A three-dimensional functionalized matrix and its preparation method, electrode and solid-state battery

By employing inverted conical, hourglass, or tilted hole structures in a three-dimensional functionalized substrate in all-solid-state batteries, the mechanical failure and mass transfer limitations of thick electrodes have been solved, resulting in improved energy density and fast charging performance.

CN123120748APending Publication Date: 2026-11-17NINGBO INST OF MATERIALS TECH & ENG CHINESE ACAD OF SCI
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611142694.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-07-30
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

In existing technologies, thick electrodes in all-solid-state batteries face mechanical failure and limited mass transfer problems. Especially under high-pressure compaction and volume expansion of active materials, simple straight holes or U-shaped grooves cannot provide effective Z-axis constraint, leading to electrode material slippage, pulverization, and interface failure.

Method used

A three-dimensional functionalized matrix is ​​adopted, and through holes and/or non-through holes are set on the conductive skeleton. The structure is designed as an inverted cone, hourglass or inclined hole structure. Combined with the mechanical limiting area and the pure ion transport area, a mechanical interlocking structure is formed to prevent the active material from sliding out, and the expansion stress is relieved by the stress conversion part.

Benefits of technology

It effectively solves the problems of powder shedding and delamination of thick electrodes, improves the interface peel strength, realizes the stability and rapid ion transport of high-load electrodes, and maintains the high energy density and fast charging performance of batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123120748A_ABST
    Figure CN123120748A_ABST
Patent Text Reader

Abstract

This invention provides a three-dimensional functionalized substrate and its preparation method, as well as an electrode and a solid-state battery, belonging to the field of battery technology. It includes: a conductive framework having a first surface and a second surface arranged opposite to each other; arrayed limiting recesses, each including through holes formed on the conductive framework and / or non-through holes formed on the first surface and / or the second surface; the angle between the opening direction of the through holes and the thickness direction of the conductive framework is 0° to 90°; when the angle is not 0°, the diameter of the through holes is constant or varies along the opening direction; when the angle is 0°, the through holes have a reduced diameter section. The advantage is that after the composite electrode material fills specific pores such as conical holes and hourglass holes, it solidifies to form a mechanical interlocking structure similar to tenons or barbs.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of battery technology, and particularly relates to a three-dimensional functionalized substrate and its preparation method, as well as electrodes and solid-state batteries. Background Technology

[0002] To achieve the goal of high energy density in all-solid-state batteries, developing thick electrode designs with high active material areal loading has become an inevitable trend in the industry. However, thick electrodes in all-solid-state batteries face severe challenges from both mechanical failure and limited mass transfer. While existing technologies have attempted to increase contact area or accommodate electrode material by creating through-holes or blind slots in the current collector, simple through-holes or U-shaped slots cannot provide effective constraint in the Z-axis direction perpendicular to the electrode surface under extremely high compaction pressures (hundreds of megapascals) and the intense volume expansion of active materials (especially silicon-based anodes) during long cycles. Expansion stress easily causes electrode material to slide outwards along the through-hole wall (i.e., the "pull-out" effect), leading to electrode pulverization, interlayer delamination, and interface failure. Furthermore, although existing technologies propose filling the holes with electrolyte to improve ion transport, this often comes at the cost of sacrificing the overall mechanical strength of the electrode. Therefore, there is an urgent need to develop a novel three-dimensional confinement integrated structure that can effectively accommodate active substances and mechanically lock them at the geometrical level, thus solving the problems of Z-axis detachment and interface peeling. Summary of the Invention

[0003] The purpose of this invention is to address the aforementioned problems in existing technologies by proposing a three-dimensional functionalized matrix for locking and preventing the extraction of active substances.

[0004] The objective of this invention can be achieved through the following technical solution: a three-dimensional functionalized matrix, comprising: A conductive framework having a first surface and a second surface disposed opposite to each other; Multiple limiting recesses, including through holes formed on the conductive skeleton and / or non-through holes formed on the first surface and / or the second surface; The angle between the opening direction of the through hole and the thickness direction of the conductive skeleton is 0° to 90°. When the included angle is not 0°, the diameter of the through hole is constant or varies along the opening direction of the through hole; When the included angle is 0°, the through hole has a reduced diameter section.

[0005] Preferably, the section with the smallest aperture in the reduced diameter section is located at the port of the through hole and / or on the inner section of the through hole.

[0006] Preferably, the axial cross-sectional profile of the reduced diameter section is composed of any one or more of straight segments, curved segments, broken line segments, and stepped segments.

[0007] Preferably, the limiting recess is divided into a connected mechanical limiting region and a pure ion transport region along the opening direction.

[0008] Preferably, a solid gap region is formed between the non-through holes on the first surface and the adjacent non-through holes on the second surface, and the solid gap region includes a stress transfer portion.

[0009] Preferably, the conductive skeleton is made of metal foil, three-dimensional woven metal mesh, porous metal foam, conductive carbon-based three-dimensional skeleton, or a polymer support skeleton modified with conductivity.

[0010] An electrode sheet includes the above-described three-dimensional functionalized matrix, wherein the limiting recess is at least filled with a positive electrode composite layer to form a positive electrode composite electrode sheet; or at least filled with a negative electrode composite layer to form a negative electrode composite electrode sheet.

[0011] A solid-state battery includes the aforementioned electrode sheets and a solid electrolyte layer. The number of electrode sheets is multiple, and the multiple electrode sheets are distributed at intervals. Adjacent electrode sheets are respectively a positive electrode composite sheet and a negative electrode composite sheet. When a through hole is provided on the three-dimensional functionalized substrate, the solid electrolyte layer fills the space between two adjacent electrodes and is connected to the corresponding electrodes respectively. When only non-through holes are provided on the three-dimensional functionalized matrix, the solid electrolyte layer fills the space between two adjacent electrodes and is connected to the corresponding electrodes respectively. Furthermore, two adjacent positive composite electrodes are connected to each other, and two adjacent negative composite electrodes are connected to each other.

[0012] A method for preparing a three-dimensional functionalized matrix, comprising: A conductive skeleton is provided, and an array of limiting recesses is constructed on the conductive skeleton using a subtractive manufacturing process; Alternatively, molding materials can be provided, and additive manufacturing processes can be used to form a skeleton structure with arrayed limiting recesses. The limiting recess includes at least one of a through hole and a non-through hole.

[0013] Preferably, the subtractive manufacturing process includes one or more of ultrafast laser etching, chemical directional etching, or microwave irradiation ablation; The additive manufacturing process includes one or more of selective laser melting, electron beam melting, direct writing, photopolymerization, or fused deposition modeling.

[0014] Compared with existing technologies, the beneficial effects of this invention are as follows: After the composite electrode material is filled into specific pores such as conical holes and hourglass holes, it solidifies to form a mechanical interlocking structure similar to tenons or barbs. The huge stress generated by the electrode sheet during compaction and cyclic expansion is fully dispersed by the limiting recess structure, and the interface peel strength is increased by several times or even orders of magnitude compared with traditional flat foil, effectively solving the problem of powder shedding and delamination of high-load electrode sheets during bending and cycling. Attached Figure Description

[0015] Figure 1 It is a schematic diagram of a three-dimensional functionalized substrate with an inverted conical through hole; Figure 2 It is a schematic diagram of a three-dimensional functionalized substrate with an hourglass-shaped through hole; Figure 3 It is a schematic diagram of a three-dimensional functionalized substrate with inclined through holes; Figure 4 It is a schematic diagram of a three-dimensional functionalized substrate with double-sided non-through holes; Figure 5 It is a schematic diagram of a three-dimensional functionalized substrate with through holes of other shapes; Figure 6 It is a schematic diagram of a three-dimensional functionalized substrate with non-through holes of other shapes; Figure 7 This is one of the structural schematic diagrams of a positive electrode composite sheet; Figure 8 This is the second schematic diagram of the positive electrode composite sheet; Figure 9 This is the third schematic diagram of the positive electrode composite sheet; Figure 10 This is a schematic diagram of the interconnected electrodes with through holes in a solid-state battery. Figure 11 This is a schematic diagram of the interconnection of electrodes in a solid-state battery that only have non-through holes.

[0016] In the figure, 100 is the conductive framework; 101 is the through hole; 102 is the non-through hole; 103 is the stress conversion part; 104 is the positive electrode composite layer; 105 is the negative electrode composite layer; and 106 is the solid electrolyte layer. Detailed Implementation

[0017] The following are specific embodiments of the present invention, which are described in conjunction with the accompanying drawings. However, the present invention is not limited to these embodiments.

[0018] It should be noted that all directional indications (such as up, down, left, right, front, back, etc.) in the embodiments of the present invention are only used to explain the relative positional relationship and movement of each component in a certain specific posture (as shown in the figure). If the specific posture changes, the directional indication will also change accordingly.

[0019] A three-dimensional functionalized substrate includes: a conductive framework 100 having a first surface and a second surface disposed opposite to each other; Multiple limiting recesses, including through holes 101 formed on the conductive skeleton 100 and / or non-through holes 102 formed on the first surface and the second surface; The angle between the opening direction of the through hole 101 and the thickness direction of the conductive skeleton 100 is 0° to 90°. When the included angle is not 0°, the diameter of the through hole 101 is constant or varies along the opening direction of the through hole 101. When the included angle is 0°, the through hole 101 has a reduced diameter section.

[0020] It should be noted that the reduced diameter section in this invention refers to a certain section of the through hole 101 in its opening direction, whose diameter is smaller than the diameters on both sides of the section, that is, the channel forms a radial contraction at that point. Its specific forms include, but are not limited to, the conical contraction section of the inverted conical hole, the middle contraction section of the hourglass hole, the stepped contraction section of the stepped hole, and the dovetail groove type limiting contraction.

[0021] For the through hole 101, its anti-slip principle includes two mechanisms: the first is a diameter reduction locking mechanism, which forms a geometric contraction structure similar to a dovetail groove or a limiting groove through the diameter reduction section, creating an axial physical barrier to the active material filling the hole and preventing it from sliding out along the opening direction; the second is an inclined guiding mechanism, which sets the channel at an inclination so that the channel direction is inconsistent with the force direction of the substrate, thereby changing the force transmission path and increasing the sliding resistance. The two can function independently or work together to enhance each other.

[0022] like Figure 1 As shown, in one specific embodiment, the limiting recess includes a plurality of through holes 101, which penetrate the first surface and the second surface. The angle between the opening direction of the through holes and the thickness direction of the conductive skeleton 100 is 0°, that is, the through holes 101 are opened parallel to the thickness direction of the conductive skeleton 100.

[0023] The through hole 101 has a reduced diameter section. Specifically, the through hole 101 has a first diameter D1 at the first surface and a second diameter D2 at the second surface, where D1 > D2. That is, the diameter of the through hole gradually decreases from the first surface to the second surface, forming an inverted conical hole (referred to as an inverted conical hole). The reduced diameter section is located on the side of the through hole 101 closest to the second surface. The dimensions of the inverted conical hole satisfy the geometric relationship: 1.2 ≤ D2 / D1 ≤ 5.0.

[0024] like Figure 2 As shown, in another specific embodiment, the limiting recess includes a plurality of through holes 101, which penetrate the first surface and the second surface. The angle between the opening direction of the through hole 101 and the thickness direction of the conductive skeleton 100 is 0°, that is, the through hole 101 is opened parallel to the thickness direction of the conductive skeleton 100.

[0025] The through hole 101 has a narrowing section. Specifically, the through hole 101 has a first diameter Dw at the first surface and a second diameter Dn at the second surface; that is, the diameter of the through hole 101 gradually decreases from the first surface towards the middle along the opening direction, and then gradually increases from the middle towards the second surface, forming an hourglass-shaped hole (referred to as an hourglass hole). The narrowing section is located in the middle or near the middle of the hole. The dimensions of the hourglass hole satisfy the geometric relationship: 1.5 ≤ Dw / Dn ≤ 10.0.

[0026] like Figure 3 As shown, in another specific embodiment, the limiting recess includes a through hole 101, which penetrates the first surface and the second surface. The angle between the opening direction of the through hole 101 and the thickness direction of the conductive skeleton 100 is not 0°, that is, the through hole 101 is inclined relative to the thickness direction of the conductive skeleton 100. Along the opening direction of the through hole 101, the diameter of the through hole 101 remains constant. The through hole 101 is an oblique straight hole, which does not have a narrowing section, and the hole wall is smooth and the hole diameter is uniform.

[0027] The section with the smallest diameter in the reduced-diameter section can be located at the port of the through hole 101 (i.e., at the opening of the through hole 101 on the first or second surface), or it can be located on the internal section of the through hole 101 (i.e., in the middle of the channel or at any non-port location). Figure 5 As shown, the axial cross-sectional profile of the reduced diameter section (i.e., the profile of the hole wall after cutting along the opening direction) can be composed of any one or more of straight segments, curved segments, broken line segments, and stepped segments, such as, but not limited to: inverted conical reduced diameter composed of straight segments, arc-shaped reduced diameter composed of curved segments, multi-segment reduced diameter composed of broken line segments, stepped reduced diameter composed of stepped segments, and combinations of the above line types.

[0028] like Figure 7 , Figure 8As shown, the limiting recess is filled in a multi-segmented, partitioned manner along its opening direction. Specifically, taking the hourglass hole and the inverted conical hole as examples, the internal space of the same hourglass hole or inverted conical hole is divided into a mechanical limiting region and a pure ion transport region. The mechanical limiting region includes the neck (i.e., the narrow part of the reduced diameter section) or the opening (i.e., the reduced diameter area of ​​the inverted conical hole near the small diameter port). This region is densely filled with composite electrode material. The geometric contraction of the reduced diameter section firmly anchors the composite electrode material inside the channel, preventing it from sliding out and detaching along the hole wall during the volume expansion during charging and discharging. The pure ion transport region is the remaining hole segment not occupied by the composite electrode material. This region is filled solely with pure solid electrolyte material.

[0029] On the one hand, the composite electrode material within the mechanically confined region is firmly locked in place by the reduced-diameter section, providing reliable mechanical support and structural interlocking for the electrode material in the thickness direction. On the other hand, the pure solid electrolyte, which is continuously filled within the pure ion transport region, provides a continuous, low-impedance transport path for lithium ions. Thanks to this, the all-solid-state battery of this invention can achieve a 10 mAh / cm² capacity on a thick electrode exceeding 200 μm. -2 The above-mentioned ultra-high limit areal capacity, while still maintaining good fast charging dynamic performance. like Figure 9 As shown, as an alternative implementation method besides the aforementioned partitioned filling scheme, the entire internal space of the hourglass or inverted conical hole within the limiting recess is completely occupied by the composite electrode material, eliminating the need for a separate pure ion transport region. In this implementation, the mechanical self-locking effect of the reduced diameter section is fully utilized. After the composite electrode material solidifies within the inverted area of ​​the hole neck or orifice, it forms an interlocking structure similar to a dovetail groove or expansion screw, ensuring that the electrode material is firmly anchored within the conductive framework 100 during the volume expansion and contraction of charging and discharging, preventing it from easily detaching or slipping out. This fully composite filling scheme has a simpler structure and a more convenient manufacturing process, making it suitable for applications where rate performance requirements are relatively low but the problem of electrode material detachment still needs to be addressed.

[0030] It should be noted that, in this invention, the non-through hole 102 refers to a blind hole structure formed on the first surface and / or the second surface of the conductive skeleton 100 and not penetrating the thickness direction of the conductive skeleton 100. The solid interval region refers to the continuous solid region maintained between the bottom wall and / or side wall of the non-through hole 102 on the first surface and the bottom wall and / or side wall of the adjacent non-through hole 102 on the second surface in the thickness direction of the conductive skeleton 100. This region is not penetrated by any hole structure, and the stress conversion part 103 refers to a specific area within the solid interval region that converts the normal expansion stress in the thickness direction of the substrate into transverse shear stress along the plane of the substrate.

[0031] like Figure 4As shown, in one specific embodiment, the limiting recess includes a non-through hole 102 formed on the first surface of the conductive frame 100 and a non-through hole 102 formed on the second surface. The non-through holes 102 on the first surface and the non-through holes 102 on the second surface are arranged alternately and staggered in the thickness direction of the conductive frame 100 (i.e., they do not overlap on the horizontal projection plane), such that a solid gap region is formed between the bottom wall of the non-through hole 102 on the first surface and the bottom wall of the adjacent non-through hole 102 on the second surface. Specifically, the stress conversion part 103 is located in the geometric center region of the solid gap region or at its interface near the bottom wall of the non-through hole 102.

[0032] The non-through hole 102 in this invention is not limited to the specific configuration shown in the above figures. For example... Figure 6 As shown, as another optional form of expression, the axial cross-sectional shape of the non-through hole 102 can also be any one of rectangle, trapezoid, or semicircle. Furthermore, multiple non-through holes 102 on the same conductive frame 100 surface can be arranged in a regular array (such as a honeycomb, rectangular, or staggered array) or randomly distributed. The area and shape of the solid interval between adjacent non-through holes 102 can be adjusted according to actual stress distribution requirements. All stress conversion and mechanical locking functions achieved based on the above-described non-through hole 102 structure fall within the protection scope of this invention.

[0033] The material of the aforementioned conductive framework 100 can be flexibly selected according to specific application scenarios. The conductive framework 100 is selected from any one or a combination of metal foils (such as aluminum foil, copper foil, nickel foil, titanium foil, stainless steel foil, or composite metal foil with carbon coating), three-dimensional woven metal meshes (such as stainless steel wire mesh, nickel mesh, etc.), porous metal foams / sponges (such as foamed nickel, foamed copper, foamed aluminum, foamed iron, or foamed iron-nickel alloy, etc.), conductive carbon-based three-dimensional frameworks (such as three-dimensional conductive carbon fiber networks, three-dimensional graphene foam, carbon nanotube three-dimensional networks, or carbon cloth / carbon paper, etc.), or high mechanical strength polymer support frameworks modified with conductivity (such as porous films, non-woven fabrics, or woven meshes with conductive coatings, doped with conductive fillers, or chemically plated / electroplated metal layers). Different conductive frameworks 100 have their own advantages in terms of conductivity, mechanical strength, flexibility, mass density, corrosion resistance, and interfacial compatibility with active materials. In practical applications, they can be rationally selected according to the battery system, energy density requirements, and mechanical performance requirements.

[0034] like Figures 7-9 As shown, an electrode sheet is provided, comprising the aforementioned three-dimensional functionalized substrate. The limiting recess (including through-hole 101 and / or non-through-hole 102) is filled with at least a positive electrode composite layer 104 to form a positive electrode composite electrode sheet, or at least filled with a negative electrode composite layer 105 to form a negative electrode composite electrode sheet.

[0035] In one embodiment, the limiting recess is completely filled with either the positive electrode composite layer 104 or the negative electrode composite layer 105. Regardless of whether the limiting recess is a through hole (hourglass hole or inverted conical hole) or a non-through hole 101 (blind hole), the positive or negative electrode composite layer slurry is filled into the entire limiting recess and coated on the first and second surfaces of the conductive skeleton 100. After drying and densification, the composite layer is firmly anchored to the conductive skeleton 100, effectively preventing the composite layer from peeling off from the surface of the conductive skeleton 100 or sliding out from the channel during the volume expansion of the charging and discharging process.

[0036] As another implementation, the limiting recess is filled in a multi-segment partitioned state: part of the area is filled with positive or negative active material (or positive composite layer 104 or negative composite layer 105), and the remaining part is filled with pure solid electrolyte to form a solid electrolyte layer 106. This partitioned filling strategy is also applicable to through holes 101 and non-through holes 102. Taking hourglass holes or inverted conical holes as examples, the reduced diameter section and its adjacent area (mechanical limiting area) are densely filled with positive or negative composite layer 105, and the geometric contraction of the reduced diameter section forms a structural interlock; the remaining hole section not occupied by the composite layer (pure ion transport area) is filled with pure solid electrolyte alone, forming a lithium ion fast transport channel that runs through the thickness direction of the substrate. Taking non-through holes 102 as an example, the area near the bottom wall is densely filled with composite layer and locked inside the blind hole, and the remaining hole section near the opening is filled with pure solid electrolyte alone, forming an ion transport channel connected to the electrolyte layer on the surface of the conductive skeleton 100.

[0037] This application also provides a solid-state battery, which includes the aforementioned electrode sheets and a solid electrolyte layer 106. The electrode sheets are multiple pieces, spaced apart along the thickness direction. Adjacent electrode sheets are respectively a positive composite electrode and a negative composite electrode, i.e., positive and negative composite electrode sheets are alternately stacked. A solid electrolyte layer 106 is disposed between adjacent positive and negative composite electrode sheets.

[0038] Depending on the type of the upper limit recess in the three-dimensional functionalized substrate, solid-state batteries can be divided into the following two categories: like Figure 10 As shown, scenario one: a three-dimensional functionalized substrate is provided with through holes 101 (including a composite structure of through holes 101 and non-through holes 101). When a through-hole 101 is provided on the three-dimensional functionalized substrate, the limiting recess includes a through-hole 101 (such as an hourglass hole or an inverted conical hole) penetrating the first and second surfaces of the conductive framework 100. The solid electrolyte layer 106 fills between two adjacent electrodes and is connected to the corresponding electrodes respectively. Specifically, a portion of the solid electrolyte layer 106 fills the gap space between adjacent positive and negative composite electrodes to form an electrolyte membrane that isolates the two electrodes; another portion of the solid electrolyte layer 106 permeates and fills the pore segment (i.e., the pure ion transport region) inside the through-hole that is not occupied by the composite electrode material, forming a continuous integrated structure with the solid electrolyte in the channel, thereby constructing a continuous lithium-ion transport channel that runs through the entire thickness of the conductive framework 100 within the through-hole.

[0039] like Figure 11 As shown, scenario two: only non-through holes 102 (no through holes 101) are provided on the three-dimensional functionalized substrate. When the three-dimensional functionalized substrate has only non-through holes 102 and no through holes 101, the limiting recess only includes blind holes formed on the first and / or second surfaces of the conductive skeleton 100, and the conductive skeleton 100 remains complete and continuous in the thickness direction (the solid spacer area is not penetrated). The solid electrolyte layer 106 also fills between two adjacent electrodes and is connected to the corresponding electrodes respectively. The difference from case one is that, since there are no through holes 101 on the three-dimensional functionalized substrate, the conductive skeleton 100 is a complete continuous metal body in the thickness direction. Two adjacent positive composite electrodes are electrically connected through the continuous metal structure of their respective conductive skeletons 100 (i.e., electrodes of the same polarity are connected to each other), and two adjacent negative composite electrodes are also electrically connected through the continuous metal structure of the conductive skeleton 100 (i.e., electrodes of the same polarity are connected to each other). This structure helps reduce the internal resistance of the battery and improve the current collection efficiency of electrons in the thickness direction. At the same time, the solid spacer area of ​​the non-through hole 102 and the stress conversion part 103 effectively alleviate the volume expansion stress during the charging and discharging process, ensuring the long-term cycle stability of the electrode.

[0040] The present invention also provides a method for preparing a three-dimensional functionalized substrate for all-solid-state batteries, comprising: A conductive skeleton 100 is provided, and an array of limiting recesses are constructed on the conductive skeleton 100 using a subtractive manufacturing process. Alternatively, molding materials can be provided, and additive manufacturing processes can be used to form a skeleton structure with arrayed limiting recesses. The limiting recess includes at least one of an inverted conical hole, an hourglass hole, and a double-sided staggered blind hole.

[0041] More specifically, subtractive manufacturing processes include one or more of ultrafast laser etching, chemical directional etching, or microwave irradiation ablation; Additive manufacturing processes include one or more of selective laser melting, electron beam melting, direct writing, photopolymerization, or fused deposition modeling.

[0042] More specifically, when constructing an inverted conical hole, the cross-sectional dimensions of the hole are controlled to gradually change along the thickness direction of the substrate during the processing, so that the formed hole has an inverted conical structure in which the cross-sectional dimensions of the hole opening are smaller than the cross-sectional dimensions of the hole bottom. For example, when constructing hourglass holes, holes are machined from opposite sides of the substrate into the substrate, and the connection position of the holes on both sides inside the substrate is controlled to form a shrinking neck, so that the formed holes have an hourglass structure with the cross-sectional dimensions of the two end openings being larger than the cross-sectional dimensions of the middle neck. For example, when constructing double-sided staggered blind holes, a first blind hole array is formed on the first surface of the substrate, and a second blind hole array is formed on the second surface of the substrate. The first blind hole array and the second blind hole array are staggered on the projection perpendicular to the substrate surface to form staggered hole walls or support walls inside the substrate.

[0043] More specifically, when polyimide is used to form a skeleton structure through additive manufacturing, a conductive layer is formed on the surface of the skeleton structure by combining it with a chemical plating process, so that the skeleton structure constitutes a conductive skeleton 100.

[0044] The following description is based on the embodiments. It is worth mentioning that the laser power, scanning speed, etching time, printing resolution, coating thickness and hole structure size in the following embodiments are only illustrative examples. Those skilled in the art can make adjustments according to the type of substrate, target hole diameter and thickness requirements. All adjustments should fall within the protection scope of the present invention without departing from the concept of the present invention. Example 1

[0045] This embodiment provides a method for fabricating a three-dimensional functionalized substrate with inverted conical blind holes, using a 200μm thick copper foil as the conductive framework 100. An array of inverted conical non-through blind holes is constructed on the surface of the copper foil using ultrafast laser processing. During the processing, the focal depth and shear radius of the ultrafast laser are dynamically changed to gradually enlarge the hole diameter along the thickness direction of the substrate, thereby forming inverted conical blind holes with an opening cross-sectional size smaller than the bottom cross-sectional size.

[0046] In this embodiment, the diameter of the formed inverted conical blind hole is 30 μm, the diameter of the bottom hole is 80 μm, and the depth is 150 μm. The resulting three-dimensional functionalized matrix has an array of inverted conical non-through blind hole structures. Example 2

[0047] This embodiment provides a method for preparing a three-dimensional functionalized substrate with hourglass-shaped through holes. A 500μm thick aluminum foil is selected as the conductive framework 100. An ultrafast laser double-sided alignment processing method is used to process holes from opposite sides of the aluminum foil towards the center, connecting the holes formed on both sides in the middle of the substrate. A constricted neck is formed at the connection point, thus creating an hourglass-shaped through-hole array that is narrow in the middle and wide at both ends.

[0048] In this embodiment, the diameter of the two end openings of the formed hourglass-shaped pores is 150 μm, and the diameter of the neck in the middle is 50 μm. The resulting three-dimensional functionalized matrix has an array of hourglass-shaped through-hole structures inside. Example 3

[0049] This embodiment provides a method for fabricating a three-dimensional functionalized substrate with double-sided staggered blind vias. An aluminum substrate with a thickness of 300 μm is selected as the conductive framework 100. Using double-sided photolithography and chemical directional etching, a first blind via array is formed on the first surface of the substrate, and a second blind via array is formed on the second surface of the substrate. The first and second blind via arrays are staggered in their projection perpendicular to the substrate surface, thereby forming staggered via walls or support walls within the substrate.

[0050] In this embodiment, the aperture of both the first and second blind hole arrays is 200 μm, and the hole depth is 160 μm. A staggered support wall with a thickness of approximately 40 μm is retained between the bottoms of the holes on both sides. The resulting three-dimensional functionalized substrate has a double-sided staggered blind hole structure. Example 4

[0051] This embodiment provides a method for preparing a three-dimensional functionalized matrix through additive manufacturing and surface conductive modification processes. Polyimide resin is selected as the molding material, and a framework structure with an inverted conical micropore array is prepared using photopolymerization 3D printing technology. By controlling the printing structure parameters, an inverted conical micropore array is formed inside the framework structure.

[0052] In this embodiment, the diameter of the inverted conical micropore opening is 100 μm, the diameter of the bottom hole is 150 μm, and the thickness of the framework is 500 μm. After printing, a 1.5 μm thick high-density copper conductive layer is deposited on the surface of the framework structure using a chemical plating process, so that the framework structure constitutes a conductive framework 100. The resulting three-dimensional functionalized substrate retains the inverted conical micropore structure and has conductivity. Example 5

[0053] This embodiment provides a method for fabricating a three-dimensional metal skeleton with hourglass-shaped holes. The method employs metal 3D printing technology, using stainless steel powder as the raw material to print a three-dimensional skeleton with an array of hourglass-shaped holes. By presetting the internal hole structure parameters of the skeleton, an hourglass-shaped hole array with larger openings at both ends and a smaller neck in the middle is formed inside the printed skeleton.

[0054] In this embodiment, the thickness of the obtained three-dimensional skeleton is 500 μm, the diameter of the two ends of the hourglass hole is 800 μm, and the diameter of the middle neck is 500 μm. Since it is directly formed using conductive metal powder, the obtained skeleton can be directly used as a conductive skeleton 100. Example 6

[0055] This embodiment provides a solid-state battery, which is prepared by the following method: A 150 μm thick high-purity titanium substrate was used as a three-dimensional functionalized matrix, and hourglass-shaped through-holes were constructed inside it. The diameter of the wide end opening of the hourglass hole, Dw, was 100 μm, and the diameter of the neck in the middle was 25 μm, satisfying Dw / Dn=4.0. LiNi0.8Co0.1Mn0.1O2 positive electrode slurry was extruded into and across the neck region of the hourglass hole, so that the composite electrode material filled the lower half of the space inside the hole, forming an anchoring structure across the neck. Subsequently, the remaining space inside the hole was filled with Li6PS5Cl pure solid electrolyte material, thereby obtaining the positive electrode composite electrode sheet.

[0056] A positive electrode composite sheet and a negative electrode composite sheet are arranged opposite each other, and a solid electrolyte layer 106 is placed between them. The solid electrolyte layer 106 is connected to both the positive electrode composite sheet and the negative electrode composite sheet, thereby assembling a solid-state battery. Since the three-dimensional functionalized substrate has through holes, the solid electrolyte layer 106 is located between adjacent positive electrode composite sheets and negative electrode composite sheets and is connected to both. Example 7

[0057] This embodiment provides a solid-state battery, which is prepared by the following method: A 50μm thick copper foil was used as the three-dimensional functionalized substrate for the negative electrode, and inverted conical blind holes were machined on its surface. The equivalent diameter D1 of the hole opening was controlled to be 20μm, the bottom diameter D2 to be 45μm, satisfying D2 / D1=2.25, and the hole depth to be 40μm. A high-energy-density silicon-carbon composite material was filled into the inverted conical blind holes, and the negative electrode composite material was pressed into the holes under high pressure. The limiting effect formed by the contraction of the hole opening allowed the negative electrode composite material to be embedded in the hole, thus obtaining the negative electrode composite electrode sheet.

[0058] A negative electrode composite sheet and a positive electrode composite sheet are arranged opposite each other, and a solid electrolyte layer 106 is placed between them. The solid electrolyte layer 106 is connected to both the negative electrode composite sheet and the positive electrode composite sheet, thereby assembling a solid-state battery. Since the three-dimensional functionalized substrate has non-through holes, the solid electrolyte layer 106 is located between adjacent electrodes and connected to them. During stacking assembly, electrodes of the same electrode can be electrically connected through corresponding current collectors. Example 8

[0059] This embodiment provides a solid-state battery, which is prepared by the following method: A 200 μm thick aluminum foil was used as a three-dimensional functionalized substrate. Blind holes with a diameter of 80 μm and a depth of 120 μm were machined on both sides of the foil, with the depth of the blind holes exceeding half the thickness of the substrate. The blind holes on both sides were staggered in the projection direction perpendicular to the substrate surface, and the overlapping area formed an interlaced hole wall of about 30 μm. The LiNi0.8Co0.1Mn0.1O2 cathode composite material was pressed into the double-sided interlaced blind holes to obtain the cathode composite electrode.

[0060] Multiple electrode sheets are spaced apart, with adjacent electrode sheets serving as positive and negative composite electrode sheets, respectively. A solid electrolyte layer 106 is placed between adjacent electrode sheets, connecting the solid electrolyte layer 106 to the adjacent positive and negative composite electrode sheets, thereby assembling a stacked solid-state battery. Because the three-dimensional functionalized substrate has non-through holes, electrode sheets of the same polarity can be electrically connected through corresponding current collectors during stacking assembly. Example 9

[0061] This embodiment provides a solid-state battery, which is prepared by the following method: A 100μm thick copper foil was used as a three-dimensional functionalized substrate, and inverted conical non-through blind holes were machined on both sides. A SiC-containing negative electrode composite material was controlled to fill the area near the surface of the blind holes to a depth of approximately 30μm, leaving approximately 20μm of free space at the bottom of the holes. The negative electrode composite material was then fitted into the blind holes by an inverted conical limiting structure near the hole opening, thus producing the negative electrode composite sheet.

[0062] A negative electrode composite sheet and a positive electrode composite sheet are arranged opposite each other, and a solid electrolyte layer 106 is placed between them. The solid electrolyte layer 106 is connected to the adjacent electrode sheets respectively, thereby assembling a solid-state battery. Since the three-dimensional functionalized substrate has non-through holes, the same electrode sheets can be electrically connected through corresponding current collectors during stacking assembly.

[0063] Comparative Example 1 This comparative example uses a conventional, flat 15μm thick aluminum foil as the positive electrode current collector, coated on one side with a LiNi0.8Co0.1Mn0.1O2 / Li6PS5Cl composite electrode material, with the electrode thickness controlled at 30μm, to prepare the positive electrode composite sheet. It is compacted at 500MPa and assembled with the negative electrode composite sheet and a solid electrolyte layer 106 to form an all-solid-state battery. Electrochemical tests show that the battery has an initial discharge specific capacity of 192 mAh g⁻¹ at 0.1C rate, corresponding to an areal capacity of approximately 2 mAh cm⁻¹. -2 Under conditions of thin electrodes and low internal structural stress, traditional flat two-dimensional current collectors can meet basic physical forming requirements and maintain normal charge and discharge performance.

[0064] Comparative Example 2 This comparative example uses a conventional, flat 15μm thick aluminum foil as the positive electrode current collector, coated on one side with a LiNi0.8Co0.1Mn0.1O2 / Li6PS5Cl composite electrode material, increasing the electrode thickness to 80μm, to obtain the positive electrode composite sheet, which is then compacted at 500MPa. Subsequently, it is assembled with the negative electrode composite sheet and a solid electrolyte layer 106 to form an all-solid-state battery. Due to the lack of mechanical support from a three-dimensional framework, slight physical peeling occurred at the electrode edges after molding. After assembling the all-solid-state battery, its initial discharge surface capacity is approximately 4.5 mAh cm⁻¹. -2 This indicates that the increased electrode thickness has led to some active materials being unable to participate in electrochemical reactions due to the obstruction of electron / ion transport pathways.

[0065] Comparative Example 3 This comparative example uses a conventional, flat 15μm thick aluminum foil as the positive electrode current collector, coated on one side with a LiNi0.8Co0.1Mn0.1O2 / Li6PS5Cl composite electrode material, further increasing the electrode thickness to 120μm to obtain a positive electrode composite sheet, which is then compacted at 500MPa. Subsequently, it is assembled with the negative electrode composite sheet and a solid electrolyte layer 106 to form an all-solid-state battery. Due to the increased electrode thickness, the internal stress accumulated during compaction cannot be effectively released through the two-dimensional flat substrate, resulting in significant macroscopic physical delamination and local warping in the center and edge areas of the electrode. After assembly into an all-solid-state battery, its initial discharge surface capacity is only 5.5mAh cm⁻¹. -2 This is significantly lower than the approximately 8.0 mAh / cm² capacity at that thickness. -2 It has the theoretical capacity, and the charge and discharge polarization is significant.

[0066] Comparative Example 4 A conventional, flat 15μm thick aluminum foil was used as the positive electrode current collector, and a LiNi0.8Co0.1Mn0.1O2 / Li6PS5Cl composite electrode material was coated on one side, further increasing the electrode thickness to 200μm, to prepare a positive electrode composite sheet. After compaction under 500MPa pressure, obvious network cracks appeared on the electrode surface, and more than 50% of the electrode coating area physically peeled off from the flat aluminum foil during the electrode transfer process. This demonstrates that without the constraint and support of a three-dimensional functionalized substrate, it is difficult for ultra-thick positive electrode composite sheets to maintain a stable forming and transfer state.

[0067] Comparative Example 5 A conventional, flat 20μm thick copper foil was used as the negative electrode current collector, and a high-energy-density nano-silicon-carbon composite material (SiC) with a single-sided coating thickness of 100μm was applied to prepare the negative electrode composite sheet, which was then compacted under a pressure of 250MPa. Because the flat copper foil surface could not provide three-dimensional physical anchoring, the 150μm thick electrode layer detached entirely during the stress release stage after compaction.

[0068] Therefore, it is evident that traditional flat current collectors are insufficient to provide adequate interfacial bonding stability for high-expansion thick anode systems. As demonstrated in the above embodiments and comparative examples, constructing positive and / or negative composite electrode sheets using a three-dimensional functionalized substrate with inverted conical holes, hourglass holes, or double-sided staggered blind holes, and forming a solid-state battery with a solid electrolyte layer 106 between adjacent electrodes, effectively enhances the mechanical interlocking and interfacial bonding stability between the composite electrode material and the substrate. Compared to the comparative examples using traditional flat current collectors, the three-dimensional functionalized substrate more effectively restricts the composite electrode material from being pulled out, peeled off, slipped, or experiencing interfacial instability due to expansion during thick electrode forming, transfer, and cycling, and helps maintain stable contact between the solid electrolyte layer 106 and the positive and negative composite electrode sheets. Especially for high-load thick electrodes and high-expansion anode materials, the three-dimensional functionalized substrate can more fully utilize the limiting, spatial buffering, and structural support functions of the pore structure, thereby improving the overall structural stability and application applicability of the solid-state battery.

[0069] It should be noted that in this invention, the use of terms such as "first," "second," and "a" is for descriptive purposes only and should not be construed as indicating or implying their relative importance or implicitly specifying the number of technical features indicated. Therefore, a feature defined as "first" or "second" may explicitly or implicitly include at least one of that feature. In the description of this invention, "a plurality of" means at least two, such as two, three, etc., unless otherwise explicitly specified. The terms "connection," "fixed," etc., should be interpreted broadly. For example, "fixed" can mean a fixed connection, a detachable connection, or an integral part; it can mean a mechanical connection or an electrical connection; it can mean a direct connection or an indirect connection through an intermediate medium; it can mean the internal communication of two elements or the interaction between two elements, unless otherwise explicitly specified. Those skilled in the art can understand the specific meaning of the above terms in this invention according to the specific circumstances.

[0070] Furthermore, the technical solutions of the various embodiments of the present invention can be combined with each other, but only if they are feasible for those skilled in the art. If the combination of technical solutions is contradictory or cannot be implemented, it should be considered that such combination of technical solutions does not exist and is not within the scope of protection claimed by the present invention.

[0071] The specific embodiments described herein are merely illustrative of the spirit of the invention. Those skilled in the art to which this invention pertains may make various modifications or additions to the described specific embodiments or use similar methods to substitute them, without departing from the spirit of the invention or exceeding the scope defined by the appended claims.

Claims

1. A three-dimensional functionalized matrix, characterized in that, include: A conductive framework having a first surface and a second surface disposed opposite to each other; Multiple limiting recesses, including through holes formed on the conductive skeleton and / or non-through holes formed on the first surface and / or the second surface; The angle between the opening direction of the through hole and the thickness direction of the conductive skeleton is 0° to 90°. When the included angle is not 0°, the diameter of the through hole is constant or varies along the opening direction of the through hole; When the included angle is 0°, the through hole has a reduced diameter section.

2. The three-dimensional functionalized matrix according to claim 1, characterized in that, The section with the smallest aperture in the reduced diameter section is located at the port of the through hole and / or on the internal section of the through hole.

3. The three-dimensional functionalized matrix according to claim 1, characterized in that, The axial cross-sectional profile of the reduced diameter section is composed of any one or more of the following: straight line segment, curved segment, broken line segment, and stepped segment.

4. The three-dimensional functionalized matrix according to claim 1, characterized in that, The limiting recess is divided into a connected mechanical limiting area and a pure ion transport area along the opening direction.

5. The three-dimensional functionalized matrix according to claim 1, characterized in that, A solid gap region is formed between the non-through hole on the first surface and the adjacent non-through hole on the second surface, and the solid gap region includes a stress transfer portion.

6. The three-dimensional functionalized matrix according to claim 1, characterized in that, The conductive framework is made of metal foil, three-dimensional woven metal mesh, porous metal foam, conductive carbon-based three-dimensional framework, or a polymer support framework modified with conductivity.

7. An electrode sheet, characterized in that, The three-dimensional functionalized matrix as described in any one of claims 1-6 includes a limiting recess filled with at least a positive electrode composite layer to form a positive electrode composite sheet; or at least filled with a negative electrode composite layer to form a negative electrode composite sheet.

8. A solid-state battery, characterized in that, Including the electrode as described in claim 7, it further includes a solid electrolyte layer, and the number of the electrode is multiple pieces, the multiple electrode pieces are distributed at intervals, and two adjacent electrode pieces are respectively a positive electrode composite electrode and a negative electrode composite electrode; When a through hole is provided on the three-dimensional functionalized substrate, the solid electrolyte layer fills the space between two adjacent electrodes and is connected to the corresponding electrodes respectively. When only non-through holes are provided on the three-dimensional functionalized matrix, the solid electrolyte layer fills the space between two adjacent electrodes and is connected to the corresponding electrodes respectively. Furthermore, two adjacent positive composite electrodes are connected to each other, and two adjacent negative composite electrodes are connected to each other.

9. A method for preparing a three-dimensional functionalized matrix, characterized in that, include: A conductive skeleton is provided, and an array of limiting recesses is constructed on the conductive skeleton using a subtractive manufacturing process; Alternatively, molding materials can be provided, and additive manufacturing processes can be used to form a skeleton structure with arrayed limiting recesses. The limiting recess includes at least one of a through hole and a non-through hole.

10. The method according to claim 9, characterized in that, The subtractive manufacturing process includes one or more of ultrafast laser etching, chemical directional etching, or microwave irradiation ablation. The additive manufacturing process includes one or more of selective laser melting, electron beam melting, direct writing, photopolymerization, or fused deposition modeling.