Sodium carboxymethylcellulose / polypyrrole composite conductive hydrogel and preparation method thereof

By using carboxymethylcellulose sodium/polypyrrole composite hydrogel as the precursor of the negative electrode material of sodium ion battery, the problem of limited use of graphite negative electrode material in sodium ion battery is solved, and high conductivity and water absorption are achieved. It is suitable for The negative electrode material of sodium ion battery.

CN118955952APending Publication Date: 2024-11-15SHANGHAI SECOND POLYTECHNIC UNIVERSITY
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411158542.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-22
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

The use of graphite anode materials in sodium ion batteries is limited by the large atomic radius of sodium ions, which makes it difficult for sodium ions to insert into the graphite layer, and it is necessary to find suitable sodium ion battery anode materials.

Method used

Using sodium carboxymethylcellulose/polypyrrole composite conductive hydrogel as the precursor of hard carbon, a composite hydrogel with a network structure and good conductivity was prepared by crosslinking reaction between sodium carboxymethylcellulose and pyrrole. , as the negative electrode material of sodium ion battery.

Benefits of technology

The composite hydrogel has good conductivity, water absorption, heat absorption and environmental stability, and is low in cost. It is suitable as the negative electrode material of sodium ion battery, improving the storage performance of sodium ions and the overall performance of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118955952A_ABST
    Figure CN118955952A_ABST
Patent Text Reader

Abstract

The invention discloses a sodium carboxymethyl cellulose / polypyrrole composite conductive hydrogel and a preparation method thereof. According to the invention, sodium carboxymethyl cellulose and polypyrrole are used for preparing composite hydrogel, and then the composite hydrogel is dried to obtain the hydrogel material with a porous network structure. The preparation method is simple in process, conditions are easy to control, and large-scale production is easy; the prepared composite hydrogel material has the advantages of sodium carboxymethyl cellulose and polypyrrole, is light and flexible, and has good water absorption, conductivity and environmental stability; the composite hydrogel material can be further used for preparing a sodium ion battery hard carbon negative electrode material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of composite hydrogel materials, and in particular to a sodium carboxymethyl cellulose / polypyrrole composite conductive hydrogel and a preparation method thereof. Background Art

[0002] Lithium-ion batteries have the advantages of high energy density, good electrochemical performance, long cycle life, no memory effect and environmental protection, and have been widely used in portable electronic devices and new energy vehicles. However, the limited lithium resources in the earth's crust restrict its large-scale application in energy storage devices. Sodium and lithium belong to the same main group and have similar properties. Compared with lithium, sodium resources are more abundant, the cost is lower, and the safety is higher. Therefore, sodium-ion batteries may replace lithium-ion batteries. Because the atomic radius of sodium ions is larger, compared with lithium ions, the distance between graphite layers is only 0.34nm, which makes it difficult for sodium ions to insert into the graphite layer, making the graphite negative electrode widely used in lithium-ion batteries unable to be used in sodium-ion batteries. Therefore, finding anode materials suitable for sodium-ion batteries has become the focus of current research.

[0003] Hard carbon has excellent sodium storage performance due to its wide interlayer spacing, porous and loose structure, and interlaced layered structure, and is considered to be the most promising negative electrode material for sodium ion batteries. Since the structure and performance of hard carbon are highly related to its precursor, the selection of a suitable precursor is key. At present, biomass with high content of cellulose, lignin and hemicellulose is the preferred precursor for the preparation of hard carbon. Conductive hydrogel is a new type of functional material formed by the polymerization and cross-linking of hydrogel and conductive polymer, which has good conductivity, stability and mechanical properties. Summary of the invention

[0004] The purpose of the present invention is to provide a sodium carboxymethyl cellulose / polypyrrole composite conductive hydrogel that can be used as a precursor of hard carbon, a negative electrode material for sodium ion batteries, and a preparation method thereof. The present invention uses sodium carboxymethyl cellulose and pyrrole as raw materials to prepare a sodium carboxymethyl cellulose / polypyrrole composite conductive hydrogel, which has the advantages of simple process, environmentally friendly materials, low cost, easy control of conditions, and easy large-scale production. The prepared sodium carboxymethyl cellulose / polypyrrole composite conductive hydrogel can be used as a precursor of hard carbon, a negative electrode material for sodium ion batteries.

[0005] To achieve the above object, the technical solution of the present invention is as follows:

[0006] A method for preparing a sodium carboxymethyl cellulose / polypyrrole composite conductive hydrogel, the specific steps are as follows:

[0007] (1) Preparation of sodium carboxymethyl cellulose hydrogel

[0008] A certain amount of sodium carboxymethyl cellulose is added to 20 mL of deionized water until the sodium carboxymethyl cellulose is completely dissolved to obtain a sodium carboxymethyl cellulose aqueous solution with a mass concentration of 0.5-1%, and then acrylamide, N, N'-methylenebisacrylamide, potassium persulfate and 8-15 μL of tetramethylethylenediamine as a co-initiator are added to the sodium carboxymethyl cellulose aqueous solution. After the addition is complete, the mixture is continuously stirred at a temperature of 35-45° C. for cross-linking reaction to obtain a sodium carboxymethyl cellulose hydrogel; wherein the mass ratio of sodium carboxymethyl cellulose, acrylamide, N, N-bismethylacrylamide and potassium persulfate is (0.1-0.2):4:(0.04-0.08):(0.2-0.4);

[0009] (2) Preparation of sodium carboxymethyl cellulose / polypyrrole composite hydrogel

[0010] The sodium carboxymethyl cellulose hydrogel prepared in step (1) is immersed in 100 mL of phytic acid solution containing pyrrole, and after standing for 3-4 hours, the sample is taken out and washed to obtain a sodium carboxymethyl cellulose / polypyrrole composite hydrogel;

[0011] (3) Preparation of sodium carboxymethyl cellulose / polypyrrole composite conductive hydrogel

[0012] The sodium carboxymethyl cellulose / polypyrrole composite hydrogel is freeze-dried to obtain the sodium carboxymethyl cellulose / polypyrrole conductive hydrogel.

[0013] In the present invention, in step (1), during the cross-linking reaction, the stirring speed is 300-500 rpm and the reaction time is 5-10 h.

[0014] In the present invention, in step (2), the phytic acid solution containing pyrrole is prepared by mixing pyrrole, phytic acid and water in a volume ratio of (0.1-0.6):(3-8):100.

[0015] In the present invention, in step (2), the phytic acid solution containing pyrrole is prepared by mixing pyrrole, phytic acid and water in a volume ratio of (0.4-0.5):5:100.

[0016] In the present invention, in step (2), washing is performed with water.

[0017] In the present invention, in step (3), the product is first placed in a refrigerator for pre-freezing for 12-24 hours, and then freeze-dried in a freeze dryer at a temperature of -30 to -50°C for 24-50 hours.

[0018] The invention also provides a sodium carboxymethyl cellulose / polypyrrole composite conductive hydrogel prepared by the preparation method.

[0019] Compared with the prior art, the present invention has the following advantages:

[0020] (1) The sodium carboxymethyl cellulose / polypyrrole composite conductive hydrogel of the present invention has a network structure, is rich in a large number of hydroxyl functional groups on the surface, and has good water absorption.

[0021] (2) Polypyrrole has good electrical conductivity and heat absorption; the sodium carboxymethyl cellulose / polypyrrole composite conductive hydrogel prepared by the present invention has the advantages of both sodium carboxymethyl cellulose and polypyrrole, and has good electrical conductivity, water absorption, heat absorption, and environmental stability.

[0022] (3) The sodium carboxymethyl cellulose / polypyrrole composite conductive hydrogel prepared by the present invention is light and flexible, and is derived from biomass materials and has low cost.

[0023] (4) The present invention uses sodium carboxymethyl cellulose to stabilize hydrophobic polypyrrole chains to obtain highly conductive hydrogels. First, pyrrole monomers are in situ polymerized into polypyrrole on the surface of sodium carboxymethyl cellulose hydrogels, and then are uniformly dispersed into the interior of carboxymethyl hydrogels through the cross-linking effect of phytic acid, thereby forming interconnected conductive pathways, thereby improving its conductivity. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 These are the test results of water absorption performance of composite conductive hydrogels with different polypyrrole contents according to the present invention.

[0025] Figure 2 This is a comparison chart of the gel swelling properties of the sodium carboxymethyl cellulose / polypyrrole composite conductive hydrogel prepared in Example 4.

[0026] Figure 3 This is a comparison chart of the water retention properties of the sodium carboxymethyl cellulose / polypyrrole composite conductive hydrogel prepared in Example 4.

[0027] Figure 4 SEM images of the sodium carboxymethyl cellulose / polypyrrole composite conductive hydrogel (a) prepared in Example 4 and the blank control sample (b).

[0028] Figure 5 This is a physical picture of the sodium carboxymethyl cellulose / polypyrrole composite conductive hydrogel prepared in Example 4 and a blank sample. DETAILED DESCRIPTION

[0029] The present invention will be further described below in conjunction with specific examples. These examples are only used to illustrate the present invention and are not intended to limit the scope of the present invention.

[0030] Instruments and equipment used in the present invention:

[0031] Low temperature constant temperature cooling bath: produced by Gongyi Jinghua Instrument, model DFY-1400;

[0032] Freeze dryer: produced by Shanghai Jingqi Instrument, model: DYYB-18;

[0033] Dielectric constant tester: produced by Shenzhen Deka Precision Measuring Instrument, model: DZ5000;

[0034] Cold field emission scanning electron microscope: Hitachi, model: S-48DD.

[0035] Example 1

[0036] (1) 0.15 g of sodium carboxymethyl cellulose was slowly added to 20 mL of deionized water and stirred at room temperature for 40 min to completely dissolve the sodium carboxymethyl cellulose, thereby preparing a sodium carboxymethyl cellulose aqueous solution with a mass concentration of 0.74%.

[0037] (2) 4 g of acrylamide, 0.06 g of N,N'-methylenebisacrylamide, 0.3 g of potassium persulfate and 10 μl of tetramethylethylenediamine were added to the above sodium carboxymethylcellulose aqueous solution and stirred to dissolve.

[0038] (3) The dissolved solution was placed in a 35°C thermostat for 6 hours to undergo a thermal crosslinking reaction to obtain a sodium carboxymethyl cellulose hydrogel. (4) 0.2 ml of pyrrole, 5 ml of phytic acid, and 100 mL of deionized water were prepared into a phytic acid solution of pyrrole (prepared and used immediately), and the sodium carboxymethyl cellulose hydrogel was placed in 100 mL of the phytic acid solution of pyrrole and allowed to stand for 3 hours to obtain a sodium carboxymethyl cellulose / polypyrrole composite hydrogel.

[0039] (5) The sodium carboxymethyl cellulose / polypyrrole composite hydrogel was washed with distilled water until neutral, and then placed in a refrigerator for pre-freezing and then dried in a freeze dryer at -50°C for 50 h to obtain the sodium carboxymethyl cellulose / polypyrrole composite conductive hydrogel PPY-CNF-1.

[0040] Example 2

[0041] (1) Slowly add 0.15 g of sodium carboxymethyl cellulose into 20 mL of deionized water and stir at room temperature for 40 min to completely dissolve the sodium carboxymethyl cellulose to prepare a sodium carboxymethyl cellulose aqueous solution with a mass concentration of 0.74%.

[0042] (2) 4 g of acrylamide, 0.06 g of N,N'-methylenebisacrylamide, 0.3 g of potassium persulfate and 10 μl of tetramethylethylenediamine were added dropwise to the above sodium carboxymethylcellulose aqueous solution and stirred to dissolve.

[0043] (3) The dissolved solution was placed in a 35°C thermostat for 6 hours to undergo a thermal crosslinking reaction to obtain a sodium carboxymethyl cellulose hydrogel. (4) 0.3 ml of pyrrole, 5 ml of phytic acid, and 100 mL of deionized water were prepared into a pyrrole phytic acid solution (prepared and used immediately), and the sodium carboxymethyl cellulose hydrogel was placed in 100 mL of the pyrrole phytic acid solution and allowed to stand for 3 hours to obtain a sodium carboxymethyl cellulose / polypyrrole composite hydrogel.

[0044] (5) The sodium carboxymethyl cellulose / polypyrrole composite hydrogel was washed with distilled water until neutral, and then placed in a refrigerator for pre-freezing and then dried in a freeze dryer at -50°C for 50 h to obtain the sodium carboxymethyl cellulose / polypyrrole composite conductive hydrogel PPY-CNF-2.

[0045] Example 3

[0046] (1) Slowly add 0.15 g of sodium carboxymethyl cellulose into 20 mL of deionized water and stir at room temperature for 40 min to completely dissolve the sodium carboxymethyl cellulose to prepare a sodium carboxymethyl cellulose aqueous solution with a mass concentration of 0.74%.

[0047] (2) 4 g of acrylamide, 0.06 g of N,N'-methylenebisacrylamide, 0.3 g of potassium persulfate and 10 μl of tetramethylethylenediamine were added dropwise to the above sodium carboxymethylcellulose aqueous solution and stirred to dissolve.

[0048] (3) The dissolved solution was placed in a 35°C thermostat for 6 hours to undergo a thermal crosslinking reaction to obtain a sodium carboxymethyl cellulose hydrogel. (4) 0.4 ml of pyrrole, 5 ml of phytic acid, and 100 mL of deionized water were prepared into a phytic acid solution of pyrrole (prepared and used immediately), and the sodium carboxymethyl cellulose hydrogel was placed in 100 mL of the phytic acid solution of pyrrole and allowed to stand for 3 hours to obtain a sodium carboxymethyl cellulose / polypyrrole composite hydrogel.

[0049] (5) The sodium carboxymethyl cellulose / polypyrrole composite hydrogel was washed with distilled water until neutral, and then placed in a refrigerator for pre-freezing and then dried in a freeze dryer at -50°C for 50 h to obtain the sodium carboxymethyl cellulose / polypyrrole composite conductive hydrogel PPY-CNF-3.

[0050] Example 4

[0051] (1) Slowly add 0.15 g of sodium carboxymethyl cellulose into 20 mL of deionized water and stir at room temperature for 40 min to completely dissolve the sodium carboxymethyl cellulose to prepare a sodium carboxymethyl cellulose aqueous solution with a mass concentration of 0.74%.

[0052] (2) 4 g of acrylamide, 0.06 g of N,N'-methylenebisacrylamide, 0.3 g of potassium persulfate and 10 μl of tetramethylethylenediamine were added to the above sodium carboxymethylcellulose aqueous solution and stirred to dissolve.

[0053] (3) The dissolved solution was placed in a 35°C thermostat for 6 hours to undergo a thermal crosslinking reaction to obtain a sodium carboxymethyl cellulose hydrogel. (4) 0.5 ml of pyrrole, 5 ml of phytic acid, and 100 mL of deionized water were prepared into a pyrrole phytic acid solution (prepared and used immediately), and the sodium carboxymethyl cellulose hydrogel was placed in 100 mL of the pyrrole phytic acid solution and allowed to stand for 3 hours to obtain a sodium carboxymethyl cellulose / polypyrrole composite hydrogel.

[0054] (5) The sodium carboxymethyl cellulose / polypyrrole composite hydrogel was washed with distilled water until neutral, and then placed in a refrigerator for pre-freezing and then placed in a freeze dryer at -50°C for 50 h to obtain the sodium carboxymethyl cellulose / polypyrrole composite conductive hydrogel PPY-CNF-4.

[0055] Example 5

[0056] (1) Slowly add 0.15 g of sodium carboxymethyl cellulose into 20 mL of deionized water and stir at room temperature for 40 min until the sodium carboxymethyl cellulose is completely dissolved to prepare a sodium carboxymethyl cellulose aqueous solution with a mass concentration of 0.74%.

[0057] (2) 4 g of acrylamide, 0.06 g of N,N'-methylenebisacrylamide, 0.3 g of potassium persulfate and 10 μl of tetramethylethylenediamine were added dropwise to the above sodium carboxymethylcellulose aqueous solution and stirred to dissolve.

[0058] (3) The dissolved solution was placed in a 35°C thermostat for 6 hours to undergo a thermal crosslinking reaction to obtain a sodium carboxymethyl cellulose hydrogel. (4) 0.6 ml of pyrrole, 5 ml of phytic acid, and 100 mL of deionized water were prepared into a phytic acid solution of pyrrole (prepared and used immediately), and the sodium carboxymethyl cellulose hydrogel was placed in 100 mL of the phytic acid solution of pyrrole and allowed to stand for 3 hours to obtain a sodium carboxymethyl cellulose / polypyrrole composite hydrogel.

[0059] (5) The sodium carboxymethyl cellulose / polypyrrole composite hydrogel was washed with distilled water until neutral, and then placed in a refrigerator for pre-freezing and then placed in a freeze dryer at -50°C for 50 h to obtain the sodium carboxymethyl cellulose / polypyrrole composite conductive hydrogel PPY-CNF-5.

[0060] Table 1 shows the density and water content of the sodium carboxymethyl cellulose / polypyrrole composite conductive hydrogels prepared in Examples 1-5 and blank samples; According to Table 1, the average density of the sodium carboxymethyl cellulose-polypyrrole composite conductive hydrogel is about 1.55 g / cm 3 , slightly higher than the PPY-CNF-K prepared in step (3), with an average moisture content of about 76.74%.

[0061] Table 1

[0062] Gel samples Pyrrole dosage (mL) <![CDATA[Density (g / cm 3 )]]> Moisture content (%) PPY-CNF-1 0.2 1.4934 76.36% PPY-CNF-2 0.3 1.4736 79.70% PPY-CNF-3 0.4 1.5872 71.2% PPY-CNF-4 0.5 1.5414 76.65% PPY-CNF-5 0.6 1.6517 76.92% PPY-CNF-K 0.0 1.4294 81.07%

[0063] Figure 1 The water absorption performance test shows that the water absorption of the hydrogel samples compounded with polypyrrole is generally lower than that of the blank samples. The 0.5 ml pyrrole monomer sample of Example 4 shows outstanding water absorption performance.

[0064] Figure 2 The swelling performance test results of the hydrogel samples are shown in Figure 2. Figure 2 It can be seen that the composite conductive hydrogel sample prepared in Example 4 has the most outstanding water absorption performance. The hydrogel with high water absorption rate can absorb more water, increase the concentration of the conductive carrier therein, and improve the conductive performance.

[0065] Figure 3 The results of the water retention test on the sample of Example 4 are as follows. Figure 3 It can be seen that after 5 days, the water retention rate is still 94.69%. The high water retention rate means that the hydrogel can effectively retain water, maintain the stability of the conductive carrier, and thus maintain its conductive properties.

[0066] Figure 4 1 is a scanning electron microscope image of the composite conductive hydrogel and a blank sample prepared in Example 4. From the analysis of the microscopic morphology, it can be seen that the composite conductive hydrogel has a significantly more honeycomb porous network structure inside than the blank hydrogel, and its pores are also larger than those of the blank sample.

[0067] Table 2

[0068]

[0069] Table 2 shows the conductivity test results of the composite conductive hydrogels prepared in Examples 1-4 and blank samples. The results show that when the pyrrole content is 0.5 ml, the conductivity can reach 6.07×10 -2 S / m, compared with 8.04×10 -3 From the comparison of S / m, the addition of polypyrrole significantly improves the conductivity of the gel, which is due to the honeycomb porous network structure that improves the effectiveness of the ion migration channel.

[0070] In the above, the present invention focuses on testing the water absorption rate and water retention rate. The water absorption performance is good, and it can fully absorb water during the preparation process to form a uniform gel structure. The water retention is strong, and the structural integrity of the gel can be maintained to a certain extent to avoid excessive shrinkage. The conductivity test can measure whether the material has a certain ion conduction channel, which lays the foundation for ion diffusion in the subsequent carbonization process. It can maintain structural stability, multi-level pore distribution, and hard carbon materials with high specific surface area during the carbonization process.

Claims

1. A method for preparing a sodium carboxymethylcellulose / polypyrrole composite conductive hydrogel, characterized in that: The specific steps are as follows: (1) Preparation of sodium carboxymethyl cellulose hydrogel A certain amount of sodium carboxymethyl cellulose is added to 20 mL of deionized water until the sodium carboxymethyl cellulose is completely dissolved to obtain a sodium carboxymethyl cellulose aqueous solution with a mass concentration of 0.5-1%, and then acrylamide, N, N'-methylenebisacrylamide, potassium persulfate and 8-15 μL of tetramethylethylenediamine as a co-initiator are added to the sodium carboxymethyl cellulose aqueous solution. After the addition, the mixture is continuously stirred at a temperature of 35-45° C. for cross-linking reaction to obtain a sodium carboxymethyl cellulose hydrogel; wherein the mass ratio of sodium carboxymethyl cellulose, acrylamide, N, N-bismethylacrylamide and potassium persulfate is (0.1-0.2):4:(0.04-0.08):(0.2-0.4); (2) Preparation of sodium carboxymethyl cellulose / polypyrrole composite hydrogel The sodium carboxymethyl cellulose hydrogel prepared in step (1) is immersed in 100 mL of phytic acid solution containing pyrrole, and after standing for 3-4 hours, the sample is taken out and washed to obtain a sodium carboxymethyl cellulose / polypyrrole composite hydrogel; (3) Preparation of sodium carboxymethyl cellulose / polypyrrole composite conductive hydrogel The sodium carboxymethyl cellulose / polypyrrole composite hydrogel is freeze-dried to obtain the sodium carboxymethyl cellulose / polypyrrole conductive hydrogel.

2. The preparation method according to claim 1, characterized in that: In step (1), during the cross-linking reaction, the stirring speed is 300-500 rpm and the reaction time is 5-10 h.

3. The preparation method according to claim 1, characterized in that: In step (2), the phytic acid solution containing pyrrole is prepared by mixing pyrrole, phytic acid and water in a volume ratio of (0.1-0.6):(3-8):

100.

4. The preparation method according to claim 3, characterized in that: In step (2), the phytic acid solution containing pyrrole is prepared by mixing pyrrole, phytic acid and water in a volume ratio of (0.4-0.5):5:

100.

5. The preparation method according to claim 1, characterized in that: In step (2), washing is performed with water.

6. The preparation method according to claim 1, characterized in that: In step (3), the product is first placed in a refrigerator for pre-freezing for 12-24 hours, and then freeze-dried in a freeze dryer at a temperature of -30 to -50°C for 24 to 50 hours.

7. A sodium carboxymethyl cellulose / polypyrrole composite conductive hydrogel prepared according to the preparation method according to any one of claims 1 to 6.

Citation Information

Cited By

  • Ionic thermoelectric gel material and preparation method and application thereof

    CN120137102A

  • Ionic thermoelectric gel material, preparation method and application thereof

    CN120137102B