Positive electrode active material and battery

By designing the La concentration ratio of particles A and B in the positive electrode active material to be 1.90×10-4<CLa/C′La<1.90×10-2, the problems of high resistance and low capacity retention in high-nickel ternary positive electrode materials were solved, and the battery performance was improved.

CN123120713APending Publication Date: 2026-11-17TOYOTA JIDOSHA KK
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202610614954.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2025-05-16
Filing Date
2026-05-07
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing battery cathode active materials have shortcomings in reducing resistance and improving capacity retention, especially in high-nickel ternary cathode materials, where uneven La distribution leads to structural instability and poor electronic conductivity.

Method used

A positive electrode active material is used, wherein primary particles A and B each contain La and satisfy a specific concentration ratio CLa/C′La range. Particle B is attached to the surface of primary particle A. By controlling the distribution of La, the structural stability and electronic conductivity are improved.

Benefits of technology

It achieves reduced resistance and improved capacity retention, especially maintaining high battery performance during cycling.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123120713A_ABST
    Figure CN123120713A_ABST
Patent Text Reader

Abstract

This disclosure provides a positive electrode active material comprising: crystalline primary particles A containing Li, TM (TM being a transition metal other than La), and O; and particles B attached to the primary particles A, wherein the particle size of the primary particles A is larger than the particle size of the particles B, and both the primary particles A and the particles B contain La. When the La concentration (atm%) in the primary particles A is set to CLa and the La concentration (atm%) in the particles B is set to C′La, a value of 1.90 × 10⁻⁶ is satisfied. ‑4 <CLa / C′La<1.90×10 ‑2 .
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This disclosure relates to positive electrode active materials and batteries. Background Technology

[0002] In recent years, battery development has been booming. For example, in the automotive industry, batteries for battery electric vehicles (BEVs), plug-in hybrid electric vehicles (PHEVs), or hybrid electric vehicles (HEVs) are being developed. As positive electrode active materials for batteries, active materials containing transition metals such as Ni, Co, and Mn are known.

[0003] For example, Japanese Patent Application Publication No. 2022-542774 discloses a W-containing high-nickel ternary cathode material, characterized in that it has the chemical formula Li. a Ni x Co y Mn 1-x-y W b M c O2 contains W-containing high-nickel ternary cathode material. The high-nickel ternary cathode material contains both spherical secondary particles and single-crystal particles. The single-crystal particles do not contain W elements, while the spherical secondary particles are doped with W elements.

[0004] Japanese Patent Application Publication No. 2024-511223 discloses a single-crystal multi-element cathode material, characterized in that the ratio of the longest diagonal length to the shortest diagonal length of the single-crystal particles of the above-mentioned single-crystal multi-element cathode material, measured by SEM, is defined as the roundness R, and R is 1 or more. The D-value of the single-crystal particles of the above-mentioned single-crystal multi-element cathode material is... 10 D 50 and D 90 Satisfying K 90 =(D 90 -D 10 ) / D 50 K 90 The product of R is 1.20~1.40. Summary of the Invention

[0005] From the viewpoint of improving battery performance, there is a demand for reduced resistance and increased capacity retention. This disclosure was made in view of the above-mentioned realities, and its main objective is to provide a positive electrode active material that can reduce resistance and improve capacity retention. [1]

[0007] A positive electrode active material,

[0008] The positive electrode active material has: crystalline primary particles A containing Li, TM (TM being a transition metal other than La) and O; and

[0009] Particle B attached to the primary particle A,

[0010] The particle size of the primary particle A is larger than the particle size of the primary particle B.

[0011] The primary particle A and the primary particle B each contain La. When the La concentration (atm%) in primary particle A is set to CLa and the La concentration (atm%) in primary particle B is set to C′La, the following condition is met: 1.90 × 10⁻⁶. -4 <CLa / C′La<1.90×10 -2 . [2]

[0013] According to the positive electrode active material described in [1], wherein W is attached to the surface of the primary particle A. [3]

[0015] According to the positive electrode active material described in [1] or [2], wherein the primary particle A contains at least one of Ni, Co and Mn as the TM. [4]

[0017] A battery has a positive electrode active material layer, a negative electrode active material layer, and an electrolyte layer disposed between the positive electrode active material layer and the negative electrode active material layer.

[0018] The positive electrode active material layer contains a positive electrode active material according to any one of [1] to [3].

[0019] In this disclosure, the positive electrode active material is provided that can reduce resistance and improve capacity retention. Attached Figure Description

[0020] The features, advantages, and technical and industrial significance of exemplary embodiments of the present invention will now be described in conjunction with the accompanying drawings, wherein the same symbols denote the same elements.

[0021] Figure 1 This is a schematic cross-sectional view illustrating the positive electrode active material in this disclosure.

[0022] Figure 2 This is a flowchart illustrating a method for manufacturing the positive electrode active material in this disclosure.

[0023] Figure 3 This is a schematic cross-sectional view illustrating the battery in this disclosure. Detailed Implementation

[0024] Hereinafter, embodiments will be described with reference to the accompanying drawings. However, this disclosure can be implemented in many different ways and is not limited to the embodiments illustrated below. In addition, in order to make the explanation clearer, the width, thickness, and shape of each part are sometimes schematically shown compared with the actual embodiment, but this is only an example and is not limiting to the interpretation.

[0025] A. Positive electrode active material

[0026] Figure 1 This is a schematic cross-sectional view illustrating the positive electrode active material in this disclosure. For example... Figure 1 As shown, the positive electrode active material 10 has crystalline primary particles A containing Li, TM (TM being a transition metal other than La), and O, and particles B attached to the primary particles A. The particle size of primary particles A is larger than that of particles B. Primary particles A and particles B each contain La. When the La concentration (atm%) in primary particles A is set as CCa and the La concentration (atm%) in particles B is set as C′La, CCa / C′La meets the specified range.

[0027] In this disclosure, the positive electrode active material has a primary particle A with a particle B attached to it. The La present in primary particle A contributes to structural stabilization during cycling, while the La present in particle B contributes to improved electronic conductivity. In this disclosure, CLa and C′La satisfy 1.90 × 10⁻⁶. -4 <CLa / C′La<1.90×10 -2 If the La concentration (CLa) in particle A is too high, the La ionic radius is large, thus increasing the strain of the initial structure. If the La concentration (C′La) in particle B is too high, it hinders Li ion conductivity. The CLa / C′La ratio can be 5.00 × 10⁻⁶. -4 That's all. On the other hand, CLa / C′La can be 2.00 × 10 -3 the following.

[0028] CLa and C′La were determined using the following steps. First, Auger electron spectroscopy (AES) was used to analyze the positive electrode active material, determining the elemental composition of any particles. Primary particles A and B were identified based on the presence or absence of TM (transition metals other than La). Next, 20 primary particles A and 20 particles B attached to primary particles A were randomly selected. Then, the average La concentration (atm%) of the 20 primary particles A was set as CLa, and the average La concentration (atm%) of the 20 particles B was set as C′La, and the ratio CLa / C′La was calculated.

[0029] In Example 3 of the aforementioned Japanese Patent Application Publication No. 2022-542774, a method using Li was disclosed. 1.0029 Ni 0.83 Co 0.11 Mn 0.0 6W 0.0009 La 0.002 O2 represents the cathode material. In Example 3 of Japanese Patent Application Publication No. 2022-542774, La is described as being uniformly distributed on the surface of single crystals and secondary spherical particles. Furthermore, Japanese Patent Application Publication No. 2024-511223 discloses a cathode material composed of Li... 1+a (Ni x Co y Mn z G b M c O 2-d The positive electrode material is indicated by Japanese Patent Application Publication No. 2024-511223. It discloses that G is one or more of Ti, W, V, Ta, Zr, La, Ce, Er, Sr, Si, Al, B, Mg, Co, F, and Y. Specifically, La is disclosed as one option for G. However, neither Japanese Patent Application Publication No. 2022-542774 nor Japanese Patent Application Publication No. 2024-511223 discloses a positive electrode active material in which both the primary particles and the particles attached thereto contain La, and the La concentration is within a specified range.

[0030] 1. Primary particle A

[0031] The primary particle A in this disclosure is a crystalline particle containing Li, TM (TM being a transition metal other than La), and O. Examples of crystal structures for primary particle A include layered rock salt type and spinel type, with layered rock salt type being preferred. Furthermore, primary particle A may have a crystal structure belonging to space group R-3m. Primary particle A in this disclosure contains La. The primary particle may or may not contain W.

[0032] Primary particle A contains Li, TM (TM being a transition metal other than La), and O. Primary particle A can contain one, two, three, or more transition metals.

[0033] Transition metals are metals belonging to groups 3 through 11 of the periodic table. The transition metals contained in a primary particle can belong to the third, fourth, or fifth period. Examples of transition metals include Ti, V, Cr, Mn, Fe, Co, Ni, Zr, Nb, and W.

[0034] Primary particle A preferably contains at least Ni. This is because it yields a positive electrode active material with excellent capacity characteristics. When all transition metals contained in the primary particle are set to 1 mole, the proportion of Ni in the primary particle is, for example, 0.25 moles or more. In this case, the proportion of Ni in the primary particle can be 0.33 moles or more, 0.50 moles or more, 0.75 moles or more, 0.80 moles or more, or 0.90 moles or more. By increasing the proportion of Ni, the capacitance characteristics are improved.

[0035] Primary particle A may or may not contain Co. When all the transition metals contained in the primary particle are set as 1 mole, the proportion of Co contained in the primary particle may be, for example, 0 moles or more, 0.05 moles or more, or 0.10 moles or more. On the other hand, the proportion of Co contained in the primary particle may be, for example, 0.40 moles or less, or 0.20 moles or less.

[0036] Primary particle A may or may not contain Mn. When the total amount of transition metal contained in the primary particle is set to 1 mole, the proportion of Mn contained in the primary particle may be, for example, 0 moles or more, 0.05 moles or more, or 0.10 moles or more. On the other hand, the proportion of Mn contained in the primary particle may be, for example, 0.40 moles or less, or 0.20 moles or less.

[0037] Primary particle A preferably contains at least one of Ni, Co, and Mn. When all metals (excluding Li) contained in the primary particle are considered to be 1 mole, the total proportion of Ni, Co, and Mn in the primary particle is, for example, 0.80 moles or more. In this case, the total proportion of Ni, Co, and Mn can be 0.90 moles or more, or 0.95 moles or more. It should be noted that "the total proportion of Ni, Co, and Mn" also includes the case where the proportion of one or two of Ni, Co, and Mn is 0.

[0038] In addition to Li and TM, primary particle A may also contain other metals M besides Li and TM. 1 (Including semi-metals). M as another metal 1 Examples of metals belonging to groups 12 through 14 of the periodic table include Zn, Al, Si, Ga, Ge, In, and Sn.

[0039] Primary particle A contains La in addition to Li, TM, and O. The La concentration (CLa) in primary particle A is lower than the La concentration (C′La) in particle B, and there is no particular limitation as long as the above-mentioned CLa / C′La concentration is satisfied. The La concentration (CLa) in primary particle A is, for example, 0.01 atm% or more and 0.5 atm% or less, or 0.03 atm% or more and 0.3 atm% or less.

[0040] The positive electrode active material in this disclosure can be a monocrystalline active material composed of the aforementioned primary particles A, or a polycrystalline material formed by the aggregation of multiple primary particles A. Monocrystalline active material refers to a material that is not a so-called polycrystalline active material (an active material formed by the seamless aggregation of multiple primary particles A). Monocrystalline active materials typically do not aggregate and exist as a single, independent particle. Preferably, monocrystalline active materials do not show grain boundaries when observed under a scanning electron microscope (SEM) (magnification: approximately 10,000 to 30,000 times). Compared to polycrystalline active materials, monocrystalline active materials have the advantage of less degradation over time.

[0041] The particle size of primary particle A can be, for example, 0.5 μm or more, 0.6 μm or more, 0.8 μm or more, or 1.0 μm or more. On the other hand, the particle size of primary particles can be, for example, 20 μm or less, 15 μm or less, 10 μm or less, or 5 μm or less. The particle size of primary particle A can be determined, for example, as the longest diameter observed in SEM. Furthermore, for example, if primary particles (positive electrode active material) are contained in the positive electrode active material layer, the particle size (longest diameter) of the primary particles can be determined from a cross-sectional image of the positive electrode active material layer.

[0042] W can exist on the surface of primary particle A. W can exist as a W compound containing W and other elements. Examples of other elements include Li, O, and La. The W compound can be disposed directly on the surface of primary particle A or disposed in the presence of other layers (other compounds), with the former being preferred.

[0043] W compounds can contain, for example, Li, W, and O. W compounds can consist solely of Li, W, and O, or they can contain other elements. As an example of the composition of a W compound, Li can be cited. a W b O c (5.5≤a≤6.5, 0.5≤b≤1.5, 5.5≤c≤6.5). A typical W compound having the above composition is Li6WO6. Other examples of W compounds with the above composition include Li... a W b O c(1.5≤a≤2.5, 0.5≤b≤1.5, 3.5≤c≤4.5). A typical W compound having the above composition is Li₂WO₄. Additionally, as other examples of the composition of W compounds, Li₂WO₄ can be cited. a W b O c (3.5≤a≤4.5, 0.5≤b≤1.5, 4.5≤c≤5.5). A typical W compound having the above composition is Li₄WO₅. Additionally, as other examples of the composition of W compounds, Li₂... a W b O c (1.5≤a≤2.5, 1.5≤b≤2.5, 6.5≤c≤7.5). W compounds with the above composition are typically Li2W2O7.

[0044] 2. Particle B

[0045] The positive electrode active material of this disclosure has particles B attached to the surface of primary particles A. The particle size of particle B is smaller than that of primary particles A. The particle size D of particle B... B The particle size D relative to the primary particle A A The ratio (D) B / D A For example, it can be 0.01 or higher and 0.5 or lower, or 0.05 or higher and 0.4 or lower, or 0.1 or higher and 0.3 or lower.

[0046] Particle B contains La. The La contained in particle B contributes to improved electronic conductivity. By having particle B on the surface of primary particle A, a reduction in electrical resistance can be achieved. Particle B can be disposed directly on the surface of primary particle A or disposed in the presence of other layers (other compounds). The La concentration in particle B (C′La) is greater than the La concentration in primary particle A (CLa), and there are no particular limitations as long as the above-mentioned CLa / C′La concentration is satisfied. The La concentration in particle B (C′La) is, for example, 10 atm% or more and 60 atm% or less, or 20 atm% or more and 40 atm% or less.

[0047] Particle B can be, for example, a La compound containing La and other elements. Examples of other elements include Ni, Li, O, and W.

[0048] La compounds can contain, for example, La, Ni, and O. La compounds can consist solely of La, Ni, and O, or they can contain other elements. As an example of the composition of a La compound, La... a Ni b O c(0.8 ≤ a ≤ 1.2, 0.8 ≤ b ≤ 1.2, 2.8 ≤ c ≤ 3.2). For example, LaNiO3 is a typical perovskite composition with good electronic conductivity. Other examples of La compounds include La... a Li b Ni c O d (3.5≤a≤4.5, 0.5≤b≤1.5, 0.5≤c≤1.5, 7.5≤d≤8.5). For example, given that La4LiNiO8 has good electronic conductivity, it is hypothesized that it has a crystalline phase similar to perovskite.

[0049] La compounds can be compounds containing both La and W.

[0050] W can exist on the surface of particle B. Particle B may or may not contain W.

[0051] 3. Positive electrode active material

[0052] The primary particles A and B of the positive electrode active material disclosed herein each contain La. When all transition metals contained in primary particle A are set to 1 mole, the proportion of La contained in the positive electrode active material (primary particles A and B) is, for example, 0.001 moles or more. In this case, the proportion of La contained in the positive electrode active material can be 0.003 moles or more, or 0.005 moles or more. On the other hand, the aforementioned proportion of La contained in the positive electrode active material is, for example, 0.100 moles or less, 0.050 moles or less, or 0.030 moles or less. When all transition metals contained in the primary particles are set to 1 mole, the proportion of W contained in the positive electrode active material is, for example, 0.001 moles or more, 0.003 moles or more, or 0.005 moles or more. On the other hand, the aforementioned proportion of W contained in the positive electrode active material is, for example, 0.100 moles or less, 0.050 moles or less, or 0.030 moles or less.

[0053] 4. Manufacturing method

[0054] Figure 2 This is a flowchart illustrating the manufacturing method of the above-mentioned positive electrode active material. Figure 2The method for manufacturing the positive electrode active material shown includes: a mixing step of mixing a transition metal hydroxide containing TM (TM being a transition metal other than La), a Li source, a La source, and a W source as needed to obtain a mixture; and a firing step of firing the obtained mixture. The firing step includes: a first firing treatment at a temperature T1; a second firing treatment at a temperature T2 lower than T1 after the first firing treatment; and a third firing treatment at a temperature T3 higher than T2 after the second firing treatment. Thus, the positive electrode active material is obtained.

[0055] (1) Mixing process

[0056] Transition metal hydroxides contain TM (TM being a transition metal other than La). Transition metal hydroxides are precursors to positive electrode active materials. Transition metal hydroxides typically do not contain Li, but may contain Li. The synthesis method of transition metal hydroxides is not particularly limited; for example, the following methods can be used. First, prepare an aqueous solution of the transition metal hydroxide as a raw material. Methods for preparing the raw material aqueous solution include, for example, dissolving a water-soluble transition metal compound in water. Transition metal compounds include, for example, metal salts such as sulfates and nitrates. Ni sources include, for example, NiSO4 and Ni(NO3)2. Co sources include, for example, CoSO4, Co(NO3)2, and Co(NO3)3. Mn sources include, for example, MnSO4 and Mn(NO3)2. The composition of the raw material aqueous solution can be appropriately adjusted according to the target positive electrode active material. A certain amount of NH3 aqueous solution is added to the reaction vessel, and nitrogen replacement is carried out while stirring with a stirrer or similar device. Next, an aqueous sodium hydroxide solution is added to the reaction vessel, maintaining the pH at an alkaline level (e.g., pH 11.3–12.0), while simultaneously adding the starting material aqueous solution and an NH3 aqueous solution. The reaction temperature is not particularly limited, but can be, for example, above 50°C and below 65°C. The reaction time is, for example, 2 hours or more and within 6 hours. After the reaction is complete, it is preferable to filter to remove the transition metal hydroxide, wash with water, and then dry.

[0057] In the mixing process, a mixture containing a transition metal hydroxide, a Li source, a La source, and a W source as needed is prepared. Examples of Li sources include lithium hydroxide, lithium carbonate, lithium nitrate, lithium acetate, lithium oxide, and lithium chloride. The Li source can be lithium hydroxide or a Li-containing compound other than lithium hydroxide. The molar ratio of Li in the Li source to the TM contained in the transition metal hydroxide is, for example, 0.8 or more and 1.2 or less, 0.9 or more and 1.1 or less, or 1.0.

[0058] Examples of La sources include hydroxides, sulfates, nitrates, and other metal salts. Examples of La sources include La(OH)3, LaSO4, and La(NO3)3. The molar ratio of La in the La source to the TM contained in the transition metal hydroxide is, for example, 0.01 or more and 0.1 or less, and may be 0.05 or more and 0.07 or less.

[0059] Examples of W sources include H2WO4. The molar ratio of W in the W source to the TM contained in the transition metal hydroxide is, for example, 0.005 or more and 0.02 or less, and may be 0.008 or more and 0.015 or less.

[0060] The mixture preferably contains a molten salt. By having the molten salt function as a flux, sufficient grain growth of primary particles is achieved. The molten salt may contain Li. Examples of molten salts include lithium hydroxide. The mixture may contain lithium hydroxide as both a Li source and a molten salt. The molar ratio (Li' / TM) of Li in the Li source and molten salt relative to the amount of transition metal hydroxide (TM) in the transition metal hydroxide is, for example, 1.01 or more, 1.05 or more, 1.10 or more, or 1.15 or more. On the other hand, the Li' / TM ratio is, for example, 1.60 or less, 1.50 or less, 1.40 or less, or 1.30 or less.

[0061] (2) Firing process

[0062] In the first firing process, the first mixture is fired at a temperature T1. Temperature T1 is typically 700°C to 900°C, but can also be 750°C to 850°C. The firing time in the first firing process is not particularly limited, but can be, for example, 3 hours to 5 hours. Next, a second firing process is performed at a temperature T2, which is lower than T1. Temperature T2 is typically 400°C to 600°C, but can also be 450°C to 550°C. The firing time in the second firing process is not particularly limited, but can be, for example, 2 hours to 4 hours. Next, a third firing process is performed at a temperature T3, which is higher than T2. ​​Temperature T3 is typically 700°C to 900°C, but can also be 750°C to 850°C. The firing time in the third firing process is not particularly limited, but can be, for example, 3 hours to 5 hours. The heating rate to temperature T1 and the heating rate from temperature T2 to T3 are, for example, 10°C / min or more and 30°C / min or less. The cooling rate from temperature T1 to temperature T2 can also be set to natural cooling. The atmosphere in the first, second, and third firing processes is usually an oxygen-containing atmosphere. Examples of firing methods include using a muffle furnace, an electric furnace, or similar firing furnace.

[0063] By combining the amount of La source in the mixing process with the firing temperature in the firing process, the amount of La entering the interior of primary particle A and the crystallinity of primary particle A can be controlled.

[0064] B. Battery

[0065] Figure 3 This is a schematic cross-sectional view illustrating the battery in this disclosure. Figure 3 The battery 20 shown includes: a positive electrode active material layer 11 having the aforementioned positive electrode active material, a negative electrode active material layer 12, an electrolyte layer 13 disposed between the positive electrode active material layer 11 and the negative electrode active material layer 12, a positive electrode current collector 14 for collecting current from the positive electrode active material layer 11, and a negative electrode current collector 15 for collecting current from the negative electrode active material layer 12. Because the positive electrode active material layer 11 has the aforementioned positive electrode active material, a battery with reduced resistance and high capacity retention is obtained.

[0066] The positive electrode active material layer contains the positive electrode active material described in "A. Positive Electrode Active Material". Additionally, the positive electrode active material layer may contain a conductive material and a binder. Conventionally known materials can be used as the conductive material and binder. The positive electrode active material layer may contain an electrolyte. The electrolyte is, for example, the electrolyte described later. The thickness of the positive electrode active material layer is, for example, 0.1 μm or more and 1000 μm or less. The method for manufacturing the positive electrode active material layer is not particularly limited; for example, a method of coating a positive electrode slurry containing the positive electrode active material and a dispersion medium onto a positive electrode current collector and then drying it can be used. The dried positive electrode active material layer can be pressed. Pressing increases the density of the positive electrode active material layer.

[0067] The negative electrode active material layer contains at least a negative electrode active material. Examples of negative electrode active materials include carbon-based, Li-based, Si-based, and oxide-based active materials. The negative electrode active material layer may contain at least one of a conductive material, a binder, and an electrolyte. Details regarding the conductive material, binder, and electrolyte are the same as described above.

[0068] The electrolyte layer contains at least an electrolyte. The electrolyte is, for example, a liquid electrolyte (electrolyte). Examples of electrolytes include non-aqueous electrolytes. Non-aqueous electrolytes may contain, for example, lithium salts and non-aqueous solvents. Examples of lithium salts include inorganic lithium salts such as LiPF6, LiBF4, LiClO4, and LiAsF6; and organic lithium salts such as LiCF3SO3, LiN(SO2CF3)2, LiN(SO2C2F5)2, and LiC(SO2CF3)3. Examples of non-aqueous solvents include, for example, carbonate solvents. The non-aqueous solvent can be a mixture of cyclic carbonates such as EC and PC, which have high dielectric constants and high viscosity, and chain carbonates such as DMC, DEC, and EMC, which have low dielectric constants and low viscosity. Additionally, non-aqueous electrolytes may contain ionic liquids. Other examples of electrolytes include aqueous electrolytes.

[0069] Materials that can be used as positive electrode current collectors include, for example, SUS, aluminum, nickel, iron, titanium, and carbon. On the other hand, materials that can be used as negative electrode current collectors include, for example, SUS, copper, nickel, and carbon.

[0070] The type of battery disclosed herein is not particularly limited, but lithium-ion batteries are typical. Furthermore, the battery in this disclosure can be a primary battery or a secondary battery, with a secondary battery being preferred. This is because it can be repeatedly charged and discharged, making it useful, for example, as a battery for vehicles. Examples of applications for the battery include power sources for vehicles such as hybrid electric vehicles (HEVs), plug-in hybrid electric vehicles (PHEVs), battery electric vehicles (BEVs), gasoline vehicles, and diesel vehicles. It is particularly preferred for use as a power source for driving hybrid electric vehicles (HEVs), plug-in hybrid electric vehicles (PHEVs), or battery electric vehicles (BEVs). Additionally, the battery can be used as a power source for mobile bodies other than vehicles (e.g., railways, ships, aircraft) and for electrical products such as information processing devices.

[0071] Furthermore, this disclosure is not limited to the embodiments described above. The embodiments described above are illustrative, and may have a structure that is substantially the same as the technical concept described in the claims of this disclosure and achieves the same effect. Any structure is included within the technical scope of this disclosure.

[0072] Comparative Example 1

[0073] Production of positive electrode active material

[0074] NiSO4, CoSO4, and MnSO4 were prepared as raw materials and dissolved in ion-exchange water to prepare a raw material aqueous solution. The molar ratio of Ni, Co, and Mn in the raw material aqueous solution was Ni:Co:Mn = 8:1:1. Furthermore, the concentration of the raw material aqueous solution (the proportion of all raw materials to the raw material aqueous solution) was 30% by mass.

[0075] Then, a certain amount of NH3 aqueous solution was added to the reaction vessel, and the mixture was stirred while nitrogen was purged from the reaction vessel. NaOH aqueous solution was added to the reaction vessel to maintain an alkaline pH. While maintaining a controlled temperature, the raw material aqueous solution and NH3 aqueous solution were added dropwise to precipitate the transition metal hydroxide. The reaction temperature was 60℃, and the reaction time was 3 hours. Next, the precipitated transition metal hydroxide was removed by filtration, and deion-exchanged water was added to disperse it with a spoon, followed by washing. After washing, the filtered transition metal hydroxide was dried at 120℃ for 16 hours to obtain the transition metal hydroxide as a precursor.

[0076] Then, a Li source (LiOH) is added to the obtained precursor and mixed in a mortar to obtain a mixture (mixing step). The amount of Li source added is adjusted so that the molar ratio (Li / NCM) of Li in the Li source relative to the total NCM (Ni, Co, Mn) in the precursor is 1.1. The obtained mixture is calcined in a calcining furnace at 900°C in an oxygen atmosphere for 10 hours to obtain a calcined body. The calcined body is then crushed using a jet mill, and the particle size is adjusted to obtain the positive electrode active material.

[0077] Battery manufacturing

[0078] Using the obtained positive electrode active material, a battery is manufactured. Specifically, a coating machine (manufactured by Allgood Co., Ltd.) with film thickness adjustment function is used for coating, and positive electrode active material (LiNi) containing conductive material in a mass ratio of positive electrode active material: conductive material: binder = 88:10:2 is coated. 0.8 Co 0.1 Mn 0.1 A positive electrode composite material consisting of O2, conductive material (acetylene black), and binder (polyvinylidene fluoride) is coated onto the surface of a metal foil serving as the positive electrode current collector. Then, it is dried at 80°C for 5 minutes using a dryer to obtain a positive electrode with both a positive electrode current collector and a positive electrode active material layer.

[0079] Next, using a coating machine (manufactured by Allgood Co., Ltd.) with film thickness adjustment function, a negative electrode composite material containing negative electrode active material (natural graphite) and binders (SBR and CMC) was coated onto the surface of a metal foil serving as the negative electrode current collector. Then, it was dried at 80°C for 5 minutes using a dryer to obtain a negative electrode with a negative electrode current collector and a layer of negative electrode active material. Next, a 1M LiPF6 solution was prepared as the electrolyte. The electrolyte solvent was a mixed solvent prepared by mixing ethylene carbonate (EC), dimethyl carbonate (DMC), and ethyl methyl carbonate (EMC) in a volume ratio of EC:DMC:EMC = 3:4:3. Using the above-described positive electrode, negative electrode, and electrolyte, a wound cylindrical battery was obtained.

[0080] Comparative Example 2

[0081] A precursor (transition metal hydroxide) was obtained in the same manner as in Comparative Example 1. A Li source (LiOH), a La source (La(OH)3), and a W source (H2WO4) were added to the obtained precursor and mixed using an agate mortar to obtain a mixture (mixing step). The amount of Li source added was adjusted so that the molar ratio (Li / NCM) of Li in the Li source relative to the total NCM (Ni, Co, Mn) in the precursor was 1.1. Furthermore, the amount of La source added was adjusted to La / NCM of 0.01, and the amount of W source added was adjusted to W / NCM of 0.01. The obtained mixture was calcined in a calcining furnace at 900°C under an oxygen atmosphere for 10 hours to obtain a calcined body. The calcined body was crushed using a jet mill, and the particle size was adjusted to obtain a positive electrode active material. A battery was obtained in the same manner as in Comparative Example 1, except that the obtained positive electrode active material was used.

[0082] Example 1

[0083] Similar to Comparative Example 1, a precursor (transition metal hydroxide) was obtained. A Li source (LiOH), a La source (La(OH)3), and a W source (H2WO4) were added to the obtained precursor and mixed using an agate mortar to obtain a mixture (mixing step). The amount of Li source added was adjusted so that the molar ratio (Li / NCM) of Li in the Li source relative to the total NCM (Ni, Co, Mn) in the precursor was 1.1. Furthermore, the amount of La source added was adjusted to make La / NCM 0.01, and the amount of W source added was adjusted to make W / NCM 0.01. The obtained mixture was fired in a firing furnace under an oxygen atmosphere in the following order: 800°C for 4 hours (first firing treatment), 500°C for 3 hours (second firing treatment), and 800°C for 4 hours (third firing treatment), thereby obtaining a fired body (firing step). The heating rate in the firing step was set to 20°C / min, and the cooling rate was set to natural cooling. The sintered material was crushed using a jet mill, and the particle size was adjusted to obtain the positive electrode active material. A battery was obtained in the same manner as in Comparative Example 1, except that the obtained positive electrode active material was used.

[0084] Example 2

[0085] In the mixing process, the amount of La source added was adjusted to make La / NCM 0.05. Otherwise, the positive electrode active material was obtained using the same method as in Example 1. Except for using the obtained positive electrode active material, a battery was obtained in the same manner as in Comparative Example 1.

[0086] Example 3

[0087] In the mixing process, the amount of La source added was adjusted to make La / NCM 0.07. Otherwise, the positive electrode active material was obtained using the same method as in Example 1. Except for using the obtained positive electrode active material, a battery was obtained in the same manner as in Comparative Example 1.

[0088] Example 4

[0089] In the mixing process, the amount of La source added was adjusted to make La / NCM 0.10. Otherwise, the positive electrode active material was obtained using the same method as in Example 1. Except for using the obtained positive electrode active material, a battery was obtained in the same manner as in Comparative Example 1.

[0090] Determination of La concentration

[0091] The elemental composition of arbitrary particles was determined by point analysis using Auger electron spectroscopy (AES). Primary particles A and B were screened based on the presence or absence of Ni, Co, and Mn. Specifically, particles containing Ni, Co, and Mn were designated as primary particles A, and particles attached to primary particles A but lacking Ni, Co, and Mn were designated as particles B. It was confirmed that the particle size of primary particles A was larger than that of particles B. Twenty primary particles A and 20 particles B attached to primary particles A were randomly selected. The average La concentration (atm%) in the 20 primary particles A was set as CLa, and the average La concentration (atm%) in the 20 particles B was set as C′La. The ratio CLa / C′La was calculated. The results are shown in Table 1.

[0092] evaluate

[0093] initial resistance

[0094] The initial resistance was measured using the batteries obtained in Comparative Examples 1, 2, and 1-4. Specifically, the batteries were charged to 4.3V and then discharged to 3.7V. The voltage drop (V) was then measured during 10-second discharge at various C-rates: 0°C, 0.1C, 0.3C, 0.5C, 0.7C, and 1.0C. The voltage drop (V) was plotted against the current value, and the slope of the approximate straight line drawn as a linear function was taken as the resistance (V resistance). The results are shown in Table 1. Note that the initial resistance values ​​in Table 1 are relative to the initial resistance of Comparative Example 1, which is set to 100%.

[0095] Capacity maintenance rate

[0096] The capacity retention rate was determined using the batteries obtained in Comparative Examples 1, 2, and Examples 1-4. Specifically, 200 cycles were performed under the following conditions: voltage range: 3.0V~4.3V, C rate: 2C, mode: CC charge / discharge, and temperature: 50°C. The capacity retention rate was determined by dividing the discharge capacity of the 200th cycle by the discharge capacity of the first cycle. The results are shown in Table 1.

[0097] (Table 1)

[0098]

[0099] As shown in Table 1, it was confirmed that Examples 1-4 had lower initial resistance and higher cycle capacity retention compared to Comparative Examples 1 and 2. This is presumably because in Examples 1-4, primary particles A and B each contained La, and the ratio CLa / C′La was within a specified range. Therefore, the La present in primary particle A contributed to structural stabilization during cycling, while the La present in particle B contributed to improved electronic conductivity. On the other hand, in Comparative Example 1, since neither primary particles A nor particle B contained La, the structural stabilization effect from the La in primary particle A and the improved electronic conductivity effect from the La in particle B were not achieved. Furthermore, it was confirmed that in Comparative Example 2, due to the excessively large CLa / C′La ratio, the initial structural strain was large, resulting in high initial resistance and low cycle capacity retention.

Claims

1. A positive electrode active material, The positive electrode active material has the following characteristics: A is a crystalline primary particle containing Li, TM (a transition metal other than La), and O; and Particle B attached to the primary particle A, The particle size of the primary particle A is larger than the particle size of the primary particle B. The primary particle A and the primary particle B each contain La. When the La concentration atm% in primary particle A is set as CLa and the La concentration atm% in primary particle B is set as C′La, the following condition is met: 1.90 × 10⁻⁶. -4 <CLa / C′La<1.90×10 -2 .

2. The positive electrode active material according to claim 1, wherein, The positive electrode active material has W attached to the surface of the primary particle A.

3. The positive electrode active material according to claim 1, wherein, The primary particle A contains at least one of Ni, Co, and Mn as the TM.

4. A battery having a positive electrode active material layer, a negative electrode active material layer, and an electrolyte layer disposed between the positive electrode active material layer and the negative electrode active material layer. The positive electrode active material layer contains the positive electrode active material as described in any one of claims 1-3.

Citation Information

Patent Citations

  • W-containing high-nickel ternary positive electrode material and its manufacturing method

    JP2022542774A

  • Single crystal type multi-element positive electrode material, its manufacturing method, and lithium ion battery

    JP2024511223A