Composite solid electrolyte membranes, their preparation methods and applications

By combining sulfide solid electrolyte, lithium salt and hexahydrotriazine polymer in the composite solid electrolyte membrane, the problems of poor interfacial contact and stability of sulfide-based solid electrolyte membrane in semi-solid batteries are solved, thereby improving the cycle life and electrochemical stability of the battery.

CN123120837APending Publication Date: 2026-11-17HUANENG ARONGQI NEW ENERGY CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202610964903.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-06-30
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

In semi-solid batteries, sulfide-based solid electrolyte membranes suffer from poor interfacial contact and increased impedance due to volume changes in the positive and negative electrode materials, which affects cycle life. They also suffer from poor air stability and a narrow electrochemical window. Existing modification methods are costly and their effects are difficult to meet industrialization requirements.

Method used

The composite solid electrolyte membrane is composed of a sulfide solid electrolyte, lithium salt, and a hexahydrotriazine polymer. The hexahydrotriazine polymer is formed by the polymerization of the first and second monomers and has a hyperbranched topology and abundant molecular cavities. Combined with the lithium salt, it forms a regular network macromolecular structure, which improves electrochemical stability and self-healing ability.

Benefits of technology

It improves the cycle life of semi-solid-state batteries by enhancing lithium-ion transport capacity through abundant molecular cavities and chemically stable hexahydrotriazine polymers, reducing impurity introduction and side reactions, and achieving efficient self-repair and oxidation-reduction resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123120837A_ABST
    Figure CN123120837A_ABST
Patent Text Reader

Abstract

This application proposes a composite solid electrolyte membrane, its preparation method, and its application. The composite solid electrolyte membrane comprises a sulfide solid electrolyte, a lithium salt, and a hexahydrotriazine polymer. The hexahydrotriazine polymer is formed by polymerization of a first monomer and a second monomer. The first monomer has the structure shown in formula (I): In formula (I), R1, R2, and R3 are each independently selected from unsubstituted or Ra-substituted C. 2‑12 Alkenyl, unsubstituted or Ra-substituted C 2‑12 Alkyne group, etc.; Ra is selected from C 1‑6 Alkyl, C 1‑6 The first monomer comprises at least one of alkoxy groups, etc.; the second monomer comprises at least one of esters, ethers, amines, alkenes, and nitriles that have polymerization properties. The composite solid electrolyte membrane described in this application, containing a sulfide solid electrolyte, a lithium salt, and a hexahydrotriazine polymer formed by the polymerization of the first and second monomers, can improve the cycle life of a semi-solid-state battery when used in such batteries.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application relates to the field of energy storage technology, and in particular to a composite solid electrolyte membrane, its preparation method, and its application. Background Technology

[0002] Semi-solid batteries use solid electrolytes instead of traditional organic liquid electrolytes, which can improve battery safety and cycle stability, and are expected to be applied in the field of large-scale energy storage.

[0003] Sulfide-based solid electrolytes exhibit excellent ionic conductivity, approaching that of liquid electrolytes. However: On the one hand, during the cycling process, the semi-solid battery with sulfide-based solid electrolyte membrane suffers from poor interfacial contact due to changes in the volume of the positive and negative electrode materials, which increases the impedance of the semi-solid battery and affects its cycle life.

[0004] On the other hand, sulfide-based solid electrolytes suffer from poor air stability and a narrow electrochemical window.

[0005] In related technologies, techniques such as modifying positive and negative electrode materials, constructing interface buffer layers, or modifying sulfide-based solid electrolytes are used to reduce the impedance growth of sulfide-based solid electrolytes during cycling. Although these methods can alleviate the interface mismatch problem of sulfide-based solid electrolytes to some extent, the raw material costs are high, the processing technology is complex, and the improvement effect achieved in dynamic cycling is difficult to meet the needs of industrial applications. Summary of the Invention

[0006] In view of this, one object of this application is to provide a composite solid electrolyte membrane containing a sulfide solid electrolyte, a lithium salt and a hexahydrotriazine polymer formed by polymerization of a first monomer and a second monomer, for use in a semi-solid battery, which can improve the cycle life of the semi-solid battery.

[0007] Another objective of this application is to provide a method for preparing a composite solid electrolyte membrane.

[0008] Another objective of this application is to provide a semi-solid-state battery.

[0009] Another object of this application is to provide an electrical device.

[0010] Another object of this application is to provide an electrical appliance.

[0011] To achieve the above objectives, the first aspect of this application proposes a composite solid electrolyte membrane comprising a sulfide solid electrolyte, a lithium salt, and a hexahydrotriazine polymer, wherein the hexahydrotriazine polymer is formed by polymerization of a first monomer and a second monomer. The first monomer has the structure shown in formula (Ⅰ): Equation (Ⅰ), In equation (I), R1, R2, and R3 are each independently selected from unsubstituted or Ra-substituted C. 2-12 Alkenyl, unsubstituted or Ra-substituted C 2-12 Alkyne group, unsubstituted or Ra-substituted C 3-13 Cycloalkyl, unsubstituted or Ra-substituted C 1-11 Cyano, unsubstituted or Ra-substituted C 1-11 Aldehyde group, unsubstituted or Ra-substituted C 1-11 Amine, unsubstituted or Ra-substituted C 3-13 Imidazole group, unsubstituted or Ra-substituted C 3-13 One of the pyridinyl groups; Ra is selected from C 1-6 Alkyl, C 1-6 Alkoxy, C 2-6 alkenyl, C 2-6 alkynyl group, C 1-6 Acyl group, C 1-6 ether group, C 6-10 At least one of aryl and halogen atoms; The second monomer includes at least one of esters, ethers, amines, alkenes, and nitriles that have polymerization properties.

[0012] The composite solid electrolyte membrane described in this application can bring at least the following beneficial effects: The product contains a sulfide solid electrolyte, a lithium salt, and a hexahydrotriazine polymer formed by polymerization of a first monomer and a second monomer. The hexahydrotriazine polymer possesses a hyperbranched topology and abundant molecular cavities. On the one hand, these abundant cavities provide channels for ions to freely shuttle, enhancing the lithium-ion transport capacity of the hexahydrotriazine polymer. On the other hand, the R groups (R1, R2, R3) in the first monomer contain polymerizable functional groups, and the R groups substitute for the nitrogen (N) position of the triazine ring. Compared to polymers where the carbon (C) adjacent to the N position in the triazine ring is substituted, the monomer of formula (I) has a higher molecular weight. The polymer composition enhances the chemical stability of the hexahydrotriazine polymer's backbone nodes, making it less prone to ring-opening during battery cycling. Furthermore, the combination of the sulfide solid electrolyte, lithium salt, and hexahydrotriazine polymer results in several advantages. First, the sulfide solid electrolyte exhibits stronger electrochemical stability, utilizing its high ionic conductivity while minimizing decomposition during charge and discharge. Second, the lithium salt generates a regularized network macromolecular structure, reducing the introduction of impurities and side reactions. In summary, the composite solid electrolyte membrane formed by the sulfide solid electrolyte, lithium salt, and hexahydrotriazine polymer in this application demonstrates highly efficient self-healing capabilities and excellent redox stability during cycling, thereby improving the cycle life of the semi-solid-state battery.

[0013] In some embodiments, the mass ratio of the first monomer to the second monomer is 1:(10 to 120).

[0014] In some embodiments, in formula (I), R1, R2, and R3 are each independently selected from unsubstituted C. 2-12 alkenyl, unsubstituted C 2-12 Alkyne group, unsubstituted C 3-13 cycloalkyl, unsubstituted C 1-11 Cyano, unsubstituted or Ra-substituted C 1-11 Aldehyde group, unsubstituted or Ra-substituted C 3-13 One of the imidazole groups.

[0015] In some embodiments, the first monomer comprises at least one of the following compounds: Equation (Ⅰ-1) Equation (Ⅰ-2), Equation (Ⅰ-3) Equation (Ⅰ-4) Equation (Ⅰ-5) Equation (Ⅰ-6) Equation (Ⅰ-7) Equation (Ⅰ-8).

[0016] In some embodiments, the second monomer includes at least one selected from methyl acrylate, methyl methacrylate, ethylene glycol dimethyl ether, diethylene glycol dimethyl ether, N,N'-methylenebisacrylamide, N,N'-ethylenebisacrylamide, N,N'-propylenebisacrylamide, vinylidene fluoride, trifluoroethylene, hexafluoropropylene, trifluorochloroethylene, 1,1-chlorofluoroethylene, difluorochloroethylene, and acrylonitrile.

[0017] In some embodiments, the composite solid electrolyte membrane includes at least one of the following features: a) Based on the mass of the composite solid electrolyte membrane, the mass percentage of the sulfide solid electrolyte is a, where 70% ≤ a ≤ 94%; b) Based on the mass of the composite solid electrolyte membrane, the mass percentage of the lithium salt is b, where 5% ≤ b ≤ 20%; c) Based on the mass of the composite solid electrolyte membrane, the mass percentage of the hexahydrotriazine polymer is c, where 1% ≤ c ≤ 10%; d) The mass ratio of the sulfide solid electrolyte to the lithium salt is (5-20):1; e) The average pore size of the composite solid electrolyte membrane is D1, and the average particle size of the sulfide solid electrolyte is D2, where 0.003 ≤ D1 / D2 ≤ 0.1; f) The thickness of the composite solid electrolyte membrane is H, where 10 μm ≤ H ≤ 80 μm.

[0018] In some embodiments, the lithium salt includes at least one of lithium hexafluorophosphate, lithium dioxaborate, lithium tetrafluoroborate, lithium difluorooxaborate, lithium trifluoromethanesulfonate, lithium bis(trifluoromethanesulfonyl)imide, and lithium bis(fluorosulfonyl)imide.

[0019] In some embodiments, the sulfide solid electrolyte includes at least one of glass-ceramic-based sulfides, sulfide-germanium sulfides, thio-ultrafast ionic compounds, and LGPS-type sulfides.

[0020] In some embodiments, the sulfide solid electrolyte includes Li2S-P2S5 and Li7P3S. 11 Li4 x A1 y M y S4, Li6PS5Cl and Li 10 GeP2S 12 At least one of them, and Li4 x A1 y M y In S4, A includes Si or Ge elements, M includes Zn, Al, or P elements, and 0 < x < 4, 0 < y < 1.

[0021] The second aspect of this application discloses a method for preparing a composite solid electrolyte membrane, comprising: The sulfide solid electrolyte, the lithium salt, and the first solvent are mixed to obtain a first slurry; The first slurry is dried and rolled to obtain a base film material; The first monomer, the second monomer, and the second solvent are mixed to obtain a post-treatment solution; The base film material is immersed in the post-treatment solution to obtain the post-treated base film material; The post-treated base film material is subjected to polymerization reaction and hot pressing to obtain the composite solid electrolyte membrane.

[0022] The method for preparing the composite solid electrolyte membrane described in this application, in addition to having the beneficial effects of the composite solid electrolyte membrane described in this application, can also bring at least the following beneficial effects: In the rolled base film material, the solid electrolyte particles are in close contact, exhibiting good mechanical strength. By introducing the first monomer, the second monomer, and the second solvent into the composite solid electrolyte membrane through a post-treatment solution, a coating layer is formed on and inside the base film material without damaging the closely contacting solid electrolyte particles or affecting the mechanical strength of the base film material itself. It also facilitates the polymerization to form a self-healing protective layer. The composite solid electrolyte membrane prepared by this method maintains its performance advantages for a longer period.

[0023] In some embodiments, during the polymerization reaction process, the first monomer and the second monomer in the post-treated base film material undergo a polymerization reaction to form the hexahydrotriazine polymer.

[0024] In some embodiments, the polymerization reaction is performed before the hot pressing treatment, or the polymerization reaction is performed simultaneously with the hot pressing treatment.

[0025] In some embodiments, the pressure of the hot pressing process is 400 to 600 MPa.

[0026] In some embodiments, when the polymerization reaction is carried out before the hot pressing treatment, the polymerization reaction temperature is 50–70°C, the polymerization reaction time is 8–22 h, the hot pressing temperature is 80–90°C, and the hot pressing time is 10–40 min.

[0027] In other embodiments, when the polymerization reaction and the hot pressing are carried out simultaneously, the temperature of the polymerization reaction and the temperature of the hot pressing are both 50-70°C, and the time of the polymerization reaction and the time of the hot pressing are both 15-20 hours.

[0028] The third aspect of this application proposes a semi-solid battery, including the composite solid electrolyte membrane described in the first aspect of this application, or including a composite solid electrolyte membrane prepared by the method described in the second aspect of this application.

[0029] In some embodiments, the semi-solid battery further includes a liquid electrolyte, and the mass ratio of the composite sulfide solid electrolyte membrane to the liquid electrolyte is 1:(0.5-10).

[0030] A fourth aspect of this application provides an energy storage device comprising a housing and at least one semi-solid-state battery as described in the third aspect of this application, the semi-solid-state battery being housed within the housing.

[0031] The fifth aspect of this application provides an electrical device including the energy storage device described in the fourth aspect of this application, wherein the energy storage device supplies power to the electrical device.

[0032] The semi-solid-state batteries, energy storage devices, and electrical equipment described in this application all have at least the beneficial effects of the composite solid electrolyte membrane and the preparation method of the composite solid electrolyte membrane described in this application.

[0033] Additional aspects and advantages of this application will be set forth in part in the description which follows, and in part will be obvious from the description, or may be learned by practice of this application. Attached Figure Description

[0034] To more clearly illustrate the technical solutions in the embodiments of this application, the drawings used in the embodiments will be briefly described below. Obviously, the drawings described below are only some embodiments of this application. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort. Among them: Figure 1 This is a flowchart illustrating a method for preparing a composite solid electrolyte membrane, which is an exemplary embodiment of this application.

[0035] Figure 2 This is a schematic diagram of the structure of an energy storage system (residential energy storage system) according to an embodiment of this application. Figure 3 This is a schematic diagram of the structure of an energy storage system (generation / distribution side energy storage system) according to another embodiment of this application.

[0036] Figure 4 This is a schematic diagram of the structure of an energy storage system (industrial and commercial energy storage system) according to another embodiment of this application.

[0037] Explanation of reference numerals in the attached figures: 400 - Energy storage system; 410 - First power conversion device; 420 - First user load; 430 - Second user load; 440 - Energy storage device; 450 - High voltage cable; 460 - Second power conversion device; 470 - Energy storage cabinet; 480 - Photovoltaic-energy storage-charging station; 490 - Automobile. Detailed Implementation

[0038] The embodiments of this application are described in detail below, with examples of the embodiments illustrated in the accompanying drawings. The embodiments described below with reference to the accompanying drawings are exemplary. Obviously, the described embodiments are only a part of the embodiments of this application, and not all of them. These embodiments are intended to explain this application, and all other embodiments obtained by those skilled in the art based on the embodiments of this application without inventive effort are within the scope of protection of this application. They should not be construed as limitations on this application.

[0039] In this application, the disclosure of numerical ranges includes all values ​​throughout the range and the disclosure of further subdivisions of the range, including the endpoints and subranges given for these ranges.

[0040] Unless otherwise specified, all raw materials and equipment involved in this application are self-made through commercial means or known methods; and all methods involved are conventional methods unless otherwise specified.

[0041] When the term “and / or” is used in a list containing two or more items, it means that any of the listed items can be used alone or in combination with any one or more of the listed items. For example, the expression “A and / or B” is intended to mean A or B or A and B, that is, A only, B only, or a combination of A and B.

[0042] <Composite Solid Electrolyte Membrane> A composite solid electrolyte membrane includes a sulfide solid electrolyte, a lithium salt, and a hexahydrotriazine polymer, wherein the hexahydrotriazine polymer is formed by polymerization of a first monomer and a second monomer. The first monomer has the structure shown in formula (Ⅰ): Equation (Ⅰ), In equation (I), R1, R2, and R3 are each independently selected from unsubstituted or Ra-substituted C. 2-12 Alkenyl, unsubstituted or Ra-substituted C 2-12 Alkyne group, unsubstituted or Ra-substituted C 3-13 Cycloalkyl, unsubstituted or Ra-substituted C 1-11 Cyano, unsubstituted or Ra-substituted C 1-11 Aldehyde group, unsubstituted or Ra-substituted C 1-11 Amine, unsubstituted or Ra-substituted C 3-13 Imidazole group, unsubstituted or Ra-substituted C 3-13 One of the pyridinyl groups; Ra is selected from C 1-6 Alkyl, C 1-6 Alkoxy, C 2-6 alkenyl, C 2-6 alkynyl group, C 1-6 Acyl group, C 1-6 ether group, C 6-10 At least one of aryl and halogen atoms; The second monomer includes at least one of esters, ethers, amines, alkenes, and nitriles that have polymerization properties.

[0043] The composite solid electrolyte membrane of this application embodiment includes a sulfide solid electrolyte, a lithium salt, and a hexahydrotriazine polymer. The hexahydrotriazine polymer has a hyperbranched topology and abundant molecular cavities. On the one hand, the abundant molecular cavities provide channels for ions to freely shuttle, enhancing the lithium-ion transport capacity of the hexahydrotriazine polymer. On the other hand, the R groups (i.e., R1, R2, R3) in the first monomer contain polymeric functional groups, and the R groups substitute for the nitrogen (N) position of the triazine ring. Compared to polymers where the carbon (C) position adjacent to the N in the triazine ring is substituted, the monomer of formula (I)... The resulting polymer enhances the chemical stability of the hexahydrotriazine polymer's backbone nodes, making it less prone to ring-opening during semi-solid-state battery cycling. Furthermore, the combination of the sulfide solid electrolyte, lithium salt, and hexahydrotriazine polymer results in several advantages. First, the sulfide solid electrolyte exhibits stronger electrochemical stability, utilizing its high ionic conductivity while reducing its decomposition during charge and discharge. Second, the lithium salt generates a regularized network macromolecular structure, which helps reduce the introduction of impurities and side reactions. In summary, the composite solid electrolyte membrane formed by the sulfide solid electrolyte, lithium salt, and hexahydrotriazine polymer in this application demonstrates highly efficient self-healing capabilities and good redox stability during cycling, thereby improving the cycle life of the semi-solid-state battery.

[0044] In some embodiments, the mass ratio of the first monomer to the second monomer is 1:(10-120). For example, the mass ratio of the first monomer to the second monomer is 1:10, 1:30, 1:50 or 1:120, which is conducive to the full reaction of the first monomer and the second monomer to obtain the hexahydrotriazine polymer of this application.

[0045] In some embodiments, in formula (I), R1, R2, and R3 are each independently selected from unsubstituted C. 2-12 alkenyl, unsubstituted C 2-12 Alkyne group, unsubstituted C 3-13 cycloalkyl, unsubstituted C 1-11 Cyano, unsubstituted or Ra-substituted C 1-11 Aldehyde group, unsubstituted or Ra-substituted C 3-13 One of the imidazole groups.

[0046] In some embodiments, the first monomer includes, but is not limited to, at least one of the following compounds: Equation (Ⅰ-1) Equation (Ⅰ-2), Equation (Ⅰ-3) Equation (Ⅰ-4) Equation (Ⅰ-5) Equation (Ⅰ-6) Equation (Ⅰ-7) Equation (Ⅰ-8).

[0047] The monomers shown in formulas (I-1) to (I-8) above are hexahydrotriazine monomers, wherein the hexahydrotriazine groups therein can polymerize with the second monomer to form the hexahydrotriazine polymer of this application.

[0048] In some embodiments, the second monomer includes, but is not limited to, at least one of methyl acrylate, methyl methacrylate, ethylene glycol dimethyl ether, diethylene glycol dimethyl ether, N,N'-methylenebisacrylamide, N,N'-ethylenebisacrylamide, N,N'-propylenebisacrylamide, vinylidene fluoride, trifluoroethylene, hexafluoropropylene, trifluorochloroethylene, 1,1-chlorofluoroethylene, difluorochloroethylene, and acrylonitrile. The aforementioned second monomer is a polymerizable monomer capable of polymerization with the hexahydrotriazine group in the first monomer, thereby forming the hexahydrotriazine polymer of this application.

[0049] In the embodiments of this application, the specific selection of the second monomer can be adjusted according to the positive and negative electrode materials of the semi-solid-state battery. For example, for a semi-solid-state battery with high voltage oxidation resistance requirements for the positive electrode, such as a battery upper limit cutoff voltage of 4V~5V and an oxidation resistance index of 4~5.5V at the highest potential on the positive electrode side during battery operation (vs. Li... + / Li), the second monomer can be selected from at least one of acrylates, halogenated acrylates, carbonates, halogenated carbonates, acrylamides, halogenated acrylamides, olefins, halogenated olefins (or oligomers). For example, it includes, but is not limited to, methyl acrylate, methyl methacrylate, vinylene carbonate, ethylene ethylene carbonate, N,N'-methylenebisacrylamide, N,N'-ethylenebisacrylamide, N,N'-propylenebisacrylamide, vinylidene fluoride, trifluoroethylene, hexafluoropropylene, trifluorochloroethylene, 1,1-chlorofluoroethylene, difluorochloroethylene, etc. For semi-solid-state batteries with reduction stability requirements for the negative electrode, for example, a lower limit cutoff voltage of 2.5V~3V, and an oxidation resistance index of -0.5~0.5V on the negative electrode side during battery operation (vs. Li). + / Li), the second monomer may be selected from at least one of ethers, cyclic ethers, halogenated ethers, nitriles, halogenated nitriles, acrylamides, halogenated acrylamides, olefins, and halogenated olefin monomers (or oligomers). For example, including but not limited to at least one of ethylene glycol dimethyl ether, diethylene glycol dimethyl ether, acrylonitrile, N,N'-methylenebisacrylamide, N,N'-ethylenebisacrylamide, N,N'-propylenebisacrylamide, vinylidene fluoride, trifluoroethylene, hexafluoropropylene, trifluorochloroethylene, 1,1-chlorofluoroethylene, and difluorochloroethylene.

[0050] In some embodiments, the composite solid electrolyte membrane includes at least one of the following features: a) Based on the mass of the composite solid electrolyte membrane, the mass percentage of the sulfide solid electrolyte is a, where 70% ≤ a ≤ 94%; b) Based on the mass of the composite solid electrolyte membrane, the mass percentage of the lithium salt is b, where 5% ≤ b ≤ 20%; c) Based on the mass of the composite solid electrolyte membrane, the mass percentage of the hexahydrotriazine polymer is c, where 1% ≤ c ≤ 10%.

[0051] For example, based on the mass of the composite solid electrolyte membrane, the mass percentage (a) of the sulfide solid electrolyte includes, but is not limited to, 70%, 80%, 90%, or 94%, the mass percentage (b) of the lithium salt includes, but is not limited to, 5%, 10%, 15%, or 20%, and the mass percentage (c) of the hexahydrotriazine polymer includes, but is not limited to, 1%, 5%, 7%, or 10%. In the embodiments of this application, if there is too much sulfide solid electrolyte or too little hexahydrotriazine polymer, the solid electrolyte membrane structure has poor stability and it is difficult to maintain a continuous low impedance characteristic during long cycles; if there is too little inorganic filler in the sulfide solid electrolyte or too much hexahydrotriazine polymer, the solid electrolyte membrane has low ionic conductivity and it is difficult to obtain a better cycling advantage than liquid electrolyte; if there is too little lithium salt, it is difficult to effectively catalyze the copolymerization reaction between the first monomer and the second monomer; if there is too much lithium salt, the residual lithium salt during charging will reduce and consume active lithium on the negative electrode side, causing a sharp drop in the capacity of the semi-solid battery. Further research revealed that the sulfide solid electrolyte, as an inorganic filler, combined with the hexahydrotriazine polymer, can maintain structural stability during long-term cycling, and is less prone to detachment and failure from the positive and negative electrode materials, thereby improving the fast-charge and fast-discharge performance of the semi-solid-state battery during long-term cycling. The combination of lithium salt and hexahydrotriazine polymer can induce the copolymerization reaction of the first and second monomers, making the polymeric segments less prone to kinking or end-capping, thus improving the mechanical strength and ionic conductivity of the hexahydrotriazine polymer. Furthermore, the residual first monomer in the electrolyte can be reduced on the negative electrode side during charging, generating a solid electrolyte interphase (SEI) layer rich in Li3N and organic matter, further strengthening the stability of the negative electrode interface. By controlling the contents of the sulfide solid electrolyte, lithium salt, and hexahydrotriazine polymer within the above-mentioned ranges, it is beneficial to form a composite solid electrolyte membrane with the performance characteristics of this application.

[0052] In some embodiments, the average pore size of the composite solid electrolyte membrane is D1, and the average particle size of the sulfide solid electrolyte is D2, where 0.003 ≤ D1 / D2 ≤ 0.1.

[0053] For example, the values ​​of D1 / D2 mentioned above include, but are not limited to, 0.003, 0.02, 0.05, or 0.1. If the average pore size of the composite solid electrolyte membrane is too large, it indicates that the sulfide solid electrolyte has agglomerated; if the average pore size of the composite solid electrolyte membrane is too small, it indicates that the sulfide solid electrolyte is difficult to form a good composite with the hexahydrotriazine polymer. By adjusting D1 / D2 within the above range, it is beneficial to achieve uniform particle dispersion of the sulfide solid electrolyte and the construction of the hexahydrotriazine polymer three-dimensional framework, thereby improving the ionic conductivity and structural stability of the solid electrolyte membrane. Based on the above analysis, there is a correlation between the average pore size D1 of the composite solid electrolyte membrane and the sulfide solid electrolyte D2. Therefore, by adjusting D1 / D2 within the above range, it is beneficial to improve the ionic conductivity and structural stability of the composite solid electrolyte membrane, thereby improving the cycle life of the semi-solid-state battery.

[0054] In some embodiments, the thickness of the composite solid electrolyte membrane is H, where 10 μm ≤ H ≤ 80 μm. For example, H can be 10 μm, 20 μm, 40 μm, 60 μm, or 80 μm. By controlling the thickness of the composite solid electrolyte membrane within the above range, it is beneficial to ensure that the composite solid electrolyte membrane has high ionic conductivity while maintaining good mechanical strength, thereby improving the cycle life of the semi-solid battery.

[0055] In some embodiments, the mass ratio of the sulfide solid electrolyte to the lithium salt is (5-20):1. For example, the mass ratio of the sulfide solid electrolyte to the lithium salt is 5:1, 10:1, 15:1, or 20:1, etc. This facilitates the control of the content of each component in the composite solid electrolyte membrane within the scope of this application, thereby obtaining the composite solid electrolyte membrane of this application.

[0056] In some embodiments, the lithium salt includes, but is not limited to, at least one of lithium hexafluorophosphate (LiPF6), lithium dioxolaneborate (LiBOB), lithium tetrafluoroborate (LiBF4), lithium dioxolaneborate (LiDFOB), lithium trifluoromethanesulfonate (LiOTf), lithium bis(trifluoromethanesulfonyl)imide (LiTFSI), and lithium bis(fluorosulfonyl)imide (LiFSI). In embodiments of this application, the lithium salt anion can be considered as a complex composed of a simple anion and a Lewis acid reagent; for example, the tetrafluoroborate ion of lithium tetrafluoroborate can be considered as composed of F... - Composed of boron trifluoride (BF3) and Lewis acids, lithium hexafluorophosphate can be considered as being composed of F- and phosphorus pentafluoride (PF5), Lewis acids that can efficiently initiate cationic polymerization. The autocatalytic reaction of these lithium salts can generate regular network macromolecular structures, which is beneficial for reducing the introduction of impurities and the occurrence of side reactions.

[0057] In some embodiments, the sulfide solid electrolyte includes, but is not limited to, at least one of glass-ceramic-based sulfides, sulfide-germanium sulfides, thio-ultrafast ionic compounds, and LGPS-type sulfides. These sulfide solid electrolytes are characterized by high ionic conductivity.

[0058] As an optional example, the sulfide solid electrolyte includes Li2S-P2S5 and Li7P3S. 11 Li4 x A1 y M y S4, Li6PS5Cl and Li 10 GeP2S 12 At least one of them, and Li4 x A1 y M y In S4, A includes Si or Ge elements, M includes Zn, Al, or P elements, and 0 < x < 4, 0 < y < 1. The above-mentioned sulfide solid electrolytes are characterized by high ionic conductivity.

[0059] <Preparation Method of Composite Solid Electrolyte Membrane> The method for preparing the composite solid electrolyte membrane of this application embodiment can be used to prepare the composite solid electrolyte membrane of this application embodiment.

[0060] Figure 1 This is a flowchart illustrating a method for preparing a composite solid electrolyte membrane, which is an exemplary embodiment of this application.

[0061] like Figure 1 As shown, the preparation method of this composite solid electrolyte membrane includes the following steps: S101. The sulfide solid electrolyte, the lithium salt and the first solvent are mixed to obtain the first slurry.

[0062] In some embodiments, the first solvent includes, but is not limited to, organic solvents.

[0063] For example, the first solvent includes, but is not limited to, at least one of dimethyl carbonate, diethyl carbonate, dipropyl carbonate, ethyl methyl carbonate, xylene, toluene, heptane, decane, and anisole.

[0064] In some embodiments, the mass ratio of the sulfide solid electrolyte to the lithium salt in the first slurry is (5-20):1. For example, the mass ratio of the sulfide solid electrolyte to the lithium salt is 5:1, 10:1, 15:1, or 20:1. This facilitates the control of the content of each component in the composite solid electrolyte membrane within the range of this application, thereby obtaining the composite solid electrolyte membrane of this application.

[0065] In some embodiments, the solid content of the first slurry is 25% to 60%, including but not limited to 35% or 45%.

[0066] S102. The first slurry is dried and rolled to obtain a base film material.

[0067] In the embodiments of this application, the first slurry is dried to evaporate the solvent in the first slurry, and then rolled to obtain the base film material.

[0068] In some embodiments, the drying temperature is 50–120°C and the drying time is 2–24 hours.

[0069] For example, the drying temperature includes, but is not limited to, 70°C or 100°C, and the drying time includes, but is not limited to, 8h, 15h or 20h.

[0070] In some embodiments, the rolling pressure is 100-600 MPa, the rolling temperature is 50-100°C, and the rolling time is 3-30 min.

[0071] For example, the pressure of the roller pressing includes, but is not limited to, 200MPa, 300MPa, 400MPa or 500MPa, the temperature of the roller pressing includes, but is not limited to, 60℃, 70℃, 80℃ or 90℃, and the time of the roller pressing includes, but is not limited to, 0.1h, 0.2h, 0.3h or 0.4h.

[0072] S103. Mix the first monomer, the second monomer, and the second solvent to obtain a post-treatment solution.

[0073] In some embodiments, the second solvent includes, but is not limited to, organic solvents.

[0074] For example, the second solvent includes, but is not limited to, at least one of dimethyl carbonate, diethyl carbonate, dipropyl carbonate, methyl ethyl carbonate, xylene, toluene, heptane, decane, and anisole.

[0075] In some embodiments, the mass ratio of the first monomer to the second monomer in the post-treatment solution is 1:(10-120). For example, the mass ratio of the first monomer to the second monomer is 1:10, 1:30, 1:50, or 1:120, which facilitates the full reaction of the first monomer and the second monomer to obtain the hexahydrotriazine polymer of this application.

[0076] In some embodiments, the post-treatment solution is a completely dissolved clear liquid, wherein the total mass content of the first monomer and the second monomer is 3% to 30%. For example, the total mass content of the first monomer and the second monomer is 3%, 5%, 10%, 15%, 20%, 25%, or 30%.

[0077] S104. Immerse the base film material in the post-treatment solution to obtain the post-treated base film material.

[0078] In some embodiments, the immersion temperature of the base film material is 25±5℃.

[0079] In some embodiments, the soaking time of the base film material is 30 min to 60 min, such as 40 min or 50 min, which is beneficial for the first monomer and the second monomer to be fully adsorbed into the pores of the base film material.

[0080] S105. The post-treated base film material is subjected to polymerization reaction treatment and hot pressing treatment to obtain the composite solid electrolyte membrane.

[0081] In some embodiments, during the polymerization reaction process, the first monomer and the second monomer in the post-treated base film material undergo a polymerization reaction to form the hexahydrotriazine polymer.

[0082] In the embodiments of this application, the polymerization reaction treatment and the hot pressing treatment can be performed step by step, or they can be performed simultaneously. The hot pressing treatment enables the hexahydrotriazine polymer generated on the surface of the base film material to enter the interior of the base film material, thereby further improving the structural stability of the composite solid electrolyte membrane.

[0083] In some embodiments, the pressure of the hot pressing process is 400 to 600 MPa, including but not limited to 450 MPa, 500 MPa or 550 MPa.

[0084] In some embodiments, the polymerization reaction is performed before the hot pressing treatment. By performing the polymerization reaction and hot pressing treatment in separate steps, especially by placing the polymerization reaction treatment before the hot pressing treatment, it is easier to adjust the polymerization reaction parameters and the hot pressing parameters, which is beneficial to improving the quality of the composite solid electrolyte membrane. In some embodiments, when the polymerization reaction is carried out before the hot pressing treatment, the polymerization temperature is 50–70°C and the polymerization time is 8–22 hours, while the hot pressing temperature is 80–90°C and the hot pressing time is 10–40 minutes. Controlling the polymerization reaction time to 8–22 hours is beneficial for the complete polymerization of the first and second monomers.

[0085] For example, when the polymerization reaction is performed before the hot pressing treatment, the temperature of the polymerization reaction includes, but is not limited to, 55°C, 60°C or 65°C, the time of the polymerization reaction includes, but is not limited to, 11h, 14h or 18h, the temperature of the hot pressing treatment includes, but is not limited to, 85°C, and the time of the hot pressing treatment includes, but is not limited to, 20min or 30min.

[0086] As an optional embodiment, the polymerization reaction treatment and hot pressing treatment steps include the following steps: (1) Under conditions of 50-70℃, the first and second monomers in the post-treated base film material undergo a polymerization reaction; (2) The base film material after polymerization reaction is subjected to hot pressing to obtain the composite solid electrolyte membrane. The hot pressing temperature is 80-90℃, the hot pressing pressure is 400-600 MPa, and the hot pressing time is 10-40 min.

[0087] In other embodiments, the polymerization reaction and the hot pressing are performed simultaneously. By performing the polymerization reaction and the hot pressing simultaneously, the preparation time of the composite solid electrolyte membrane can be shortened, which is beneficial for the industrial-scale preparation of the composite solid electrolyte membrane.

[0088] In other embodiments, when the polymerization reaction and the hot pressing are carried out simultaneously, the temperature of the polymerization reaction and the temperature of the hot pressing are both 50-70°C, and the time of the polymerization reaction and the time of the hot pressing are both 15-20 hours.

[0089] For example, when the polymerization reaction and the hot pressing are performed simultaneously, the temperature of the polymerization reaction and the temperature of the hot pressing are, but are not limited to, 55°C, 60°C or 65°C, and the time of the polymerization reaction and the time of the hot pressing are, but are not limited to, 17h or 19h.

[0090] As another alternative example, the polymerization reaction treatment and hot pressing steps include: At 50–70°C, while the first and second monomers in the post-treated base membrane material undergo polymerization, the base membrane material is subjected to hot pressing for 15–20 hours to obtain the composite solid electrolyte membrane, with a hot pressing pressure of 400–600 MPa.

[0091] This application does not impose any particular limitations on the method for controlling the average particle size of sulfide solid electrolytes. For example, commercially available sulfide solid electrolytes can be ground using a grinding device, and then sulfide solid electrolyte particles with the desired particle size distribution can be obtained using a particle size sieving tool (e.g., a sieve). This application also does not impose any particular limitations on the method for controlling the thickness of the composite solid electrolyte membrane. For example, the thickness of the composite solid electrolyte membrane usually decreases as the pressure of the hot pressing process increases and the hot pressing time decreases. Based on this, the thickness of the composite solid electrolyte membrane can be controlled by adjusting the above-mentioned process parameters during the preparation of the composite solid electrolyte membrane.

[0092] The average pore size of the composite solid electrolyte membrane in this application is affected by the particle size of the sulfide solid electrolyte particles and the membrane thickness. For example, when the thickness of the composite solid electrolyte membrane is fixed, the average pore size of the composite solid electrolyte membrane usually decreases as the particle size of the sulfide solid electrolyte particles increases; when the particle size of the sulfide solid electrolyte particles is fixed, the average pore size of the composite solid electrolyte membrane usually increases as the thickness of the composite solid electrolyte membrane increases.

[0093] Semi-solid-state batteries The semi-solid battery of this application embodiment includes the composite solid electrolyte membrane described in any embodiment of this application, or the composite solid electrolyte membrane prepared by the method described in any embodiment of this application embodiment.

[0094] In some embodiments, the semi-solid-state battery can be a rechargeable battery. A rechargeable battery refers to a battery cell that can be recharged after discharge to activate the active materials and continue to be used. The battery cell can be a lithium-ion battery, sodium-ion battery, sodium-lithium-ion battery, lithium metal battery, sodium metal battery, lithium-sulfur battery, magnesium-ion battery, nickel-metal hydride battery, nickel-cadmium battery, lead-acid battery, etc., and this application does not specifically limit it.

[0095] In some embodiments, the semi-solid-state battery further includes a liquid electrolyte, and the mass ratio of the composite sulfide solid electrolyte membrane to the liquid electrolyte is 1:(0.5-10). For example, the mass ratio of the composite sulfide solid electrolyte membrane to the liquid electrolyte is 1:0.5, 1:1, 1:2, 1:5, or 1:10, which facilitates further lithium-ion transport in the electrolyte and improves the cycle life of the semi-solid-state battery.

[0096] This application does not impose any particular limitation on the liquid electrolyte; those skilled in the art can choose according to actual needs, as long as the purpose of this application can be achieved. As an optional example, the liquid electrolyte includes a non-aqueous organic solvent and an electrolyte. For example, at least one of ethylene carbonate (EC), propylene carbonate (PC), diethyl carbonate (DEC), ethyl propionate (EP), propyl propionate (PP), ethyl methyl carbonate (EMC), dimethyl carbonate (DMC), vinylene carbonate (VC), or fluoroethylene carbonate (FEC) is mixed in a certain mass ratio to obtain the non-aqueous organic solvent of the liquid electrolyte; as for the electrolyte in the liquid electrolyte, it can be at least one of lithium hexafluorophosphate (LiPF6), lithium bis(oxalato)borate (LiBOB), lithium tetrafluoroborate (LiBF4), lithium difluorooxalato)borate (LiDFOB), lithium trifluoromethanesulfonate (LiOTf), lithium bis(trifluoromethanesulfonyl)imide (LiTFSI), and lithium bis(fluorosulfonyl)imide (LiFSI).

[0097] The semi-solid-state battery of this application also includes a positive electrode sheet. This application does not impose any particular limitation on the positive electrode sheet, as long as it achieves the purpose of this application. For example, the positive electrode sheet typically includes a positive current collector and a positive electrode material layer. The positive electrode material layer can be disposed on one or both surfaces along the thickness direction of the positive current collector. In this application, the positive electrode material layer is disposed on the surface of the positive current collector; that is, the positive electrode material layer can be disposed on a portion of one surface of the positive current collector, or it can be disposed on the entire surface of one surface of the positive current collector. In this application, there is no particular limitation on the positive current collector, as long as it achieves the purpose of this application. For example, it can include, but is not limited to, aluminum foil, aluminum alloy foil, or composite current collectors. In this application, there is no particular limitation on the thickness of the positive current collector, as long as it achieves the purpose of this application. For example, the thickness can be 4μm to 12μm. The single-sided thickness of the positive electrode material layer in this application can be 100μm to 200μm.

[0098] In this application, the positive electrode material layer includes a positive electrode active material. This application does not have any particular restrictions on the positive electrode active material, as long as it can achieve the purpose of this application. For example, it may include at least one of lithium iron phosphate, lithium-rich manganese-based materials, lithium cobalt oxide, lithium manganese oxide, and lithium manganese iron phosphate.

[0099] In this application, the positive electrode material layer may further include a positive electrode conductive agent. This application does not impose any particular limitation on the positive electrode conductive agent, as long as it can achieve the purpose of this application. For example, it may include, but is not limited to, at least one of conductive carbon black (Super P), carbon nanotubes (CNTs), carbon fibers, acetylene black, and graphene. The aforementioned carbon nanotubes may include, but are not limited to, single-walled carbon nanotubes and / or multi-walled carbon nanotubes. In this application, the positive electrode material layer may further include a positive electrode binder. This application does not impose any particular limitation on the positive electrode binder, as long as it can achieve the purpose of this application. For example, it may include, but is not limited to, at least one of fluorinated resins, polypropylene resins, fiber-type binders, rubber-type binders, or polyimide-type binders.

[0100] The semi-solid-state battery of this application also includes a negative electrode sheet. This application does not impose any particular limitation on the negative electrode sheet, as long as it achieves the purpose of this application. For example, the negative electrode sheet typically includes a negative current collector and a negative electrode material layer. The negative electrode material layer can be disposed on one or both surfaces along the thickness direction of the negative current collector. In this application, the negative electrode material layer is disposed on the surface of the negative current collector; that is, the negative electrode material layer can be disposed on a portion of one surface of the negative current collector, or it can be disposed on the entire surface of one surface of the negative current collector. This application does not impose any particular limitation on the negative current collector, as long as it achieves the purpose of this application. For example, it can include, but is not limited to, copper foil, copper alloy foil, nickel foil, or composite current collectors. In this application, there is no particular limitation on the thickness of the negative current collector, as long as it achieves the purpose of this application, for example, a thickness of 4μm to 12μm. The single-sided thickness of the negative electrode material layer in this application can be 70μm to 200μm.

[0101] In this application, the negative electrode material layer includes a negative electrode active material. The negative electrode active material is not particularly limited, as long as it can achieve the purpose of this application. For example, it may include at least one of artificial graphite, natural graphite, mesophase carbon microspheres, soft carbon, hard carbon, silicon, and silicon-carbon.

[0102] In this application, the negative electrode material layer may also include a negative electrode conductive agent. This application does not have any particular limitation on the negative electrode conductive agent, as long as it can achieve the purpose of this application. For example, it may include, but is not limited to, at least one of conductive carbon black (Super P), carbon nanotubes (CNTs), carbon fiber, acetylene black and graphene.

[0103] In this application, the negative electrode material layer may also include a negative electrode binder. This application does not impose any particular limitation on the negative electrode binder, as long as it can achieve the purpose of this application. For example, it may include, but is not limited to, at least one of acrylate, polyamide, polyimide, polyamide-imide, polyvinylidene fluoride, styrene-butadiene rubber, sodium alginate, polyvinyl alcohol, polytetrafluoroethylene, polyacrylonitrile, sodium carboxymethyl cellulose, and potassium carboxymethyl cellulose.

[0104] The battery of this application also includes a casing. This application does not impose any particular restrictions on the casing, and those skilled in the art can choose one according to actual needs, as long as it can achieve the purpose of this application. For example, the casing may include a steel casing, an aluminum alloy casing, or an aluminum-plastic film.

[0105] This application does not impose any particular limitation on the preparation method of the semi-solid-state battery. Any preparation method known in the art can be used, as long as it can achieve the purpose of this application. For example, the preparation method of the battery includes, but is not limited to, the following steps: stacking the negative electrode sheet, the composite sulfide solid electrolyte membrane, and the positive electrode sheet in sequence, assembling them into an outer package to obtain a bare battery; hot-pressing the bare battery and then performing vacuum drying treatment, followed by injecting liquid electrolyte, and then encapsulating, settling, forming, and capacity testing of the cell to obtain a semi-solid-state battery.

[0106] <Energy Storage Device> The energy storage device of the present application includes a housing and at least one semi-solid battery as described in any embodiment of the present application, wherein the semi-solid battery is housed in the housing.

[0107] Energy storage devices incorporating this semi-solid-state battery exhibit superior performance, which is beneficial for their use. Containing the semi-solid-state battery within a housing enhances its stability and protection, thereby extending the lifespan of the energy storage device. It is understood that an energy storage device can contain one or more semi-solid-state batteries; when multiple semi-solid-state batteries are present, they can be connected in at least one manner, such as parallel or series connection.

[0108] <Electrical Equipment> The electrical equipment described in the embodiments of this application, including the energy storage device described in the embodiments of this application, is beneficial to improving the product competitiveness and performance of the electrical equipment.

[0109] In one optional embodiment, the electrical device includes a device body, and an energy storage device is used to supply power to the device body. In another optional embodiment, the device body includes a positive terminal and a negative terminal, the positive electrode of the semi-solid-state battery in the energy storage device is used to electrically connect to the positive terminal of the device body, and the negative electrode of the semi-solid-state battery in the energy storage device is used to electrically connect to the negative terminal of the device body, so as to supply power to the electrical device.

[0110] The electrical equipment covered by this application may include, but is not limited to: containers, electric vehicles, electric cars, ships, spacecraft, electric toys, power tools, lighting fixtures, and household appliances, etc. Among them, spacecraft include, for example, airplanes, rockets, space shuttles, etc.; electric toys include, for example, stationary or mobile electric toys, specifically, electric car toys, electric ship toys, and electric airplane toys, etc.; power tools include, for example, metal cutting power tools, grinding power tools, assembly power tools, and railway power tools, specifically, electric drills, electric grinders, electric wrenches, electric screwdrivers, electric hammers, impact drills, concrete vibrators, and electric planers.

[0111] Because the energy we need is highly time- and space-dependent, in order to utilize energy rationally and improve energy efficiency, it is necessary to store one form of energy in the same way or by converting it into another, and then release it in a specific energy form for future applications. Currently, the main way to generate green electricity is to develop green energy sources such as photovoltaics and wind power to replace fossil fuels. Currently, the generation of green electricity generally relies on solar, wind, and hydropower. However, wind and solar power are generally characterized by strong intermittency and large fluctuations, which can cause grid instability, insufficient power during peak demand periods, and excessive power during off-peak periods. Unstable voltage can also damage the power grid. Therefore, insufficient electricity demand or insufficient grid capacity may lead to the problem of "wind and solar curtailment." Solving these problems requires energy storage. This involves converting electrical energy into other forms of energy through physical or chemical means and storing it. When needed, this energy can be converted back into electrical energy and released. Simply put, energy storage is like a large "power bank," storing electrical energy when solar and wind power are abundant and releasing the stored electricity when needed.

[0112] Taking electrochemical energy storage as an example, this solution provides an energy storage device that is applied to an energy storage system containing the aforementioned electrical devices. The energy storage device is equipped with a set of chemical batteries, which mainly utilize the chemical elements in the batteries as the energy storage medium. The charging and discharging process is accompanied by the chemical reaction or change of the energy storage medium. Simply put, the electrical energy generated by wind and solar energy is stored in the chemical batteries. When the external power consumption reaches its peak, the stored power is released for use, or transferred to places with power shortages for use.

[0113] Current energy storage applications are quite widespread, including generation-side energy storage, grid-side energy storage, and consumption-side energy storage. The corresponding types of energy storage devices include: (1) Large-scale energy storage power stations applied to wind power and photovoltaic power stations can help renewable energy power generation meet grid connection requirements and improve the utilization rate of renewable energy. As a high-quality active / reactive power regulation power source on the power supply side, energy storage power stations can achieve load matching of power in time and space, enhance the absorption capacity of renewable energy, reduce instantaneous power changes, reduce the impact on the power grid, improve the absorption of new energy power generation, and are of great significance in power grid system backup, alleviating peak load power supply pressure and peak regulation and frequency regulation.

[0114] (2) Energy storage containers applied on the grid side mainly function as peak shaving, frequency regulation and grid congestion relief. In terms of peak shaving, they can realize peak shaving and valley filling of electricity load, that is, charging the energy storage battery when the electricity load is low and releasing the stored electricity during the peak electricity load period, thereby achieving a balance between power production and consumption.

[0115] (3) Small energy storage cabinets applied to the electricity consumption side mainly function as self-consumption of electricity, peak-valley price arbitrage, capacity cost management, and improvement of power supply reliability. Depending on the application scenario, electricity consumption side energy storage can be divided into industrial and commercial energy storage cabinets, household energy storage devices, energy storage charging piles, etc., which are generally used in conjunction with distributed photovoltaics. Industrial and commercial users can use energy storage for peak-valley price arbitrage and capacity cost management. In the electricity market implementing peak-valley pricing, by charging the energy storage system when the electricity price is low and discharging the energy storage system when the electricity price is high, peak-valley price arbitrage can be achieved, reducing electricity costs. In addition, industrial enterprises subject to two-part tariffs can use energy storage systems to store energy during off-peak hours and discharge during peak loads, thereby reducing peak power and the maximum demand declared, achieving the goal of reducing capacity costs. Household photovoltaics with energy storage can improve the level of self-consumption of electricity. Due to high electricity prices and poor power supply stability, the demand for household photovoltaic installations is driven. Given that photovoltaic power generation occurs during the day, while user load is generally higher at night, configuring energy storage can better utilize photovoltaic power, improve self-consumption levels, and reduce electricity costs. Furthermore, energy storage devices are needed in fields such as communication base stations and data centers for backup power.

[0116] In some embodiments, see Figure 2 , Figure 2 This is a schematic diagram of the structure of an energy storage system according to an embodiment of this application. Figure 2 The embodiments are illustrated using a home energy storage scenario in user-side energy storage as an example. The energy storage device 440 of this application is not limited to the home energy storage scenario.

[0117] This application provides an energy storage system 400, which includes a first power conversion device 410 (e.g., a photovoltaic panel, optionally a photovoltaic panel), a first user load 420 (e.g., a household lighting fixture, optionally a household lighting fixture), a second user load 430 (e.g., a household appliance such as an air conditioner), and an energy storage device 440. The energy storage device 440 is a small energy storage box that can be wall-mounted on an outdoor wall. However, the energy storage device 440 is not limited to wall mounting and can also be placed in a user's residence in other ways. Specifically, when the first power conversion device 410 is a photovoltaic panel, the photovoltaic panel can convert solar energy into electrical energy during periods of low electricity prices. The energy storage device 440 stores this electrical energy and supplies it to lighting fixtures and household appliances during peak electricity prices, or provides power during power outages / power interruptions.

[0118] In some embodiments, see Figure 3 , Figure 3 This is a schematic diagram of the structure of an energy storage system according to another embodiment of this application, and this application Figure 3 The embodiments are illustrated using a shared energy storage scenario on the generation / distribution side as an example. The energy storage device 440 of this application is not limited to the energy storage scenario on the generation / distribution side.

[0119] This application provides an energy storage system 400, which includes: a high-voltage cable 450, a first power conversion device 410, a second power conversion device 460, and an energy storage device 440 provided in this application. In some embodiments of the power generation scenario, the second power conversion device 460 can be a wind power conversion device. Since the electricity generated by wind power conversion is volatile, random, and intermittent, the unstable electricity output by the wind power conversion device can be stored in the energy storage device 440 through grid connection. The energy storage device 440 is connected to the high-voltage cable and outputs smooth electricity to the power consumption side of the distribution network, realizing peak shaving and frequency regulation, and stable grid operation; or, wind power... The conversion device is always connected to the high-voltage cable. Under normal power generation conditions, the power output of the wind power conversion device is supplied to the power consumption side of the distribution network through the high-voltage cable. When the current power load is low and the wind power conversion device generates excess power, the excess power is first stored in the energy storage device 440 to reduce wind and solar curtailment rates and improve the problem of new energy power generation consumption. When the power load is high, the power grid issues an instruction to transmit the power stored in the energy storage device 440 together with the high-voltage cable 450 in grid-connected mode to supply power to the power consumption side. This provides the power grid with various services such as peak shaving, frequency regulation, and backup, giving full play to the peak shaving role of the power grid, promoting peak shaving and valley filling, and alleviating the power supply pressure of the power grid.

[0120] In some embodiments on the distribution network side, the first power conversion device 410 can be a photovoltaic power conversion device, and the energy storage device 440 is connected to the high-voltage cable 450 and installed downstream of the high-voltage cable 450 and between the user load. The power output of the photovoltaic power conversion device is stored in the energy storage device 440, which can respond in a timely manner to act as a backup power source when the power grid / distribution network fails; or, it can provide power supply support to alleviate line congestion when the high-voltage cable 450 transmission line is blocked, and to delay the economic pressure caused by the expansion of the power grid / distribution capacity when the power grid is planned to be expanded.

[0121] In some embodiments, see Figure 4 , Figure 4 This is a schematic diagram of the structure of an energy storage system according to another embodiment of this application, and this application Figure 4 The embodiments are illustrated using an industrial and commercial energy storage scenario as an example. The energy storage device 440 of this application is not limited to its power generation / distribution side energy storage scenario.

[0122] This application provides an energy storage system 400, which includes: an energy storage cabinet 470 (an energy storage cabinet is a type of energy storage device), a high-voltage cable 450, a factory equipped with a first power conversion device 410, a photovoltaic-energy storage-charging station 480 equipped with a second power conversion device 460, and a vehicle 490. In some embodiments of industrial and commercial scenarios, the first power conversion device 410 can be a photovoltaic panel, which converts solar energy into electrical energy and stores it in the energy storage cabinet 470 in the factory. In the event of a power grid failure, the energy storage cabinet 470 can transmit the energy to the factory. The power supply ensures the safe and stable operation of the factory without interruption of production; or when the factory's power load is high, the power grid issues an instruction to transmit the electricity stored in the energy storage cabinet 470 together with the high-voltage cable 450 in a grid-connected mode to supply the factory with electricity, providing various services such as peak shaving / frequency regulation and backup for the power grid operation; in addition, the second power conversion device 460 can also be a photovoltaic panel, which converts solar energy into electrical energy and stores it in the energy storage cabinet 470 of the photovoltaic-storage-charging station 480, and directly charges the car 490 through the photovoltaic-storage-charging station 480, which is fast and convenient.

[0123] Optionally, the first power conversion device 410 and the second power conversion device 460 may include, but are not limited to, photovoltaic power conversion devices. The first power conversion device 410 can convert at least one of solar energy, light energy, wind energy, thermal energy, tidal energy, biomass energy, and mechanical energy into electrical energy.

[0124] Optionally, the energy storage cabinet 470 may include, but is not limited to, energy storage application scenarios such as energy storage power stations, hydropower / thermal / wind power generation systems, solar power generation systems, mobile power systems, smart home systems, or temporary power supply systems, and is also used in multiple fields such as data centers, military equipment, aerospace, charging piles, and electric vehicles.

[0125] Optionally, the energy storage cabinet 470 may include, but is not limited to, battery modules, battery packs, battery clusters, power banks, energy storage cabinets / containers, and other battery integrated systems composed of single semi-solid-state batteries. The actual application form of the energy storage cabinet 470 provided in this application embodiment can be, but is not limited to, the listed products, and can also be other application forms. This application embodiment does not strictly limit the application form of the energy storage cabinet 470. This application embodiment only uses a multi-cell battery in the energy storage cabinet 470 as an example for illustration.

[0126] Optionally, the single semi-solid-state battery constituting the energy storage cabinet 470 can be, but is not limited to, at least one of cylindrical, square, prismatic, or other shaped batteries.

[0127] The following non-limiting embodiments further illustrate certain features of the present technology.

[0128] I. Examples and Comparative Examples Table A Compounds

[0129] Preparation Example 1 Ethylene carbonate (EC), ethyl methyl carbonate (EMC), and dimethyl carbonate (DMC) were mixed in a mass ratio of 1:1:1. Then, vinylene carbonate (VC) and vinyl sulfate (DTD) were added, followed by lithium hexafluorophosphate (LiPF6) and lithium bis(fluorosulfonyl)imide (LiFSI) to obtain a liquid electrolyte. The concentrations of LiPF6, LiFSI, VC, and DTD in the liquid electrolyte were all 0.5 wt%.

[0130] Preparation Example 2 Fluoroethylene carbonate (FEC) and ethyl difluorocarbonate (DFEA) were mixed in a mass ratio of 3:7. Then, vinylene carbonate (VC), vinyl sulfate (DTD), and 1,3,6-hexanetrionitrile (HTCN) were added. Lithium hexafluorophosphate (LiPF6) and lithium bis(fluorosulfonyl)imide (LiFSI) were then added to obtain a liquid electrolyte. The concentrations of LiPF6, LiFSI, VC, DTD, and HTCN in the liquid electrolyte were all 0.8 mol / L, 0.2 mol / L, 0.5 wt%, and 0.5 wt%, respectively.

[0131] Preparation Example 3 Ethyl carbonate (EC), ethyl difluoroacetate (DFEA), and diethyl carbonate (DEC) were mixed in a mass ratio of 1:1:3. Then, vinylene carbonate (VC), vinyl sulfate (DTD), and 1,3,6-hexanetrionitrile (HTCN) were added, followed by the addition of lithium hexafluorophosphate (LiPF6) to obtain a liquid electrolyte. The concentrations of LiPF6, VC, DTD, and HTCN in the liquid electrolyte were all 1 mol / L and 0.5 wt%, respectively.

[0132] Preparation Example 4 Ethylene carbonate (EC), ethyl methyl carbonate (EMC), and dimethyl carbonate (DMC) were mixed in a mass ratio of 1:1:1. Then, vinylene carbonate (VC), vinyl sulfate (DTD), and fluoroethylene carbonate (FEC) were added. Lithium hexafluorophosphate (LiPF6) and lithium bis(fluorosulfonyl)imide (LiFSI) were then added to obtain a liquid electrolyte. The concentrations of LiPF6, LiFSI, VC, DTD, and FEC in the liquid electrolyte were all 0.8 wt% and 0.2 wt%, respectively.

[0133] Preparation Example 5 Ethylene carbonate (EC), ethyl methyl carbonate (EMC), and dimethyl carbonate (DMC) were mixed in a mass ratio of 1:1:1. Then, vinylene carbonate (VC), vinyl sulfate (DTD), and the compound shown in formula (I-7) were added. Lithium hexafluorophosphate (LiPF6) and lithium bis(fluorosulfonyl)imide (LiFSI) were then added to obtain a liquid electrolyte. The concentrations of LiPF6, LiFSI, VC, DTD, and the compound shown in formula (I-7) in the liquid electrolyte were all 0.5 wt%.

[0134] Example 1-1 <Preparation of Composite Solid Electrolyte Membranes> The sulfide solid electrolyte Li6PS5Cl and lithium salt LiPF6 were added to dimethyl carbonate at a mass ratio of 10:1 to obtain a first slurry with a solid content of 55wt%. The first slurry was dried to evaporate the solvent dimethyl carbonate, and then rolled to obtain the base film material. The drying temperature was 80℃, the drying time was 10h, the rolling pressure was 400MPa, the rolling temperature was 60℃, and the rolling time was 10min. The first monomer and the second monomer were added to dimethyl carbonate at a mass ratio of 1:50 to obtain a post-treatment solution. The total content of the first monomer and the second monomer in the post-treatment solution was 15 wt%. The first monomer was the compound shown in formula (I-7), and the second monomer was acrylonitrile. The prepared base film material was immersed in the post-treatment solution for 40 min to allow the first monomer and the second monomer to be fully adsorbed into the pores of the base film material, resulting in a post-treated base film material. The first monomer and the second monomer in the post-treated base film material were subjected to a polymerization reaction at 60°C for 20 h. Then, the base film material after the polymerization reaction was subjected to hot pressing treatment to obtain the composite solid electrolyte membrane. The hot pressing temperature was 85°C, the hot pressing pressure was 500 MPa, and the hot pressing time was 20 min. The average particle size D2 of the sulfide solid electrolyte and the average pore size D1 of the composite solid electrolyte membrane are shown in Table 1.

[0135] <Preparation of Semi-Solid-State Batteries> The method for preparing the semi-solid-state battery in this embodiment includes the following steps: (1) Preparation of positive electrode sheet: The positive electrode active material lithium iron phosphate (LiFePO4), conductive agent conductive carbon black (Super-P), and binder polyvinylidene fluoride (PVDF) were dispersed in the solvent N-methylpyrrolidone (NMP) at a mass ratio of 97:0.5:2.5 and mixed evenly to form a positive electrode slurry with a solid content of 65wt%. The slurry was then coated onto one surface of a positive electrode current collector aluminum foil with a thickness of 9μm. The coating weight per unit area of ​​the positive electrode slurry was 33mg / cm². 2 After drying, cold pressing, slitting, and cutting, positive electrode sheets are obtained.

[0136] (2) Preparation of negative electrode sheet: The negative electrode active materials artificial graphite, conductive carbon black (SP), thickener (CMC) and binder (SBR) are dispersed in deionized water at a mass ratio of 96.5:0.5:1:2 to prepare a negative electrode slurry with a solid content of 60wt%, and stirred evenly to obtain the negative electrode slurry; then the negative electrode slurry is coated on a negative electrode current collector copper foil with a thickness of 6μm, and the coating weight per unit area of ​​the negative electrode slurry is 16mg / cm². 2 After drying, cold pressing, slitting, and cutting, negative electrode sheets are obtained.

[0137] (3) Battery assembly: The positive electrode, composite solid electrolyte membrane and negative electrode are stacked in sequence and assembled into the outer packaging to obtain a bare battery. The bare battery is hot-pressed and then vacuum dried. Then the liquid electrolyte prepared in Preparation Example 1 is injected. The cell is then packaged, left to stand, formed and capacity tested to obtain a solid-liquid battery with a capacity of about 1.5Ah, also known as a stacked solid-liquid battery assembled with lithium iron phosphate and graphite.

[0138] Examples 1-2 to 1-7 Except for adjusting the average particle size D2 of the sulfide solid electrolyte and the average pore size D1 of the composite solid electrolyte membrane according to Table 1 in the <Preparation of Composite Solid Electrolyte Membrane>, the rest is the same as in Example 1-1.

[0139] The sulfide solid electrolytes of different particle sizes were sourced from raw materials of various specifications from conventional solid electrolyte manufacturers. The particle size parameters were provided by the manufacturers and can be verified using the particle size testing methods described later. Because the average particle size of the selected sulfide solid electrolytes differs, the average pore size of the composite solid electrolyte membrane also differs.

[0140] Examples 1-8 to 1-36 Except for adjusting the preparation parameters of the base membrane material and post-treatment solution according to Table 2 in the <Preparation of Composite Solid Electrolyte Membrane>, the rest is the same as in Example 1-1.

[0141] Examples 1-37 This embodiment is basically the same as Embodiment 1-1, except that: In the preparation method of the composite solid electrolyte membrane, the following is replaced: "At 60°C, the first and second monomers in the post-treated base membrane material undergo a polymerization reaction for 20 hours; then the base membrane material after polymerization is subjected to hot pressing to obtain the composite solid electrolyte membrane, wherein the hot pressing temperature is 85°C, the hot pressing pressure is 500 MPa, and the hot pressing time is 20 min" At 60°C, while the first and second monomers in the post-treated base film material undergo polymerization, the base film material is subjected to hot pressing for 20 hours to obtain the composite solid electrolyte membrane. The hot pressing pressure is 500 MPa.

[0142] Examples 2-1 to 2-12 Except for the following adjustments in <Preparation of Semi-Solid-State Batteries>, which involve modifying the types of positive active materials used in the preparation of the positive electrode, the types of negative active materials used in the preparation of the negative electrode, and the liquid electrolyte as per Table 3, the rest of the process is the same as in Examples 1-1.

[0143] Among them, the composition of artificial graphite + silicon oxide is artificial graphite: silicon oxide = 85:15 (mass ratio), and silicon oxide is silicon suboxide (VoltXpert® SOC1600); the composition of artificial graphite + silicon carbon is artificial graphite: silicon carbon = 85:15 (mass ratio), and silicon carbon is a composite nano-silicon and carbon material (Shenzhen Kejing SL450B-SC chemically pure).

[0144] Comparative Examples 1-1 to 1-3 Except for adjusting the average particle size D2 of the sulfide solid electrolyte and the average pore size D1 of the composite solid electrolyte membrane according to Table 1 in the <Preparation of Composite Solid Electrolyte Membrane>, the rest is the same as in Example 1-1.

[0145] Comparative Examples 1-4 Except for the fact that in the <Preparation of Composite Solid Electrolyte Membrane>, no sulfide solid electrolyte is added when preparing the base membrane material and no first monomer is added when preparing the post-treatment solution (as shown in Table 2), the rest is the same as in Example 1-1.

[0146] Comparative Examples 1-5 Except for the preparation of the composite solid electrolyte membrane, in which only the second monomer is added and not the first monomer is added when preparing the post-treatment solution (as shown in Table 2), the rest is the same as in Example 1-1.

[0147] Comparative Examples 1-6 Except for the preparation of the composite solid electrolyte membrane, in which only the first monomer is added and the second monomer is not added when preparing the post-treatment solution (as shown in Table 2), the rest is the same as in Example 1-1.

[0148] Comparative Example 2-1 Except for replacing the composite solid electrolyte membrane with a 16 μm thick porous PP membrane (commercially available wet-process membrane with a porosity of 42%) in the <Preparation of Semi-Solid Cells> section (as shown in Table 3), the rest is the same as in Example 2-1.

[0149] Comparative Example 2-2 Except for replacing the composite solid electrolyte membrane with a porous PP membrane with a thickness of 16 μm (as shown in Table 3) in the <Preparation of Semi-Solid Cells>, the rest is the same as in Example 2-2.

[0150] Comparative Examples 2-3 Except for replacing the composite solid electrolyte membrane with a porous PP membrane with a thickness of 16 μm (as shown in Table 3) in the <Preparation of Semi-Solid Cells>, the rest is the same as in Examples 2-4.

[0151] Comparative Examples 2-4 Except for replacing the composite solid electrolyte membrane with a porous PP membrane with a thickness of 16 μm (as shown in Table 3) in the <Preparation of Semi-Solid Cells>, the rest is the same as in Examples 2-5.

[0152] Comparative Examples 2-5 Except for replacing the composite solid electrolyte membrane with a porous PP membrane with a thickness of 16 μm (as shown in Table 3) in the <Preparation of Semi-Solid Cells>, the rest is the same as in Examples 2-11.

[0153] Table 1: Relevant preparation parameters of Examples 1-1 to 1-7 and Comparative Examples 1-1 to 1-3

[0154] Table 2: Relevant preparation parameters for Examples 1-1, 1-8 to 1-36, and Comparative Examples 1-4 to 1-6

[0155] Note: In Table 2, " / " indicates that no relevant preparation parameters exist; the mass ratio in the base film material refers to the mass ratio of the sulfide solid electrolyte to the lithium salt, and the mass ratio in the post-treatment solution refers to the mass ratio of the first monomer and the second monomer. A+B (molar ratio a:b) means that the raw materials (lithium salt or first monomer or second monomer) are composed of substance A and substance B, and the molar ratio of substance A to substance B is a:b, for example: Examples 1-11 The lithium salt type is "LiBF4 + LiBOB (molar ratio 1:1)", which means that the lithium salt in Examples 1-11 is composed of LiBF4 and LiBOB, and the molar ratio of LiBF4 to LiBOB is 1:1; the first monomer type in Examples 1-31 is "Formula (I-4) + Formula (I-8) (molar ratio 1:1)", which means that the first monomer in Examples 1-31 is composed of the compound shown in Formula (I-4) and the compound shown in Formula (I-8), and the molar ratio of the compound shown in Formula (I-4) to the compound shown in Formula (I-8) is 1:1; the second monomer in Examples 1-31 is "Pentaerythritol glycidyl ether + acrylonitrile (molar ratio 1:1)", which means that the second monomer in Examples 1-31 is composed of pentaerythritol glycidyl ether and acrylonitrile, and the mass ratio of pentaerythritol glycidyl ether to acrylonitrile is 1:1.

[0156] Table 3: Relevant preparation parameters for Examples 1-2, Examples 2-1 to 2-12, and Comparative Examples 2-1 to 2-5

[0157] Note: In Table 3, " / " indicates that the relevant preparation parameters do not exist.

[0158] II. Test methods and equipment: 1. Average particle size test of sulfide solid electrolytes: Referring to industry standard T / SPSTS 019-2021 "Performance Requirements and Test Methods for Solid Electrolytes for Solid-State Lithium Batteries - Inorganic Oxide Solid Electrolytes", the particle size and distribution of sulfide solid electrolytes were tested using a Mastersizer 3000 laser particle size analyzer, and the median particle size D was used. 50 (μm) represents the average particle size D2 of the powder. The test results are shown in Table 1.

[0159] 2. Average pore size test of composite solid electrolyte membrane: According to the national standard GB / T 19587 According to the 2017 standard, the specific pore size distribution of the solid electrolyte membranes obtained in each embodiment and comparative example was tested using a BELPREP VAC III-MINI X specific surface area analyzer. The ratio of total adsorption pore volume to specific surface area was calculated from the obtained adsorption lines to obtain the average pore size D1 of the membrane. The test results are shown in Table 1.

[0160] 3. Thickness testing of composite solid electrolyte membranes: The thickness of the composite solid electrolyte membrane was tested according to industry standard T / SPSTS 020-2021 "Performance Requirements and Test Methods for Solid Electrolytes for Solid-State Lithium Batteries - Polymers and Composite Solid Electrolytes". The test results are shown in Table 1.

[0161] 4. Room temperature ionic conductivity test: The prepared composite solid electrolyte membrane was punched in a glove box. Following the "Assembly Method of Mold Cells for Semi-Solid Battery Material Evaluation," conductivity tests were performed using mold cells. The test conditions were: mold cell diameter 10 mm, test pressure 50 MPa, temperature 25 ± 2 °C, using an impedance analyzer (model Bio). logic MTZ 35) Tests were conducted at frequencies ranging from 0.1 Hz to 3.5 MHz. The test results are shown in Table 4.

[0162] 5. Cyclic performance test: For a stacked semi-solid-state battery assembled from lithium iron phosphate and graphite, it is charged at 0.5C constant current to 3.65V at 55℃, and then discharged at 0.5C constant current to 2.5V. The capacity of the third discharge cycle is recorded as the initial capacity DC3, and the capacity of the Xth discharge cycle is recorded as DC... xThe cycle life was monitored until the cycle capacity retention λ (=DCx / DC3) decayed to below 80%, and the number of cycles X at this point was recorded for comparison. For other stacked semi-solid-state batteries assembled with positive and negative electrode materials, the test temperature and charge / discharge rate were kept consistent with the above system. The cycle cutoff voltage of the semi-solid-state batteries corresponding to each test example / comparative example is shown in Table 4.

[0163] Table 4: Performance data for each comparative example and embodiment

[0164] According to Tables 1 and 4: As can be seen from Examples 1-1 to 1-7 and Comparative Examples 1-1 to 1-3, the ionic conductivity and cycle number of Comparative Examples 1-1 to 1-3 are relatively low. This may be because the D1 / D2 ratio of Comparative Example 1-1 is relatively large, while the D1 / D2 ratio of Comparative Examples 1-2 and 1-3 is relatively small. This makes it difficult for the sulfide solid electrolyte particles to be evenly dispersed and for the hexahydrotriazine polymer stereo framework to be constructed, thus affecting the ionic conductivity and structural stability of the solid electrolyte membrane.

[0165] As can be seen from Examples 1-1 to 1-7 and Comparative Examples 1-4 to 1-6, Comparative Examples 1-4 have low ionic conductivity and low cycle count. This may be because Comparative Examples 1-4 do not add sulfide solid electrolyte when preparing the base film material and do not add the first monomer when preparing the post-treatment solution, making it difficult to form the composite solid electrolyte membrane of this application. Comparative Examples 1-5 also have low ionic conductivity and low cycle count. This may be because Comparative Examples 1-5 do not add the first monomer when preparing the post-treatment solution, making it difficult to form the hexahydrotriazine polymer of this application, and thus also difficult to form the composite solid electrolyte membrane of this application. Although the cycle count of Comparative Examples 1-6 has improved to some extent, its ionic conductivity is still low. This may be because Comparative Examples 1-6 do not add the second monomer when preparing the post-treatment solution, making it difficult to form the hexahydrotriazine polymer of this application, and thus also difficult to form the composite solid electrolyte membrane of this application. In contrast, the semi-solid battery of this application has a higher cycle life while maintaining a higher ionic conductivity.

[0166] The average particle size of the sulfide solid electrolyte, the average pore size of the composite solid electrolyte membrane, their ratio, and the thickness of the composite solid electrolyte membrane also typically affect the performance of the semi-solid-state battery. As can be seen from Examples 1-1 to 1-7, by adjusting the above parameters within the scope of this application, based on the composite solid electrolyte membrane comprising sulfide solid electrolyte, lithium salt, and hexahydrotriazine polymer, it is beneficial to obtain a semi-solid-state battery with good cycle life.

[0167] The type of sulfide solid electrolyte, the type of lithium salt, the mass ratio of sulfide solid electrolyte to lithium salt, the type of the first monomer, the type of the second monomer, and the mass ratio of the first monomer to the second monomer, etc., generally affect the performance of semi-solid-state batteries. As can be seen from Examples 1-1, 1-8, and 1-36, based on the composite solid electrolyte membrane of this application, which includes sulfide solid electrolyte, lithium salt, and hexahydrotriazine polymer, adjusting the above parameters within the range of this application is beneficial to obtaining a semi-solid-state battery with good cycle life.

[0168] As can be seen from Examples 2-1 and Comparative Examples 2-1, 2-2 and Comparative Examples 2-2, 2-4 and Comparative Examples 2-3, 2-5 and Comparative Examples 2-4, and 2-11 and Comparative Examples 2-5, the semi-solid-state battery of this application has significantly improved cycle performance compared with the semi-solid-state battery using a common PP separator.

[0169] The type of positive electrode material, the type of negative electrode material, the composition of the liquid electrolyte, and the mass ratio of the solid electrolyte membrane to the liquid electrolyte typically affect the performance of semi-solid-state batteries. As can be seen from Examples 1-2 and Examples 2-1 to 2-12, based on the composite solid electrolyte membrane of this application comprising a sulfide solid electrolyte, lithium salt, and hexahydrotriazine polymer, adjusting the aforementioned parameters within the range of this application is beneficial for obtaining semi-solid-state batteries with good cycle life.

[0170] The above provides a detailed description of the composite solid electrolyte membrane, its preparation method, semi-solid battery, and energy storage device disclosed in this application. Specific examples have been used to illustrate the principles and implementation methods of this application. The descriptions of the above embodiments are only for the purpose of helping to understand the technical solutions and core inventive points of the embodiments of this application. At the same time, for those skilled in the art, there will be changes in the specific implementation methods and application scope based on the ideas of this application. Therefore, the content of this specification should not be construed as a limitation of this application.

[0171] In this application, the terms "one embodiment," "some embodiments," "example," "specific example," or "some examples," etc., refer to a specific feature, structure, material, or characteristic described in connection with that embodiment or example, which is included in at least one embodiment or example of this application. In this specification, the illustrative expressions of the above terms do not necessarily refer to the same embodiment or example. Furthermore, the specific features, structures, materials, or characteristics described may be combined in any suitable manner in one or more embodiments or examples. Moreover, without contradiction, those skilled in the art can combine and integrate the different embodiments or examples described in this specification, as well as the features of different embodiments or examples.

[0172] In this application, the terms "upper," "lower," "left," "right," "front," "rear," "top," "bottom," "inner," "outer," "vertical," "horizontal," "lateral," and "longitudinal" indicate the orientation or positional relationship based on the orientation or positional relationship shown in the accompanying drawings. These terms are primarily for the purpose of better describing this application and its embodiments, and are not intended to limit the indicated device, element, or component to having a specific orientation, or to be constructed and operated in a specific orientation.

[0173] Furthermore, in addition to indicating location or positional relationship, some of the aforementioned terms may also have other meanings. For example, the term "above" may also be used in some cases to indicate a certain dependency or connection relationship. Those skilled in the art can understand the specific meaning of these terms in this application based on the specific circumstances.

[0174] Furthermore, the terms "installation," "setup," "equipped with," "connection," and "linked" should be interpreted broadly. For example, they can refer to a fixed connection, a detachable connection, or an integral structure; they can refer to a mechanical connection or an electrical connection; they can refer to a direct connection or an indirect connection through an intermediate medium, or an internal connection between two devices, components, or parts. Those skilled in the art can understand the specific meaning of these terms in this application based on the specific circumstances.

[0175] Furthermore, the terms "first," "second," etc., are primarily used to distinguish different devices, components, or parts (which may be the same or different in specific type and construction), and are not intended to indicate or imply the relative importance or quantity of the indicated devices, components, or parts. Unless otherwise stated, "a plurality of" means two or more.

[0176] Although embodiments of this application have been shown and described above, it is understood that the above embodiments are exemplary and should not be construed as limiting this application. Those skilled in the art can make changes, modifications, substitutions and variations to the above embodiments within the scope of this application.

Claims

1. A composite solid electrolyte membrane, characterized in that, The mixture includes a sulfide solid electrolyte, a lithium salt, and a hexahydrotriazine polymer, wherein the hexahydrotriazine polymer is formed by polymerization of a first monomer and a second monomer. The first monomer has the structure shown in formula (Ⅰ): Equation (Ⅰ), In equation (I), R1, R2, and R3 are each independently selected from unsubstituted or Ra-substituted C. 2-12 Alkenyl, unsubstituted or Ra-substituted C 2-12 Alkyne group, unsubstituted or Ra-substituted C 3-13 Cycloalkyl, unsubstituted or Ra-substituted C 1-11 Cyano, unsubstituted or Ra-substituted C 1-11 Aldehyde group, unsubstituted or Ra-substituted C 1-11 Amine, unsubstituted or Ra-substituted C 3-13 Imidazole group, unsubstituted or Ra-substituted C 3-13 One of the pyridinyl groups; Ra is selected from C 1-6 Alkyl, C 1-6 Alkoxy, C 2-6 alkenyl, C 2-6 alkynyl group, C 1-6 Acyl group, C 1-6 ether group, C 6-10 At least one of aryl and halogen atoms; The second monomer includes at least one of esters, ethers, amines, alkenes, and nitriles that have polymerization properties.

2. The composite solid electrolyte membrane according to claim 1, characterized in that, The mass ratio of the first monomer to the second monomer is 1:(10-120); And / or, in equation (I), R1, R2, and R3 are each independently selected from unsubstituted C 2-12 alkenyl, unsubstituted C 2-12 Alkyne group, unsubstituted C 3-13 Cycloalkyl, unsubstituted C 1-11 Cyano, unsubstituted or Ra-substituted C 1-11 Aldehyde group, unsubstituted or Ra-substituted C 3-13 One of the imidazole groups; And / or, the second monomer comprises at least one of methyl acrylate, methyl methacrylate, ethylene glycol dimethyl ether, diethylene glycol dimethyl ether, N,N'-methylenebisacrylamide, N,N'-ethylenebisacrylamide, N,N'-propylenebisacrylamide, vinylidene fluoride, trifluoroethylene, hexafluoropropylene, trifluorochloroethylene, 1,1-chlorofluoroethylene, difluorochloroethylene, and acrylonitrile.

3. The composite solid electrolyte membrane according to claim 1, characterized in that, The first monomer includes at least one of the following compounds: Equation (Ⅰ-1) Equation (Ⅰ-2), Equation (Ⅰ-3) Equation (Ⅰ-4) Equation (Ⅰ-5) Equation (Ⅰ-6) Equation (Ⅰ-7) Equation (Ⅰ-8).

4. The composite solid electrolyte membrane according to claim 1, characterized in that, The composite solid electrolyte membrane includes at least one of the following features: a) Based on the mass of the composite solid electrolyte membrane, the mass percentage of the sulfide solid electrolyte is a, where 70% ≤ a ≤ 94%; b) Based on the mass of the composite solid electrolyte membrane, the mass percentage of the lithium salt is b, where 5% ≤ b ≤ 20%; c) Based on the mass of the composite solid electrolyte membrane, the mass percentage of the hexahydrotriazine polymer is c, where 1% ≤ c ≤ 10%; d) The mass ratio of the sulfide solid electrolyte to the lithium salt is (5-20):1; e) The average pore size of the composite solid electrolyte membrane is D1, and the average particle size of the sulfide solid electrolyte is D2, where 0.003 ≤ D1 / D2 ≤ 0.1; f) The thickness of the composite solid electrolyte membrane is H, where 10 μm ≤ H ≤ 80 μm.

5. The composite solid electrolyte membrane according to any one of claims 1 to 4, characterized in that, The lithium salt includes at least one of lithium hexafluorophosphate, lithium dioxaborate, lithium tetrafluoroborate, lithium dioxaborate, lithium trifluoromethanesulfonate, lithium bis(trifluoromethanesulfonyl)imide, and lithium bis(fluorosulfonyl)imide. And / or, the sulfide solid electrolyte includes at least one of glass ceramic-based sulfides, sulfogermanium sulfides, thio-ultrafast ionic compounds, and LGPS-type sulfides; Optionally, the sulfide solid electrolyte includes Li2S-P2S5 and Li7P3S. 11 Li4 x A1 y M y S4, Li6PS5Cl and Li 10 GeP2S 12 At least one of them, and Li4 x A1 y M y In S4, A includes Si or Ge elements, M includes Zn, Al, or P elements, and 0 < x < 4, 0 < y < 1.

6. A method for preparing a composite solid electrolyte membrane as described in any one of claims 1 to 5, characterized in that, include: The sulfide solid electrolyte, the lithium salt, and the first solvent are mixed to obtain a first slurry; The first slurry is dried and rolled to obtain a base film material; The first monomer, the second monomer, and the second solvent are mixed to obtain a post-treatment solution; The base film material is immersed in the post-treatment solution to obtain the post-treated base film material; The post-treated base film material is subjected to polymerization reaction and hot pressing to obtain the composite solid electrolyte membrane.

7. The preparation method according to claim 6, characterized in that, During the polymerization reaction process, the first monomer and the second monomer in the post-treated base film material undergo a polymerization reaction to form the hexahydrotriazine polymer. And / or, the polymerization reaction is performed before the hot pressing treatment, or the polymerization reaction is performed simultaneously with the hot pressing treatment; And / or, the pressure of the hot pressing treatment is 400-600 MPa; Optionally, when the polymerization reaction is carried out before the hot pressing treatment, the polymerization reaction temperature is 50-70°C, the polymerization reaction time is 8-22 h, the hot pressing temperature is 80-90°C, and the hot pressing time is 10-40 min. Optionally, when the polymerization reaction and the hot pressing are carried out simultaneously, the temperature of the polymerization reaction and the temperature of the hot pressing are both 50-70°C, and the time of the polymerization reaction and the time of the hot pressing are both 15-20 hours.

8. A semi-solid-state battery, characterized in that, Includes the composite solid electrolyte membrane according to any one of claims 1 to 5, or includes the composite solid electrolyte membrane prepared by the preparation method according to claim 6 or 7; Optionally, the semi-solid battery further includes a liquid electrolyte, and the mass ratio of the composite sulfide solid electrolyte membrane to the liquid electrolyte is 1:(0.5-10).

9. An energy storage device, characterized in that, It includes a housing and at least one semi-solid battery as described in claim 8, the semi-solid battery being housed within the housing.

10. An electrical appliance, characterized in that, The device includes the energy storage device of claim 9, wherein the energy storage device supplies power to the electrical equipment.