A low contact resistance metal connector and its flow field structure

By setting a double-layer protective coating, a biomimetic dendritic flow field, and lateral heat-conducting ribs on the metal connector, the problems of matrix element diffusion and thermal stress concentration under high temperature environment are solved, achieving low contact resistance and uniform gas distribution, thus extending the service life and operating efficiency of the fuel cell stack.

CN123120768APending Publication Date: 2026-11-17HUANENG CLEAN ENERGY RES INST
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611252198.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-18
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

In existing high-temperature solid oxide fuel cells, the single-layer coating structure of the metal interconnect cannot effectively prevent the diffusion of matrix elements outward, leading to increased interfacial contact resistance and poisoning and degradation of the electrode structure, thus reducing the stack's operating life.

Method used

It adopts a double-layer protective coating structure, including a conductive bottom layer and a composite barrier surface layer, combined with a biomimetic dendritic flow field and transverse integrated thermal ribs to enhance electron conduction, gas distribution and heat conduction, and suppress element volatilization and thermal stress concentration.

Benefits of technology

It effectively reduces interfacial contact resistance, improves gas distribution uniformity and heat distribution stability, extends stack life, and maintains high-efficiency operation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123120768A_ABST
    Figure CN123120768A_ABST
Patent Text Reader

Abstract

This application relates to the field of solid oxide fuel cell technology and discloses a low-contact-resistance metal connector and flow field structure, including a substrate, a double-layer protective coating, a biomimetic dendritic flow field, and a transversely integrated thermally conductive rib. The double-layer protective coating, from the inside out, includes a conductive underlayer adhered to the substrate and a composite barrier surface layer covering the outside of the conductive underlayer. The conductive underlayer reduces contact resistance, and the composite barrier surface layer blocks the outward diffusion of gaseous chromium. The biomimetic dendritic flow field is disposed on the working surface of the substrate, divided into three differentiated flow channel distribution regions, achieving uniform gas distribution through density differences. The transversely integrated thermally conductive rib is integrally stamped from the back of the substrate and extends laterally along the surface to conduct heat. This application suppresses the outward volatilization of chromium, reduces interfacial contact resistance and in-plane temperature difference, and improves the uniformity of reactant gas distribution.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application relates to the field of solid oxide fuel cell technology, specifically to a low contact resistance metal connector and flow field structure. Background Technology

[0002] Metal connectors are core structural components in solid oxide electrolyzers and solid oxide fuel cell stacks. Within the stack, these connectors connect individual cells in series for current collection, distribute reactant gases, and conduct system heat. Their normal operating environment is a high-temperature condition of 700 to 850°C.

[0003] In existing high-temperature fuel cell stack systems, high-chromium ferritic alloys are typically used as the base material for the metal interconnects to maintain the structural strength of the components and match the thermal expansion coefficients of the remaining cell assemblies. To meet the operational requirements of the fuel cell stack, existing technologies typically prepare a single-layer manganese-cobalt coating on the outer surface of the ferritic alloy substrate. This single-layer coating structure is used to conduct current during high-temperature reactions and provide basic physical isolation.

[0004] In existing technologies, single-layer coating structures cannot effectively prevent the outward diffusion of elements from the substrate under long-term high-temperature operation. The continuous formation of an oxide film at the substrate interface leads to a continuous increase in interfacial contact resistance. At the same time, chromium elements inside the substrate are converted into gaseous chromium oxides at high temperatures. These gaseous chromium oxides penetrate the single-layer coating structure and overflow outward, depositing at the oxygen electrode and causing poisoning and degradation of the electrode structure, thus reducing the overall lifespan of the fuel cell stack. Summary of the Invention

[0005] To address the shortcomings of existing technologies, this application provides a low contact resistance metal connector and flow field structure, which solves the problems mentioned in the background art.

[0006] To achieve the above objectives, this application provides the following technical solution: The first aspect of this application provides a low contact resistance metal connector, comprising: a substrate, a double-layer protective coating, a biomimetic dendritic flow field, and a transversely integrated thermal rib.

[0007] The double-layer protective coating is attached to the outer surface of the substrate; the double-layer protective coating includes, from the inside to the outside, a conductive underlayer that adheres to the surface of the substrate and a composite barrier layer that covers the outside of the conductive underlayer.

[0008] The biomimetic dendritic flow field is disposed on the working surface of the substrate; the biomimetic dendritic flow field includes a main flow channel and branch flow channels.

[0009] The horizontal integrated heat-conducting rib is disposed on the back side of the substrate; the horizontal integrated heat-conducting rib is integrally stamped from the substrate.

[0010] Furthermore, the conductive substrate is Mn 1.5 Co 1.5 The composite barrier layer has an O4 spinel structure; the composite barrier layer has a Ce-Mn composite structure; the composite barrier layer and the conductive underlayer are combined to form a dense coating.

[0011] Furthermore, the thickness of the conductive bottom layer is 5 μm to 30 μm; the thickness of the composite barrier surface layer is 5 μm to 15 μm.

[0012] Furthermore, the substrate is made of Crofer 22 APU high-chromium ferritic alloy; the thickness of the substrate is 0.3 mm to 1.0 mm; the outer surface of the substrate is provided with surface microstructures, and the surface roughness Ra of the surface microstructures is 0.5 μm to 2 μm.

[0013] Furthermore, the lateral integrated thermally conductive ribs are distributed laterally in-plane along the substrate.

[0014] Furthermore, the thickness of the lateral integrated heat-conducting rib is 0.3 mm to 1 mm, the height of the lateral integrated heat-conducting rib is 0.8 mm to 1.5 mm, and the spacing between adjacent lateral integrated heat-conducting ribs is 8 mm to 15 mm.

[0015] A second aspect of this application provides a flow field structure for a low contact resistance metal connector, wherein the biomimetic dendritic flow field is divided into three differentiated flow channel distribution regions along the surface of the substrate; the three flow channel distribution regions include a central region, a transition region, and an edge region.

[0016] Furthermore, the central region has a low-porosity structure, and the main flow channels and branch flow channels within the central region are arranged in a high-density configuration; the transition region has a medium-porosity structure, and the branch flow channels within the transition region are arranged in a medium-density configuration; the edge region has a high-porosity structure, and the branch flow channels within the edge region are arranged in a low-density configuration.

[0017] Furthermore, the width of the main flow channel is 4mm to 8mm, and the depth of the main flow channel is 0.8mm to 1.5mm; the branch flow channel extends outward from the main flow channel; the width of the branch flow channel is 1mm to 3mm, and the depth of the branch flow channel is 0.5mm to 1.0mm; the spacing between adjacent branch flow channels is 8mm to 15mm.

[0018] This application provides a low contact resistance metal connector and flow field structure. It has the following advantages: 1. This application addresses the issues of high-temperature oxidation and element volatilization in a ferritic alloy substrate by applying a double-layer protective coating. The inner manganese-cobalt spinel conductive underlayer provides an electron conduction pathway under high-temperature conditions. Combined with the micro-undulation structure formed by sandblasting the substrate surface, it increases the physical contact area at the interface and reduces the interfacial contact resistance between the metal connector and the battery cell. The outer cerium-manganese composite barrier layer forms a dense isolation layer that blocks the outward diffusion path of gaseous chromium oxides from within the substrate under high-temperature conditions, inhibits chromium volatilization, and prevents electrode structure degradation.

[0019] 2. This application achieves balanced distribution of large-area reactive gases by setting a dendritic flow field on the working surface of the metal connector. The flow field is divided into three regions with different pore structures and densities: a central region, a transition region, and an edge region. The main channel reduces the gas transmission pressure drop, the high-density arrangement in the central region maintains uniform flow velocity and suppresses local carbon deposition, and the low-density arrangement in the edge region increases the gas supply to the outer area. The differentiated zoning configuration controls the gas flow velocity deviation within the overall working surface within the limited process parameters, eliminates the problem of local reactive gas deficiency caused by conventional equal-width straight groove flow channels, and improves the uniformity of fluid distribution.

[0020] 3. This application solves the problems of thermal stress concentration and plate warping during thermal cycling by integrally stamping a transverse heat-conducting rib structure on the back of the metal connector. The integral stamping process maintains the original support strength of the base without adding additional assembly parts. The transverse heat-conducting ribs extend laterally along the surface of the base, increasing the in-plane transverse heat-conducting area inside the metal connector. Under high-temperature reaction conditions, the locally generated heat is conducted to both sides along the heat-conducting rib structure, reducing the overall in-plane temperature difference of the metal connector, suppressing local overheating, and maintaining stable structural contact pressure during thermal cycling. Attached Figure Description

[0021] Figure 1 This is a plan view of the overall structure of the metal connector in this application; Figure 2 This is a cross-sectional view of the double-layer protective coating of this application; Figure 3 This is a schematic diagram of the biomimetic dendritic flow field fluid distribution of this application; Figure 4 This is a cross-sectional view of the horizontally integrated heat-conducting rib structure of this application; Figure 5 This is a microscopic view of the coating cross-section of this application.

[0022] Among them, 100 is the substrate; 200 is the double-layer protective coating; 210 is the conductive bottom layer; 220 is the composite barrier surface layer; 300 is the biomimetic dendritic flow field; 310 is the main flow channel; 320 is the branch flow channel; 400 is the transverse integrated heat-conducting rib; 510 is the gas inlet; and 520 is the gas outlet. Detailed Implementation

[0023] The technical solutions in the embodiments of this application will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of this application, and not all embodiments. Based on the embodiments of this application, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of this application.

[0024] Please see the appendix Figure 1 -Appendix Figure 5 This application provides a low contact resistance metal connector and flow field structure, including a substrate 100, a double-layer protective coating 200, a biomimetic dendritic flow field 300, and a transverse integrated thermal rib 400.

[0025] The substrate 100 serves as the load-bearing and supporting foundation of the overall structure. A double-layer protective coating 200 is attached to the outer surface of the substrate 100. The double-layer protective coating 200 includes, from the inside out, a conductive underlayer 210 adhered to the surface of the substrate 100 and a composite barrier surface layer 220 covering the outside of the conductive underlayer 210.

[0026] A biomimetic dendritic flow field 300 is disposed on the working surface of the substrate 100. The biomimetic dendritic flow field 300 includes a main flow channel 310 and branch flow channels 320.

[0027] The horizontal integrated heat-conducting rib 400 is disposed on the back side of the substrate 100. The horizontal integrated heat-conducting rib 400 is integrally stamped from the substrate 100.

[0028] In the overall workflow, the metal connector performs functions such as gas distribution, current conduction, and heat conduction.

[0029] The reactant gas enters through the gas inlet 510 of the metal connector. The reactant gas first enters the main channel 310 of the biomimetic dendritic flow field 300. The main channel 310 transports the gas and reduces the fluid pressure drop.

[0030] The reactant gas is diverted from the main flow channel 310 to the branch flow channel 320. The branch flow channel 320 distributes the gas to the cell reaction area. The reacted gas is discharged through the gas outlet 520.

[0031] During current conduction, the current passes through the double protective coating 200 and the substrate 100. The conductive underlayer 210 provides an electron conduction path, reducing the contact resistance between the substrate 100 and the battery cell.

[0032] In an operating environment of 700 to 850°C, the substrate 100 generates vaporized chromium. The composite barrier layer 220 forms a barrier layer on the outside of the conductive bottom layer 210, blocking the outward diffusion of vaporized chromium and preventing electrode attenuation.

[0033] The heat generated during operation is conducted to the metal connector. The integrated transverse heat-conducting rib 400 receives the heat and conducts it along the transverse cross-section of the base 100. The integrated transverse heat-conducting rib 400 increases the in-plane conduction area, making the heat distribution more even in the metal connector.

[0034] The metal connector has a substrate 100 comprising: an alloy material body and surface microstructures disposed on the outer surface of the alloy material body.

[0035] The matrix 100 is made of Crofer 22 APU high-chromium ferritic alloy. This high-chromium ferritic alloy provides high-temperature oxidation resistance and creep resistance in high-temperature environments of 700 to 850°C, while maintaining the mechanical strength of the matrix 100.

[0036] The thickness of the substrate 100 is set to 0.3 mm to 1.0 mm. Preferably, the thickness of the substrate 100 is 0.5 mm.

[0037] The outer surface of the substrate 100 is provided with surface microstructures. The surface microstructures are formed by sandblasting the outer surface of the substrate 100.

[0038] After sandblasting, the surface roughness Ra value of the outer surface of the substrate 100 is controlled between 0.5μm and 2μm.

[0039] The surface microstructure increases the contact area between the substrate 100 and the battery cell. The increased contact area reduces the contact resistance between the substrate 100 and the battery cell.

[0040] The dual-layer protective coating 200 includes a conductive underlayer 210 and a composite barrier surface layer 220.

[0041] A conductive substrate 210 is disposed on the outer surface of the substrate 100. The conductive substrate 210 is Mn 1.5 Co 1.5 O4 spinel structure. The thickness of the conductive underlayer 210 is set to 5 μm to 30 μm; preferably, the thickness of the conductive underlayer 210 is 15 μm.

[0042] The conductive underlayer 210 reduces the contact resistance at the interface of the substrate 100 and provides adhesion between the double-layer protective coating 200 and the substrate 100. Under high-temperature conditions, the conductive underlayer 210 and the substrate 100 form a dense Cr2O3 layer at their interface.

[0043] A composite barrier layer 220 is disposed on the outer surface of the conductive substrate 210. The composite barrier layer 220 has a Ce-Mn composite structure, and Ce and Mn elements are uniformly distributed in the composite barrier layer 220. The thickness of the composite barrier layer 220 is set to 5 μm to 15 μm; preferably, the thickness of the composite barrier layer 220 is 8 μm.

[0044] The composite barrier surface layer 220 and the conductive underlayer 210 are combined to form a dense coating. The cross-sectional structure of this dense coating is continuous, and there are no obvious cracks or pores inside.

[0045] At high temperatures of 700 to 850°C, the composite barrier layer 220 inhibits the growth of oxides on the surface of the substrate 100. As a barrier layer, the composite barrier layer 220 blocks the outward diffusion path of CrO3 in the gas phase, inhibiting the volatilization of chromium to the external electrode.

[0046] The conductive bottom layer 210 and the composite barrier surface layer 220 together form a double-layer protective structure system. The double-layer protective coating 200 maintains the high-temperature stability of the metal connector.

[0047] A biomimetic dendritic flow field 300 is disposed on the working surface of the substrate 100. The biomimetic dendritic flow field 300 has a branching structure, including a main flow channel 310 and branch flow channels 320 that are interconnected.

[0048] The main channel 310 has a width of 4mm to 8mm and a depth of 0.8mm to 1.5mm. The main channel 310 conveys a large flow rate of gas, reducing fluid pressure drop.

[0049] Branch channels 320 extend outward from the main channel 310. The width of the branch channels 320 is 1 mm to 3 mm, and the depth is 0.5 mm to 1.0 mm. The spacing between adjacent branch channels 320 is 8 mm to 15 mm. The branch channels 320 uniformly distribute the gas, improving reaction uniformity.

[0050] The biomimetic dendritic flow field 300 is divided into three differentiated flow channel distribution regions along the surface of the substrate 100. These three flow channel distribution regions include a central region, a transition region, and an edge region.

[0051] The central region has a low-porosity structure, with the main flow channel 310 and branch flow channels 320 arranged in a high-density configuration. The central region maintains a uniform gas flow rate and inhibits carbon buildup.

[0052] The transition zone has a mesoporous structure, and the branch channels 320 are arranged with a medium density. The transition zone smoothly transitions and evenly distributes the gas.

[0053] The edge region has a high-porosity structure, while the branch channels 320 are arranged in a low-density configuration. The edge region enhances the gas supply to the edge area.

[0054] The basic dimensions of the metal connector are 200mm × 200mm, with an effective reaction area of ​​400cm²; the extended dimensions are 250mm × 250mm, with an effective reaction area of ​​625cm². 2 .

[0055] The biomimetic dendritic flow field 300 controls the uniformity of gas flow velocity across the working surface of the metal connector within ±5% through differentiated arrangement and size characteristics.

[0056] A horizontally integrated thermal rib 400 is disposed on the back side of the substrate 100.

[0057] The transverse integrated heat-conducting rib 400 and the substrate 100 are integrally stamped structures. The transverse integrated heat-conducting rib 400 extends laterally along the in-plane distribution of the substrate 100.

[0058] The thickness of the horizontal integrated heat-conducting rib 400 is 0.3mm to 1mm, and the height is 0.8mm to 1.5mm; the spacing between adjacent horizontal integrated heat-conducting ribs 400 is 8mm to 15mm.

[0059] The integrally stamped transverse thermally conductive rib 400 maintains the structural strength of the base 100 and reduces contact resistance.

[0060] The lateral integrated thermal rib 400 increases the lateral thermal conduction area of ​​the metal connector, and conducts local reaction heat laterally in the plane of the substrate 100. The lateral integrated thermal rib 400 reduces the in-plane temperature difference of the metal connector and suppresses local overheating.

[0061] By incorporating lateral integrated thermal ribs 400, the maximum temperature difference inside the fuel cell stack is reduced by 50%, thus extending the lifespan of the cells.

[0062] This application provides a method for preparing a metal connector, the method comprising: Crofer 22 APU alloy sheet was selected as the substrate 100. The substrate 100 was integrally formed using laser stamping. A biomimetic dendritic flow field 300 was formed on the working surface of the substrate 100, and transverse integrated heat-conducting ribs 400 were formed on the back surface of the substrate 100. The dimensional accuracy of the laser stamping process was controlled within ±0.05 mm.

[0063] The outer surface of the substrate 100 after laser stamping is sandblasted to control the surface roughness Ra of the outer surface of the substrate 100 to be 0.5μm to 2μm.

[0064] A conductive underlayer 210 is prepared on the outer surface of the substrate 100 using a plasma spraying process. This spraying process uses Mn... 1.5 Co 1.5 O4 deposition forms a conductive underlayer 210.

[0065] A composite barrier surface layer 220 is prepared on the outer surface of the conductive substrate 210 using an impregnation process. This impregnation process uses a Ce-Mn precursor solution to coat the conductive substrate 210.

[0066] The substrate 100, to which the conductive underlayer 210 and the composite barrier surface layer 220 are attached, is subjected to heat treatment. The heat treatment is carried out in an air atmosphere at a temperature of 900°C for 2 hours. This heat treatment process promotes the crystallization of the conductive underlayer 210 and the composite barrier surface layer 220, forming a double-layer protective coating 200.

[0067] Example 1: High-Temperature Oxidation and Contact Resistance Test Metal connector samples with a double-layer protective coating on the outer surface were prepared. The testing environment was configured as an air atmosphere, and the internal temperature of the heating equipment was set to 800℃. The testing cycle was set to continuous operation for 3000 hours.

[0068] The contact resistance of the metal connector interface was recorded as 8.4 mΩ·cm during the initial stage of operation. 2 After 1000 hours of operation, the interface contact resistance test value changed to 9.7 mΩ·cm. 2 After 3000 hours of operation, the final measured value of the interface contact resistance was 12.8 mΩ·cm. 2 During the 3000-hour high-temperature operation cycle, the cumulative increase in contact resistance was 4.4 mΩ·cm. 2 Test data shows that the ASR increase of the double-coated connector after 3000 hours of high-temperature operation was controlled within 5 mΩ·cm. 2 Within.

[0069] Table 1. High-Temperature Oxidation and Contact Resistance Test Data Testing phase Continuous runtime (h) <![CDATA[Interfacial contact resistance test value (mΩ·cm 2 )]]> <![CDATA[Stage resistance increase (mΩ·cm 2 )]]> <![CDATA[Cumulative resistance increase (mΩ·cm 2 )]]> initial stage 0 8.4 - 0 Mid-term monitoring 1000 9.7 1.3 1.3 End of cycle 3000 12.8 3.1 4.4 Example 2: Fluid Pressure Drop and Distribution Test A metal connector with a biomimetic dendritic flow field on its working surface was prepared, and the effective reaction area of ​​the metal connector was adapted to a 400 cm² area. 2 The individual battery cell. An air source was connected to the fluid testing platform, and the inlet gas flow rate was set to a fixed process parameter.

[0070] A conventional straight-slot flow field metal connector was used as a comparison sample, and its inlet and outlet fluid pressure drop was measured to be 1284 Pa. Subsequently, the biomimetic dendritic flow field metal connector provided in this embodiment was used, and its inlet and outlet fluid pressure drop was measured to be 827 Pa under the same gas source conditions. Compared to the conventional straight-slot flow field structure, this embodiment is adapted to a 400 cm... 2 The biomimetic dendritic flow field of the battery cell reduces the fluid pressure drop by 35.6%.

[0071] Table 2 Comparison of Fluid Pressure Drop and Distribution Tests Flow field structure type <![CDATA[Adapted effective reaction area (cm 2 )]]> Inlet and outlet fluid pressure drop measurements (Pa) Calculated value of pressure drop (%) Traditional constant-width straight groove flow field structure (comparative example) 400 1284 - Bionic dendritic flow field structure (this application) 400 827 35.6% Example 3: Thermal Cycling Deformation Resistance Test A metal connector with integrated horizontal thermal ribs on the back was selected as the test sample. A programmed temperature rise furnace was used for testing. Each thermal cycle was set to heat from room temperature (25℃) to 800℃, hold at that temperature, and then cool back to room temperature. A total of 500 thermal cycles were performed on the test sample.

[0072] The geometric deformation data of the metal connector sample before and after thermal cycling were recorded using a coordinate measuring machine. The initial flatness error of the sample before testing was 0.03 mm. After 500 thermal cycles from room temperature to 800℃, the flatness error of the sample changed to 0.08 mm. After the test, the metal connector plate remained flat overall, with no obvious warping deformation.

[0073] Table 3. Thermal Cycling Deformation Resistance Test Data test node Total number of thermal cycles (times) Sample flatness error measurement (mm) Macroscopic Deformation Status Assessment Pre-loop test 0 0.03 Initial flat state Post-loop test 500 0.08 No obvious warping or deformation Example 4: System-level long-term operation test The metal interconnects provided in this application are alternately stacked and assembled with solid oxide single cells. 120 cells are used to form a short-reactor system with a nominal power of 8 kW. Multiple 8 kW short-reactor combinations are then used to construct a modular system with a power output of 25 kW.

[0074] The system operating temperature was set to 750℃. The modular unit operated continuously for 5000 hours under constant load conditions. The energy conversion efficiency was recorded as 92.1% during the initial stage of operation. After 5000 hours of continuous operation, the continuous operating efficiency of the 25kW module with 120 cells and an 8kW short stack was measured to be 91.5%.

[0075] Table 4 System-level Long-Cycle Operation Efficiency Record Table Operational phase Cumulative continuous runtime (h) Modular overall energy conversion efficiency (%) Operational status assessment Initial stage of grid connection 0 92.1 Stable rated output End of cycle 5000 91.5 Stable rated output Example Test Conclusion A technical analysis is conducted based on the test data from the above specific embodiments and the structural innovation mechanism of this application.

[0076] At the material interface protection level, the conductive bottom layer in the double-layer protective coating maintains the electron transport channel between the metal connector and the battery cell, while the composite barrier layer limits the excessive growth of oxides on the outer surface of the substrate in a high-temperature environment and cuts off the outward diffusion path of vapor-phase chromium. The test data of Example 1 confirms that this double-layer microscopic physical barrier mechanism maintains the conductivity stability of the coating interface in a long-term high-temperature oxidation environment, preventing the sharp increase in contact resistance caused by continuous oxidation in traditional structures.

[0077] At the fluid dynamics distribution level, the biomimetic dendritic flow field utilizes a differentiated density arrangement design in three regions—center, transition, and edge—to alter the flow resistance distribution of gas within a large reaction area. Test data from Example 2 confirms that this partitioned arrangement structure, while maintaining uniform gas distribution across the entire domain, reduces frictional resistance and eliminates the problem of excessively high local fluid pressure drop caused by straight flow channel structures.

[0078] At the thermodynamic conduction level, the transversely integrated thermally conductive ribs form transverse thermal conduction channels on the back of the substrate. The test data of Example 3 confirms that the increase in the in-plane transverse thermal conduction area of ​​the metal connector accelerates the diffusion of local reaction heat, reduces the in-plane temperature difference of the substrate structure, eliminates the concentration of thermal stress inside the material, and maintains the macroscopic geometric stability of the plate after undergoing hundreds of extreme thermal shocks.

[0079] At the overall system integration level, the three physical mechanisms of antioxidant barrier at the material interface, balanced flow field distribution on the working surface, and structural heat conduction on the back side work together to maintain the consistency of electrochemical reaction conditions inside the fuel cell stack. The test data in Example 4 confirms that the low contact resistance metal connector and flow field structure of this application effectively suppress electrode poisoning and local thermal failure during long-term operation of a 25kW high-power module, maintaining the high-efficiency and stable operation of the fuel cell stack system.

[0080] Although embodiments of this application have been shown and described, it will be understood by those skilled in the art that various changes, modifications, substitutions and variations can be made to these embodiments without departing from the principles and spirit of this application, the scope of which is defined by the appended claims and their equivalents.

Claims

1. A low contact resistance metal connector, characterized in that, include: The substrate (100), double-layer protective coating (200), biomimetic dendritic flow field (300), and transverse integrated thermal ribs (400) are all included. The double-layer protective coating (200) is attached to the outer surface of the substrate (100); the double-layer protective coating (200) includes, from the inside to the outside, a conductive bottom layer (210) attached to the surface of the substrate (100) and a composite barrier surface layer (220) covering the outside of the conductive bottom layer (210); The biomimetic dendritic flow field (300) is disposed on the working surface of the substrate (100); the biomimetic dendritic flow field (300) includes a main flow channel (310) and branch flow channels (320) connected to each other; The transverse integrated heat-conducting rib (400) is disposed on the back side of the substrate (100); the transverse integrated heat-conducting rib (400) is integrally stamped from the substrate (100).

2. The low contact resistance metal connector according to claim 1, characterized in that, The conductive substrate (210) is Mn 1.5 Co 1.5 The composite barrier layer (220) has an O4 spinel structure; the composite barrier layer (220) has a Ce-Mn composite structure; the composite barrier layer (220) and the conductive bottom layer (210) are combined to form a dense coating.

3. A low contact resistance metal connector according to claim 2, characterized in that, The thickness of the conductive bottom layer (210) is 5 μm to 30 μm; the thickness of the composite barrier surface layer (220) is 5 μm to 15 μm.

4. A low contact resistance metal connector according to claim 1, characterized in that, The substrate (100) is made of Crofer 22 APU high-chromium ferritic alloy; the thickness of the substrate (100) is 0.3 mm to 1.0 mm; The outer surface of the substrate (100) is provided with surface microstructures, and the surface roughness Ra of the surface microstructures is 0.5 μm to 2 μm.

5. A low contact resistance metal connector according to claim 1, characterized in that, The transverse integrated thermal ribs (400) are distributed in a transverse direction along the in-plane of the substrate (100).

6. A low contact resistance metal connector according to claim 5, characterized in that, The thickness of the transverse integrated heat-conducting rib (400) is 0.3 mm to 1 mm, and the height of the transverse integrated heat-conducting rib (400) is 0.8 mm to 1.5 mm; the spacing between adjacent transverse integrated heat-conducting ribs (400) is 8 mm to 15 mm.

7. A flow field structure for a low contact resistance metal connector, used to achieve a low contact resistance metal connector as described in any one of claims 1-6, characterized in that, The biomimetic dendritic flow field (300) is divided into three differentiated flow channel distribution regions along the surface of the substrate (100); the three flow channel distribution regions include a central region, a transition region, and an edge region.

8. The flow field structure of a low contact resistance metal connector according to claim 7, characterized in that, The central region has a low porosity structure, and the main flow channel (310) and the branch flow channel (320) in the central region are arranged in a high density. The transition zone has a mesoporous structure, and the branch channels (320) within the transition zone are arranged with a medium density. The edge region has a high porosity structure, and the branch channels (320) within the edge region are arranged in a low density.

9. The flow field structure of a low contact resistance metal connector according to claim 8, characterized in that, The width of the main channel (310) is 4 mm to 8 mm, and the depth of the main channel (310) is 0.8 mm to 1.5 mm.

10. The flow field structure of a low contact resistance metal connector according to claim 8, characterized in that, The branch channel (320) extends outward from the main channel (310); the width of the branch channel (320) is 1 mm to 3 mm, and the depth of the branch channel (320) is 0.5 mm to 1.0 mm; the spacing between adjacent branch channels (320) is 8 mm to 15 mm.