A bimetallic ion-doped manganese-based mixed phosphate material, its preparation method, positive electrode sheet, and sodium-ion battery.
By doping Fe2+ and Ti4+ ions into manganese-based mixed phosphate materials and then coating them with carbon, the problems of poor conductivity and structural instability of manganese-based mixed phosphate materials were solved, and the electrochemical performance of the materials was improved.
Patent Information
- Application Number
- CN202611490505.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-23
- Publication Date
- 2026-11-17
AI Technical Summary
Existing manganese-based mixed phosphate materials have poor conductivity, resulting in low specific capacity and poor high-rate performance. Furthermore, the Jahn-Teller effect of Mn3+ causes structural degradation and irreversible phase transitions, leading to poor cycle stability.
By doping NMPP materials with Fe2+ and Ti4+ bimetallic ions and partially coating the surface with carbon, Na4Mn1.8-xFe1.2Tix(PO4)2P2O7/C materials are formed. Combining bulk doping and carbon coating strategies improves the conductivity and structural stability of the materials.
Excellent electrical conductivity and structural stability of the material were achieved, and the specific capacity, rate performance and cycle stability were improved.
Smart Images

Figure CN123120722A_ABST
Abstract
Description
Technical Field
[0001] This application belongs to the field of sodium-ion battery cathode material technology, and relates to a manganese-based mixed phosphate material, and more particularly to a bimetallic ion-doped manganese-based mixed phosphate material, its preparation method, cathode sheet and sodium-ion battery. Background Technology
[0002] Sodium-ion batteries are considered an important supplementary system to lithium-ion batteries due to their abundant resources and low cost, and the development of high-performance cathode materials is the key to their commercial application.
[0003] Manganese-based mixed phosphate Na4Mn3(PO4)2P2O7 (abbreviated as NMPP) has high abundance, high voltage (the electron-withdrawing P2O7 groups around the Mn octahedrons can generate an inductive effect, providing a high redox potential), and is prone to multi-electron transfer (Mn 2+ / Mn 3+ / Mn 4+ With advantages such as high conductivity, NMPP materials are considered a high-performance cathode material. However, the intrinsic defect of poor conductivity leads to low specific capacity and poor high-rate performance, and Mn... 3+ The Jahn-Teller effect causes unavoidable structural degradation and irreversible phase transitions, resulting in poor cycle stability.
[0004] Synthesizing NMPP / C composites via carbon coating can improve electronic conductivity. CN110085849A discloses a carbon-coated sodium manganese pyrophosphate @SWCNT composite material with a network structure, its preparation, and its application. By uniformly coating sodium manganese pyrophosphate with a carbon layer and in-situ composite it on the surface of a network-shaped single-walled carbon nanotube, the thermal stability, chemical stability, and conductivity of sodium manganese pyrophosphate are improved, resulting in higher capacity utilization, rate performance, and cycling performance.
[0005] However, carbon coating and composite strategies with carbon materials can only improve the electronic conductivity of the material surface, but cannot improve the intrinsic electrical conductivity of the material.
[0006] Elemental doping of NMPP materials can reduce the Mn content and strengthen the crystal structure, potentially suppressing structural degradation and irreversible phase transitions caused by the Jahn-Teller effect and improving the electronic conductivity from within, thereby enhancing its electrochemical performance. CN121698318A discloses an iron-manganese-based mixed phosphate micro / nano secondary sphere, its preparation method, and its applications. The chemical formula of the iron-manganese-based mixed phosphate micro / nano secondary sphere is Na4Fe. x Mn 3-x(PO4)2P2O7, 0<x<3, which combines the excellent cycling stability of Na4Fe3(PO4)2P2O7 (NFPP) and the high voltage platform of NMPP, inhibits the formation of the electrochemically inert NaMnPO4 impurity phase, ensures the purity of the final product, and can simultaneously achieve high specific capacity, excellent rate performance and long-term cycling stability when used as a cathode for sodium-ion batteries.
[0007] However, doping only iron element into the NMPP material has a poor inhibition effect on the distortion caused by the Jahn-Teller effect, and the doping amount of iron element still needs further investigation.
[0008] Therefore, how to combine the bulk phase doping and carbon coating strategies to effectively inhibit the Jahn-Teller effect and simultaneously improve the internal and external conductivity of NMPP particles is an urgent problem to be solved in the art. Contents of the Invention
[0009] In view of the deficiencies existing in the prior art, the purpose of the present application is to provide a bimetallic ion-doped manganese-based mixed phosphate material, preparation method, cathode pole piece and sodium-ion battery. In the present application, an appropriate amount of Fe 2+ , Ti 4+ bimetallic ion doping is performed, and at least part of the surface of the bimetallic ion-doped manganese-based mixed phosphate is carbon-coated. The obtained bimetallic ion-doped manganese-based mixed phosphate material has excellent conductivity and structural stability, so that when applied to sodium-ion batteries, it can exhibit excellent specific capacity, rate performance and cycling stability.
[0010] To achieve the above purpose of the invention, the present application adopts the following technical solutions:
[0011] In a first aspect, the present application provides a bimetallic ion-doped manganese-based mixed phosphate material, the chemical general formula of the bimetallic ion-doped manganese-based mixed phosphate material is Na4Mn 1.8-x Fe 1.2 Ti x (PO4)2P2O7 / C, 0.15≤x≤0.2; the bimetallic ion-doped manganese-based mixed phosphate material comprises a bimetallic ion-doped manganese-based mixed phosphate inner core and a carbon coating layer located on at least part of the surface of the bimetallic ion-doped manganese-based mixed phosphate inner core.
[0012] Exemplarily, the value of x may be 0.15, 0.16, 0.17, 0.18, 0.19 or 0.2, etc.
[0013] In the present application, Fe is introduced at the Mn site in the NMPP material 2+Doping with Fe, an element with similar physicochemical properties and ionic radii to Mn, and its superior stability, can reduce the proportion of Mn while stabilizing the crystal structure, thus reducing the Mn content. 3+ The Jahn-Teller effect enhances the electronic conductivity of the material from within. Specifically, when the Mn / Fe molar ratio is 6:4 (Fe... 2+ When the doping amount is 1.2%, the material can have both excellent conductivity and structural stability, thereby improving its specific capacity, rate performance and cycle stability.
[0014] This application involves Ti injection into Mn sites in NMPP materials. 4+ Doping with Ti allows it to generate Na vacancies within the material through charge compensation, which facilitates rapid ion / electron transport. This achieves overall charge balance and improves the material's conductivity from within. Furthermore, the Ti-O bond is stronger than the Fe-O and Mn-O bonds, and Ti, being an inert element, acts as a support and buffer within the material, helping to mitigate the effects of Na doping. + Lattice volume changes caused by insertion / extraction and Mn 3+ The Jahn-Teller effect. Where, when Ti... 4+ When the doping amount is 0.15~0.2, the conductivity and structural stability of the material can be further improved, thereby further improving its specific capacity, rate performance and cycle stability.
[0015] This application improves the surface / interface electronic conductivity of the material and suppresses side reactions between the bimetallic ion-doped manganese-based mixed phosphate and the electrolyte by coating at least part of the surface of the bimetallic ion-doped manganese-based mixed phosphate core with a carbon coating layer.
[0016] In some embodiments, the carbon coating layer in the bimetallic ion-doped manganese-based mixed phosphate material has a mass fraction of 5wt% to 8wt%, for example, it can be 5wt%, 6wt%, 7wt%, or 8wt%.
[0017] In the bimetallic ion-doped manganese-based mixed phosphate material provided in this application, the mass fraction of the carbon coating layer should be controlled to be 5wt%~8wt%. If the mass fraction of the carbon coating layer is too low, it is difficult to form a continuous and complete carbon conductive layer on the particle surface, resulting in limited improvement in material conductivity and inability to construct an effective conductive network. At the same time, the carbon layer provides insufficient protection for the active material, allowing the electrolyte to easily come into direct contact with the active material, exacerbating manganese ion dissolution. During charge and discharge, the lattice deformation is not effectively buffered, and the crystal structure is easily damaged, leading to a decrease in the material's rate performance and cycle stability. If the mass fraction of the carbon coating layer is too high, the proportion of non-sodium-storage active carbon components is too high, which will dilute the active material, reduce the material's specific capacity and energy density. In addition, an excessively thick carbon layer will increase the sodium ion diffusion resistance, degrade the powder tap density and electrode processing performance, and easily induce additional electrolyte side reactions, reducing the initial coulombic efficiency.
[0018] In some embodiments, the particle size distribution of the bimetallic ion-doped manganese-based mixed phosphate material is 3μm to 8μm, and the particle size of the bimetallic ion-doped manganese-based mixed phosphate material can be, for example, 3μm, 4μm, 5μm, 6μm, 7μm or 8μm.
[0019] Secondly, this application provides a method for preparing a bimetallic ion-doped manganese-based mixed phosphate material as described in the first aspect, comprising the following steps:
[0020] Sodium, manganese, iron, titanium, and phosphorus sources were added to a solvent in stoichiometric ratios, and a carbon source was added. The mixture was then sequentially mixed, spray-dried, and calcined in stages to obtain the bimetallic ion-doped manganese-based mixed phosphate material.
[0021] This application utilizes spray drying to achieve atomic-level homogenization of all raw materials, enabling precise control of the stoichiometry of raw material components and maintaining uniform distribution, thus avoiding localized component segregation. Through segmented calcination, stepwise dehydration, decomposition, and ordered crystal phase growth are achieved. The initial low-temperature stage removes solvents and organic impurities from the precursor, preventing particle agglomeration and abnormal crystal growth caused by excessively rapid heating. The subsequent high-temperature stage ensures the full crystallization of the target manganese-based mixed phosphate phase, while also considering Fe... 2+ Ti 4+ Uniform lattice doping with bimetallic ions suppresses manganese volatilization and impurity phase formation, promotes the production of powder materials with moderate grain size and controllable defects, thereby improving the structural stability and sodium ion transport capacity of the material, and improving the rate and cycle performance of the battery.
[0022] In some embodiments, the sodium source includes any one or a combination of at least two of sodium pyrophosphate, sodium oxalate, or sodium acetate. Typical but non-limiting combinations include combinations of sodium pyrophosphate and sodium oxalate, combinations of sodium oxalate and sodium acetate, combinations of sodium pyrophosphate and sodium acetate, combinations of sodium pyrophosphate, sodium oxalate, and sodium acetate, etc.
[0023] In some embodiments, the manganese source includes any one or a combination of at least two of manganese acetate, manganese oxalate, or manganese nitrate. Typical but non-limiting combinations include combinations of manganese acetate and manganese oxalate, combinations of manganese oxalate and manganese nitrate, combinations of manganese acetate and manganese nitrate, combinations of manganese acetate, manganese oxalate, and manganese nitrate, etc.
[0024] In some embodiments, the iron source includes any one or a combination of at least two of ferric nitrate, ferric phosphate, or ferrous oxalate. Typical but non-limiting combinations include combinations of ferric nitrate and ferric phosphate, combinations of ferric phosphate and ferrous oxalate, combinations of ferric nitrate and ferrous oxalate, and combinations of ferric nitrate, ferric phosphate, and ferrous oxalate.
[0025] In some embodiments, the titanium source includes tetrabutyl titanate.
[0026] In some embodiments, the phosphorus source includes sodium dihydrogen phosphate and / or ammonium dihydrogen phosphate.
[0027] In some embodiments, the solvent includes a nitric acid solution.
[0028] In some embodiments, the concentration of the nitric acid solution is 0.5 mol / L to 1 mol / L, for example, it can be 0.5 mol / L, 0.6 mol / L, 0.7 mol / L, 0.8 mol / L, 0.9 mol / L or 1 mol / L, etc.
[0029] In some embodiments, the carbon source includes any one or a combination of at least two of citric acid, glucose, sucrose, or oxalic acid. Typical but non-limiting combinations include combinations of citric acid and glucose, combinations of sucrose and oxalic acid, combinations of citric acid, glucose, sucrose, and oxalic acid, etc.
[0030] In some embodiments, the molar ratio of the carbon source to the total molar ratio of the manganese source, the iron source and the titanium source is (0.8~1.2):1, for example, it can be 0.8:1, 0.9:1, 1:1, 1.1:1 or 1.2:1, etc.
[0031] In some embodiments, the mixing includes ultrasonic dispersion and / or magnetic stirring.
[0032] In some embodiments, the segmented calcination includes a first calcination and a second calcination.
[0033] In some implementations, the mixing time is 2h to 4h, for example, it can be 2h, 2.5h, 3h, 3.5h or 4h.
[0034] In some embodiments, the ultrasonic dispersion time is 1h to 4h, for example, it can be 1h, 1.5h, 2h, 2.5h, 3h, 3.5h or 4h.
[0035] In some embodiments, the magnetic stirring time is 1h to 4h, for example, it can be 1h, 1.5h, 2h, 2.5h, 3h, 3.5h or 4h.
[0036] In some embodiments, the atmosphere for the first calcination and the second calcination is independently nitrogen and / or argon, respectively.
[0037] In some embodiments, the heating rate of the first calcination is 2℃ / min to 3℃ / min, for example, it can be 2℃ / min, 2.5℃ / min or 3℃ / min, etc.
[0038] In some embodiments, the temperature of the first calcination is 320°C to 380°C, for example, it can be 320°C, 340°C, 350°C, 360°C or 380°C.
[0039] In some embodiments, the holding time for the first calcination is 4h to 7h, for example, it can be 4h, 5h, 6h or 7h.
[0040] In some embodiments, the heating rate of the second calcination is 2℃ / min to 3℃ / min, for example, it can be 2℃ / min, 2.5℃ / min or 3℃ / min, etc.
[0041] In some embodiments, the second calcination temperature is 620°C to 680°C, for example, it can be 620°C, 640°C, 650°C, 660°C or 680°C.
[0042] In some embodiments, the holding time for the second calcination is 8h to 12h, for example, it can be 8h, 9h, 10h, 11h or 12h.
[0043] In some embodiments, the inlet air temperature of the spray dryer is 215°C to 225°C, for example, it can be 215°C, 220°C or 225°C.
[0044] In some embodiments, the outlet air temperature of the spray dryer is 105°C to 115°C, for example, it can be 105°C, 110°C or 115°C.
[0045] In some embodiments, the feed rate of the spray dryer is 280 mL / h to 320 mL / h, for example, it can be 280 mL / h, 290 mL / h, 300 mL / h, 310 mL / h or 320 mL / h.
[0046] In some embodiments, after the spray drying is completed and before the segmented calcination, a drying process is also included.
[0047] In some embodiments, the drying temperature is 60°C to 100°C, for example, it can be 60°C, 70°C, 80°C, 90°C or 100°C.
[0048] In some embodiments, the drying time is 1 hour to 3 hours, for example, it can be 1 hour, 2 hours or 3 hours.
[0049] Thirdly, this application provides a positive electrode sheet comprising a bimetallic ion-doped manganese-based mixed phosphate material as described in the first aspect.
[0050] In some embodiments, the positive electrode sheet further includes a conductive agent and a binder.
[0051] In some embodiments, the mass ratio of the bimetallic ion-doped manganese-based mixed phosphate material, the conductive agent, and the binder is (70~85):(10~20):(5~10), for example, it can be 70:20:10, 75:15:10, 80:10:10, 80:15:5, or 85:10:5, etc.
[0052] Fourthly, this application provides a sodium-ion battery, the sodium-ion battery comprising a positive electrode as described in the third aspect.
[0053] In some embodiments, the sodium-ion battery further includes a sodium-containing electrolyte and a negative electrode.
[0054] In some embodiments, the sodium-containing electrolyte includes sodium salts, organic solvents, and additives.
[0055] In some embodiments, the sodium salt includes NaClO4, and the concentration of the sodium salt is 0.5 mol / L to 2 mol / L, for example, it can be 0.5 mol / L, 1 mol / L, 1.5 mol / L or 2 mol / L, etc.
[0056] In some embodiments, the organic solvent comprises equal volumes of EC (ethylene carbonate) and DMC (dimethyl carbonate).
[0057] In some embodiments, the additive includes FEC (fluoroethylene carbonate), and the mass fraction of the additive is 3wt% to 8wt%, for example, it can be 3wt%, 4wt%, 5wt%, 6wt%, 7wt%, or 9wt%.
[0058] The numerical range described in this application includes not only the point values listed above, but also any point values between the above numerical ranges that are not listed. Due to space limitations and for the sake of brevity, this application will not exhaustively list the specific point values included in the range.
[0059] Compared with the prior art, this application has the following advantages:
[0060] (1) This application involves Fe injection into Mn sites in NMPP materials. 2+ Doping with Fe, an element with similar physicochemical properties and ionic radii to Mn, and its superior stability, can reduce the proportion of Mn while stabilizing the crystal structure, thus reducing the Mn content. 3+ The Jahn-Teller effect enhances the electronic conductivity of the material from within. Specifically, when the Mn / Fe molar ratio is 6:4 (Fe... 2+ When the doping amount is 1.2%, the material can have both excellent conductivity and structural stability, thereby improving its specific capacity, rate performance and cycle stability.
[0061] (2) This application involves Ti injection into Mn sites in NMPP materials. 4+ Doping with Ti allows it to generate Na vacancies within the material through charge compensation, which facilitates rapid ion / electron transport. This achieves overall charge balance and improves the material's conductivity from within. Furthermore, the Ti-O bond is stronger than the Fe-O and Mn-O bonds, and Ti, being an inert element, acts as a support and buffer within the material, helping to mitigate the effects of Na doping. + Lattice volume changes caused by insertion / extraction and Mn 3+ The Jahn-Teller effect. Where, when Ti... 4+ When the doping amount is 0.15~0.2, the conductivity and structural stability of the material can be further improved, thereby further improving its specific capacity, rate performance and cycle stability.
[0062] (3) This application improves the surface / interface electronic conductivity of the material and suppresses side reactions between the bimetallic ion-doped manganese-based mixed phosphate and the electrolyte by coating at least part of the surface of the bimetallic ion-doped manganese-based mixed phosphate core with a carbon coating layer. Attached Figure Description
[0063] Figure 1This is a schematic diagram of the process flow for preparing the bimetallic ion-doped manganese-based mixed phosphate material provided in this application.
[0064] Figure 2 These are XRD comparison images of the bimetallic / monometallic ion-doped manganese-based mixed phosphate materials provided in Examples 1-2 and Comparative Examples 1-3 of this application.
[0065] Figure 3 These are SEM images of the bimetallic ion-doped manganese-based mixed phosphate materials provided in Examples 1-2 and Comparative Examples 2-3 of this application.
[0066] Among them, (a) - Example 1, (b) - Example 2, (c) - Comparative Example 2, and (d) - Comparative Example 3. Detailed Implementation
[0067] The technical solution of this application will be further described below through specific embodiments. Those skilled in the art should understand that the embodiments described are merely to help understand this application and should not be regarded as specific limitations on this application.
[0068] The scope of this application can be defined by lower and upper limits. The selected lower and upper limits define the boundaries of a specific range. The range defined in this way can be defined by the inclusion or exclusion of endpoints. Any endpoint can be independently selected for inclusion or exclusion, and all lower and upper limits can be arbitrarily combined to form new ranges. That is, any lower limit can be combined with any upper limit to form a valid range. For example, if the ranges of 60~120 and 80~110 are listed for specific parameters, it should be understood that the ranges of 60~110 and 80~120 also fall within the scope of this application. In addition, if the minimum range values 1 and 2 are listed, and the maximum range values 3, 4 and 5 are also listed, then all ranges of 1~3, 1~4, 1~5, 2~3, 2~4 and 2~5 fall within the scope of this application. In this application, the numerical range "a~b" represents a shortened representation of any combination of real numbers between a and b, where a and b are both real numbers. For example, the numerical range "0~5" means that all real numbers between 0 and 5 have been fully listed in this document, and "0~5" is only a shortened representation of this set of numerical combinations. When a parameter is expressed as an integer ≥2, it is equivalent to listing positive integers that meet the requirements, such as 2, 3, 4, 5, 6, 7, 8, 9, 10, etc. When a parameter is expressed as an integer selected from "2~10", it is equivalent to listing any integer among 2, 3, 4, 5, 6, 7, 8, 9, and 10.
[0069] Unless otherwise specified, the term "at least two combinations" in this application refers to a quantity greater than or equal to 2. For example, "any one or at least two combinations" means any one of the listed items, or a combination of at least two of the listed items in a manner that does not conflict and enables the implementation of this application.
[0070] In this application, unless otherwise specified, the features or solutions corresponding to "and / or" cover any one of two or more related listed items, as well as any and all combinations of the related listed items. These arbitrary and all combinations include any two related listed items, any more related listed items, or a combination of all related listed items. For example, "A and / or B" represents a set consisting of A, B, and combinations of A and B. "Including A and / or B" can be understood, depending on the context of the statement, as including A, including B, or including both A and B. In this application, "optional" means that the corresponding feature, component, step, or solution is not essential, i.e., selected from either "present" or "absent" parallel solutions. If multiple "optional" limitations appear in a technical solution, unless otherwise specified and without technical conflict or mutual constraint, each "optional" limitation is independent and does not affect the others.
[0071] In this application, technical features or solutions described using open-ended terms such as "comprising" or "including" do not exclude additional non-conflicting elements beyond those listed unless otherwise specified. They are considered to disclose both closed-ended features or solutions consisting solely of the listed elements and open-ended features or solutions that may include additional non-conflicting elements beyond those listed. For example, if A includes a1, a2, and a3, unless otherwise specified, this means that A may consist only of a1, a2, and a3, or it may include other non-conflicting elements based on a1, a2, and a3. This corresponds to the disclosure of technical solutions such as "A consists of a1, a2, and a3," "A is selected from a1, a2, and a3," and "A not only includes a1, a2, and a3, but may also include other non-conflicting elements."
[0072] All embodiments and optional embodiments of this application, unless otherwise specified and without technical conflict, can be combined to form new technical solutions, and such combinations fall within the scope of this application. The term "embodiment" mentioned in this application means that a specific feature, structure, or characteristic described in connection with an embodiment can be included in at least one embodiment or implementation of this application. The appearance of this phrase in various positions in the specification does not necessarily refer to the same embodiment, nor is it an independent or alternative embodiment mutually exclusive with other embodiments. Those skilled in the art can explicitly and implicitly understand that the embodiments described in this application can be combined with other embodiments without technical conflict.
[0073] In this application, the ordinal numbers “first,” “second,” “third,” and “fourth” used in expressions such as “first aspect,” “second aspect,” “third aspect,” and “fourth aspect” are used for descriptive purposes only and should not be construed as indicating or implying relative importance or quantity, nor should they be construed as implicitly indicating the importance or quantity of the indicated technical features. They serve only as a non-exhaustive enumeration and do not constitute a closed limitation on quantity.
[0074] In this application, the order in which the steps are written in the methods described in the various embodiments does not imply a strict execution order. The actual execution order of each step should be determined according to its function and possible internal logic. Unless otherwise specified, all steps in this application can be executed in the order they are written, or in any order without technical conflict. For example, if the method includes steps (a) and (b), it means that the method may include steps (a) and (b) executed sequentially, or it may include steps (b) and (a) executed sequentially. If the method also includes step (c), then step (c) can be added to the method in any order without conflict, including but not limited to the execution order of steps (a), (b), and (c), steps (a), (c), and (b), steps (c), (a), and (b), etc.
[0075] Figure 1 This is a schematic diagram of the process flow for preparing the bimetallic ion-doped manganese-based mixed phosphate material provided in this application. The process includes the following steps: adding sodium, manganese, iron, titanium, and phosphorus sources to a solvent in stoichiometric ratios; adding a carbon source and mixing; then spray drying followed by segmented calcination to obtain the bimetallic ion-doped manganese-based mixed phosphate material.
[0076] Example 1
[0077] This embodiment provides a bimetallic ion-doped manganese-based mixed phosphate material with the general chemical formula Na₄Mn. 1.65 Fe 1.2 Ti 0.15 (PO4)2P2O7 / C; it includes Na4Mn 1.65 Fe 1.2 Ti 0.15 (PO4)2P2O7 core and located in Na4Mn 1.65 Fe 1.2 Ti 0.15 (PO4)2P2O7 has a carbon coating layer on at least part of its surface, with a carbon coating layer mass fraction of 6 wt%; and its particle size distribution is 3 μm to 8 μm.
[0078] The preparation method of the bimetallic ion-doped manganese-based mixed phosphate material provided in this embodiment includes the following steps:
[0079] (1) Combine Na4P2O7, Mn(CH3COO)2·4H2O, Fe(NO3)3·9H2O, C 16 H 36 O4Ti and NH4H2PO4 were added to an appropriate amount of 0.5mol / L nitric acid solution in stoichiometric ratio, followed by the addition of C6H8O7·H2O. The mixture was then magnetically stirred for 2 hours and ultrasonically dispersed for 2 hours to obtain a mixed solution.
[0080] Among them, the molar amount of C6H8O7·H2O is related to that of Mn(CH3COO)2·4H2O, Fe(NO3)3·9H2O and C 16 H 36 The total molar ratio of O4Ti is 1:1.
[0081] (2) The mixed solution is spray-dried and then placed in a forced-air drying oven and dried at 60°C for 2 hours until the residual moisture is completely evaporated. Finally, it is ground to obtain the precursor.
[0082] During spray drying, the equipment's inlet air temperature is set to 220℃, the outlet air temperature to 110℃, and the feed rate to 300mL / h.
[0083] (3) The precursor was placed in a tube furnace and heated to 350°C at 2°C / min and held for 6 hours in a nitrogen atmosphere. Then it was heated to 650°C at 2°C / min and held for 10 hours. After cooling in the furnace, a bimetallic ion-doped manganese-based mixed phosphate material was obtained.
[0084] Example 2
[0085] This embodiment provides a bimetallic ion-doped manganese-based mixed phosphate material with the general chemical formula Na₄Mn. 1.6 Fe 1.2 Ti 0.2 (PO4)2P2O7 / C; it includes Na4Mn 1.6 Fe 1.2 Ti 0.2 (PO4)2P2O7 / C core and located in Na4Mn 1.6 Fe 1.2 Ti 0.2 (PO4)2P2O7 / C has a carbon coating layer on at least part of its surface, with a carbon coating layer mass fraction of 5 wt% and a particle size distribution of 3 μm to 8 μm.
[0086] The preparation method of the bimetallic ion-doped manganese-based mixed phosphate material provided in this embodiment includes the following steps:
[0087] (1) Combine CH3COONa·3H2O, MnC2O4·2H2O, FeC2O4·2H2O, C 16 H36 O4Ti and NH4H2PO4 were added to an appropriate amount of 0.8 mol / L nitric acid solution in stoichiometric ratio, followed by the addition of C6H4PO4. 12 O6 was used to magnetically stir for 1 hour and ultrasonically disperse for 3 hours to obtain a mixed solution.
[0088] Among them, C6H 12 The molar amount of O6 is related to MnC2O4·2H2O, FeC2O4·2H2O, and C. 16 H 36 The total molar ratio of O4Ti is 0.8:1.
[0089] (2) The mixed solution is spray-dried and then placed in a forced-air drying oven and dried at 100°C for 1 hour until the residual moisture is completely evaporated. Finally, it is ground to obtain the precursor.
[0090] During spray drying, the equipment's inlet air temperature is set at 225℃, the outlet air temperature at 115℃, and the feed rate at 320mL / h.
[0091] (3) The precursor was placed in a tube furnace and heated to 320°C at 2.5°C / min and held for 7 hours in a nitrogen atmosphere. Then it was heated to 620°C at 2.5°C / min and held for 12 hours. After cooling in the furnace, a bimetallic ion-doped manganese-based mixed phosphate material was obtained.
[0092] Example 3
[0093] This embodiment provides a bimetallic ion-doped manganese-based mixed phosphate material with the general chemical formula Na₄Mn. 1.62 Fe 1.2 Ti 0.18 (PO4)2P2O7 / C; it includes Na4Mn 1.62 Fe 1.2 Ti 0.18 (PO4)2P2O7 core and located in Na4Mn 1.62 Fe 1.2 Ti 0.18 (PO4)2P2O7 has a carbon coating layer on at least part of its surface, with a carbon coating layer mass fraction of 8 wt%; and its particle size distribution is 3 μm to 8 μm.
[0094] The preparation method of the bimetallic ion-doped manganese-based mixed phosphate material provided in this embodiment includes the following steps:
[0095] (1) Combine Na2C2O4, Mn(NO3)2·4H2O, FePO4·2H2O, C 16 H 36O4Ti and NaH2PO4 were added to an appropriate amount of 1mol / L nitric acid solution in stoichiometric ratio, followed by the addition of H2C2O4·2H2O. The mixture was then magnetically stirred for 3 hours and ultrasonically dispersed for 1 hour to obtain a mixed solution.
[0096] Among them, the molar amount of H2C2O4·2H2O is related to that of Mn(NO3)2·4H2O, FePO4·2H2O and C 16 H 36 The total molar ratio of O4Ti is 1.2:1.
[0097] (2) The mixed solution is spray-dried and then placed in a forced-air drying oven and dried at 80°C for 3 hours until the residual moisture is completely evaporated. Finally, it is ground to obtain the precursor.
[0098] During spray drying, the equipment's inlet air temperature is set at 215℃, the outlet air temperature at 105℃, and the feed rate at 280mL / h.
[0099] (3) The precursor was placed in a tube furnace and heated to 380°C at 3°C / min and held for 4 hours in a nitrogen atmosphere. Then it was heated to 680°C at 3°C / min and held for 8 hours. After cooling with the furnace, a bimetallic ion-doped manganese-based mixed phosphate material was obtained.
[0100] Example 4
[0101] This embodiment provides a bimetallic ion-doped manganese-based mixed phosphate material, which is the same as that in Example 1 except that the mass fraction of the carbon coating layer is adjusted to 2 wt%.
[0102] The bimetallic ion-doped manganese-based mixed phosphate material provided in this embodiment, except that the molar amount of C6H8O7·H2O in step (1) is the same as that of Mn(CH3COO)2·4H2O, Fe(NO3)3·9H2O and C 16 H 36 Except for adjusting the total molar ratio of O4Ti to 0.5:1, everything else is the same as in Example 1.
[0103] Example 5
[0104] This embodiment provides a bimetallic ion-doped manganese-based mixed phosphate material, which is the same as that in Example 1 except that the mass fraction of the carbon coating layer is adjusted to 10 wt%.
[0105] The bimetallic ion-doped manganese-based mixed phosphate material provided in this embodiment, except that the molar amount of C6H8O7·H2O in step (1) is the same as that of Mn(CH3COO)2·4H2O, Fe(NO3)3·9H2O and C 16 H 36Except for adjusting the total molar ratio of O4Ti to 1.5:1, everything else is the same as in Example 1.
[0106] Comparative Example 1
[0107] This comparative example provides a single-metal ion-doped manganese-based mixed phosphate material, except that its general chemical formula is Na₄Mn. 1.8 Fe 1.2 Except for (PO4)2P2O7 / C, everything else is the same as in Example 1.
[0108] The single-metal ion-doped manganese-based mixed phosphate material provided in this comparative example, except that C is not added in step (1). 16 H 36 Except for the addition of O4Ti and the amount of Mn(CH3COO)2·4H2O adjusted according to the stoichiometric ratio, everything else is the same as in Example 1.
[0109] Comparative Example 2
[0110] This comparative example provides a bimetallic ion-doped manganese-based mixed phosphate material, except that its general chemical formula is Na4Mn. 1.7 Fe 1.2 Ti 0.1 Except for (PO4)2P2O7 / C, everything else is the same as in Example 1.
[0111] The bimetallic ion-doped manganese-based mixed phosphate material provided in this comparative example, except for step (1) where Mn(CH3COO)2·4H2O and C are adjusted according to stoichiometric ratio, is... 16 H 36 Except for the amount of O4Ti added, everything else is the same as in Example 1.
[0112] Comparative Example 3
[0113] This comparative example provides a bimetallic ion-doped manganese-based mixed phosphate material, except that its general chemical formula is Na4Mn. 1.5 Fe 1.2 Ti 0.3 Except for (PO4)2P2O7 / C, everything else is the same as in Example 1.
[0114] The bimetallic ion-doped manganese-based mixed phosphate material provided in this comparative example, except for step (1) where Mn(CH3COO)2·4H2O and C are adjusted according to stoichiometric ratio, is... 16 H 36 Except for the amount of O4Ti added, everything else is the same as in Example 1.
[0115] Comparative Example 4
[0116] This comparative example provides a bimetallic ion-doped manganese-based mixed phosphate material, except that its general chemical formula is Na4Mn. 1.65 Fe 1.2 Ti 0.15 (PO4)2P2O7, that is, except for the carbon coating layer, everything else is the same as in Example 1.
[0117] The bimetallic ion-doped manganese-based mixed phosphate material provided in this comparative example is the same as that in Example 1, except that C6H8O7·H2O is not added in step (1).
[0118] Comparative Example 5
[0119] This comparative example provides a single-metal ion-doped manganese-based mixed phosphate material, except that its general chemical formula is Na₄Mn. 2.1 Fe 0.9 Except for (PO4)2P2O7 / C, everything else is the same as in Comparative Example 1.
[0120] The single-metal ion-doped manganese-based mixed phosphate material provided in this comparative example is the same as that in Comparative Example 1, except that the amount of Mn(CH3COO)2·4H2O and Fe(NO3)3·9H2O added is adjusted according to the stoichiometric ratio in step (1).
[0121] Comparative Example 6
[0122] This comparative example provides a single-metal ion-doped manganese-based mixed phosphate material, except that its general chemical formula is Na₄Mn. 1.5 Fe 1.5 Except for (PO4)2P2O7 / C, everything else is the same as in Comparative Example 1.
[0123] The single-metal ion-doped manganese-based mixed phosphate material provided in this comparative example is the same as that in Comparative Example 1, except that the amount of Mn(CH3COO)2·4H2O and Fe(NO3)3·9H2O added is adjusted according to the stoichiometric ratio in step (1).
[0124] Figure 2 These are XRD comparison images of the bimetallic / monometallic ion-doped manganese-based mixed phosphate materials provided in Examples 1-2 and Comparative Examples 1-3. It can be seen that the XRD spectra of the five materials are similar, all exhibiting obvious characteristic peaks, and corresponding well to the standard card (PDF#97-009-2836) of Na4Mn3(PO4)2P2O7, indicating that Fe... 2+ and Ti 4+ After replacing some Mn sites, the crystal structure of the material remains unchanged, still belonging to the orthorhombic crystal system, space group Pn21a. Furthermore, due to Ti... 4+ The ionic radius (0.68 Å) and Mn2+ The ionic radii (0.80 Å) of Ti differ significantly, with Ti... 4+ With increasing doping concentration, the diffraction peaks shift to the right overall. According to Bragg's equation sinθ = nλ / 2d, as the diffraction angle θ increases, the corresponding interplanar spacing d decreases, i.e., Ti... 4+ The doping of Ti leads to a decrease in the interplanar spacing of the material, indicating that Ti 4+ Successfully doped and replaced some Mn sites and incorporated them into the NMPP crystal structure.
[0125] Figure 3 These are SEM images of the bimetallic ion-doped manganese-based mixed phosphate materials provided in Examples 1-2 and Comparative Examples 2-3. It can be seen that the four materials have roughly the same microstructure, consisting of irregularly sized micron-sized spherical or quasi-spherical particles with a particle size distribution ranging from 3 μm to 8 μm.
[0126] The materials provided in Examples 1-5 and Comparative Examples 1-6 were precisely weighed with acetylene black (conductive agent) and polyvinylidene fluoride (binder) at a mass ratio of 80:15:5. N-methylpyrrolidone (solvent) was added, and the mixture was continuously mechanically ball-milled in a planetary ball mill at a speed of 300 r / min for 4 hours to form a stable slurry system. This slurry system was then uniformly and smoothly coated onto the surface of carbon-coated aluminum foil. Subsequently, it was dried in a 60°C forced-air drying oven for 6 hours to initially remove volatile components, and then dried in a 110°C vacuum oven for 12 hours. After naturally cooling to room temperature, it was cut into tablets with a diameter of 12 mm and a surface density of approximately 2 mg / cm³ using a tablet press. 2 The standard circular electrode sheet is used as the positive electrode sheet.
[0127] In an argon atmosphere glove box with strict oxygen and humidity control (H2O < 1ppm, O2 < 1ppm), assemble the CR2032 button half cell in the following order: with the positive electrode shell as the base, stack the positive electrode plates, then place the glass fiber separator, inject sodium electrolyte, stack the metallic sodium negative electrode, stainless steel gasket, and wave spring sheet, and finally cover with the negative electrode shell to seal and form the cell.
[0128] The sodium-containing electrolyte consists of a 1:1 volume ratio of EC / DMC mixed organic solvent, 5 wt% FEC additive, and 1 mol / L NaClO4 sodium salt.
[0129] After the assembled CR2032 button cell was left to stand at room temperature until the open-circuit voltage stabilized, the electrochemical performance was tested, with the voltage test range being 1.5V~4.4V.
[0130] The test results are shown in Tables 1 and 2.
[0131]
[0132]
[0133] As can be seen from Tables 1 and 2, the bimetallic ion-doped manganese-based mixed phosphate materials provided in Examples 1 to 3 exhibit high specific capacity, excellent rate performance, and cycle stability when used as active materials for positive electrode sheets in sodium-ion batteries.
[0134] Compared to Example 1, Examples 4 and 5 adjusted the amount of carbon source added, resulting in a carbon coating mass fraction outside the range of 5wt% to 8wt%, which led to a decrease in specific capacity, rate performance, and cycle stability. This indicates that when the carbon coating mass fraction is too low, it is difficult to form a continuous and complete carbon conductive layer on the particle surface, limiting the improvement in material conductivity and making it impossible to construct an effective conductive network. Simultaneously, the carbon layer provides insufficient protection for the active material, allowing the electrolyte to directly contact the active material, exacerbating manganese ion dissolution. During charge and discharge, the lattice deformation is not effectively buffered, and the crystal structure is easily damaged, resulting in a decrease in the material's rate performance and cycle stability. When the carbon coating mass fraction is too high, the proportion of non-sodium-storing active carbon components is too high, diluting the active material and reducing the material's specific capacity and energy density. An excessively thick carbon layer also increases sodium ion diffusion resistance, degrades powder tap density and electrode processing performance, and easily induces additional electrolyte side reactions, reducing the initial coulombic efficiency.
[0135] Compared to Example 1, Comparative Examples 1, 5, and 6 only doped NMPP materials with Fe. 2+ Undoped Ti 4+ While its specific capacity and rate performance decreased slightly, its cycling performance decreased significantly. This indicates that the high valence state of Ti allows it to generate Na vacancies within the material through charge compensation, which is conducive to the rapid transport of ions / electrons. This achieves overall charge balance and improves the conductivity of the material from within, thereby further enhancing specific capacity and rate performance. Simultaneously, the Ti-O bond strength is higher than that of the Fe-O and Mn-O bonds, and Ti is an inert element, which can act as a support and buffer in the material, significantly mitigating the Na vacancies. + Lattice volume changes caused by insertion / extraction and Mn 3+ The Jahn-Teller effect can significantly improve structural stability and cyclic stability.
[0136] Furthermore, compared to Comparative Example 1, Comparative Examples 5 and 6 doped NMPP materials with Fe. 2+ Insufficient or excessive doping of Fe results in a decrease in specific capacity, rate performance, and cycle stability. This indicates that when the Mn / Fe molar ratio is 6:4 (Fe... 2+ When the Fe doping level is 1.2%, the material can possess both excellent conductivity and structural stability, thereby improving its specific capacity, rate performance, and cycle stability. And when Fe...2+ When the doping amount is too low (e.g., 1.0), Fe 2+ Insufficient lattice regulation makes it difficult to effectively suppress Mn. 3+ The Jahn-Teller distortion provides limited improvement in lattice structure stability, while the increase in electronic conductivity is small, resulting in significant charge-discharge polarization and poor rate performance and cycle stability of the material; when Fe 2+ When the doping amount is too high (e.g., 1.5), excess Fe... 2+ It can easily cause lattice distortion, generate impurities, destroy the original crystal structure, crowd out sodium storage active sites, reduce the reversible specific capacity of the material, and exacerbate the structural degradation during the charge and discharge process, leading to a decrease in cycle stability.
[0137] Compared with Example 1, Comparative Examples 2 and 3 showed differences in Fe 2+ Under the same doping amount, doping Ti into NMPP material 4+ When Ti is doped too little or too much, its specific capacity, rate performance, and cycle stability all decrease significantly. This indicates that when Ti... 4+ When the doping amount of Ti is 0.15~0.2%, the conductivity and structural stability of the material can be further improved, thereby further enhancing its specific capacity, rate performance, and cycle stability. And when Ti... 4+ When the doping amount is too low (e.g., 0.1), high-priced Ti... 4+ Insufficient lattice regulation makes it difficult to effectively broaden sodium ion diffusion channels and buffer Mn during charging and discharging. 3+ The Jahn-Teller distortion caused by this process results in limited improvement in the material's ion transport performance and structural stability, with no significant improvement in electronic conductivity and excessive charge-discharge polarization, leading to lower-than-expected rate performance and cycle stability. 4+ When the doping amount is too high (e.g., 0.3), excessive high-valence Ti will result in an excess of high-valence Ti. 4+ This can cause excessive lattice distortion, easily leading to the formation of titanate impurities at grain boundaries, disrupting the integrity of the original phosphate crystal structure, and simultaneously causing excessive Ti... 4+ It will crowd out the sodium storage active sites of Mn and Fe, reduce the reversible specific capacity of the material, and exacerbate the accumulation of lattice stress during the charge and discharge process, accelerate structural collapse, and lead to a significant deterioration in cycle performance.
[0138] Compared to Example 1, Comparative Example 4, which did not include a carbon source to obtain a carbon coating layer, showed a significant decrease in specific capacity, rate performance, and cycle stability. This indicates that coating at least part of the surface of the bimetallic ion-doped manganese-based mixed phosphate core with a carbon coating layer is beneficial for improving the surface / interface electronic conductivity of the material and suppressing side reactions between the bimetallic ion-doped manganese-based mixed phosphate and the electrolyte.
[0139] In summary, this application achieves this by injecting Fe into the Mn sites in NMPP materials. 2+ Doping with Fe, an element with similar physicochemical properties and ionic radii to Mn, and its superior stability, can reduce the proportion of Mn while stabilizing the crystal structure, thus reducing the Mn content. 3+ The Jahn-Teller effect enhances the electronic conductivity of the material from within. Specifically, when the Mn / Fe molar ratio is 6:4 (Fe... 2+ When the doping amount is 1.2%, the material can have both excellent conductivity and structural stability, thereby improving its specific capacity, rate performance and cycle stability.
[0140] This application involves Ti injection into Mn sites in NMPP materials. 4+ Doping with Ti allows it to generate Na vacancies within the material through charge compensation, which facilitates rapid ion / electron transport. This achieves overall charge balance and improves the material's conductivity from within. Furthermore, the Ti-O bond is stronger than the Fe-O and Mn-O bonds, and Ti, being an inert element, acts as a support and buffer within the material, helping to mitigate the effects of Na doping. + Lattice volume changes caused by insertion / extraction and Mn 3+ The Jahn-Teller effect. Where, when Ti... 4+ When the doping amount is 0.15~0.2, the conductivity and structural stability of the material can be further improved, thereby further improving its specific capacity, rate performance and cycle stability.
[0141] This application improves the surface / interface electronic conductivity of the material and suppresses side reactions between the bimetallic ion-doped manganese-based mixed phosphate and the electrolyte by coating at least part of the surface of the bimetallic ion-doped manganese-based mixed phosphate core with a carbon coating layer.
[0142] The applicant declares that the above description is only a specific implementation of this application, but the protection scope of this application is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily conceived by those skilled in the art within the scope of the technology disclosed in this application fall within the protection and disclosure scope of this application.
Claims
1. A bimetallic ion-doped manganese-based mixed phosphate material, characterized in that, The chemical formula of the bimetallic ion-doped manganese-based mixed phosphate material is Na₄Mn₄. 1.8-x Fe 1.2 Ti x (PO4)2P2O7 / C, 0.15≤x≤0.2; The bimetallic ion-doped manganese-based mixed phosphate material includes a bimetallic ion-doped manganese-based mixed phosphate core and a carbon coating layer located on at least a portion of the surface of the bimetallic ion-doped manganese-based mixed phosphate core.
2. The bimetallic ion-doped manganese-based mixed phosphate material according to claim 1, characterized in that, In the bimetallic ion-doped manganese-based mixed phosphate material, the mass fraction of the carbon coating layer is 5wt%~8wt%.
3. The bimetallic ion-doped manganese-based mixed phosphate material according to claim 1 or 2, characterized in that, The particle size distribution of the bimetallic ion-doped manganese-based mixed phosphate material is 3 μm to 8 μm.
4. A method for preparing a bimetallic ion-doped manganese-based mixed phosphate material as described in any one of claims 1 to 3, characterized in that, Includes the following steps: Sodium, manganese, iron, titanium, and phosphorus sources were added to a solvent in stoichiometric ratios, and a carbon source was added. The mixture was then sequentially mixed, spray-dried, and calcined in stages to obtain the bimetallic ion-doped manganese-based mixed phosphate material.
5. The preparation method according to claim 4, characterized in that, The sodium source includes any one or a combination of at least two of sodium pyrophosphate, sodium oxalate, or sodium acetate. And / or, the manganese source includes any one or a combination of at least two of manganese acetate, manganese oxalate, or manganese nitrate; And / or, the iron source includes any one or a combination of at least two of ferric nitrate, ferric phosphate, or ferrous oxalate; And / or, the titanium source includes tetrabutyl titanate; And / or, the phosphorus source includes sodium dihydrogen phosphate and / or ammonium dihydrogen phosphate; And / or, the solvent includes a nitric acid solution; And / or, the carbon source includes any one or a combination of at least two of citric acid, glucose, sucrose or oxalic acid; And / or, the molar ratio of the carbon source to the total molar ratio of the manganese source, the iron source and the titanium source is (0.8~1.2):
1.
6. The preparation method according to claim 4 or 5, characterized in that, The mixing includes ultrasonic dispersion and / or magnetic stirring; And / or, the segmented calcination includes a first calcination and a second calcination.
7. The preparation method according to claim 6, characterized in that, The mixing time is 2h~4h; And / or, the ultrasonic dispersion time is 1h to 4h; And / or, the magnetic stirring time is 1h to 4h; And / or, the atmosphere for the first calcination and the second calcination is independently nitrogen and / or argon, respectively; And / or, the heating rate of the first calcination is 2℃ / min to 3℃ / min; And / or, the temperature of the first calcination is 320℃~380℃; And / or, the holding time for the first calcination is 4h~7h; And / or, the heating rate of the second calcination is 2℃ / min to 3℃ / min; And / or, the second calcination temperature is 620℃~680℃; And / or, the holding time for the second calcination is 8h~12h.
8. The preparation method according to any one of claims 4 to 7, characterized in that, The inlet air temperature for the spray drying is 215℃~225℃; And / or, the outlet air temperature of the spray dryer is 105℃~115℃; And / or, the feed rate of the spray dryer is 280 mL / h to 320 mL / h.
9. A positive electrode sheet, characterized in that, The positive electrode comprises the bimetallic ion-doped manganese-based mixed phosphate material as described in any one of claims 1 to 3.
10. A sodium-ion battery, characterized in that, The sodium-ion battery includes the positive electrode as described in claim 9.
Citation Information
Patent Citations
Carbon-coated sodium manganese phosphate pyrophosphate@SWCNT (Single Walled Carbon Nanotube) composite material with net structure and preparation and application thereof
CN110085849A
Iron-manganese-based mixed phosphate micro-nano secondary sphere as well as preparation method and application thereof
CN121698318A