A lithium iron phosphate-ternary hybrid cathode slurry, its preparation method, and a power battery
By employing premixing dispersion, separate dissolution of conductive binders, vacuum homogenization and degassing processes, and the use of polyether-type block copolymers, the dispersion problem of lithium manganese iron phosphate and ternary materials was solved, resulting in a positive electrode slurry with high safety and high energy density, thus improving the battery's electrical performance and cycle life.
Patent Information
- Application Number
- CN202611567327.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-10-10
- Publication Date
- 2026-11-17
AI Technical Summary
Existing technologies cannot simultaneously achieve the high safety and high energy density of lithium manganese iron phosphate and ternary cathode materials, resulting in poor dispersion of cathode slurry, insufficient battery consistency and cycle life.
A step-by-step process of premixing and dispersion, separate dissolution of conductive binder, and vacuum homogenization and degassing is adopted, combined with polyether block copolymer dispersant, to optimize the material ratio, form a uniform conductive network, and prevent the active material from stratifying and agglomerating.
It improves the dispersion uniformity and conductivity of the positive electrode slurry, reduces interfacial impedance, and enhances the energy density and cycle performance of the battery.
Smart Images

Figure SMS_2
Abstract
Description
Technical Field
[0001] This invention relates to the field of lithium-ion cathode material technology, and in particular to a lithium manganese iron phosphate-ternary hybrid cathode slurry, its preparation method, and a power battery. Background Technology
[0002] With the rapid development of the new energy vehicle industry, the comprehensive performance requirements for power batteries are becoming increasingly stringent. High energy density is needed not only to meet range demands but also high safety to ensure reliable operation. The selection and design of the cathode material is one of the main factors determining the performance of lithium-ion power batteries. Lithium manganese iron phosphate (LFP) cathode material is a new type of cathode material obtained by doping a large amount of manganese into LFP cathode material. It inherits the advantages of high safety and long cycle life of LFP, effectively improving the voltage platform and energy density. However, the inherent olivine structure of LFP results in low electronic conductivity and a low ion diffusion coefficient. When used alone as a cathode material, its rate performance in power batteries is poor, making it difficult to meet fast-charging requirements.
[0003] Ternary cathode materials have a layered structure, which can ensure efficient conduction of electrons and ions and have high conductivity. However, ternary cathode materials have poor thermal stability and insufficient safety. During charging and discharging, they are prone to generating gas. When the generated oxygen comes into contact with the flammable electrolyte in the battery, a violent chemical reaction occurs and heat is released. If heat dissipation is not timely, thermal runaway can easily occur, posing a significant safety hazard.
[0004] To achieve complementary performance, existing technologies often blend lithium manganese iron phosphate (LMP) with ternary cathode materials. However, the preparation process of the slurry in existing technologies is simple and crude, mostly using direct mechanical stirring. However, the tap density of LMP and ternary materials differs significantly, and their particle size distributions are also different. This leads to severe stratification or agglomeration of the two active materials during the preparation and coating of the cathode slurry, when the mechanical stirring shear force is insufficient to overcome the gravitational sedimentation effect. Consequently, the distribution of active materials on the cathode sheet is uneven, resulting in poor battery consistency. Furthermore, the poor dispersibility of the obtained cathode slurry leads to a significant increase in interfacial impedance, affecting the lithium-ion transport efficiency and accelerating the degradation rate of battery cycle life.
[0005] Alternatively, lithium manganese iron phosphate can be first coated onto the ternary material using a high-speed mixer via a dry coating process to form a composite material, which is then used to fabricate the electrode sheets using conventional stirring processes. While this method offers high safety performance, the lack of a conductive network covering the coated area results in higher battery resistance and poorer electrical performance. Furthermore, an improper composition ratio of the blended cathode slurry makes it difficult to fully leverage the synergistic effect of the two materials, failing to achieve a balance between high safety and high energy density.
[0006] Therefore, obtaining a positive electrode slurry with high conductivity, good dispersibility, and a balance between high safety and high energy density is of great significance for improving the consistency and cycle life of power batteries. Summary of the Invention
[0007] The purpose of this invention is to provide a lithium manganese iron phosphate-ternary blended cathode slurry, its preparation method, and a power battery, so as to solve the technical problem that it is difficult to simultaneously achieve high safety and high energy density in the prior art, and to obtain a cathode slurry with uniform dispersion and good conductivity.
[0008] The technical problem to be solved by this invention can be achieved through the following technical solution: In a first aspect, the present invention provides a method for preparing a lithium manganese iron phosphate-ternary blended cathode slurry, comprising the following process steps: S1. Mix lithium manganese iron phosphate and nickel cobalt manganese ternary materials and add them to 10-15% solvent, stir and disperse for 30-60 minutes to obtain a premixed slurry; S2. Add conductive agent and binder to the remaining solvent, and shear and disperse for 1-2 hours to obtain conductive binder slurry; S3. Add conductive binder slurry to the premixed slurry, stir at 800-1000 r / min for 1-2 h, and then vacuum homogenize at 1000-1500 r / min for 2-3 h under a vacuum of -0.08--0.1 MPa to obtain lithium iron phosphate-ternary mixed cathode slurry.
[0009] Preferably, the molar ratio of lithium manganese iron phosphate to nickel cobalt manganese ternary material is (7.5-8.5):(1.5-2.5).
[0010] More preferably, the molar ratio of lithium manganese iron phosphate to nickel cobalt manganese ternary material is 8:2.
[0011] Preferably, the lithium manganese iron phosphate-ternary blended cathode slurry comprises the following raw materials in parts by weight: 115-135 parts of lithium manganese iron phosphate, 14-24 parts of nickel-cobalt-manganese ternary material, 1-3 parts of conductive agent, 2-4 parts of binder, and 35-45 parts of solvent.
[0012] More preferably, the nickel-cobalt-manganese ternary material includes one or more combinations of NCM523, NCM622 and NCM811.
[0013] More preferably, the conductive agent includes one or more combinations of acetylene black, Ketjen black, and carbon nanotubes.
[0014] More preferably, the adhesive includes polyvinylidene fluoride.
[0015] More preferably, the molecular weight of polyvinylidene fluoride is 0.7 × 10⁻⁶. 6~1.2×10 6 .
[0016] More preferably, the solvent includes N-methylpyrrolidone.
[0017] Preferably, the raw materials for the lithium manganese iron phosphate-ternary blended cathode slurry have all undergone drying pretreatment.
[0018] More preferably, the drying pretreatment specifically includes: vacuum drying lithium manganese iron phosphate and nickel cobalt manganese ternary materials at 100-120°C for 8-12 hours; drying the conductive agent and adhesive at 60-80°C for 4-6 hours; and dehydrating the solvent to a moisture content ≤50ppm.
[0019] More preferably, the viscosity of the lithium manganese iron phosphate-ternary blended cathode slurry is 3.0 × 10⁻⁶. 4 ~5.0×10 4 mPa·s.
[0020] By adopting the above technical solution, in preparing the lithium manganese iron phosphate-ternary blended cathode slurry, the active material particles, namely lithium manganese iron phosphate and nickel cobalt manganese ternary materials, are first premixed with a small amount of solvent to form a slurry with high solid content. The Brownian motion of the active material particles in the solvent in the slurry is very significant, which leads to an increase in sedimentation resistance and greatly slows down the sedimentation rate of the active material particles. This effectively prevents the two active materials with different densities from stratifying and settling in the liquid phase due to the difference in gravity.
[0021] Then, the conductive agent and binder are dissolved and dispersed separately with the remaining solvent to form a conductive binder slurry. The conductive agent contained therein can be pre-stabilized and dispersed in the binder solution to form a uniform conductive colloidal solution. Subsequently, a second homogenization is performed between the conductive agent and the premixed slurry, which can make the pre-activated conductive agent uniformly coat the surface of the active material particles, forming a continuous electronic conduction path between the particles. This effectively reduces the contact resistance between the active material particles and avoids local agglomeration of the conductive agent, thus improving the overall dispersion uniformity of the positive electrode slurry.
[0022] Finally, the premixed slurry and conductive binder slurry are repeatedly stirred and dispersed. Pre-dispersion is carried out at room temperature and pressure, followed by homogenization and degassing under vacuum conditions. The vacuum environment helps to remove air bubbles introduced by stirring, thereby eliminating bubble defects and reducing pinholes or cracks formed during the coating and drying processes of the cathode sheet. This reduces the impact on cathode sheet quality, interface consistency, and battery cycle performance. Furthermore, simultaneous uniform dispersion under vacuum conditions further improves the dispersion and homogenization of active material particles, ultimately resulting in a uniform cathode slurry.
[0023] This invention effectively solves the stratification problem caused by the density difference between the two active material particles through a distribution process of premixing and dispersion, separate dissolution of conductive binder, and vacuum homogenization and degassing, resulting in a uniform and consistent distribution of active material in the obtained positive electrode sheet.
[0024] Furthermore, this invention also limits the ratio of lithium manganese iron phosphate and nickel cobalt manganese ternary materials. By optimizing the blending ratio, the high safety of lithium manganese iron phosphate and the high conductivity of ternary materials can be fully combined to improve the overall energy density.
[0025] Preferably, in step S101, a polyether-type block copolymer dispersant is also added; the polyether-type block copolymer dispersant is a polyethylene oxide-polyacrylonitrile block copolymer; the amount of polyether-type block copolymer dispersant added is 2 to 5% of the total mass of lithium manganese iron phosphate and nickel cobalt manganese ternary materials.
[0026] Preferably, the raw materials for the polyethylene oxide-polyacrylonitrile block copolymer include terminal amine polyethylene oxide prepolymer and acrylonitrile monomer in a mass ratio of 1:(0.8-1).
[0027] During the premixing and dispersion stage, due to the high solid content of the slurry, small-diameter lithium manganese iron phosphate particles will fill the gaps in the nickel-cobalt-manganese ternary material. The outer layer of the secondary particles of the ternary material is easily filled by the fine particles of lithium manganese iron phosphate, or some lithium manganese iron phosphate particles may directly adhere to the surface of the ternary material. This can easily prevent the coated ternary material from directly contacting the external conductive network, resulting in a decrease in conductivity. Although the resulting positive electrode sheet has high safety, its resistance is relatively high.
[0028] By adopting the above technical solution, this invention also introduces a polyether-type block copolymer dispersant, specifically a polyethylene oxide-polyacrylonitrile block copolymer, in the premixing and dispersion stage. The polyacrylonitrile segments in the dispersant have a strong affinity for the lithium manganese iron phosphate particles, enabling the dispersant to selectively anchor on the surface of the active material particles. The polyethylene oxide segments contain a large number of ether bonds, exhibiting good flexibility. In a solvent medium, they can form a dense steric hindrance layer around the lithium manganese iron phosphate active material particles, effectively preventing uncontrolled agglomeration or localized adsorption of the active material particles during the premixing stage.
[0029] Furthermore, by forming an adsorption barrier on the surface of lithium manganese iron phosphate, it is possible to ensure that the two active material particles can maintain a relatively independent dispersion state, effectively avoid coating, increase the effective contact area, significantly reduce interfacial resistance, and also directly improve the wettability and dispersibility of lithium manganese iron phosphate in solvents, thereby greatly reducing the possibility of aggregation between small-diameter lithium manganese iron phosphate particles.
[0030] By using a relatively independent dispersion system, the conductive agent can be uniformly distributed among the active material particles when blended with the conductive binder slurry, forming a continuous conductive network. This prevents increased resistance due to the lack of conductive pathways in certain areas. Furthermore, the polyethylene oxide segments themselves possess a certain ability to conduct lithium ions, thus providing numerous lithium ion conduction channels. The introduction of the dispersant can construct a highly efficient three-dimensional electron-ion transport network, improving electron and ion transport efficiency and thereby enhancing the electrical performance of the power battery.
[0031] Preferably, the raw materials for the polyethylene oxide-polyacrylonitrile block copolymer also include acrylamide monomer; the amount of acrylamide monomer added is 5 to 10 wt% of the mass of acrylamide monomer.
[0032] Preferably, the polyethylene oxide-polyacrylonitrile block copolymer is prepared according to the following method: Preparation of amine-terminated polyethylene oxide prepolymer: Benzaldehyde and ethanolamine were mixed under a nitrogen atmosphere and reacted at room temperature for 10–15 h, followed by vacuum distillation. Then, potassium metal was mixed and dissolved in benzene solvent. The temperature was adjusted to 60–65 °C, and the reaction was stirred to obtain an ethanolamine initiator. The ethanolamine initiator was added to ethylene oxide and reacted at 70–75 °C for 20–24 h. After end-capping to terminate the reaction, the prepolymer was dissolved in chloroform. Acetic acid was added, and the reaction was continued at room temperature with stirring for another 20–24 h to obtain the amine-terminated polyethylene oxide prepolymer. Preparation of block copolymers: Acrylonitrile monomer, acrylamide monomer and amine-terminated polyethylene oxide prepolymer are mixed in water, and an initiator is added dropwise under a nitrogen atmosphere at 40-50°C. The reaction is carried out in the dark for 2-4 hours to obtain the copolymer.
[0033] More preferably, the mass ratio of ethanolamine, benzaldehyde and potassium metal is 1:(1.7-2.0):(0.6-0.7).
[0034] More preferably, the mass ratio of ethylene oxide to ethanolamine initiator is 100:(0.5 to 1).
[0035] More preferably, the initiator includes any one of cerium ammonium nitrate, potassium persulfate, and ammonium persulfate; the amount of initiator added is 1 to 1.5% of the total mass of the monomer.
[0036] By adopting the above technical solution, the polyethylene oxide-polyacrylonitrile block copolymer of the present invention can also introduce acrylamide monomers during the preparation process, thereby introducing amide groups into the block copolymer. During the preparation process, benzaldehyde is used to protect the amino group in ethanolamine, which then reacts with metallic potassium to generate potassium alkoxide active centers, which can initiate the ring-opening polymerization of ethylene oxide. The protecting groups are then removed by acetic acid treatment to obtain an amino-terminated polyethylene oxide prepolymer. Subsequently, under the action of an initiator, acrylonitrile and acrylamide monomers undergo free radical polymerization to form the block copolymer.
[0037] The introduction of amide groups can provide stronger hydrogen bond anchoring ability, which can improve the binding force between block copolymers and lithium manganese iron phosphate particles, effectively reduce the probability of dispersant molecules desorbing from the particle surface during subsequent high-speed homogenization, thereby ensuring that the two active material particles in the cathode slurry can always maintain effective steric hindrance, significantly reduce the tendency of sedimentation and stratification of the two in the cathode slurry, and improve the viscosity stability and storage stability of the cathode slurry.
[0038] Uniformly dispersed positive electrode slurry is a prerequisite for constructing a uniform conductive network. The introduction of dispersants can effectively prevent the agglomeration of active material particles and conductive agent particles, inhibiting secondary agglomeration and forming a more efficient conductive network. During long-term charge-discharge cycles, the battery is less prone to failure due to increased local impedance, improving capacity retention and rate performance, reducing interface impedance, and resulting in a power battery that balances high safety and high energy density.
[0039] Secondly, the present invention provides a lithium manganese iron phosphate-ternary blended cathode slurry, which is prepared according to the above-mentioned preparation method of lithium manganese iron phosphate-ternary blended cathode slurry.
[0040] Thirdly, the present invention provides a power battery, including a positive electrode, a negative electrode and a separator. The positive electrode is prepared by the above-mentioned method for preparing lithium manganese iron phosphate-ternary mixed positive electrode slurry, which is uniformly coated on a carbon aluminum foil current collector, and then dried, rolled and cut.
[0041] More preferably, the coating surface density is 150–200 g / m². 2 The drying temperature is 120–150℃, and the drying time is 1–2 hours; the compacted density after roller pressing is 2.6–3.2 g / cm³. 3 .
[0042] More preferably, the raw material for the negative electrode sheet includes graphite; the raw material for the separator includes a polyethylene / polypropylene composite separator.
[0043] More preferably, the power battery is assembled according to the following method: A battery cell is obtained by winding or stacking positive electrode sheets, separators, and negative electrode sheets; the battery cell is then placed in an aluminum shell or a soft-pack shell, injected with electrolyte, sealed, and subjected to formation and aging to obtain a power battery.
[0044] The beneficial effects of this invention are: 1. The lithium manganese iron phosphate-ternary blended cathode slurry provided by this invention employs a step-by-step process of premixing and dispersion, separate dissolution of the conductive binder, and vacuum homogenization and degassing. High-solids premixing treatment suppresses the gravitational sedimentation and stratification of the two different active material particles. A three-dimensional continuous conductive network is constructed through pre-activation of the conductive agent. Finally, vacuum degassing eliminates the barrier of interfacial gases, resulting in a cathode slurry with uniform and consistent dispersion of active materials. Furthermore, the blending ratio of lithium manganese iron phosphate and ternary materials is optimized, thereby fully combining the high safety and high conductivity of both, and improving the overall energy density.
[0045] 2. The lithium manganese iron phosphate-ternary blended cathode slurry provided by this invention also introduces a polyether-type block copolymer dispersant in the premixing and dispersion stage. This dispersant can form a dense steric hindrance layer around the lithium manganese iron phosphate active material particles, ensuring that the two active material particles can maintain a relatively independent dispersion state. At the same time, the polyethylene oxide segments themselves have a certain ability to conduct lithium ions, thereby helping to build an efficient three-dimensional electron / ion transport network, improving the electron and ion transport efficiency, thereby reducing interface impedance and improving rate performance.
[0046] 3. The polyether-type block copolymer dispersant of the present invention also introduces acrylamide monomers during the preparation process, thereby introducing amide groups into the block copolymer, thereby improving dispersion stability, enhancing the uniformity of the conductive network and reducing contact resistance. Detailed Implementation
[0047] The specific embodiments of the present invention will be described in detail below, but it should be understood that the scope of protection of the present invention is not limited to the specific embodiments.
[0048] Preparation Example Preparation Example 1: A polyethylene oxide-polyacrylonitrile block copolymer was prepared according to the following method: Preparation of amine-terminated polyethylene oxide prepolymer: Under a nitrogen atmosphere, 1.8 g benzaldehyde and 1 g ethanolamine were mixed and reacted at room temperature for 12 h. Then, the mixture was distilled under reduced pressure. 0.6 g potassium metal was then mixed and dissolved in benzene solvent. The temperature was adjusted to 60 °C and the reaction was stirred to obtain the ethanolamine initiator. Add 0.8g of ethanolamine initiator to 100g of ethylene oxide, react at 70℃ for 24h, end-cap to terminate the reaction, dissolve in chloroform, add 12g of acetic acid, and continue stirring at room temperature for 24h to obtain the terminal amine polyethylene oxide prepolymer. Preparation of block copolymer: 10g of acrylonitrile monomer and 10g of the above-obtained amine-terminated polyethylene oxide prepolymer were mixed in water, and cerium ammonium nitrate was added dropwise for 1 hour under nitrogen atmosphere at 45°C. After reacting in the dark for 3 hours, the mixture was filtered, washed and dried to obtain the desired product.
[0049] Preparation Example 2 is a polyethylene oxide-polyacrylonitrile block copolymer, which differs from Preparation Example 1 only in that the amount of acrylonitrile monomer added is 8g.
[0050] Preparation Example 3 is a polyethylene oxide-polyacrylonitrile block copolymer, which differs from Preparation Example 1 only in that the amount of acrylonitrile monomer added is 5g.
[0051] Preparation Example 4 is a polyethylene oxide-polyacrylonitrile block copolymer, which differs from Preparation Example 1 only in that the amount of acrylonitrile monomer added is 12g.
[0052] Preparation Example 5: A polyethylene oxide-polyacrylonitrile block copolymer was prepared according to the following method: Preparation of amine-terminated polyethylene oxide prepolymer: Under a nitrogen atmosphere, 1.8 g benzaldehyde and 1 g ethanolamine were mixed and reacted at room temperature for 12 h. Then, the mixture was distilled under reduced pressure. 0.6 g potassium metal was then mixed and dissolved in benzene solvent. The temperature was adjusted to 60 °C and the reaction was stirred to obtain the ethanolamine initiator. Add 0.8g of ethanolamine initiator to 100g of ethylene oxide, react at 70℃ for 24h, end-cap to terminate the reaction, dissolve in chloroform, add 12g of acetic acid, and continue stirring at room temperature for 24h to obtain the terminal amine polyethylene oxide prepolymer. Preparation of block copolymer: 10g of acrylonitrile monomer, 0.7g of acrylamide monomer and 10g of the above-obtained amine-terminated polyethylene oxide prepolymer were mixed in water. Cerium ammonium nitrate was added dropwise for 1 hour under nitrogen atmosphere at 45°C. After reacting in the dark for 3 hours, the mixture was filtered, washed and dried to obtain the desired product.
[0053] Preparation Example 6 is a polyethylene oxide-polyacrylonitrile block copolymer, which differs from Preparation Example 4 only in that the amount of acrylamide monomer added is 0.5g.
[0054] Preparation Example 7 is a polyethylene oxide-polyacrylonitrile block copolymer, which differs from Preparation Example 4 only in that the amount of acrylamide monomer added is 1g.
[0055] Preparation Example 8 is a polyethylene oxide-polyacrylonitrile block copolymer, which differs from Preparation Example 4 only in that the amount of acrylamide monomer added is 1.5g.
[0056] Example Example 1: A lithium manganese iron phosphate-ternary blended cathode slurry was prepared according to the following method: S1. Pre-drying pretreatment was performed by vacuum drying lithium manganese iron phosphate particles and nickel cobalt manganese ternary material NCM523 particles at 110℃ for 10h. Then, 12.6g of lithium manganese iron phosphate and 1.9g of nickel cobalt manganese ternary material were mixed and added to 4g of N-methylpyrrolidone (moisture content ≤50ppm). The molar ratio of lithium manganese iron phosphate to nickel cobalt manganese ternary material was 8:2. The mixture was stirred and dispersed for 40min to obtain a premixed slurry. S2. Mix 0.2g of conductive agent and 0.3g of adhesive polyvinylidene fluoride (average molecular weight 1.0×10⁻⁶) 6 The mixture was dried at 70°C for 4 hours and then added to the remaining 36g of N-methylpyrrolidone (moisture content ≤50ppm). The conductive agent included carbon nanotubes and Ketjen black in a mass ratio of 1:1. After shearing and dispersing for 2 hours, a conductive adhesive slurry was obtained. S3. Add conductive binder slurry to the premixed slurry, stir at 900 r / min for 2 h, and then vacuum homogenize at 1200 r / min for 3 h under a vacuum of -0.08 MPa to obtain lithium iron phosphate-ternary blended cathode slurry.
[0057] Example 2: A lithium manganese iron phosphate-ternary blended cathode slurry, which differs from Example 1 only in that the molar ratio of lithium manganese iron phosphate to nickel cobalt manganese ternary material is 7.5:2.5; the amount of lithium manganese iron phosphate added is 11.8g; and the amount of nickel cobalt manganese ternary material NCM523 added is 2.4g.
[0058] Example 3: A lithium manganese iron phosphate-ternary hybrid cathode slurry, which differs from Example 1 only in that the molar ratio of lithium manganese iron phosphate and nickel cobalt manganese ternary material is 8.5:1.5; the amount of lithium manganese iron phosphate added is 13.4g; and the amount of nickel cobalt manganese ternary material NCM523 added is 1.4g.
[0059] Example 4: A lithium manganese iron phosphate-ternary blended cathode slurry was prepared according to the following method: S1. The lithium manganese iron phosphate particles and nickel cobalt manganese ternary material NCM523 particles were vacuum dried at 110℃ for 10h for drying pretreatment. Then, 12.6g of lithium manganese iron phosphate, 1.9g of nickel cobalt manganese ternary material and 0.4g of polyethylene oxide-polyacrylonitrile block copolymer prepared in Preparation Example 1 were mixed and added to 4g of N-methylpyrrolidone (moisture content ≤50ppm). The molar ratio of lithium manganese iron phosphate to nickel cobalt manganese ternary material was 8:2. The mixture was stirred and dispersed for 40min to obtain a premixed slurry. S2. Mix 0.2g of conductive agent and 0.3g of adhesive polyvinylidene fluoride (average molecular weight 1.0×10⁻⁶) 6The mixture was dried at 70°C for 4 hours and then added to the remaining 36g of N-methylpyrrolidone (moisture content ≤50ppm). The conductive agent included carbon nanotubes and Ketjen black in a mass ratio of 1:1. After shearing and dispersing for 2 hours, a conductive adhesive slurry was obtained. S3. Add conductive binder slurry to the premixed slurry, stir at 900 r / min for 2 h, and then vacuum homogenize at 1200 r / min for 3 h under a vacuum of -0.08 MPa to obtain lithium iron phosphate-ternary blended cathode slurry.
[0060] Example 5, a lithium manganese iron phosphate-ternary blended cathode slurry, differs from Example 4 only in that an equal amount of polyethylene oxide-polyacrylonitrile block copolymer prepared in Preparation Example 2 is used to replace the polyethylene oxide-polyacrylonitrile block copolymer prepared in Preparation Example 1.
[0061] Example 6, a lithium manganese iron phosphate-ternary blended cathode slurry, differs from Example 4 only in that the amount of polyethylene oxide-polyacrylonitrile block copolymer obtained in Preparation Example 1 added is 0.2g.
[0062] Example 7, a lithium manganese iron phosphate-ternary blended cathode slurry, differs from Example 4 only in that the amount of polyethylene oxide-polyacrylonitrile block copolymer prepared in Example 1 added is 0.5g.
[0063] Example 8, a lithium manganese iron phosphate-ternary blended cathode slurry, differs from Example 4 only in that an equal amount of polyethylene oxide-polyacrylonitrile block copolymer prepared in Preparation Example 3 is used to replace the polyethylene oxide-polyacrylonitrile block copolymer prepared in Preparation Example 1.
[0064] Example 9, a lithium manganese iron phosphate-ternary blended cathode slurry, differs from Example 4 only in that an equal amount of polyethylene oxide-polyacrylonitrile block copolymer prepared in Example 4 is used to replace the polyethylene oxide-polyacrylonitrile block copolymer prepared in Example 1.
[0065] Example 10, a lithium manganese iron phosphate-ternary blended cathode slurry, differs from Example 4 only in that an equal amount of polyethylene oxide is used to replace the polyethylene oxide-polyacrylonitrile block copolymer prepared in Example 1.
[0066] Example 11, a lithium manganese iron phosphate-ternary blended cathode slurry, differs from Example 4 only in that an equal amount of polyethylene oxide-polyacrylonitrile block copolymer prepared in Preparation Example 5 is used to replace the polyethylene oxide-polyacrylonitrile block copolymer prepared in Preparation Example 1.
[0067] Example 12, a lithium manganese iron phosphate-ternary blended cathode slurry, differs from Example 4 only in that an equal amount of polyethylene oxide-polyacrylonitrile block copolymer prepared in Preparation Example 6 is used to replace the polyethylene oxide-polyacrylonitrile block copolymer prepared in Preparation Example 1.
[0068] Example 13, a lithium manganese iron phosphate-ternary blended cathode slurry, differs from Example 4 only in that an equal amount of polyethylene oxide-polyacrylonitrile block copolymer prepared in Preparation Example 7 is used to replace the polyethylene oxide-polyacrylonitrile block copolymer prepared in Preparation Example 1.
[0069] Example 14, a lithium manganese iron phosphate-ternary blended cathode slurry, differs from Example 4 only in that an equal amount of polyethylene oxide-polyacrylonitrile block copolymer prepared in Preparation Example 8 is used to replace the polyethylene oxide-polyacrylonitrile block copolymer prepared in Preparation Example 1.
[0070] Comparative Example Comparative Example 1: A lithium manganese iron phosphate-ternary blended cathode slurry, differing from Example 1 only in that the molar ratio of lithium manganese iron phosphate to nickel cobalt manganese ternary material is 9:1; the amount of lithium manganese iron phosphate added is 14g, and the amount of nickel cobalt manganese ternary material NCM523 added is 9.5g.
[0071] Comparative Example 2, a lithium manganese iron phosphate-ternary blended cathode slurry, differs from Example 1 only in that the molar ratio of lithium manganese iron phosphate to nickel cobalt manganese ternary material is 7:3; the amount of lithium manganese iron phosphate added is 11g, and the amount of nickel cobalt manganese ternary material NCM523 added is 2.9g.
[0072] Comparative Example 3: A lithium manganese iron phosphate-ternary blended cathode slurry was prepared according to the following method: S1. The lithium manganese iron phosphate particles and nickel cobalt manganese ternary material NCM523 particles were vacuum dried at 110℃ for 10h for drying pretreatment, and then 12.6g of lithium manganese iron phosphate and 1.9g of nickel cobalt manganese ternary material were mixed to obtain a premix. S2. Mix 0.2g of conductive agent and 0.3g of adhesive polyvinylidene fluoride (average molecular weight 1.0×10⁻⁶) 6 The conductive adhesive slurry was dried at 70°C for 4 hours and then added to 40g of N-methylpyrrolidone (moisture content ≤50ppm). The conductive agent included carbon nanotubes and Ketjen black in a mass ratio of 1:1. After shearing and dispersing for 2 hours, the conductive adhesive slurry was obtained. S3. Add the premixed material to the conductive binder slurry, stir at 900 r / min for 2 h, and then vacuum homogenize at 1200 r / min for 3 h under a vacuum of -0.08 MPa to obtain the lithium iron phosphate ternary blended cathode slurry.
[0073] Comparative Example 4: A lithium manganese iron phosphate-ternary blended cathode slurry was prepared according to the following method: S1. Pre-drying pretreatment was performed by vacuum drying lithium manganese iron phosphate particles and nickel cobalt manganese ternary material NCM523 particles at 110℃ for 10h. Then, 12.6g of lithium manganese iron phosphate and 1.9g of nickel cobalt manganese ternary material were mixed and added to 4g of N-methylpyrrolidone (moisture content ≤50ppm). The molar ratio of lithium manganese iron phosphate to nickel cobalt manganese ternary material was 8:2. The mixture was stirred and dispersed for 40min to obtain a premixed slurry. S2. Mix 0.2g of conductive agent and 0.3g of adhesive polyvinylidene fluoride (average molecular weight 1.0×10⁻⁶) 6 The mixture was dried at 70℃ for 4 hours, then added to the premixed slurry along with the remaining 36g of N-methylpyrrolidone (moisture content ≤50ppm). It was stirred at 900r / min for 2 hours, and then vacuum homogenized at 1200r / min for 3 hours under a vacuum of -0.08MPa to obtain the lithium iron phosphate ternary blended cathode slurry.
[0074] Comparative Example 5: A lithium manganese iron phosphate-ternary blended cathode slurry was prepared according to the following method: Lithium manganese iron phosphate particles and nickel-cobalt-manganese ternary material NCM523 particles were pretreated by vacuum drying at 110℃ for 10h. 0.2g of conductive agent and 0.3g of binder polyvinylidene fluoride (average molecular weight 1.0×10⁻⁶) were then added. 6 The raw materials were dried at 70℃ for 4 hours, wherein the molar ratio of lithium manganese iron phosphate and nickel cobalt manganese ternary materials was 8:2, and the conductive agents included carbon nanotubes and Ketjen black in a mass ratio of 1:1. The dried raw materials were added to 40g of N-methylpyrrolidone (moisture content ≤50ppm), and stirred at 1000r / min for 2 hours to obtain lithium manganese iron phosphate-ternary mixed cathode slurry.
[0075] Performance testing Sample preparation: (1) The lithium iron phosphate-ternary hybrid cathode slurry obtained in the examples and comparative examples was uniformly coated onto carbon aluminum foil current collectors, with a coating surface density of 180 g / m². 2 Then dry at 130℃ for 1.5 hours, at 3.0 g / cm³. 3 The positive electrode sheet is obtained by compacting the density using a roller and then cutting it. (2) The positive electrode sheet, graphite negative electrode and polyethylene / polypropylene composite separator prepared by the lithium manganese iron phosphate-ternary mixed positive electrode slurry obtained in the examples and comparative examples are stacked to obtain the battery cell; then the battery cell is put into an aluminum shell, and an electrolyte is injected. The electrolyte is 1 mol / L ethylene carbonate / dimethyl carbonate / ethyl methyl carbonate electrolyte. After encapsulation and formation, the battery cell is aged to obtain the power battery.
[0076] Performance testing: 1. Peel strength test: According to the relevant records in GB / T 2792-2014 "Test method for peel strength of adhesive tape", the peel strength of the positive electrode slurry cured on the surface of the obtained positive electrode sample was tested. 2. Resistance test: The obtained positive electrode sample is tested for film resistance using an electrode resistance meter; 3. Battery performance test: (1) 3C rate performance test: At 25℃, the battery capacity was first obtained by charging and discharging at a 1C rate and recorded as C0. Then, the battery capacity was obtained by charging at a 1C rate and discharging at a 3C rate, resulting in a 3C discharge capacity C1. The battery capacity was obtained by charging at a 3C rate and discharging at a 1C rate, resulting in a 3C charge capacity C2. The 3C rate charge and discharge retention rate was calculated using the following method: ; (2) Cyclic performance test: 700 cycles of charge and discharge at 1C rate at 25℃, the specific capacity before and after the test is obtained, and the capacity retention rate is calculated.
[0077] The results of the above experiments are shown in Table 1: Table 1 Performance test results
[0078] According to Table 1, and in conjunction with Example 1, Comparative Examples 3 to 5, it can be seen that the performance of Comparative Examples 3 to 5 is significantly lower than that of Example 1. The reason may be that in Comparative Example 3, the two active material particles were directly dry-mixed, which not only easily led to the adhesion of lithium manganese iron phosphate to the surface of the ternary material, but also caused uneven distribution of active materials, resulting in decreased peel strength, increased resistance, and decreased battery performance. In Comparative Example 4, the conductive agent and binder were not mixed and dissolved first, and it was difficult to form a uniform and continuous conductive network when directly mixed with the active material, which blocked the electron transport path and led to decreased performance. In Comparative Example 5, a direct mechanical mixing method was used, which could not overcome the problem of uneven dispersion caused by the density difference of the two active material particles, and could not construct an effective conductive network.
[0079] Based on Examples 1, 2, and 3, as well as Comparative Examples 1 and 2, it can be seen that the performance of Examples 2 and 3 is slightly lower than that of Example 1, while the performance of Comparative Examples 1 and 2 is significantly lower than that of Example 1. The reason for this may be that the ratio of lithium manganese iron phosphate and nickel cobalt manganese ternary materials in Examples 2 and 3 is still within the range allowed by the process, while in Comparative Example 1, an excessive amount of lithium manganese iron phosphate was added, resulting in insufficient overall electronic conductivity of the obtained positive electrode, increased resistance, and decreased rate performance; while in Comparative Example 2, an excessive amount of nickel cobalt manganese ternary materials was added, resulting in decreased thermal stability and decreased cycle performance.
[0080] Combining Examples 1, 4, and 11, it can be seen that the performance of Examples 4 and 11 is slightly improved compared to Example 1. This may be because Examples 4 and 10 also added a dispersant of polyethylene oxide-polyacrylonitrile block copolymer during the premixing and dispersion stage. After the polyacrylonitrile chain segments are anchored, the steric hindrance of the polyethylene oxide chain segments can improve the dispersion uniformity of the active material particles and ensure that the two active material particles can maintain a relatively independent dispersion state, providing a continuous electron / ion transport network and improving battery performance. Example 11, based on Example 4, also has amide groups, which can not only improve the adhesion performance with the positive electrode current collector, thereby improving the peel strength, but also further improve the dispersion stability, reduce the interface resistance, and improve battery performance.
[0081] Combining Examples 4 and 10, it can be seen that the performance of Example 10 is lower than that of Example 4. The reason may be that polyethylene oxide is used as a dispersant in Example 10, which lacks polyacrylonitrile segments compared to Example 4. Although polyethylene oxide can play a certain dispersing role in the premixing and dispersion stage and coating process, the binding force between it and the active material is poor, and the peel strength will decrease. Moreover, the lack of the adhesion effect of polyacrylonitrile leads to a decrease in the ion transport efficiency of polyethylene oxide, resulting in a decrease in rate performance.
[0082] The above-disclosed embodiments are merely a few specific examples of the present invention. However, the embodiments of the present invention are not limited thereto, and any variations that can be conceived by those skilled in the art should fall within the protection scope of the present invention.
Claims
1. A method for preparing a lithium iron manganese phosphate - ternary blended cathode slurry, characterized by, The process includes the following steps: S1. Mix lithium manganese iron phosphate and nickel cobalt manganese ternary materials and add them to 10-15% solvent, stir and disperse for 30-60 minutes to obtain a premixed slurry; S2. Add conductive agent and binder to the remaining solvent, and shear and disperse for 1-2 hours to obtain conductive binder slurry; S3. Add conductive binder slurry to the premixed slurry, stir at 800-1000 r / min for 1-2 h, and then vacuum homogenize at 1000-1500 r / min for 2-3 h under a vacuum of -0.08--0.1 MPa to obtain lithium iron phosphate-ternary mixed cathode slurry.
2. The method for preparing the lithium iron phosphate-ternary blended cathode slurry according to claim 1, characterized in that, The molar ratio of lithium manganese iron phosphate and nickel cobalt manganese ternary material is (7.5-8.5):(1.5-2.5).
3. The method of claim 1, wherein the lithium iron manganese phosphate-ternary blended cathode slurry is prepared by mixing the lithium iron manganese phosphate, the ternary cathode active material, the binder, and the solvent. The lithium iron phosphate-ternary blended cathode slurry comprises the following raw materials in parts by weight: 115-135 parts of lithium iron phosphate, 14-24 parts of nickel-cobalt-manganese ternary material, 1-3 parts of conductive agent, 2-4 parts of binder, and 35-45 parts of solvent.
4. The method for preparing the lithium manganese iron phosphate-ternary blended cathode slurry according to claim 1, characterized in that, In step S101, a polyether-type block copolymer dispersant is also added; the polyether-type block copolymer dispersant is a polyethylene oxide-polyacrylonitrile block copolymer; the amount of the polyether-type block copolymer dispersant added is 2 to 5% of the total mass of lithium manganese iron phosphate and nickel cobalt manganese ternary materials.
5. The method for preparing the lithium iron phosphate-ternary blended cathode slurry according to claim 4, characterized in that, The raw materials for the polyethylene oxide-polyacrylonitrile block copolymer include amine-terminated polyethylene oxide prepolymer and acrylonitrile monomer in a mass ratio of 1:(0.8-1).
6. The method for preparing the lithium iron phosphate-ternary blended cathode slurry according to claim 5, characterized in that, The raw materials for the polyethylene oxide-polyacrylonitrile block copolymer also include acrylamide monomer; the amount of acrylamide monomer added is 5 to 10 wt% of the mass of acrylamide monomer.
7. The method for preparing the lithium iron phosphate-ternary blended cathode slurry according to claim 6, characterized in that, The polyethylene oxide-polyacrylonitrile block copolymer was prepared according to the following method: Preparation of amine-terminated polyethylene oxide prepolymer: Benzaldehyde and ethanolamine were mixed under a nitrogen atmosphere and reacted at room temperature for 10–15 h, followed by vacuum distillation. Then, potassium metal was mixed and dissolved in benzene solvent. The temperature was adjusted to 60–65 °C, and the reaction was stirred to obtain an ethanolamine initiator. The ethanolamine initiator was added to ethylene oxide and reacted at 70–75 °C for 20–24 h. After end-capping to terminate the reaction, the prepolymer was dissolved in chloroform. Acetic acid was added, and the reaction was continued at room temperature with stirring for another 20–24 h to obtain the amine-terminated polyethylene oxide prepolymer. Preparation of block copolymers: Acrylonitrile monomer, acrylamide monomer and amine-terminated polyethylene oxide prepolymer are mixed in water, and an initiator is added dropwise under a nitrogen atmosphere at 40-50°C. The reaction is carried out in the dark for 2-4 hours to obtain the copolymer.
8. The method for preparing the lithium iron phosphate-ternary blended cathode slurry according to claim 1, characterized in that, The raw materials for the lithium iron phosphate-ternary blended cathode slurry have all undergone drying pretreatment.
9. A lithium iron phosphate-ternary blended cathode slurry, characterized in that, The slurry was prepared according to the method for preparing lithium manganese iron phosphate-ternary blended cathode slurry according to any one of claims 1 to 8.
10. A power battery, comprising a positive electrode, a negative electrode, and a separator, characterized in that, The positive electrode sheet is prepared by the method of preparing lithium manganese iron phosphate-ternary blended positive electrode slurry according to any one of claims 1 to 8. The slurry is uniformly coated on a carbon aluminum foil current collector, and then dried, rolled, and cut.