Modified silicon-carbon negative electrode slurry and its preparation method, and its application in negative electrode sheets and lithium-ion batteries.

By coating a Li3PO4 interface modification layer and treating it with a silane coupling agent in silicon-carbon slurry with a modified garnet-type solid electrolyte functional additive, a negative electrode sheet was prepared. This solved the problems of volume expansion of silicon-based materials and SEI film rupture, improved the cycle life and electrochemical performance of lithium-ion batteries, and is suitable for large-scale application in existing production lines.

CN123120738APending Publication Date: 2026-11-17SHANDONG MAOHUA NEW ENERGY TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611624057.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-20
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

In existing technologies, the theoretical specific capacity of graphite anodes is insufficient. The volume expansion of silicon-based materials during lithiation leads to structural damage and repeated rupture of the SEI film, increasing interfacial impedance. Furthermore, existing silicon-carbon composite technologies suffer from complex equipment, high costs, and poor safety, making them difficult to apply on a large scale in the field of power batteries.

Method used

A modified silicon-carbon negative electrode slurry is used. Modified garnet-type solid electrolyte functional additives, such as LLZO or LLZTO, are added to an aqueous solvent. The surface is coated with a Li3PO4 interface modification layer and treated with a silane coupling agent to prepare a negative electrode sheet, forming a stable SEI film and suppressing volume expansion and active lithium loss.

Benefits of technology

It significantly improves the cycle life and electrochemical performance of lithium-ion batteries, solves the problems of volume expansion and SEI film rupture in silicon-carbon anodes, is suitable for large-scale application in existing production lines, has controllable costs, and is compatible with different systems of aqueous binders and liquid electrolytes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123120738A_ABST
    Figure CN123120738A_ABST
Patent Text Reader

Abstract

This invention belongs to the field of lithium-ion battery technology, specifically relating to modified silicon-carbon anode slurry, its preparation method, anode sheets, and lithium-ion batteries. The modified silicon-carbon anode slurry includes silicon-carbon anode active materials; the modified garnet-type solid electrolyte functional additive is one or both of first modified particles and second modified particles; the first modified particles are particles whose surface has been phosphorylated to form an in-situ Li3PO4 interface modification layer; the second modified particles are particles whose surface has been coated with a silane coupling agent. The modified silicon-carbon anode slurry and its preparation method of this invention solve the processing problems of lithium ion dissolution, sudden increase in slurry viscosity, and particle agglomeration and sedimentation when garnet solid electrolyte powder is added to aqueous slurries; using this slurry to prepare anode sheets can mitigate the volume expansion of silicon-carbon anodes, stabilize the SEI interface, and reduce active lithium loss; using the anode sheets in lithium-ion batteries significantly improves the cycle life and electrochemical performance of lithium-ion batteries.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of lithium-ion battery technology, specifically relating to modified silicon-carbon negative electrode slurry and its preparation method, as well as negative electrode sheets and lithium-ion batteries. Background Technology

[0002] Lithium-ion batteries are widely used in electric vehicles, portable electronic devices, and large-scale energy storage power stations. Graphite anode materials have stable cycle performance and low cost; however, the theoretical specific capacity of traditional graphite anodes is only 372 mAh / g, which is insufficient to meet the development requirements of high-energy-density batteries. Silicon-based materials have higher theoretical specific capacity and suitable lithium intercalation potential, making them the preferred anode materials. However, silicon-based materials face two major obstacles in practical applications: First, silicon undergoes a huge volume expansion (up to 300% or more) during lithiation, and this drastic volume change leads to particle cracking, pulverization, and even detachment from the current collector. Second, the dramatic volume change causes repeated rupture and reconstruction of the solid electrolyte interphase (SEI) film, continuously consuming electrolyte and active lithium ions, forming an excessively thick SEI film, significantly increasing interfacial impedance and reducing coulombic efficiency. Finally, the overall structural integrity of the electrode is compromised, leading to serious problems such as cracking, detachment, and even electrode breakage.

[0003] Currently, the preparation of silicon-carbon anodes involves uniformly dispersing nano-silicon within a carbon matrix and achieving effective coating. Different process routes exhibit significant differences in dispersion uniformity, interfacial bonding strength, production cost, and scalability. Mechanical ball milling is primarily used to produce low-capacity (400-600 mAh / g) silicon-carbon anodes for consumer electronics and low-end power applications. Its advantages include simple process, low equipment investment, and ease of scaling. However, uneven silicon particle dispersion and agglomeration lead to poor cycle performance. Chemical vapor deposition (CVD) utilizes a porous carbon framework to effectively buffer volume expansion, controlling the expansion rate to within 8%. However, it involves complex equipment, high investment costs, and the flammability and explosiveness of silane gas necessitate stringent safety requirements. Despite significant progress in silicon-carbon composite technology, its substantial volume expansion effect remains the most fundamental problem hindering large-scale application.

[0004] To address these issues, various silicon-carbon composite structures have been proposed, such as core-shell structures, yolk-shell structures, porous structures, embedded structures, and three-dimensional conductive network structures. These structures utilize conductive agents such as single-walled carbon nanotubes, graphene, and conductive polymers to optimize cycle stability. Alternatively, pre-lithiation of the negative electrode and lithium supplementation of the positive electrode can improve the battery's chemical performance. However, these technologies focus on the complex modification of the silicon-carbon materials themselves and significant adjustments to the battery system, increasing the complexity and cost of battery production. This has resulted in slow industrialization of silicon-carbon anodes, high costs, and limited large-scale application in the power battery field.

[0005] CN114639868A discloses a negative electrode sheet for lithium batteries, which directly introduces oxide solid electrolyte particles into the negative electrode material layer and disperses them between the negative electrode active material particles. It mainly uses lithium aluminum phosphorus oxygen materials containing hydrogen and halogens, focusing on improving the thermal stability and safety of the battery. However, some additive preparation routes have long sintering times and many post-processing steps, and lack systematic verification of the long-term storage stability of the slurry and the effect of improving the rate and cycle performance of silicon-based negative electrodes.

[0006] The paper "Mechanism Study on Garnet-type Li" was published in the *Journal of Inorganic Materials*, Volume 37, Issue 7, July 2022, DOI: 10.15541 / jim20220196. 6.4 La3Zr 1.4 Ta 0.6 O 12 Regulating the Solid Electrolyte Interphases of Si / C Anodes (Garnet-type Li) 6.4 La3Zr 1.4 Ta 0.6 O 12 The study on the mechanism of regulating the solid electrolyte interface of silicon-carbon anode disclosed the use of LLZTO (tantalum-doped garnet-type lithium lanthanum zirconium oxide solid electrolyte) to regulate the SEI of Si / C anode. However, this method involves mixing LLZTO with PVDF and coating it onto the surface of a polypropylene separator to form a PP-LLZTO separator. The LLZTO is located on the separator side rather than being directly added to the silicon-carbon anode slurry. The additional separator coating and drying process increases the mass and thickness of the inactive components. At the same time, since the LLZTO is fixed on the separator side and not directly distributed inside the silicon-carbon anode, it cannot provide direct structural support between the anode particles, nor does it solve the dispersion and processing compatibility problems when the solid electrolyte particles are directly added to the aqueous silicon-carbon slurry. Summary of the Invention

[0007] The technical problem to be solved by this invention is to overcome the above-mentioned defects in the prior art and to provide a modified silicon-carbon negative electrode slurry and its preparation method to solve the processing problem of the sudden increase in slurry viscosity and particle agglomeration and sedimentation caused by residual alkali when adding garnet solid electrolyte powder to aqueous silicon-carbon slurry; using this slurry to prepare negative electrode sheets can suppress the volume expansion of silicon-carbon negative electrodes, stabilize the SEI interface, and reduce the loss of active lithium; when the prepared negative electrode sheets are used in lithium-ion batteries, the cycle life and electrochemical performance of lithium-ion batteries are significantly improved.

[0008] The modified anode silicon-carbon slurry of the present invention includes an anode active material, an aqueous binder, a modified garnet-type solid electrolyte functional additive, a conductive agent, and an aqueous solvent, wherein the aqueous solvent adjusts the solid content of the slurry to be 45-55%.

[0009] The aqueous solvent is a mixture of anhydrous ethanol and water in a volume ratio of 2:8.

[0010] The negative electrode active material is a silicon-carbon composite material; according to the supplier's technical specifications, its first reversible capacity (1.5V) quality standard is ≥1800mAh / g, its first coulombic efficiency (1.5V) quality standard is ≥92%, and its particle size D50 quality standard is 8.0±2.0μm.

[0011] The modified garnet-type solid electrolyte functional additive is one or both of the first modified particles and the second modified particles; the first modified particles are LLZO (lithium lanthanum zirconium oxide solid electrolyte) or LLZTO (tantalum-doped garnet-type lithium lanthanum zirconium oxide solid electrolyte) particles whose surface has been phosphorylated to form a Li3PO4 interface modification layer in situ; the second modified particles are LLZO or LLZTO particles whose surface has been coated with a silane coupling agent.

[0012] The modified silicon-carbon anode slurry, based on 100% solids mass, comprises the following components: 90% silicon-carbon anode active material. 95%, modified garnet-type solid electrolyte functional additive 1% 5%, conductive agent 1% 5%, water-based adhesive 3% 6%.

[0013] The particle size D50 of the modified garnet-type solid electrolyte functional additive is 50 nm. 5μm, preferably 100nm 1μm; The water-based binder is one or more of the following compound systems: polyacrylic acid (PAA), lithium-ionized polyacrylic acid (PAA-Li), and carboxymethyl cellulose (CMC). The conductive agent is selected from Super P, KS 6. At least one of carbon black, carbon nanofibers, carbon nanotubes, acetylene black, and graphene.

[0014] The Li3PO4 interface modification layer on the surface of the first modified particle is generated by reacting a phosphorus source with LLZO or LLZTO particles in an organic solvent system.

[0015] The silane coupling agent of the second modified particle is selected from KH 550, KH 560, KH One or more of 570 in combination.

[0016] The method for preparing the modified negative electrode silicon-carbon slurry includes the following steps: S1: Add the modified garnet-type solid electrolyte functional additive to an aqueous solvent and disperse it at 1000 rpm for 2 hours to obtain a solid electrolyte dispersion. The modified garnet-type solid electrolyte functional additive is one or both of the first modified particles and the second modified particles. S2: Add the negative electrode active material, conductive agent, and aqueous binder to the solid electrolyte dispersion obtained in step S1, mix evenly, and prepare a modified negative electrode silicon-carbon slurry with a solid content of 45%~55%. Solid content refers to mass content.

[0017] The preparation steps of the first modified particles include: (1) Disperse LLZO or LLZTO with citric acid (the mass ratio of LLZO or LLZTO to citric acid is 1:1.14) in anhydrous ethanol and / or isopropanol organic solvent, with a powder concentration of 100 g / L; when the two are combined, the volume ratio of anhydrous ethanol to isopropanol is 1:1; stir in the organic solvent at 50°C and 800 rpm for 2 h to obtain a suspension; (2) Continue to add phosphoric acid so that the molar ratio of phosphoric acid to citric acid is 1:3, and react at a constant temperature of 50℃ and a rotation speed of 800rpm for 4 hours. (3) Finally, wash with anhydrous ethanol and centrifuge at high speed at least three times; (4) Drying the solid powder in a vacuum oven at 70°C for 12 hours to obtain the first modified particles with phosphorylation treatment and in-situ Li3PO4 interface modification layer, labeled as LLZO@LPO or LLZTO@LPO.

[0018] The preparation steps of the second modified particles include: (1) Disperse 10g of LLZO or LLZTO powder in 50mL of isopropanol and stir at 50℃ and 800rpm for 2h to obtain a suspension; (2) Add acetic acid to the ethanol-water solution (anhydrous ethanol to water volume ratio 9:1) to adjust the pH to 4.5. 5. Add silane coupling agent and pre-hydrolyze for 30 min to obtain a pre-hydrolyzed solution; the silane coupling agent is one of KH-550, KH-560, and KH-570.

[0019] (3) Add 10 mL of pre-hydrolyzed solution dropwise to 50 mL of suspension and stir at 60 °C for 5 h; (4) After the reaction is complete, centrifuge and wash three times with anhydrous ethanol, and collect the solid; (5) Dry in a vacuum oven at 80°C for 12 hours, then place in a drying oven at 150°C for 2 hours to obtain the second modified particles coated with silane coupling agent, LLZO@KH or LLZTO@KH.

[0020] The modified silicon-carbon slurry is used to prepare the negative electrode sheet. The modified silicon-carbon slurry is coated on the surface of the current collector copper foil, and then baked, rolled, die-cut, and baked again. The negative electrode sheet is then dried in a vacuum drying oven at 120°C for 12 hours and cut into 12mm round sheets.

[0021] The lithium-ion battery includes a negative electrode, a positive electrode (NCM811), a separator made of microporous polypropylene membrane (Celgard2500), and an electrolyte of 1 mol / L LiPF6EC:DMC:EMC=1:1:1 containing 10 wt% FEC from Shanghai Songjing New Energy Technology Co., Ltd.

[0022] The modified particles of this invention utilize phosphoric acid modification to convert the residual LiOH and Li2CO3 alkali on the LLZO / LLZTO surface into near-neutral Li3PO4; silane coating introduces organic functional groups; and the slurry pH is reduced from the original 11. 13 dropped to 8 9. Weakly alkaline range; avoids excessive swelling and chain breakage of CMC, completely solving the pain points of viscosity spikes and flocculation failure when unmodified garnet powder is added to aqueous slurries; improves the dispersion of powder in the aqueous phase, reducing sedimentation, particle protrusion, and coating defects. Maintains PAA / PAA in a weakly alkaline environment. The charge properties of Li, together with CMC and silicon-carbon particles, form a stable colloidal network, which constrains the volume expansion of silicon lithium intercalation and inhibits particle pulverization.

[0023] The in-situ Li3PO4 of this invention is a fast lithium-ion conductor, which is tightly bonded to the garnet matrix and has low interfacial contact impedance. It forms a diffusely distributed lithium-ion transport network inside the negative electrode, improving ion conduction at high rates.

[0024] The modified particles of this invention can induce the formation of a thin, dense, and stable SEI film on the surface of silicon-carbon anodes, reducing SEI cracking caused by repeated expansion and contraction of silicon. Regeneration cycle significantly reduces electrolyte consumption and irreversible loss of active lithium, mitigating the capacity decay of silicon-carbon anodes during cycles.

[0025] Compared with the prior art, the beneficial effects of the present invention are: (1) This invention has good processing adaptability and is designed for phosphorylation and silane surface modification of garnet solid electrolyte powder, thus solving the problem of Li-oxidation when LLZO or LLZTO powder comes into contact with water. + / H + The ion exchange reaction releases LiOH into the aqueous solution, causing the pH of the slurry to rise rapidly to a strong alkaline state. This ultimately leads to a technical challenge of the viscosity of the aqueous silicon-carbon slurry soaring and causing agglomeration and sedimentation. The slurry has a wide processing window and is suitable for existing industrial coating production of aqueous silicon-carbon anodes.

[0026] (2) This invention does not require modification of existing materials and production lines, nor does it require complex modifications such as coating or nano-sizing of silicon-carbon active materials; the electrode uses the existing coating, drying and rolling process, without the need for new equipment, and is directly compatible with existing liquid lithium-ion battery production lines, which can be quickly scaled up.

[0027] (3) The present invention significantly improves the cycle performance. The modified garnet solid electrolyte is directly doped into the negative electrode slurry, and a diffuse ion conduction network is constructed inside the silicon-carbon negative electrode to induce the formation of a stable SEI film, reduce the loss of active lithium, and effectively suppress the cycle capacity decay of the silicon-carbon negative electrode.

[0028] (4) This invention has strong versatility and controllable cost. The amount of solid electrolyte added is low, and the overall cost increase is small. It can be compatible with different systems of aqueous binders, commercial silicon carbon materials and conventional liquid electrolytes. It is suitable for both traditional liquid lithium batteries and solid-liquid hybrid lithium batteries. Attached Figure Description

[0029] Figure 1 The images show X-ray diffraction (XRD) patterns of the LLZTO powder used in this invention, the LLZTO@LPO powder prepared in Example 1, and the LLZTO standard PDF card.

[0030] Figure 2 This is a high-resolution transmission electron microscope (TEM) image of the first modified particle LLZTO@LPO prepared in Example 1 of the present invention.

[0031] Figure 3 The image shows the Raman spectrum of the first modified particle LLZTO@LPO prepared in Example 1 of this invention.

[0032] Figure 4 The image shows the scanning electron microscope (SEM) morphology of the second modified particle LLZTO@KH prepared in Example 2 of this invention.

[0033] Figure 5 The image shows the Fourier Transform Infrared (FTIR) spectrum of the second modified particle LLZTO@KH prepared in Example 2 of this invention. Detailed Implementation

[0034] The present invention will be further described below with reference to specific embodiments. Unless otherwise specified, all raw materials used in the present invention are commercially available raw materials.

[0035] Si / C composite material: specific capacity of 1800 mAh / g, initial efficiency of 92%, and D50 of 8.0±2.0 μm.

[0036] LLZTO powder: particle size D50 is 500 nm, specific surface area is 25.2462 m². 2 / g, with a residual alkali content of 20.26%.

[0037] LLZO powder: particle size D50 is 500 nm, specific surface area is 22.4731 m². 2 / g, with a residual alkali content of 22.59%.

[0038] Phosphoric acid: content >85wt%.

[0039] Positive electrode: NCM811, supplier COA; Current collector: copper foil, 8μm thick.

[0040] Separator: Celgard 2500 microporous polypropylene membrane.

[0041] Electrolyte: 1 mol / L LiPF6EC:DMC:EMC = 1:1:1 from Shanghai Songjing New Energy Technology Co., Ltd., containing 10 wt% FEC.

[0042] I. The general slurry preparation method of the present invention: S1: Add the modified garnet-type solid electrolyte functional additive to an aqueous solvent and disperse it at high speed at 1000 rpm for 2 hours to obtain a solid electrolyte dispersion. S2: Add the negative electrode active material, conductive agent, and aqueous binder to the solid electrolyte dispersion obtained in step S1, disperse at 1000 rpm for 5 min, then mix at 200 rpm for 2 h, and adjust the solid content to 45%-55% to obtain the modified negative electrode silicon-carbon slurry; the aqueous solvent is a mixture of deionized water and anhydrous ethanol, with anhydrous ethanol:water = 2:8 (volume ratio); the solid content of the slurry is 45%~55%.

[0043] II. The general method for preparing the first modified particles of the present invention: (1) Disperse 10g of LLZO or LLZTO powder in 100ml of a mixture of anhydrous ethanol and isopropanol in a volume ratio of 1:1. Add 11.4g of citric acid, stir at a constant temperature of 800rpm and 50℃ for 2h to obtain a suspension. (2) Add 1.35 mL of phosphoric acid; react at a constant temperature of 50 °C, at a speed of 800 rpm, for 4 h; (3) Solid-liquid separation, washing three times with anhydrous ethanol; (4) Dry at 70℃ for 12 hours to obtain the first modified particles.

[0044] III. The general method for preparing the second modified particles of the present invention: (1) Disperse 10g of LLZO or LLZTO powder in 50mL of isopropanol, stir at 50℃ for 2h at a constant speed of 800rpm to obtain a suspension; (2) Prepare an ethanol aqueous solution with anhydrous ethanol:water volume ratio of 9:1, adjust the pH to 4.5-5 with acetic acid, add silane coupling agent, pre-hydrolyze for 30 min to obtain a pre-hydrolyzed solution; (3) Add the pre-hydrolyzed solution dropwise to the suspension and stir at a constant temperature of 60℃ for 5 hours; (4) Centrifuge and wash three times with anhydrous ethanol, then collect the solid; (5) After drying at 80℃ for 12 hours, the particles were placed in a drying oven and cured at 150℃ for 2 hours to obtain the second modified particles.

[0045] Example 1 The specific steps for preparing the lithium-ion battery according to this invention are as follows: (1) Preparation of the first modified particle LLZTO@LPO: Weigh LLZTO powder (Li 6.4 La3Zr 1.4 Ta 0.6 O 12 10g of LLZTO (with a D50 of 500nm) was dispersed in 100mL of a mixed organic solvent of anhydrous ethanol and isopropanol in a 1:1 volume ratio. 11.4g of citric acid was added, and the mixture was stirred at 50℃ and 800rpm for 2 hours to obtain a suspension. 1.35mL of phosphoric acid was added, and the reaction was carried out at 50℃ and 800rpm for 4 hours, allowing the LiOH and Li2CO3 residues on the LLZTO surface to react in situ with the phosphorus source to form a Li3PO4 interface modification layer. After the reaction, the solid and liquid phases were separated by centrifugation, washed three times with anhydrous ethanol, and dried at 70℃ for 12 hours to obtain the first modified particle with the in-situ Li3PO4 interface modification layer, denoted as LLZTO@LPO. The TEM image of LLZTO@LPO is shown below. Figure 2 As shown, a Li3PO4 layer with a thickness of approximately 8-15 nm is uniformly coated on the surface of the particles. XRD (X-ray diffraction) analysis was performed on the LLZTO powder and the prepared LLZTO@LPO powder, and their spectra are shown below. Figure 1 As shown, Figure 1 From top to bottom, the images show the raw LLZTO powder, the prepared LLZTO@LPO powder, and the LLZTO standard PDF card (PDF#80-0457) spectrum. The spectra show that the diffraction peak positions of the samples before and after coating match well with the standard card. (The text then repeats itself, so the translation stops.) Figure 3 The Raman spectrum shown clearly shows the disappearance of lithium carbonate and the formation of Li3PO4 (LPO).

[0046] (2) Preparation of modified silicon-carbon anode slurry: The formula, based on the percentage of solids by mass, is as follows: silicon-carbon anode active material Si / C 92%, first modified particles LLZTO@LPO 3%, conductive agent Super P 2%, water-based binder (CMC 1.5% and PAA) Li 1.5% compounded, total 3%; added water-based solvent (deionized water and anhydrous ethanol, volume ratio 8:2) to adjust the solid content to 50%.

[0047] First, add LLZTO@LPO to an aqueous solvent according to S1, and disperse at 1000 rpm for 2 hours to obtain a solid electrolyte dispersion; then, add Si / C and Super... P, CMC and PAA Li was added to the dispersion and mixed at 1000 rpm for 5 min, then stirred at 200 rpm for 2 h to obtain the modified silicon-carbon negative electrode slurry. The slurry had a viscosity of 3500 mPa·s at 25℃, showed no sedimentation after standing for 72 h, and had a wide processing window.

[0048] (3) Preparation of negative electrode sheet: The slurry is prepared with an areal density of 0.8 mg / cm³. 2 (Based on negative electrode active material) Coated onto 8μm copper foil, baked at 120℃ to remove solvent, and rolled to a compaction density of 1.5g / cm³. 3 The negative electrode sheet is obtained by die-cutting and vacuum drying at 80℃ for 12 hours.

[0049] (4) Preparation of lithium-ion batteries: Using the negative electrode as the working electrode, commercial NCM811 positive electrode as the positive electrode, Celgard2500 microporous polypropylene membrane as the separator, and 1 mol / L LiPF6 EC:DMC:EMC=1:1:1 (volume ratio) containing 10 wt% FEC as the electrolyte, CR2032 button batteries were assembled in an argon glove box (H2O<0.1ppm, O2<0.1ppm).

[0050] In this embodiment, the battery retains 86.5% capacity after 100 cycles at 2.5-4.3V and 0.5C (1C=200mA / g), with an initial efficiency of 87%, which is significantly better than the additive-free system. Figure 1-3 The presence of the Li3PO4 interface modification layer and its close bonding with the garnet matrix can be observed.

[0051] Example 2 The specific steps for preparing the lithium-ion battery according to this invention are as follows: (1) Preparation of the second modified particle LLZTO@KH: Weigh LLZTO powder (Li 6.4 La3Zr 1.4 Ta 0.6 O 1210 g of a LLZTO particle (D50 = 500 nm) was dispersed in 50 mL of isopropanol solvent and stirred at 50 °C and 800 rpm for 2 h to obtain a suspension. Separately, an ethanol-water solution (anhydrous ethanol:water = 9:1, volume ratio) was prepared, pH adjusted to 4.8 with acetic acid, and 1.10 mL of silane coupling agent KH-560 was added. The solution was pre-hydrolyzed for 30 min to obtain a pre-hydrolyzed solution. This pre-hydrolyzed solution was added dropwise to the suspension and stirred at 60 °C and 500 rpm for 5 h to allow KH-560 to hydrolyze and condense onto the LLZTO surface. After the reaction, the particle was centrifuged, washed three times with anhydrous ethanol, and the solid was collected. After drying at 80 °C for 12 h, the solid was cured at 150 °C for 2 h in a drying oven to obtain the second modified LLZTO@KH particle. Its SEM morphology is shown below. Figure 4 As shown, a continuous organosilicon layer is clearly visible on the particle surface. After centrifugation, the pH of the supernatant decreased to 8.8 when the powder was dispersed in an aqueous solvent at a solid-liquid ratio of 1:10. The second modified particle, LLZTO@KH, was characterized by FTIR infrared spectroscopy, and its spectrum is shown below. Figure 5 As shown, the KH coating was successfully applied to the surface of LLZTO particles.

[0052] (2) Preparation of modified silicon-carbon negative electrode slurry: The formula is as follows based on the percentage of solid mass: silicon-carbon negative electrode active material Si / C 92%, second modified particles LLZTO@KH 3%, conductive agent Super-P 2%, water-based binder (CMC 1.5% and PAA 1.5% compounded, total 3%) 3%; an external water-based solvent (deionized water and anhydrous ethanol volume ratio 8:2) is added to adjust the solid content to 50%.

[0053] First, LLZTO@KH was added to an aqueous solvent according to step S1 and dispersed at 1500 rpm for 60 min to obtain a solid electrolyte dispersion. Then, Si / C, Super-P, CMC, and PAA were added to the dispersion according to step S2 and mixed at 500 rpm for 4 h to obtain a modified silicon-carbon negative electrode slurry. The viscosity of the slurry at 25℃ was approximately 3600 mPa·s.

[0054] (3) Preparation of negative electrode sheet: The slurry with an areal density of 0.8 mg / cm² (based on the negative electrode active material) is coated on an 8 μm copper foil, baked at 120℃ to remove the solvent, and rolled to a compaction density of 1.5 g / cm². 3 The negative electrode sheet is obtained by die-cutting and vacuum drying at 80℃ for 12 hours.

[0055] (4) Preparation of lithium-ion batteries: Using the negative electrode as the working electrode, a commercial NCM811 positive electrode as the positive electrode, a Celgard 2500 microporous polypropylene membrane as the separator, and a 1 mol / L LiPF6 electrolyte containing EC:DMC:EMC = 1:1:1 (volume ratio) and 10 wt% FEC, CR2032 button batteries were assembled in an argon glove box (H2O < 0.1 ppm, O2 < 0.1 ppm). In this embodiment, only the aqueous binder system is CMC-PAA.

[0056] In this embodiment, the battery maintained a capacity retention of 83.5% and an initial efficiency of 85.0% after 100 cycles at 2.5-4.3V and 0.5C (1C=200mA / g), proving that silane coating modification is also effective and compatible with different aqueous binder systems.

[0057] Example 3 The specific steps for preparing the lithium-ion battery according to this invention are as follows: (1) Preparation of modified garnet-type solid electrolyte functional additives: Preparation of the first modified particle LLZTO@LPO: Weigh LLZTO powder (Li 6.4 La3Zr 1.4 Ta 0.6 O 12 10g of LLZTO (with a D50=500nm) was dispersed in 100mL of a mixed organic solvent of anhydrous ethanol and isopropanol in a 1:1 volume ratio. 11.4g of citric acid was added, and the mixture was stirred at 50℃ and 800rpm for 2 hours to obtain a suspension. 1.35mL of phosphoric acid was added, and the reaction was carried out at 50℃ and 800rpm for 4 hours, allowing the LiOH and Li2CO3 residues on the LLZTO surface to react in situ with the phosphorus source to form a Li3PO4 interface modification layer. After the reaction, the solid and liquid phases were separated by centrifugation, washed three times with anhydrous ethanol, and dried at 70℃ for 12 hours to obtain the first modified particle with the in-situ Li3PO4 interface modification layer, denoted as LLZTO@LPO.

[0058] Preparation of the second modified particle LLZTO@KH: Weigh LLZTO powder (Li 6.4 La3Zr 1.4 Ta 0.6 O 1210g of anhydrous ethanol (D50=500nm) was dispersed in 50mL of isopropanol solvent and stirred at 50℃ and 800rpm for 2h to obtain a suspension. Separately, an ethanol-water solution (anhydrous ethanol:water = 9:1, volume ratio) was prepared, pH adjusted to 4.8 with acetic acid, and 1.10mL of silane coupling agent KH-560 was added. The solution was pre-hydrolyzed for 30min to obtain a pre-hydrolyzed solution. This pre-hydrolyzed solution was added dropwise to the suspension and stirred at 60℃ and 500rpm for 5h to allow KH-560 to hydrolyze and condense onto the LLZTO surface. After the reaction, the mixture was centrifuged, washed three times with anhydrous ethanol, and the solid was collected. After drying at 80℃, the solid was cured at 150℃ for 2h in a drying oven to obtain the second modified particle, LLZTO@KH.

[0059] (2) Preparation of modified silicon-carbon negative electrode slurry: The formula is as follows based on the percentage of solid mass: silicon-carbon negative electrode active material Si / C 92%, first modified particle LLZTO@LPO 1.5%, second modified particle LLZTO@KH 1.5% (total functional additives 3%), conductive agent Super-P 2%, water-based binder (CMC 1.5% and PAA-Li 1.5% compounded, total 3%) 3%; an external water-based solvent (deionized water and anhydrous ethanol volume ratio 8:2) is added to adjust the solid content to 50%.

[0060] First, according to step S1, both types of modified particles were added together to an aqueous solvent and dispersed at 1500 rpm for 60 min to obtain a solid electrolyte dispersion. Then, according to step S2, Si / C, Super-P, CMC, and PAA-Li were added to the dispersion and mixed at 500 rpm for 4 h to obtain a modified negative electrode silicon-carbon slurry. Testing showed that the pH of the mixed modified powder was 8.5, and the viscosity of the slurry at 25℃ was approximately 3400 mPa·s.

[0061] Synergistic effect of two modified particles: Li3PO4 fast ion conductor layer (inorganic hydrophilic) solves Li + / H + Ion exchange reaction and ion network construction, organosilicon layer (hydrophobic) enhance interfacial compatibility with PAA / CMC organic binder and silicon carbon, play a role at the inorganic / organic interface, solve lithium ion dissolution and enhance organic compatibility.

[0062] (3) Preparation of negative electrode sheet: The slurry with a surface density of 0.8 mg / cm² (based on the negative electrode active material) is coated on an 8 μm copper foil, baked at 120°C to remove the solvent, rolled to a compaction density of 1.5 g / cm³, die-cut, and vacuum dried at 80°C for 12 h to obtain the negative electrode sheet.

[0063] (4) Preparation of lithium-ion batteries: Using the negative electrode as the working electrode, commercial NCM811 positive electrode as the positive electrode, Celgard2500 microporous polypropylene membrane as the separator, and 1 mol / L LiPF6 EC:DMC:EMC=1:1:1 (volume ratio) containing 10 wt% FEC as the electrolyte, CR2032 button batteries were assembled in an argon glove box (H2O<0.1ppm, O2<0.1ppm).

[0064] In this embodiment, the battery retains 87.0% capacity after 100 cycles at 2.5-4.3V and 0.5C (1C=200mA / g), has an initial efficiency of 88.0%, and an electrode thickness expansion rate of 26%.

[0065] Example 4 The specific steps for preparing the lithium-ion battery according to this invention are as follows: (1) Preparation of the first modified particle LLZTO@LPO: Weigh LLZTO powder (Li 6.4 La3Zr 1.4 Ta 0.6 O 12 10g of LLZTO (with a D50=500nm) was dispersed in 100mL of a mixed organic solvent of anhydrous ethanol and isopropanol in a 1:1 volume ratio. 11.4g of citric acid was added, and the mixture was stirred at 50℃ and 800rpm for 2 hours to obtain a suspension. 1.35mL of phosphoric acid was added, and the reaction was carried out at 50℃ and 800rpm for 4 hours, allowing the LiOH and Li2CO3 residues on the LLZTO surface to react in situ with the phosphorus source to form a Li3PO4 interface modification layer. After the reaction, the solid and liquid phases were separated by centrifugation, washed three times with anhydrous ethanol, and dried at 70℃ for 12 hours to obtain the first modified particle with the in-situ Li3PO4 interface modification layer, denoted as LLZTO@LPO.

[0066] (2) Preparation of modified silicon-carbon negative electrode slurry: The formula is as follows based on the percentage of solid mass: silicon-carbon negative electrode active material Si / C 90%, first modified particle LLZTO@LPO 5%, conductive agent Super-P 2%, water-based binder (CMC 1.5% and PAA-Li 1.5% compounded, total 3%) 3%; an external water-based solvent (deionized water and anhydrous ethanol volume ratio 8:2) is added to adjust the solid content to 50%.

[0067] First, LLZTO@LPO was added to an aqueous solvent according to step S1 and dispersed at 1500 rpm for 60 min to obtain a solid electrolyte dispersion. Then, Si / C, Super-P, CMC, and PAA-Li were added to the dispersion according to step S2 and mixed at 500 rpm for 4 h to obtain a modified silicon-carbon negative electrode slurry. The powder pH was measured to be 8.4, and the slurry viscosity at 25℃ was approximately 3700 mPa·s.

[0068] (3) Preparation of negative electrode sheet: The slurry with a surface density of 0.8 mg / cm² (based on the negative electrode active material) is coated on an 8 μm copper foil, baked at 120°C to remove the solvent, rolled to a compaction density of 1.5 g / cm³, die-cut, and vacuum dried at 80°C for 12 h to obtain the negative electrode sheet.

[0069] (4) Preparation of lithium-ion batteries: Using the negative electrode as the working electrode, commercial NCM811 positive electrode as the positive electrode, Celgard2500 microporous polypropylene membrane as the separator, and 1 mol / L LiPF6 EC:DMC:EMC=1:1:1 (volume ratio) containing 10 wt% FEC as the electrolyte, CR2032 button batteries were assembled in an argon glove box (H2O<0.1ppm, O2<0.1ppm).

[0070] In this embodiment, the battery retains 85.5% capacity after 100 cycles at 2.5-4.3V and 0.5C (1C=200mA / g), with an initial efficiency of 86% and an electrode thickness expansion rate of 27.5%.

[0071] Example 5 The specific steps for preparing the lithium-ion battery according to this invention are as follows: (1) Preparation of the second modified particle LLZTO@KH: Weigh LLZTO powder (Li 6.4 La3Zr 1.4 Ta 0.6 O 12 10g of anhydrous ethanol (D50=500nm) was dispersed in 50mL of isopropanol solvent and stirred at 50℃ and 800rpm for 2h to obtain a suspension. Separately, an ethanol-water solution (anhydrous ethanol:water = 9:1, volume ratio) was prepared, pH adjusted to 4.8 with acetic acid, and 1.10mL of silane coupling agent KH-560 was added. The solution was pre-hydrolyzed for 30min to obtain a pre-hydrolyzed solution. This pre-hydrolyzed solution was added dropwise to the suspension and stirred at 60℃ and 500rpm for 5h to allow KH-560 to hydrolyze and condense onto the LLZTO surface. After the reaction, the mixture was centrifuged, washed three times with anhydrous ethanol, and the solid was collected. After drying at 80℃, the solid was cured at 150℃ for 2h in a drying oven to obtain the second modified particle, LLZTO@KH.

[0072] (2) Preparation of modified silicon-carbon negative electrode slurry: The formula is as follows based on the percentage of solid mass: silicon-carbon negative electrode active material Si / C 90%, second modified particles LLZTO@KH 5%, conductive agent Super-P 2%, water-based binder (CMC 1.5% and PAA 1.5% compounded, totaling 3%) 3%; an external water-based solvent (deionized water and anhydrous ethanol volume ratio 8:2) is added to adjust the solid content to 50%.

[0073] First, LLZTO@KH was added to an aqueous solvent according to step S1 and dispersed at 1500 rpm for 60 min to obtain a solid electrolyte dispersion. Then, Si / C, Super-P, CMC, and PAA were added to the dispersion according to step S2 and mixed at 500 rpm for 4 h to obtain a modified negative electrode silicon-carbon slurry. The powder pH was measured to be 8.7, and the slurry viscosity at 25℃ was approximately 3650 mPa·s.

[0074] (3) Preparation of negative electrode sheet: The slurry with a surface density of 0.8 mg / cm² (based on the negative electrode active material) is coated on an 8 μm copper foil, baked at 120°C to remove the solvent, rolled to a compaction density of 1.5 g / cm³, die-cut, and vacuum dried at 80°C for 12 h to obtain the negative electrode sheet.

[0075] (4) Preparation of lithium-ion batteries: Using the negative electrode as the working electrode, a commercial NCM811 positive electrode as the positive electrode, a Celgard 2500 microporous polypropylene membrane as the separator, and a 1 mol / L LiPF6 electrolyte containing EC:DMC:EMC = 1:1:1 (volume ratio) and 10 wt% FEC, CR2032 button batteries were assembled in an argon glove box (H2O < 0.1 ppm, O2 < 0.1 ppm). In this embodiment, the aqueous binder system is CMC-PAA.

[0076] In this embodiment, the battery retains 81.0% capacity after 100 cycles at 2.5-4.3V and 0.5C (1C=200mA / g), has an initial efficiency of 83.5%, and an electrode thickness expansion rate of 29.5%.

[0077] Example 6 The specific steps for preparing the lithium-ion battery according to this invention are as follows: (1) Preparation of the first modified particle LLZO@LPO: 10g of LLZO powder (D50=500nm) was weighed and dispersed in 100mL of anhydrous ethanol and isopropanol in a 1:1 volume ratio organic solvent. 11.4g of citric acid was added, and the mixture was stirred at 50℃ and 800rpm for 2h to obtain a suspension. 1.35mL of phosphoric acid was added, and the mixture was reacted at 50℃ and 800rpm for 4h to allow the LiOH and Li2CO3 residue on the LLZO surface to react in situ with the phosphorus source to generate Li3PO4 interface modification. After the reaction, the solid and liquid were separated by centrifugation, washed three times with anhydrous ethanol, and dried at 70℃ for 12h to obtain the first modified particle with an in situ Li3PO4 interface modification layer, denoted as LLZO@LPO.

[0078] (2) Preparation of modified silicon-carbon negative electrode slurry: The formula is as follows based on the percentage of solid mass: silicon-carbon negative electrode active material Si / C 92%, first modified particle LLZO@LPO 3%, conductive agent Super-P 2%, water-based binder (CMC 1.5% and PAA-Li 1.5% compounded, total 3%) 3%; an external water-based solvent (deionized water and anhydrous ethanol volume ratio 8:2) is added to adjust the solid content to 50%.

[0079] First, LLZO@LPO was added to an aqueous solvent according to step S1 and dispersed at 1500 rpm for 60 min to obtain a solid electrolyte dispersion. Then, Si / C, Super-P, CMC, and PAA-Li were added to the dispersion according to step S2 and mixed at 500 rpm for 4 h to obtain a modified silicon-carbon negative electrode slurry. Testing showed that the powder had a pH of 8.4, the slurry viscosity at 25℃ was approximately 3620 mPa·s, and it remained stable without settling after standing for 72 h.

[0080] (3) Preparation of negative electrode sheet: The slurry with a surface density of 0.8 mg / cm² (based on the negative electrode active material) is coated on an 8 μm copper foil, baked at 120°C to remove the solvent, rolled to a compaction density of 1.5 g / cm³, die-cut, and vacuum dried at 80°C for 12 h to obtain the negative electrode sheet.

[0081] (4) Preparation of lithium-ion batteries: Using the negative electrode as the working electrode, commercial NCM811 positive electrode as the positive electrode, Celgard2500 microporous polypropylene membrane as the separator, and 1 mol / L LiPF6 EC:DMC:EMC=1:1:1 (volume ratio) containing 10 wt% FEC as the electrolyte, CR2032 button batteries were assembled in an argon glove box (H2O<0.1ppm, O2<0.1ppm).

[0082] In this embodiment, the battery retains 82.0% capacity after 100 cycles at 2.5-4.3V and 0.5C (1C=200mA / g), has an initial efficiency of 84.5%, and an electrode thickness expansion rate of 28.5%.

[0083] Comparative Example 1 In this comparative example, no garnet-type solid electrolyte functional additives were added to the negative electrode slurry. The formulation of the negative electrode silicon-carbon slurry in step (2) of Example 1 was replaced with Si / C 95%, Super P 2%, CMC 1.5%, PAA Li 1.5%, the rest of the formulation and process are the same as in Example 1. Because it does not contain residual alkali powder, the slurry pH is about 8.0 and the viscosity is about 3200 mPa·s, and the processability is good; however, there is no dispersed ion network in the negative electrode, and the volume expansion of silicon carbon is not constrained.

[0084] The battery retains only 77.5% of its capacity after 100 cycles, with an initial efficiency of 80.5%. The electrode thickness expansion rate reaches 34% after 100 cycles, indicating that the capacity decays rapidly without functional additives.

[0085] Comparative Example 2 In this comparative example, in the negative electrode silicon-carbon slurry of step (2) of Example 2, 3% of unmodified LLZTO raw powder (D50=500 nm, residual alkali about 20.26%) directly replaced the second modified particles LLZTO@KH. That is, the negative electrode silicon-carbon slurry formula was replaced with Si / C 92%, unmodified LLZTO raw powder 3%, conductive agent Super-P 2%, CMC 1.5%, PAA 1.5%, and the rest of the process was the same as in Example 2. Due to the LiOH and Li2CO3 on the LLZTO surface causing the slurry pH to rise to 12.5, the CMC excessively swelled, the charge characteristics of PAA were destroyed, the slurry viscosity soared, the capacity retention rate of the coated electrode after 100 cycles was only 73.0%, the initial efficiency was 80.0%, and the thickness expansion rate was 38%.

[0086] Comparative Example 3 In this comparative example, in the negative electrode silicon-carbon slurry of Example 1 (2), 3% of the unmodified LLZTO raw powder (D50=500 nm, residual alkali approximately 20.26%) directly replaced the first modified particles LLZTO@LPO. That is, the formula was Si / C 92%, unmodified LLZTO raw powder 3%, conductive agent Super-P 2%, CMC 1.5%, PAA 1.5%, and the rest of the process was the same as in Example 1. The resulting slurry had a pH of 12.8, a capacity retention rate of 75.5% after 100 cycles, an initial efficiency of 81.0%, and an electrode thickness expansion rate of 37.5%.

[0087] Comparative Example 4 In this comparative example, 6% of unmodified LLZTO raw powder (D50=500 nm, residual alkali approximately 20.26%) directly replaced the second modified LLZTO@KH particles in Example 2. That is, the anode silicon-carbon slurry formulation was replaced with 89% silicon-carbon anode active material Si / C, 6% unmodified LLZTO raw powder, 2% Super-P conductive agent, 1.5% CMC, 1.5% PAA, and the remaining formulation and process were the same as in Example 2.

[0088] The resulting slurry had a pH of 13.2 and a continuously increasing viscosity. After 100 cycles of film formation, the capacity retention rate was only 68.0%, and the electrode thickness expansion rate was 42%.

[0089] (1) The pH and viscosity of the negative electrode slurry prepared in the above examples and comparative examples were tested, and the results are shown in Table 1; (2) The CR2032 coin cells assembled in the examples and comparative examples were tested according to conventional methods in the art and with reference to GB / T 18287. Electrochemical performance was tested in 2013, specifically the initial efficiency and the capacity retention rate after 100 cycles. The results are shown in Table 1. (3) After preparing the negative electrode samples of the examples and comparative examples, the thickness of the negative electrode was measured by micrometer, and the thickness of the corresponding negative electrode after disassembly after 100 cycles of battery electrochemical cycling was measured. The thickness expansion rate after 100 cycles was calculated. Specifically, it was calculated as (thickness after cycling - thickness before cycling) × 100% / thickness before cycling. The calculation results are shown in Table 1.

[0090] Table 1 Test Results

[0091] As can be seen from Table 1 above, the surface modification of the garnet-type solid electrolyte of the present invention is the key to solving the processing problem of its aqueous silicon-carbon slurry and improving battery performance.

Claims

1. A modified silicon-carbon negative electrode slurry, characterized in that, Including negative electrode active material, aqueous binder, modified garnet-type solid electrolyte functional additive, and conductive agent; The negative electrode active material is a silicon-carbon composite material; The modified garnet-type solid electrolyte functional additive is one or both of the first modified particles and the second modified particles; the first modified particles are LLZO or LLZTO particles whose surface has been phosphorylated to form a Li3PO4 interface modification layer in situ; the second modified particles are LLZO or LLZTO particles whose surface has been coated with a silane coupling agent.

2. The modified silicon-carbon negative electrode slurry according to claim 1, characterized in that, Based on the percentage of solids by mass, the content of each component is as follows: negative electrode active material 90%. 95%, modified garnet-type solid electrolyte functional additive 1% 5%, conductive agent 1% 5%, water-based adhesive 3% 6%.

3. The modified silicon-carbon negative electrode slurry according to claim 1, characterized in that, The particle size D50 of the modified garnet-type solid electrolyte functional additive is 50 nm. 5μm; the aqueous binder is one or more of the following compound systems: polyacrylic acid, lithium-ionized polyacrylic acid, and carboxymethyl cellulose; the conductive agent is selected from Super P, KS 6. At least one of carbon black, carbon nanofibers, carbon nanotubes, acetylene black, and graphene.

4. The modified silicon-carbon negative electrode slurry according to claim 1, characterized in that, The Li3PO4 on the surface of the first modified particles is generated by reacting a phosphorus source with LLZO or LLZTO particles in an organic solvent system; the silane coupling agent of the second modified particles is selected from KH. 550, KH 560, KH One or more of 570 in combination.

5. The modified silicon-carbon negative electrode slurry according to claim 1, characterized in that, It also includes water-based solvents, which adjust the solid content of the slurry to 45-55%.

6. A method for preparing the modified negative electrode silicon-carbon slurry according to any one of claims 1-5, characterized in that, Includes the following steps: S1: The modified garnet-type solid electrolyte functional additive is added to an aqueous solvent and dispersed to obtain a solid electrolyte dispersion; The modified garnet-type solid electrolyte functional additive is one or both of the first modified particles and the second modified particles. S2: Add the negative electrode active material, conductive agent, and aqueous binder to the solid electrolyte dispersion obtained in step S1, mix them evenly, and obtain the modified negative electrode silicon-carbon slurry.

7. The method for preparing the modified negative electrode silicon-carbon slurry according to claim 6, characterized in that, The preparation steps of the first modified particles include: (1) Disperse LLZO or LLZTO powder with citric acid in an organic solvent and stir at a constant temperature to obtain a suspension; (2) Add phosphoric acid to the suspension and continue the reaction at a constant temperature; (3) After the reaction is complete, solid-liquid separation is performed; (4) The solid powder is dried to obtain the first modified particles.

8. The method for preparing the modified negative electrode silicon-carbon slurry according to claim 6, characterized in that, The preparation steps of the second modified particles include: (1) Disperse LLZO or LLZTO powder in an organic solvent and stir at a constant temperature to obtain a suspension; (2) Adjust the pH of the ethanol-water solution to 4.

5.

5. Add silane coupling agent and pre-hydrolyze to obtain a pre-hydrolyzed solution; (3) Add the pre-hydrolyzed solution dropwise to the suspension and stir at a constant temperature; (4) After the reaction is complete, centrifuge, wash, and collect the solid; (5) Dry and solidify to obtain the second modified particles.

9. A negative electrode sheet prepared using the modified silicon-carbon slurry according to any one of claims 1-5, characterized in that, Modified silicon-carbon slurry for the negative electrode is coated onto the surface of copper foil for the current collector, and the negative electrode sheet is obtained through baking, rolling, die cutting and drying processes.

10. A lithium-ion battery prepared using the negative electrode sheet according to claim 9, characterized in that, The battery includes a negative electrode, a positive electrode, a separator, and an electrolyte.