A thermally stable negative electrode for an energy storage battery and its preparation method

By using corona-treated three-dimensional foamed copper and partially lithiated poly(pyrrole-3-carboxylic acid) conductive adhesive to form a covalently bonded three-dimensional flexible network in silicon-based anode sheets, the structural damage caused by volume expansion during charging and discharging of silicon-based anodes and the failure of adhesives at high temperatures are solved, thereby improving the stability and lifespan of batteries at high temperatures.

CN123120734APending Publication Date: 2026-11-17广东嘉尚新能源科技有限公司
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611329970.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-31
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing silicon-based anodes suffer structural damage due to volume expansion during charging and discharging, and traditional binders are prone to softening and failure at high temperatures, affecting battery safety and lifespan.

Method used

A three-dimensional foamed copper current collector treated with corona and a partially lithium-ionized poly(pyrrole-3-carboxylic acid) conductive adhesive are combined with a flexible crosslinking agent to form a covalently bonded three-dimensional flexible crosslinking network. Hydroxyl groups are generated on the copper surface through corona treatment. The epoxy groups of the crosslinking agent react with the hydroxyl groups and the silanol groups on the surface of silicon particles to form a ring-opening crosslinking reaction, thus forming a strong and tough three-dimensional network.

Benefits of technology

It effectively inhibits electrode powdering and shedding, improves thermal stability during high-temperature cycling, and balances structural flexibility with electronic/ionic dual conductivity, thereby enhancing the thermal stability and cycle life of the electrode.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123120734A_ABST
    Figure CN123120734A_ABST
Patent Text Reader

Abstract

This invention discloses a high thermal stability negative electrode for energy storage batteries and its preparation method. The negative electrode comprises a negative electrode current collector and a negative electrode active material layer. The negative electrode current collector is a three-dimensional foamed copper with hydroxyl groups on its inner and outer surfaces after corona discharge treatment. The negative electrode active material layer mainly consists of a silicon-based negative electrode active material, a lithium-containing conductive binder, and a flexible crosslinking agent. The lithium-containing conductive binder is a partially lithium-modified poly(pyrrole-3-carboxylic acid), whose molecular structure includes a polypyrrole conjugated conductive backbone, lithium carboxylic acid functional groups, and free carboxyl functional groups. The flexible crosslinking agent is a flexible polymer containing diepoxy groups, and the flexible crosslinking agent forms a covalently bonded three-dimensional crosslinked network with the lithium-containing conductive binder, the three-dimensional foamed copper, and the silicon-based negative electrode active material. This invention not only effectively suppresses pulverization and peeling during the charging and discharging process of the silicon-based negative electrode, controlling the expansion rate to an extremely low level, but also improves the electrode's resistance to softening and thermal stability under high-temperature conditions.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of energy storage battery technology, specifically to an energy storage battery negative electrode sheet with high thermal stability and its preparation method. Background Technology

[0002] With the rapid development of new energy vehicles and large-scale energy storage systems, the energy density requirements for lithium-ion batteries are constantly increasing. Silicon-based materials, due to their extremely high theoretical specific capacity (approximately 3580 mAh / g at room temperature), are considered the most promising next-generation high-energy-density anode materials. However, silicon-based anodes undergo significant volume expansion (up to 300%) during charging and discharging. This drastic volume change leads to silicon particle pulverization, cracking, and detachment from the current collector, resulting in a sharp increase in battery internal resistance and rapid decay of cycle capacity.

[0003] In existing technologies, polyvinylidene fluoride (PVDF) or sodium carboxymethyl cellulose / styrene-butadiene rubber (CMC / SBR) are commonly used as negative electrode binders. However, these traditional binders have the following significant drawbacks: First, traditional binders are all insulators, requiring the addition of large amounts of conductive agents (such as conductive carbon black). This not only reduces the proportion of active material in the electrode but also makes it difficult to maintain a stable conductive network when silicon particles expand drastically. Second, traditional binders mostly rely on intermolecular van der Waals forces or hydrogen bonds to bind with the active material, resulting in weak binding forces that cannot effectively resist the volume expansion of silicon. Finally, traditional binders with linear structures are prone to softening, swelling, or even partial dissolution under high-temperature (e.g., 60°C and above) cycling conditions, exhibiting poor thermal stability. This leads to the rapid collapse of the electrode structure during high-temperature charge and discharge processes, severely restricting the safety and lifespan of silicon-based energy storage batteries. Summary of the Invention

[0004] The purpose of this invention is to provide a thermally stable negative electrode sheet for energy storage batteries and its preparation method, aiming to solve the technical problems of structural damage caused by volume expansion during charging and discharging of existing silicon-based negative electrodes, as well as the easy softening and failure of traditional binders at high temperatures and their poor thermal stability.

[0005] To achieve the above objectives, the present invention adopts the following technical solution:

[0006] A negative electrode sheet for an energy storage battery with high thermal stability includes a negative electrode current collector and a negative electrode active material layer disposed on at least one surface of the negative electrode current collector.

[0007] The negative electrode current collector is a three-dimensional foamed copper that has undergone corona discharge treatment, and the inner and outer surfaces of the three-dimensional skeleton of the three-dimensional foamed copper have hydroxyl groups.

[0008] The negative electrode active material layer is mainly composed of silicon-based negative electrode active material, lithium-containing conductive adhesive and flexible crosslinking agent;

[0009] The lithium-containing conductive adhesive is a partially lithium-modified poly(pyrrole-3-carboxylic acid), whose molecular structure includes a polypyrrole conjugated conductive backbone, a lithium carboxylic acid functional group, and a free carboxyl functional group.

[0010] The flexible crosslinking agent is a flexible polymer containing two epoxy groups; the epoxy groups of the flexible crosslinking agent can undergo ring-opening crosslinking reactions with the free carboxyl groups of the lithium-containing conductive adhesive, the hydroxyl groups on the surface of the three-dimensional copper foam, and the silanol groups on the surface of the silicon-based negative electrode active material to form a covalently bonded three-dimensional flexible crosslinking network.

[0011] Furthermore, in the partially lithiated poly(pyrrole-3-carboxylic acid), the degree of lithiation of the side chain carboxyl groups is 30% to 55%, and the remainder consists of free carboxyl functional groups.

[0012] The lithiation degree is controlled between 30% and 55% to achieve an optimal balance between ionic conductivity and the active sites of the cross-linking reaction. Precise control of this parameter is crucial in the specific preparation process. Specifically, the total molar amount of free carboxyl groups in the unlithiated poly(pyrrole-3-carboxylic acid) can be pre-determined using acid-base titration. Then, based on the target lithiation degree (30%–55%), the required molar amount of lithium hydroxide is calculated using stoichiometry. The calculated amount of lithium hydroxide is prepared into an aqueous solution and slowly added dropwise to the poly(pyrrole-3-carboxylic acid) dispersion, thus achieving precise control over the neutralization reaction endpoint (i.e., lithiation degree). If the lithiation degree is below 30%, there are insufficient lithium-ion channels in the system, affecting the battery's rate performance. If the lithiation degree is above 55%, there are too few free carboxyl functional groups, which not only fail to provide a sufficient acidic autocatalytic environment but also lead to a sharp decrease in the density of cross-linking points with epoxy groups, preventing the formation of a dense, three-dimensional flexible cross-linked network and weakening the inhibitory effect on silicon particle expansion.

[0013] Further, the flexible crosslinking agent is one or more of polyethylene glycol diglycidyl ether, 1,4-butanediol diglycidyl ether, or polypropylene glycol diglycidyl ether.

[0014] The selected crosslinking agents all have highly active epoxy groups at the end groups, with aliphatic or polyether flexible segments in the middle. These flexible segments act as "molecular springs" in the three-dimensional network, capable of stretching to dissipate stress when silicon particles expand and springing back to their original shape when silicon particles contract, ensuring that the electrode does not experience fatigue cracking during long-term cycling.

[0015] Furthermore, in the negative electrode active material layer, the mass ratio of the silicon-based negative electrode active material to the lithium-containing conductive adhesive is (92~96):(4~8); the added mass of the flexible crosslinking agent is 1%~5% of the mass of the lithium-containing conductive adhesive.

[0016] Because the adhesive of this invention has excellent conductivity, no additional conductive agent is needed, allowing the active material content in the electrode to reach over 92%, thus improving the volumetric energy density. The crosslinking agent ratio is controlled at 1% to 5%, ensuring network crosslinking without introducing excessive insulating inactive materials that would increase the electrode's internal resistance.

[0017] Furthermore, the silicon-based anode active material is selected from one or more of nano-silicon, silicon suboxide, or silicon-carbon composite materials.

[0018] Furthermore, the porosity of the three-dimensional copper foam is 80%~90%, and the pore size is 50~200μm.

[0019] Among them, the three-dimensional skeleton can accommodate silicon-based materials within the pores, further providing a physical confinement effect; the porosity of 80%~90% and the specific pore size range can ensure the full wetting and filling of the slurry, and also have sufficient skeleton strength to withstand the tableting process.

[0020] A second aspect of the present invention provides a method for preparing the above-mentioned energy storage battery negative electrode sheet with high thermal stability, comprising the following steps:

[0021] S1. Place the three-dimensional foamed copper in a corona treatment device for discharge treatment to generate hydroxyl groups on the surface of the three-dimensional foamed copper skeleton, thus obtaining the activated negative electrode current collector.

[0022] S2. The 1H-pyrrole-3-carboxylic acid monomer is subjected to oxidative polymerization in a solvent under the action of an initiator to obtain poly(pyrrole-3-carboxylic acid); then a lithium-ionizing agent is added to carry out a partial neutralization reaction to obtain the lithium-containing conductive adhesive.

[0023] S3. Add the silicon-based negative electrode active material and the lithium-containing conductive adhesive to a solvent, add the flexible crosslinking agent, stir and disperse to obtain a negative electrode slurry;

[0024] S4. The negative electrode slurry is filled into the pores and surface of the negative electrode current collector after step S1, and then a step baking is performed to allow the epoxy groups of the flexible crosslinking agent to undergo ring-opening crosslinking reactions with the free carboxyl groups in the lithium-containing conductive adhesive, the hydroxyl groups on the surface of the negative electrode current collector, and the silanol groups on the surface of the silicon-based negative electrode active material, respectively. After in-situ curing, the energy storage battery negative electrode sheet with high thermal stability is obtained.

[0025] The preparation method of this invention utilizes in-situ crosslinking and curing technology. First, the surface activity of the current collector is activated by corona discharge. Then, various components are mixed in the slurry system. Finally, chemical bonding is achieved by thermal drive during the baking stage after coating. This eliminates the need to introduce complex chemical reaction equipment during the slurry preparation stage. It not only achieves close integration of multiphase interfaces but also has good process compatibility and is suitable for industrial promotion.

[0026] Furthermore, in step S1, the conditions for the corona discharge treatment are: in an air atmosphere, the discharge power is 500~1000W, and the treatment time is 2~5min.

[0027] Among them, high-voltage corona discharge ionizes the air, producing high-energy electrons and strong oxidizing substances such as ozone, which bombard the three-dimensional foam copper surface, removing surface oil and oxidizing to generate active Cu-OH functional groups, significantly increasing the free energy of the copper surface and providing chemical grafting sites for subsequent epoxy etherification crosslinking.

[0028] Further, the specific preparation process of step S2 is as follows: under ice-water bath conditions of 0~5℃, using deionized water as solvent, ammonium persulfate aqueous solution is added dropwise to a solution containing 1H-pyrrole-3-carboxylic acid monomer as an initiator for oxidative polymerization for 8~12h. After washing and drying, the polymerization product is obtained as poly(pyrrole-3-carboxylic acid); the poly(pyrrole-3-carboxylic acid) is dispersed in deionized water, and lithium hydroxide aqueous solution is slowly added dropwise to control the neutralization reaction so that the degree of lithiumization of the side chain carboxyl groups reaches 30%~55%. Then, the solvent is removed by drying to obtain the lithium-containing conductive adhesive.

[0029] Oxidative polymerization at 0~5℃ effectively reduces side reactions. Since the 2 and 5 positions of the 1H-pyrrole-3-carboxylic acid monomer are not substituted, ammonium persulfate can smoothly induce α-α coupling to form a long-chain conjugated polymer backbone, ensuring the high intrinsic conductivity of the material. Partial neutralization is performed using lithium hydroxide aqueous solution, and the reaction conditions are mild and controllable, allowing for precise adjustment of the degree of lithiation of the product.

[0030] Further, in step S4, the stepped baking process is specifically as follows: First stage: baking at 60~80℃ under normal pressure for 1~2h; Second stage: heating to 140~160℃ and holding at a vacuum of -0.09MPa~-0.1MPa for 4~6h to carry out ring-opening crosslinking curing.

[0031] The first stage (60~80℃) mainly involves gentle physical dehydration, slowly evaporating the solvent to prevent the water inside the slurry from boiling due to instantaneous high temperature, which would damage the microporous structure of the electrode. The second stage (140~160℃) enters the chemical curing zone. After the residual moisture is eliminated in the vacuum and its interference with the esterification reaction is removed, the free carboxyl groups catalyze the rapid ring opening of the epoxy groups, forming a high-density covalent network with the hydroxyl and carboxyl groups at each interface, achieving a qualitative change from physical mixing to chemical bonding.

[0032] Compared with the prior art, the present invention has at least the following beneficial effects:

[0033] 1) Constructing a multi-interface covalent anchoring network to effectively suppress electrode pulverization and detachment: This invention abandons the traditional van der Waals force or hydrogen bonding methods, utilizing a flexible crosslinking agent containing bi-epoxy groups to undergo a ring-opening reaction at a specific baking temperature. The crosslinking agent not only undergoes esterification crosslinking with the free carboxyl groups in the conductive adhesive, but more importantly, it can also undergo etherification crosslinking with the hydroxyl groups (Cu-OH) on the surface of the corona-treated copper foam and the silanol groups (Si-OH) on the surface of the silicon particles. This comprehensive chemical covalent bonding, from the current collector framework to the adhesive and then to the surface of the active material, forms an extremely strong three-dimensional network that firmly anchors the silicon particles, effectively preventing them from peeling off from the current collector during drastic volume expansion.

[0034] 2) Improved thermal stability during high-temperature cycling: Traditional thermoplastic linear binders are prone to molecular chain slippage and softening at high temperatures. In this invention, the cross-linked and cured electrode forms a three-dimensional cross-linked network structure similar to thermosetting resin. This strongly covalently cross-linked network restricts the thermal movement of polymer molecular chains at high temperatures. Even when the energy storage battery faces abnormally high-temperature operating conditions, the adhesive network can still maintain excellent mechanical support properties, greatly improving the thermal stability of the electrode.

[0035] 3) Balancing structural flexibility with dual electronic / ionic conductivity: A flexible crosslinking agent is used as a bridge, giving the three-dimensional network a flexible buffer space similar to a "spring," which can adaptively absorb the expansion stress of silicon particles and avoid rigid fracture. At the same time, the partially lithiated poly(pyrrole-3-carboxylic acid) not only achieves efficient electron conduction by utilizing its polypyrrole conjugated backbone, replacing traditional inactive conductive agents, but also its side chain lithium carboxylic acid (-COOLi) functional group provides a fast migration channel for lithium ions, achieving efficient dual conduction of electrons and ions.

[0036] 4) In-situ autocatalysis using free carboxyl groups: During the thermosetting stage at 140-160℃, the ring-opening reaction between epoxy groups and inorganic surface hydroxyl groups (Si-OH, Cu-OH) is usually kineticly slow. However, in the system of this invention, the abundant free carboxyl groups (-COOH) inherent in the conductive adhesive create a slightly acidic environment. The trace protons dissociated from these groups can protonate the oxygen atoms on the epoxy groups, significantly reducing the activation energy of the ring-opening reaction and ensuring that the multi-interface covalent cross-linking reaction can be completed efficiently and thoroughly at conventional electrode baking temperatures. Attached Figure Description

[0037] Figure 1 This is a schematic diagram of the negative electrode sheet in one embodiment of the present invention.

[0038] In the figure, 1 is the negative electrode current collector; 2 is the negative electrode active material layer. Detailed Implementation

[0039] To make the objectives, technical solutions, and advantages of this invention clearer, the technical solutions of the embodiments of this invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of this invention, and not all embodiments. Based on the embodiments of this invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of this invention.

[0040] The core inventive concept and mechanism of action of this invention are explained below:

[0041] like Figure 1 As shown, the present invention provides a high thermal stability negative electrode sheet for an energy storage battery, comprising a negative electrode current collector 1 and a negative electrode active material layer 2 disposed on at least one surface of the negative electrode current collector 1. The negative electrode current collector 1 is a three-dimensional foamed copper treated with corona discharge, and the inner and outer surfaces of the three-dimensional skeleton of the three-dimensional foamed copper have hydroxyl groups. The negative electrode active material layer 2 is mainly composed of a silicon-based negative electrode active material, a lithium-containing conductive adhesive, and a flexible crosslinking agent. The lithium-containing conductive adhesive is a partially lithium-modified poly(pyrrole-3-carboxylic acid), whose molecular structure includes a polypyrrole conjugated conductive backbone, a lithium carboxylic acid functional group, and a free carboxyl functional group. The flexible crosslinking agent is a flexible polymer containing a diepoxy group. The epoxy group of the flexible crosslinking agent can undergo a ring-opening crosslinking reaction with the free carboxyl group of the lithium-containing conductive adhesive, the hydroxyl group on the surface of the three-dimensional foamed copper, and the silanol group on the surface of the silicon-based negative electrode active material to form a covalently bonded three-dimensional flexible crosslinking network.

[0042] The core of this invention lies in breaking through the limitations of existing technologies that rely solely on physical bonding for silicon-based electrodes. The applicant's in-depth research revealed that to fundamentally suppress the expansion and peeling of silicon-based anodes and improve high-temperature stability, strong chemical bonds must be established within the electrode.

[0043] Based on this, the negative electrode current collector 1 of this application uses three-dimensional foamed copper that has undergone corona treatment. Corona discharge is essentially a non-equilibrium plasma technology. In an air atmosphere (500~1000W, 2~5min), the bombardment of high-energy electrons ionizes the air, and the generated highly reactive oxygen atoms and ozone react with the copper framework surface, not only removing the adsorbed hydrocarbons, but also densely generating hydroxyl groups (Cu-OH) on its surface. Compared with two-dimensional planar copper foil, three-dimensional foamed copper (porosity 80%~90%, pore size 50~200μm) provides a larger specific surface area, greatly increasing the effective anchoring sites.

[0044] For lithium-containing conductive adhesives, this application presents a partially lithium-modified poly(pyrrole-3-carboxylic acid) synthesized via chemical synthesis. The synthesis mechanism is as follows: Under ammonium persulfate (APS) oxidation, the unsubstituted 2,5-position (α-position) of the 1H-pyrrole-3-carboxylic acid monomer undergoes a radical coupling reaction, losing electrons and protons to form a conjugated polyene skeleton composed of pyrrole rings, providing electronic conductivity; while the carboxyl group at the 3-position remains intact in the side chain after polymerization. Subsequently, a measured amount of LiOH is added to neutralize some of the carboxyl group to -COOLi. The free carboxyl group serves two purposes: firstly, as an acidic catalyst to lower the activation energy of subsequent crosslinking reactions; and secondly, to provide crosslinking reaction sites. The role of lithium carboxylic acid is to reduce the lithium-ion interfacial migration resistance.

[0045] During pulping and subsequent baking, the added flexible polymers containing diepoxy groups (such as polyethylene glycol diglycidyl ether) act as a central pivot. In the 60–80°C range, only physical dehydration occurs on the electrode; however, when the temperature jumps to 140–160°C under vacuum, the chemical kinetics of the system undergo a sudden change. Trace amounts of H+ ionized from the free carboxyl groups... + The process first attacks the epoxy group, causing its oxygen atom to become positively charged, thereby polarizing the adjacent carbon-oxygen bond. This in-situ protonation process greatly reduces the energy barrier of nucleophilic attack, allowing the normally slow-reacting inorganic hydroxyl groups (Si-OH and Cu-OH) to rapidly launch a nucleophilic attack on the epoxy carbon atom to form an ether bond; simultaneously, some free carboxyl groups also directly undergo esterification and ring-opening with the epoxy group. As a result, the flexible polyether chain of the crosslinking agent is firmly locked by chemical bonds between the silicon particle surface, the copper backbone surface, and the polymer backbone, forming a three-dimensional flexible network in situ inside the electrode.

[0046] To verify the technical effects of the present invention, several embodiments and comparative examples are provided below for further explanation.

[0047] Example 1

[0048] This embodiment provides a thermally stable negative electrode sheet for an energy storage battery and its preparation method. The specific steps are as follows:

[0049] (1) Current collector activation: Three-dimensional copper foam with a porosity of 85% and a pore size of 100μm was placed in a corona treatment machine and treated for 3 minutes in an air atmosphere with a power of 800W to obtain the activated negative electrode current collector;

[0050] (2) Synthesis of lithium-containing conductive adhesive: In a 0℃ ice-water bath, an appropriate amount of 1H-pyrrole-3-carboxylic acid monomer was dissolved in deionized water, and an equimolar amount of ammonium persulfate aqueous solution was slowly added dropwise with stirring. The reaction was carried out for 10 h. After centrifugation, washing, and vacuum drying, poly(pyrrole-3-carboxylic acid) was obtained. It was redispersed in water, and 0.5 mol / L LiOH aqueous solution was slowly added dropwise for partial neutralization. After acid-base titration and calculation, the degree of lithiumization of the side chain carboxyl groups in the product was controlled to be 40%. After spray drying, lithium-containing conductive adhesive was obtained.

[0051] (3) Slurry preparation: 94 parts by weight of silicon-carbon composite material (Si / C composite material with silanol content on surface) and 6 parts by weight of the above lithium-containing conductive adhesive are added to deionized water, followed by 3% by weight of polyethylene glycol diglycidyl ether (PEGDE) by the adhesive. The mixture is dispersed at high speed by a planetary mixer to obtain a uniform negative electrode slurry.

[0052] (4) Coating and stepped baking curing: The above negative electrode slurry is uniformly filled and coated into the activated three-dimensional foamed copper. It is then placed in a vacuum oven and baked at 70°C and atmospheric pressure for 1.5 hours; then the temperature is raised to 155°C, the vacuum is reduced to -0.095 MPa, and the temperature is maintained for 5 hours for ring-opening crosslinking curing. After cooling, it is rolled and die-cut to obtain the energy storage battery negative electrode sheet with high thermal stability.

[0053] Example 2

[0054] The only difference between this embodiment and Example 1 is the type of flexible crosslinking agent used in step (3): polyethylene glycol diglycidyl ether is replaced with an equal mass of 1,4-butanediol diglycidyl ether. The intermediate chain segment of 1,4-butanediol diglycidyl ether is shorter and its flexibility is slightly lower than that of PEGDE. The remaining steps and parameters are exactly the same as in Example 1.

[0055] Example 3

[0056] The only difference between this embodiment and Example 1 is the degree of lithiation of the adhesive in step (2): the amount of LiOH aqueous solution added is adjusted to control the degree of lithiation of the side chain carboxyl groups in the product to 20%, resulting in more free carboxyl groups but fewer ion conduction channels. The remaining steps are the same as in Example 1.

[0057] Comparative Example 1

[0058] The difference between this comparative example and Example 1 is the lack of a three-dimensional flexible cross-linked network: in step (3), polyethylene glycol diglycidyl ether is not added (no cross-linking agent is added), and the material is physically mixed with the lithium-containing conductive adhesive. The remaining steps are the same as in Example 1.

[0059] Comparative Example 2

[0060] This comparative example uses traditional insulating adhesive and two-dimensional current collector as benchmarks for comparison:

[0061] The current collector is made of conventional flat two-dimensional copper foil that has not undergone corona treatment.

[0062] Slurry preparation and coating: A slurry was prepared by uniformly mixing 94 parts by weight of silicon-carbon composite material, 2 parts by weight of conductive carbon black (Super P), 2 parts by weight of sodium carboxymethyl cellulose (CMC), and 2 parts by weight of styrene-butadiene rubber (SBR) with water. The slurry was then coated onto a two-dimensional copper foil and vacuum-baked at 85°C for 12 hours. Lithium-containing conductive adhesives with conductive, self-catalytic, and multi-site crosslinking capabilities were not used.

[0063] Comparative Example 3

[0064] The difference between this comparative example and Example 1 is that the current collector surface is chemically inactive: the corona discharge treatment step is omitted in step (1), and untreated three-dimensional foamed copper is used directly. The remaining steps are the same as in Example 1. Since no corona treatment is performed, almost no hydroxyl groups (Cu-OH) are generated on the surface of the copper skeleton.

[0065] The negative electrode sheets prepared in Examples 1-3 and Comparative Examples 1-3 were assembled with lithium metal counter electrodes to form CR2032 coin cells. The electrolyte consisted of 1 mol / L LiPF6 dissolved in a mixed solvent of EC / DEC / EMC (volume ratio 1:1:1), with 10% FEC added as a film-forming additive. The following performance tests were performed on each electrode and the cell:

[0066] 1. Electrode peel strength (N / m): A 180° peel test was conducted using a tensile testing machine. The electrode was fixed on one side to a double-sided adhesive steel strip, and the current collector was peeled from the active layer at a speed of 50 mm / min. The average peel force was recorded and divided by the electrode width.

[0067] 2. Electrode thickness expansion rate (%) after cycling. The macroscopic thickness of the electrode before cycling at room temperature (fully discharged state) and after 200 cycles (fully charged state) was measured using a high-precision micrometer, and the relative expansion percentage was calculated.

[0068] 3. Capacity retention rate during room temperature cycling (%): After activation at 0.1C for 3 cycles in a 25℃ constant temperature chamber, charge-discharge cycles were performed at a current density of 1.0C within a voltage range of 0.01~1.5V. The discharge specific capacity of the first cycle and the discharge specific capacity of the 200th cycle were recorded. Capacity retention rate = (capacity of the 200th cycle / capacity of the first cycle) × 100%.

[0069] 4. High-temperature cycle capacity retention rate (%): After activation at 0.1C for 3 cycles in a 60℃ high-temperature constant temperature chamber, charge and discharge cycles were performed at a current density of 1.0C. The discharge specific capacity of the first cycle and the 100th cycle were recorded. Capacity retention rate = (capacity of the 100th cycle / capacity of the 1st cycle) × 100%.

[0070] The test results are shown in Table 1 below.

[0071] Table 1

[0072] serial number Peel strength (N / m) Electrode thickness expansion rate (%) Capacity retention rate (%) after 200 cycles at room temperature High-temperature 100-cycle capacity retention (%) Example 1 125 32% 89.2% 85.6% Example 2 102 39% 86.4% 83.1% Example 3 148 30% 84.1% 81.2% Comparative Example 1 45 98% 62.5% 45.3% Comparative Example 2 22 125% 48.7% 31.4% Comparative Example 3 76 82% 71.3% 66.8%

[0073] The analysis of the above test results is as follows:

[0074] 1) A comparison of Example 1 and Comparative Examples 1-2 shows that, in terms of peel strength and thickness expansion rate, the traditional system in Comparative Example 2 has a peel strength of only 22 N / m, and the cyclic expansion rate of silicon particles is as high as 125%, resulting in complete structural pulverization and failure, leading to significant capacity decay. Comparative Example 1 used three-dimensional copper and conductive adhesive, and although the expansion rate was reduced to 98%, the lack of a crosslinking agent meant that the molecules relied solely on physical entanglement, which could not prevent microscopic slippage caused by long cycles, resulting in a peel strength of only 45 N / m. In contrast, Example 1, due to the formation of a chemically covalently bonded three-dimensional crosslinked network during high-temperature vacuum curing, achieved a peel strength of 125 N / m, while simultaneously suppressing the cyclic thickness expansion rate to 32%, and maintaining a capacity retention rate of 85.6% at 60°C. This demonstrates that the three-dimensional crosslinked structure, similar to a high-strength spring mesh, can effectively suppress expansion and impart excellent high-temperature softening resistance to the electrode.

[0075] 2) A comparison between Example 1 and Comparative Example 3 shows that both Example 1 and Comparative Example 3 have cross-linked networks, but the current collector in Comparative Example 3 was not corona activated and lacked Cu-OH groups. Data indicates that the peel strength of Comparative Example 3 decreased to 76 N / m, and the thickness expansion rate reached 82%. This indicates that although the active material layer in Comparative Example 3 underwent internal cross-linking, it did not "root" itself on the three-dimensional copper framework. The expansion stress caused the entire coating to peel off from the copper wall, demonstrating the necessity of corona treatment-induced interfacial anchoring. Interfacial covalent bonding can effectively maintain structural stability.

[0076] 3. A comparison of Examples 1 and 2 shows that the thickness expansion rate of Example 1 (32%) is lower than that of Example 2 (39%). This may be because the PEGDE used in Example 1 has longer flexible polyethylene glycol segments in the middle, allowing for greater freedom in segment conformational transformation and more effective absorption and dissipation of localized stress concentration caused by the expansion of the silicon material. In contrast, the 1,4-butanediol diglycidyl ether segments in Example 2 are shorter and more rigid, resulting in insufficient buffering capacity. Therefore, the macroscopic expansion is slightly larger, and the cycle retention rate is slightly lower, but the overall performance remains at a very high level.

[0077] 4. A comparison of Examples 1 and 3 shows that: the degree of lithiation in Example 3 decreased to 20% (due to the presence of a large number of unneutralized carboxyl groups), but its peel strength (148 N / m) was even higher than that of Example 1, and its expansion rate (30%) was lower. This may be because more free carboxyl groups provide denser cross-linking nodes, making the network more robust. However, its battery cycle capacity retention was lower than that of Example 1. This is precisely because the low lithiation resulted in very little -COOLi, severely hindering lithium-ion conduction within the active layer, leading to a surge in concentration polarization during high-rate cycling and triggering localized lithium plating dead zones. This demonstrates that precisely titrating and controlling the degree of lithiation within the range of 30% to 55% can balance network mechanical strength and electrochemical kinetic performance.

[0078] In summary, this invention, through ingenious molecular-level design and a mild preparation process, constructs a flexible three-dimensional conductive network with multi-interface conjugated crosslinking, effectively solving the problems of volume expansion and pulverization and poor high-temperature thermal stability of silicon-based materials, and has extremely high industrial application prospects.

[0079] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention and not to limit it. Although the present invention has been described in detail with reference to the above embodiments, those skilled in the art should understand that modifications or equivalent substitutions can still be made to the specific embodiments of the present invention, and any modifications or equivalent substitutions that do not depart from the spirit and scope of the present invention should be covered within the scope of the claims of the present invention.

Claims

1. A negative electrode sheet for an energy storage battery with high thermal stability, comprising a negative electrode current collector and a negative electrode active material layer disposed on at least one surface of the negative electrode current collector, characterized in that: The negative electrode current collector is a three-dimensional foamed copper that has undergone corona discharge treatment, and the inner and outer surfaces of the three-dimensional skeleton of the three-dimensional foamed copper have hydroxyl groups. The negative electrode active material layer is mainly composed of silicon-based negative electrode active material, lithium-containing conductive adhesive and flexible crosslinking agent; The lithium-containing conductive adhesive is a partially lithium-modified poly(pyrrole-3-carboxylic acid), whose molecular structure includes a polypyrrole conjugated conductive backbone, a lithium carboxylic acid functional group, and a free carboxyl functional group. The flexible crosslinking agent is a flexible polymer containing two epoxy groups; the epoxy groups of the flexible crosslinking agent can undergo ring-opening crosslinking reactions with the free carboxyl groups of the lithium-containing conductive adhesive, the hydroxyl groups on the surface of the three-dimensional copper foam, and the silanol groups on the surface of the silicon-based negative electrode active material to form a covalently bonded three-dimensional flexible crosslinking network.

2. The high-heat-stable energy storage battery negative electrode sheet according to claim 1, characterized by: In the partially lithiated poly(pyrrole-3-carboxylic acid), the degree of lithiation of the side chain carboxyl groups is 30% to 55%, and the remainder consists of free carboxyl functional groups.

3. The high-heat-stable high-performance energy storage battery anode sheet according to claim 1, characterized by: The flexible crosslinking agent is one or more of polyethylene glycol diglycidyl ether, 1,4-butanediol diglycidyl ether, or polypropylene glycol diglycidyl ether.

4. The high-thermal-stability energy storage battery anode sheet according to claim 1, characterized in that: In the negative electrode active material layer, the mass ratio of the silicon-based negative electrode active material to the lithium-containing conductive adhesive is (92~96):(4~8); the mass of the flexible crosslinking agent added is 1%~5% of the mass of the lithium-containing conductive adhesive.

5. The high thermal stability negative electrode of the energy storage battery according to claim 1, characterized in that: The silicon-based anode active material is selected from one or more of nano-silicon, silicon suboxide, or silicon-carbon composite materials.

6. The high thermal stability negative electrode of the energy storage battery according to claim 1, characterized in that: The porosity of the three-dimensional copper foam is 80%~90%, and the pore size is 50~200μm.

7. A method for preparing a negative electrode sheet for an energy storage battery with high thermal stability as described in any one of claims 1 to 6, characterized in that, Includes the following steps: S1. Place the three-dimensional foamed copper in a corona treatment device for discharge treatment to generate hydroxyl groups on the surface of the three-dimensional foamed copper skeleton, thus obtaining the activated negative electrode current collector. S2. The 1H-pyrrole-3-carboxylic acid monomer is subjected to oxidative polymerization in a solvent under the action of an initiator to obtain poly(pyrrole-3-carboxylic acid); then a lithium-ionizing agent is added to carry out a partial neutralization reaction to obtain the lithium-containing conductive adhesive. S3. Add the silicon-based negative electrode active material and the lithium-containing conductive adhesive to a solvent, add the flexible crosslinking agent, stir and disperse to obtain a negative electrode slurry; S4. The negative electrode slurry is filled into the pores and surface of the negative electrode current collector after step S1, and then a step baking is performed to allow the epoxy groups of the flexible crosslinking agent to undergo ring-opening crosslinking reactions with the free carboxyl groups in the lithium-containing conductive adhesive, the hydroxyl groups on the surface of the negative electrode current collector, and the silanol groups on the surface of the silicon-based negative electrode active material, respectively. After in-situ curing, the energy storage battery negative electrode sheet with high thermal stability is obtained.

8. The preparation method according to claim 7, characterized in that: In step S1, the conditions for the corona discharge treatment are: in an air atmosphere, the discharge power is 500~1000W, and the treatment time is 2~5min.

9. The preparation method according to claim 7, characterized in that: The specific preparation process of step S2 is as follows: Under ice-water bath conditions of 0~5℃, with deionized water as solvent, ammonium persulfate aqueous solution was added dropwise to a solution containing 1H-pyrrole-3-carboxylic acid monomer as an initiator for oxidative polymerization for 8~12h. The polymerization product was washed and dried to obtain poly(pyrrole-3-carboxylic acid). The poly(pyrrole-3-carboxylic acid) was dispersed in deionized water, and an aqueous solution of lithium hydroxide was slowly added dropwise to control the neutralization reaction so that the degree of lithiation of the side chain carboxyl groups reached 30% to 55%. The solvent was then removed by drying to obtain the lithium-containing conductive adhesive.

10. The preparation method according to claim 7, characterized in that: In step S4, the stepped baking process specifically involves: First stage: Bake at 60~80℃ under normal pressure for 1~2 hours; Second stage: Heat to 140~160℃ and keep at a vacuum of -0.09MPa~-0.1MPa for 4~6 hours to carry out ring-opening crosslinking and curing.