Implementation
[0041] The technical solutions in the embodiments of the invention are described clearly and completely below. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.
[0042] Example 1
[0043] The proportions of each raw material are as follows:
[0044] Lithium source: 1 mol lithium acetate.
[0045] Iron source: 0.5 mol ferrous sulfate.
[0046] Manganese source: 0.47 mol manganese acetate.
[0047] Boron source: 0.025 mol boric acid.
[0048] The phosphorus source was 0.0965 mol of phosphoric acid, in the form of an 85% phosphoric acid solution.
[0049] Complexing agent: 2.561 mol citric acid, 1.3 times the sum of the amounts of lithium, iron, and manganese ions.
[0050] Carbon source: 1.2 mol sucrose.
[0051] The specific preparation steps are as follows:
[0052] Step 1: Mix manganese acetate, D-gluconic acid and water at a ratio of 1 mol: 0.65 mol: 2 L, stir in a water bath at 75 °C and 150 rpm to evaporate to 1 / 3 of the original volume, let stand for 3 h to cool and crystallize, filter, remove the filtrate, and dry the precipitate at 40 °C for 4 h to obtain pretreated manganese acetate.
[0053] Step 2: Boric acid, mannitol and anhydrous ethanol are mixed at a ratio of 1 mol: 1.75 mol: 1 L, refluxed at 75 °C for 3.5 h, and the ethanol is removed by vacuum distillation to obtain pretreated boric acid.
[0054] Step 3: Dissolve pretreated manganese acetate in deionized water to prepare a solution with a manganese concentration of 0.4 mol / L. Add 35% of the total amount of citric acid and stir at 50℃ and 150 rpm for 1.5 h. This solution is labeled as Solution A. Mix pretreated boric acid, phosphoric acid solution, and anhydrous ethanol. The amount of anhydrous ethanol used is 1.6 L / mol boron. Stir at 45℃ and 150 rpm for 1.5 h. Add lithium acetate and the remaining citric acid and continue stirring until completely dissolved. Adjust the pH to 4 ± 0.5. This solution is labeled as Solution B. Dissolve ferrous sulfate in deionized water to prepare a solution with a ferrous ion concentration of 0.5 mol / L. Add 0.75% of the total amount of ascorbic acid and stir at 75 rpm for 30 min under nitrogen protection. This solution is labeled as Solution C.
[0055] Step 4: Under nitrogen protection, solution C is added dropwise to solution A under continuous stirring at a rate of 2.5% total volume / min. After the addition is complete, stirring is continued at 75 rpm for 45 min. Then, solution B is added dropwise to the above solution at a rate of 2% total volume / min. During the addition, the pH value is maintained at 4-4.5. After all the addition is complete, sucrose is added. The mixture is then microwaved at 500W and 65℃ for 20 min, dried at 115℃ for 12 h, heated to 320℃ at a heating rate of 2℃ / min under nitrogen protection, held at this temperature for 2.5 h, ground at 150 rpm for 18 min, and heated to 720℃ at a heating rate of 1.5℃ / min under a nitrogen-hydrogen mixed atmosphere (nitrogen and hydrogen volume ratio of 95:5), held at this temperature for 8 h to obtain the positive electrode material.
[0056] Comparative Example 1
[0057] The difference from Example 1 is that no boron source is added, but the remaining raw material ratios and preparation steps are exactly the same as in Example 1.
[0058] Comparative Example 2
[0059] The difference from Example 1 is that boric acid was not pretreated and was directly mixed with other raw materials to form a sol-gel, while the other conditions were the same as in Example 1.
[0060] Experimental Example 1
[0061] Electrode preparation: The LMFP-BO positive electrode material obtained in Example 1, conductive carbon black (Super P), and polyvinylidene fluoride (PVDF) were mixed at a mass ratio of 8:1:1. An appropriate amount of N-methylpyrrolidone (NMP) was added and ground into a uniform slurry. The slurry was then coated onto aluminum foil using a scraper, with the areal density controlled to be approximately 2.5 mg·cm³. -2 Dry at 120℃ for 12 hours, roll press and cut into circular electrode sheets with a diameter of 14mm.
[0062] Battery Assembly: In an argon-filled glove box (water and oxygen content both <0.1ppm), lithium metal sheets were used as the counter electrode, Celgard 2400 as the separator, and 1M LiPF6 dissolved in EC / EMC / DMC (volume ratio 1:1:1) was used to assemble CR2032 coin cells. After assembly, the cells were allowed to stand for 12 hours to allow the electrolyte to fully impregnate them.
[0063] Constant current charge-discharge test: The test was conducted using a NEWARE battery testing system within a voltage range of 2.5-4.3V. The discharge specific capacity was tested at 0.1C, 0.5C, 1C, 2C, and 5C rates, and the capacity retention rate after 200 cycles at 1C rate was also tested.
[0064] Cyclic voltammetry (CV) testing: An electrochemical workstation (CHI760E) was used at a scan rate of 0.1 mV·s. -1 With a voltage range of 2.5-4.3V, it is used to analyze the redox peak position and polarization degree.
[0065] Electrochemical impedance spectroscopy (EIS): After activation at 0.1C for 3 cycles, AC impedance was measured at 50% state of charge (SOC) with a frequency range of 100-10 mHz and an amplitude of 5 mV. The equivalent circuit was fitted using Zview software to obtain the charge transfer impedance (Rct) and lithium-ion diffusion coefficient (DLi). + ).
[0066] Table 1. First discharge specific capacity at different discharge rates (mAh·g) -1 )
[0067] Example 1 Comparative Example 1 Comparative Example 2 0.1C 158.6 143.2 148.9 0.5C 151.3 130.5 138.7 1C 144.8 118.4 128.1 2C 135.2 100.6 113.5 5C 118.7 78.3 95.2
[0068] Table 2. Capacity retention and average coulombic efficiency after 200 cycles at 1C rate.
[0069] Example 1 Comparative Example 1 Comparative Example 2 <![CDATA[Initial capacity (mAh·g -1 )]]> 144.8 118.4 128.1 <![CDATA[Capacity after 200 cycles (mAh·g -1 )]]> 138.2 96.7 110.3 Capacity retention rate (%) 95.4 81.7 86.1 Average Coulomb efficiency (%) 99.86 99.52 99.68
[0070] Table 3 Electrochemical impedance fitting parameters (50% SOC)
[0071] Rs(Ω) Rct(Ω) <![CDATA[DLi + (×10 -14 cm 2 ·S -1 )]]> Example 1 2.8 42.5 6.37 Comparative Example 1 3.5 78.3 2.15 Comparative Example 2 3.1 61.7 3.86
[0072] Table 4. Cyclic voltammetry (CV) redox peak potential difference (ΔE) p )
[0073] Oxidation peak potential (V) Reduction peak potential (V) <![CDATA[ΔE p (mV)]]> Example 1 3.98 3.42 560 Comparative Example 1 4.05 3.28 770 Comparative Example 2 4.01 3.35 660
[0074] As shown in Tables 1-4, the materials of this invention exhibit extremely high specific capacity at all rates, especially at high rates (5C), where the cathode material prepared in Example 1 still maintains 118.7 mAh·g. -1 The discharge capacity of Comparative Example 1 and Comparative Example 2 was only 78.3 and 95.2 mAh·g, respectively. -1 This fully demonstrates that the lattice substitution of borate and the synergistic effect of the molecularly dispersed carbon network have solved the "double low" bottleneck of low electronic conductivity and slow ion diffusion in LMFP materials.
[0075] After 200 cycles at 1C, the cathode material prepared in Example 1 exhibited a capacity retention of 95.4% and an average coulombic efficiency of 99.86%, significantly higher than Comparative Examples 1 and 2. This result validates the BO3... 3- Replace PO4 3- The site-induced lattice prestress shrinkage and reserved transition metal vacancies effectively suppressed Mn 3+ The Jahn-Teller distortion and lattice fatigue ensured the integrity of the particle structure and the stability of the interface during long-term cycling.
[0076] The charge transfer impedance of the cathode material prepared in Example 1 was only 42.5 Ω, and the lithium-ion diffusion coefficient was as high as 6.37 × 10⁻⁶. -14 cm 2 ·S -1 Compared to the comparative example, its interfacial impedance is significantly reduced, and the diffusion rate is increased several times. This is due to the molecular-level pre-complexation treatment of the precursor, which allows boron to precisely enter the lattice, broadening the ion migration channels, while the in-situ anchored carbon layer provides a continuous high-speed electron pathway.
[0077] The redox peak potential difference of the cathode material prepared in Example 1 was only 560 mV, significantly smaller than that in Comparative Examples 1 and 2. The smaller ΔEp indicates that electrode polarization is suppressed, the reaction has excellent reversibility, and the voltage plateau can be kept stable and energy loss is low even at high power output.
[0078] In summary, this invention utilizes BO3 3- By employing a multi-pronged strategy of precise lattice substitution, transition metal vacancy synergy, precursor atomic dispersion, and in-situ carbon network anchoring, LMFP-BO cathode materials with high specific capacity, ultra-long cycle life, excellent fast charging capability, and low polarization characteristics have been successfully prepared, possessing extremely high application value and industrialization prospects for power batteries.
[0079] The above description of the disclosed embodiments enables those skilled in the art to make or use the invention. Various modifications to these embodiments will be readily apparent to those skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the invention. Therefore, the invention is not to be limited to the embodiments shown herein, but is to be accorded the widest scope consistent with the principles and novel features disclosed herein.
Claims
1. A borate-doped LMFP-BO cathode material, characterized in that, The proportions of each raw material in the cathode material are as follows: The amount of lithium source added, calculated as elemental lithium, is 0.98-1.06 mol. The amount of iron source added, calculated as elemental iron, is 0.46-0.52 mol. The amount of manganese source added, calculated as manganese element, is 0.44-0.5 mol, and the total amount of iron and manganese elements is 0.96-0.99 mol. The amount of boron source added, calculated as elemental boron, is 0.018-0.032 mol. The amount of phosphorus source added, calculated as elemental phosphorus, is 0.95-0.99 mol. The total amount of phosphorus source and boron source added must meet the requirement that the total number of anion sites occupied is 0.98-1.01 mol. The amount of complexing agent added is 1.1-1.6 times the sum of the total amount of metal ions. When the amount of lithium source added is >1.03 mol, the amount of complexing agent is 1.5-1.6 times. When the amount of lithium source added is <1.00 mol, the amount of complexing agent is 1.1-1.3 times. The amount of carbon source added, calculated as carbon element, is 0.85-1.6 mol.
2. The borate-doped LMFP-BO cathode material of claim 1, wherein, The lithium source is one or more of lithium acetate, lithium carbonate, lithium hydroxide, and lithium nitrate.
3. The borate-doped LMFP-BO cathode material of claim 1, wherein, The iron source is one or more of ferrous sulfate, ferrous oxalate, ferrous nitrate, and ferrous chloride.
4. The borate-doped LMFP-BO cathode material of claim 1, wherein, The manganese source is one or more of manganese acetate, manganese sulfate, manganese nitrate, and manganese chloride.
5. The borate-doped LMFP-BO cathode material of claim 1, wherein, The boron source is one or more of boric acid, trimethyl borate, triethyl borate, and lithium metaborate.
6. The LMFP-BO cathode material doped with borate according to claim 1, characterized in that, The phosphorus source is one or more of phosphoric acid, ammonium dihydrogen phosphate, and diammonium hydrogen phosphate.
7. The LMFP-BO cathode material doped with borate according to claim 1, characterized in that, The complexing agent is one or more of citric acid, tartaric acid, EDTA, and gluconic acid.
8. A method of producing the LMFP-BO cathode material according to any one of claims 1 to 7, characterized in that, Includes the following steps: Step 1: Mix manganese, D-gluconic acid and water at a ratio of 1 mol:(0.5-0.8) mol:(1.5-2.5) L, stir in a water bath and evaporate to 1 / 4-1 / 3 of the original volume, let stand to crystallize, filter, and dry the precipitate to obtain the pretreated manganese source. Step 2: Mix boron, mannitol and anhydrous ethanol at a ratio of 1 mol:(1.5-2.0) mol:(0.8-1.2) L, reflux, and distill to remove the ethanol to obtain the pretreated boron source; Step 3: Dissolve the pretreated manganese source in deionized water to prepare a solution with a manganese concentration of 0.3-0.5 mol / L, and then add 30-40% of the total amount of complexing agent to obtain solution A; Pretreated boron source, phosphorus source and anhydrous ethanol are mixed, with the amount of anhydrous ethanol being 1.2-2 L / mol boron. Then lithium source and the remaining complexing agent are added, and the pH is adjusted to 3.5-4.5 to obtain solution B. Iron source is dissolved in deionized water to prepare a solution with a ferrous ion concentration of 0.4-0.6 mol / L. An antioxidant of 0.5-1.0% of the amount of iron source is added to obtain solution C. Step four: Under the protection of an inert gas, solution C is slowly added dropwise to solution A while stirring. Then, solution B is slowly added dropwise to the above solution while maintaining the pH value at 4-4.5 during the addition process. Then, a carbon source is added, and microwave irradiation, drying, pre-carbonization, grinding, and carbonization are performed in sequence to obtain the LMFP-BO cathode material.
9. The preparation method according to claim 8, characterized in that, When manganese acetate is used in step one, the water bath temperature is 60-80℃; when manganese sulfate, manganese nitrate or manganese chloride is used, the water bath temperature is 70-90℃. When boric acid or lithium metaborate is used in step two, reflux at 50-70℃ for 2-4 hours. When borate esters are used, there is no need to add ethanol, and reflux at 80-100℃ for 3-5 hours. In step four, when using ammonium phosphate, deionized water is used as the solvent; The antioxidant mentioned in step five is ascorbic acid.
10. The preparation method according to claim 8, characterized in that, Step six describes the following steps: microwave irradiation treatment, which involves irradiating at 400-600W and 60-70℃ for 15-25 minutes; drying treatment, which involves drying at 110-120℃ for 10-14 hours; pre-carbonization treatment, which involves heating to 300-350℃ at a rate of 1.5-2.5℃ / min under inert gas protection and holding at that temperature for 2-3 hours; and carbonization treatment, which involves heating to 700-750℃ at a rate of 1-2℃ / min under a nitrogen-hydrogen mixed atmosphere and holding at that temperature for 6-10 hours.