A PI / PVDF-HFP based composite solid electrolyte, its preparation method and application
By introducing fast ion conductor fillers, porous PI membranes, and interface stabilizers into the PVDF-HFP matrix, the problems of insufficient ion transport capacity, insufficient mechanical support, and limited interface stability of PVDF-HFP-based electrolytes are solved, thus realizing a high-performance lithium-ion battery electrolyte.
Patent Information
- Application Number
- CN202611023100.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-07-10
- Publication Date
- 2026-11-17
AI Technical Summary
Existing PVDF-HFP based electrolytes in lithium-ion batteries suffer from insufficient ion transport capacity, insufficient mechanical support, and limited interfacial stability. In particular, they are difficult to meet the requirements of high-performance batteries in systems containing residual high-boiling-point solvents or plasticizers.
By employing a ternary synergistic design, a more efficient Li⁺ transport pathway is constructed by introducing fast ion conductor fillers (such as Li1.3Al0.3Ti1.7(PO4)3), porous PI membrane framework materials, and interface stabilizers (such as lithium difluorooxalate borate), thereby enhancing the mechanical stability of the membrane and optimizing the chemical stability of the electrode/electrolyte interface.
The ionic conductivity and mechanical strength of the PVDF-HFP matrix were improved, the electrochemical stability window was extended, the cycle performance and interfacial stability of lithium metal batteries were improved, and a composite solid electrolyte with excellent overall performance was achieved.
Smart Images

Figure CN123120838A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of composite solid electrolyte technology, and in particular to a PI / PVDF-HFP based composite solid electrolyte, its preparation method, and its application. Background Technology
[0002] With the rapid development of new energy vehicles and large-scale energy storage industries, higher requirements have been placed on the energy density, safety, and cycle life of rechargeable lithium-ion batteries. Replacing traditional liquid electrolytes and separators with solid-state electrolytes to construct solid-state or quasi-solid-state batteries has become an important research direction in the field of lithium metal batteries. Compared with liquid systems, solid-state electrolytes have significant advantages in reducing leakage and combustion risks, and their higher mechanical strength also helps to suppress dendrite growth to some extent, solving the problem of insufficient compatibility between traditional organic liquid electrolytes and lithium metal. This allows for the use of lithium metal as the negative electrode, significantly improving the energy density of lithium-ion batteries.
[0003] When an electrolyte transitions from a liquid to a solid state, the ion transport mechanism changes accordingly, often leading to problems such as insufficient room-temperature ionic conductivity, poor solid-solid interface contact, and complex interfacial side reactions. Among numerous solid-state electrolyte candidates, polymer electrolytes have attracted widespread attention due to their good flexibility, ease of processing into films, and ability to maintain good contact with electrode surfaces. Polyvinylidene fluoride-hexafluoropropylene copolymer (PVDF-HFP) is particularly noteworthy for its combination of high dielectric constant, wide electrochemical stability window, and good film-forming properties. However, single PVDF-HFP-based electrolytes still face some common problems: First, PVDF-HFP materials are semi-crystalline polymers with limited chain segment mobility at room temperature, thus the ion transport capacity of a single PVDF-HFP system is often insufficient to meet the requirements of high-performance batteries. Second, PVDF-HFP electrolytes still face insufficient film mechanical support and limited interfacial stability during long-term cycling, especially in systems containing residual high-boiling-point solvents or plasticizers, where improving the bulk transport performance of PVDF-HFP often comes at the cost of interfacial side reactions. Therefore, research on the modification of PVDF-HFP based electrolytes has become a consensus.
[0004] CN 121839864 A provides a composite solid electrolyte membrane, its preparation method and application, and a solid lithium metal battery. The composite solid electrolyte membrane provided by this invention includes a polymer matrix, a functional filler, and a lithium salt; wherein the functional filler is a cellulose-based derivative. CN 121642141 A uses polyvinylidene fluoride-hexafluoropropylene copolymer or polyvinylidene fluoride as the polymer matrix, LiTFSI or LiFSI as the lithium salt, sodium niobate or lithium niobate as the dielectric filler, and lithium nitrate as the interface stabilizer. Under solvent conditions, the polymer matrix, lithium salt, dielectric filler, and interface stabilizer are mixed to obtain a solid polymer electrolyte. CN202511572727.1 dissolves a PVDF-HFP matrix in DMF, stirs, transfers to a glove box, adds an active filler and a dual lithium salt system, stirs to obtain a suspension; MOF808 is added to the obtained suspension in the glove box, ultrasonically stirred; a film is formed using solution casting, and vacuum dried to obtain a composite polymer solid electrolyte.
[0005] Analysis shows that current research on the modification of PVDF-HFP mainly includes inorganic filler modification, interfacial additive regulation, and plasticizer introduction. However, these modification strategies are mostly single or binary combinations, lacking systematic ternary synergistic design, and the prepared composite solid electrolytes are difficult to simultaneously meet the requirements of structural enhancement, improved ion conduction, and interfacial stability. Summary of the Invention
[0006] This invention aims to address the shortcomings of existing technologies by providing a ternary system solution. Firstly, it employs active inorganic fillers to improve the ion transport performance of the PVDF-HFP matrix. Secondly, it introduces a three-dimensional porous PI membrane framework material to enhance the mechanical strength and thermal stability of the membrane, improve structural integrity, and optimize ion transport channels. Thirdly, it adds an interface stabilizer to regulate the electrode / electrolyte interface chemistry and improve interface stability. In summary, through the synergistic effect of these three modification methods, a PI / PVDF-HFP-based composite solid electrolyte with excellent overall performance is obtained.
[0007] To achieve the above objectives, the present invention adopts the following technical solution:
[0008] This invention discloses a PI / PVDF-HFP composite solid electrolyte, which includes a PVDF-HFP polymer matrix, a porous PI membrane, a fast ion conductor filler, a lithium salt, and an interface stabilizing additive.
[0009] The fast ion conductor filler in this invention includes Li 1.3 Al 0.3 Ti 1.7 (PO4)3, Li 1.5 A1 0.5 Ge1.5 (PO4)3, Li 6.5 La3Zr 1.5 Nb 0.5 O 12 Li 6.4 La3Zr 1.4 Ta 0.6 O 12 Li7 La3 Zr2 O 12 Li 0.5 La 0.5 Any one of TiO3.
[0010] The mass of the fast ion conductor filler in this invention is 5% to 100% of the mass of the PVDF-HFP polymer matrix in this invention.
[0011] Preferably, the mass of the fast ion conductor filler in this invention is 20% to 50% of the mass of the PVDF-HFP polymer matrix in this invention.
[0012] The lithium salt in this invention is at least one of lithium bis(trifluoromethanesulfonyl)imide, lithium bis(fluorosulfonyl)imide, lithium hexafluorophosphate, lithium perchlorate, lithium tetrafluoroborate, lithium hexafluoroarsenate, lithium bis(oxalateborate), and lithium fluoroalkyl phosphate.
[0013] The mass ratio of lithium salt to PVDF-HFP polymer matrix in this invention is 1:3 to 1:1.
[0014] The interface stabilizing additive in this invention is at least one of vinyl ethylene carbonate, fluoroethylene carbonate, lithium bis(oxalate)borate, lithium difluorooxalateborate, lithium nitrate, and lithium di(salicylic acid)borate.
[0015] The additive in this invention is 0.1% to 5% of the total mass of the PVDF-HFP polymer matrix, lithium salt, and fast ion conductor filler in this invention.
[0016] The PI porous membrane in this invention has a porosity of 30% to 90% and a thickness of 5 μm to 150 μm.
[0017] Preferably, the PI porous membrane in this invention has a porosity of 50% to 80% and a thickness of 10 μm to 30 μm.
[0018] This invention provides a method for preparing a PI / PVDF-HFP composite solid electrolyte membrane, the method comprising the following steps:
[0019] S1: Under a protective atmosphere, the first organic solvent and the PVDF-HFP polymer matrix are added to a container and stirred to dissolve, resulting in a homogeneous solution A.
[0020] S2: Add the interface stabilizing additive, lithium salt and fast ion conductor filler to the solution A and stir to obtain a uniform and transparent solution B.
[0021] S3: After degassing solution B, it is cast into a PI porous membrane and dried to obtain a PI / PVDF-HFP composite solid electrolyte membrane.
[0022] The first organic solvent in this invention is selected from any one of anhydrous acetonitrile, ethylene carbonate, N-methylpyrrolidone, N,N-dimethylformamide, acetone, tetrahydrofuran, dimethyl sulfoxide, and dichloroethane.
[0023] The concentration of the PVDF-HFP polymer matrix in the first organic solvent in this invention is 0.05 g / mL to 1.00 g / mL.
[0024] In step S1, the stirring temperature of the solution is 30℃~60℃, and the stirring time is more than 0.5h.
[0025] In step S2, the stirring temperature of the solution is 30℃~60℃, and the stirring time is more than 0.5h.
[0026] In step S3, the drying temperature is 30℃~80℃, and the drying time is 6h~25h.
[0027] This invention provides an application of a PI / PVDF-HFP composite solid electrolyte in lithium metal batteries.
[0028] The solid-state lithium metal battery of the present invention includes a positive electrode, a lithium metal negative electrode, and the PI / PVDF-HFP composite solid electrolyte membrane described in the present invention.
[0029] The method for preparing the solid-state lithium metal battery of the present invention includes the following steps:
[0030] S4: Prepare a PI / PVDF-HFP composite solid electrolyte membrane using the preparation method of the PI / PVDF-HFP composite solid electrolyte membrane described in this invention, and then cut it into circular pieces with a diameter of 19 mm for later use.
[0031] S5: Grind the positive electrode active material, conductive agent and binder, add the second organic solvent to obtain the electrode slurry, coat it evenly on the current collector by scraping, and dry the coated current collector at high temperature under vacuum to obtain the positive electrode sheet, and then cut the electrode sheet into round pieces with a diameter of 12mm for later use.
[0032] S6: Prepare a lithium metal negative electrode, and assemble the solid electrolyte membrane from step S4, the positive electrode sheet from step S5, and the lithium metal negative electrode to obtain a solid-state lithium metal battery.
[0033] The conductive agent is selected from at least one of carbon black (Super P, acetylene black, Ketjen black), conductive graphite, carbon fiber, carbon nanotubes, graphene, and vapor-grown carbon fiber.
[0034] The adhesive is selected from at least one of PVDF, PTFE, and SBR.
[0035] The active substance is selected from LiNi 0.8 Co 0.1 Mn 0.1 O2, LiNi 0.8 Co 0.15 Al 0.05 Any one of O2, LiFePO4, LiMnPO4, LiNiPO4, LiCoPO4, LiCoO2, and MoS2.
[0036] The mass ratio of the active substance, conductive agent, and binder in step S5 is 8:1:1.
[0037] In step S5, the thickness set for the scraping coating is 100 μm.
[0038] In step S5, the vacuum drying temperature is set to 80℃ and the drying time is 24h.
[0039] In this invention, the second solvent is selected from any one of anhydrous acetonitrile, ethylene carbonate, N-methylpyrrolidone, N,N-dimethylformamide, acetone, tetrahydrofuran, dimethyl sulfoxide, and dichloroethane.
[0040] The beneficial effects of this invention are as follows: This invention provides a composite solid electrolyte membrane comprising a fast ion conductor filler, a lithium salt, an interface stabilizer, a PVDF-HFP polymer, and a porous PI membrane, as well as its preparation method and applications. Firstly, this invention constructs a more efficient Li⁺ transport path by introducing a fast ion conductor filler into the polymer matrix. Simultaneously, the rigid fast ion conductor also enhances the mechanical stability of the membrane. Therefore, introducing the fast ion conductor filler can improve the bulk properties of the PVDF-HFP polymer matrix to a certain extent. Secondly, under long-term cycling or temperature fluctuation conditions, the polymer / fast ion conductor filler blend system is prone to local stress concentration, dimensional shrinkage, and structural inhomogeneity, which is detrimental to maintaining stable ion transport channels. Introducing a three-dimensional framework material is an effective way to improve the structural stability of the polymer electrolyte. The PI membrane has good thermal stability, mechanical strength, and structural integrity; therefore, introducing a porous PI membrane can provide a continuous supporting framework for the composite electrolyte, helping to improve the dimensional stability and overall strength of the membrane. Third, when composite electrolyte membranes are applied to lithium metal batteries, without effective interface control methods, the active components and residual solvation structures in the electrolyte may still induce continuous side reactions, leading to increased interfacial impedance and decreased cycle performance. Therefore, introducing interface stabilizers can improve the interfacial stability of the lithium metal anode and high-voltage cathode by regulating the local solvation structure and preferential interfacial decomposition behavior, forming a more stable inorganic-rich interfacial layer on the electrode surface. Through the above measures, the PI / PVDF-HFP-based composite solid electrolyte provided by this invention achieves a synergistic effect in improving the ionic conductivity of the polymer matrix, enhancing the stability of the membrane structure, and regulating the interface, thereby obtaining a composite solid electrolyte and lithium metal battery with excellent overall electrochemical performance.
[0041] The test results of the embodiments and comparative examples of this invention show that, after introducing a fast ion conductor, the ionic conductivity of the PVDF-HFP matrix at 30°C increases from 0.91 × 10⁻⁶ to 0.91 × 10⁻⁶. -4 S cm -1 Increased to 1.64×10 -4 S cm -1 The lithium-ion transference number increased from 0.205 to 0.567. The tensile strength of the membrane increased from 4.6 MPa to 6.7 MPa after introducing a porous PI membrane framework. The electrochemical stability window of the invented PI / PVDF-HFP-based composite solid electrolyte was extended from 4.91 V to 5.03 V after employing multiple measures. The Li||Li symmetric battery assembled using the PI / PVDF-HFP-based composite solid electrolyte of this invention performed well at 30 °C and 0.2 mA cm⁻¹. -2Under certain conditions, it can be stably cycled for over 800 h. The assembled LiFePO4||Li battery still retains 135 mAh g⁻¹ after 220 cycles at 30 ℃ and 0.5 C. -1 The discharge specific capacity of the [specific capacity] battery was 83.9%; conversely, the discharge specific capacity of the LiFePO4||Li battery assembled using the comparative example was only 14 mAh g after 220 cycles. -1 The capacity retention rate is less than 10%. Attached Figure Description
[0042] The technical solution of the present invention will be further described in detail below with reference to the accompanying drawings and embodiments.
[0043] Figure 1 These are scanning electron microscope images. (a) Porous PI membrane; (b) PVDF-HFP solid electrolyte membrane; (c) PI / PVDF-HFP based composite solid electrolyte membrane.
[0044] Figure 2 These are the XRD patterns of porous PI membranes, PVDF-HFP solid electrolyte membranes, and PI / PVDF-HFP based composite solid electrolyte membranes.
[0045] Figure 3 This is a diagram showing the thermal shrinkage of the diaphragm.
[0046] Figure 4 These are the stress-strain curves of porous PI membranes, PVDF-HFP solid electrolyte membranes, and PI / PVDF-HFP based composite solid electrolyte membranes.
[0047] Figure 5 These are the AC impedance spectra of PVDF-HFP solid electrolyte membranes and PI / PVDF-HFP-based composite solid electrolyte membranes at 30℃.
[0048] Figure 6 These are the LSV curves of PVDF-HFP solid electrolyte membranes and PI / PVDF-HFP-based composite solid electrolyte membranes.
[0049] Figure 7 The constant current cycling performance of Li||Li symmetric cells assembled with PVDF-HFP solid electrolyte membrane and PI / PVDF-HFP based composite solid electrolyte membrane is shown.
[0050] Figure 8 The rate performance and charge / discharge curves of LiFePO4||Li full cells assembled with PVDF-HFP solid electrolyte membrane and PI / PVDF-HFP based composite solid electrolyte membrane are presented.
[0051] Figure 9The cycling performance of LiFePO4||Li full cells assembled with PVDF-HFP solid electrolyte membrane and PI / PVDF-HFP based composite solid electrolyte membrane is shown. Detailed Implementation
[0052] The following provides a detailed description of specific embodiments of the present invention. It should be understood that the specific embodiments described herein are for illustration and explanation only and are not intended to limit the scope of protection of the present invention.
[0053] In this invention, unless otherwise specified, all equipment and raw materials are commercially available or commonly used in the industry. The methods described in the following embodiments are conventional methods in the art, unless otherwise specified.
[0054] Specific Implementation Method 1: This embodiment of the invention provides a PI / PVDF-HFP-based composite solid electrolyte, comprising a PVDF-HFP polymer matrix, a porous PI membrane, a fast ion conductor filler, a lithium salt, and an interface stabilizing additive. The PVDF-HFP has a weight-average molecular weight of 450,000, the porous PI membrane has a porosity of 80% and a thickness of 20 μm, and the fast ion conductor filler is Li. 1.3 Al 0.3 Ti 1.7 (PO4)3, the lithium salt is lithium bis(trifluoromethanesulfonylimide), and the interface stabilizing additive is lithium difluorooxalateborate.
[0055] This invention provides a method for preparing a PI / PVDF-HFP based composite solid electrolyte, specifically including the following steps:
[0056] S1: Under a protective atmosphere, 750 wt% of N,N-dimethylformamide and a certain amount of PVDF-HFP polymer matrix were added to a container and stirred to dissolve. The stirring temperature was 60 ℃ and the stirring time was 1 h to obtain solution A.
[0057] S2: Lithium difluorooxalate borate (2 wt% of PVDF-HFP polymer matrix), lithium bis(trifluoromethanesulfonylimide) (100 wt% of PVDF-HFP polymer matrix), and Lithium difluorooxalate (25 wt% of PVDF-HFP polymer matrix) are added. 1.3 Al 0.3 Ti 1.7 (PO4)3 was added to solution A and stirred at 60 °C for 8 h to obtain a uniform and transparent solution B.
[0058] S3: After degassing solution B, it is cast into a PI porous membrane and dried at 60°C for 12 h to obtain a PI / PVDF-HFP composite solid electrolyte membrane.
[0059] This invention provides an application of a PI / PVDF-HFP based composite solid electrolyte, characterized by its application in solid-state lithium metal batteries. The preparation method of this solid-state lithium metal battery includes the following steps:
[0060] S4: Cut the above PI / PVDF-HFP composite solid electrolyte membrane into 19 mm diameter discs for later use.
[0061] S5: LiFePO4, carbon black, and PVDF were weighed at a mass ratio of 8:1:1. N-methylpyrrolidone was added and the mixture was ground to obtain an electrode slurry. This slurry was then uniformly coated onto an aluminum foil current collector using a blade coating method, with a coating thickness of 100 μm. The coated current collector was then dried at high temperature under vacuum to obtain the positive electrode sheet. The drying temperature was set to 80℃, and the drying time was 24 h. Finally, the dried electrode sheet was cut into round pieces with a diameter of 12 mm for later use.
[0062] S6: Prepare a lithium metal negative electrode, and assemble the solid electrolyte membrane from step S4, the positive electrode sheet from step S5, and the lithium metal negative electrode to obtain a solid-state lithium metal battery.
[0063] Specific Implementation Method Two: This implementation method differs from Specific Implementation Method One in that: in step S2, Li... 1.3 Al 0.3 Ti 1.7 The amount of (PO4)3 added is 36 wt% of the weight of the PVDF-HFP polymer matrix, and the other steps and conditions are the same as in Specific Embodiment 1.
[0064] Specific Implementation Method Three: This implementation method differs from Specific Implementation Method One in that: in step S2, 25 wt% of Li based on the weight of the PVDF-HFP polymer matrix is added. 6.4 La3Zr 1.4 Ta 0.6 O 12 The other steps and conditions are the same as in Specific Implementation Method 1.
[0065] Specific Implementation Method Four: This implementation method differs from Specific Implementation Method One in that: in step S2, 3 wt% of lithium difluorooxalate borate is added to the PVDF-HFP polymer matrix, while the other steps and conditions are the same as in Specific Implementation Method One.
[0066] Specific Implementation Method 5: This implementation method differs from Specific Implementation Method 1 in that: in step S2, 2 wt% of lithium nitrate based on the weight of the PVDF-HFP polymer matrix is added, while the other steps and conditions are the same as in Specific Implementation Method 1.
[0067] Specific Implementation Method Six: This implementation method differs from Specific Implementation Method One in that: in step S3, after degassing, solution B is cast into a PI porous membrane with a porosity of 70% and a thickness of 16 μm. Other steps and conditions are the same as in Specific Implementation Method One.
[0068] Specific Implementation Method Seven: This implementation method differs from Specific Implementation Method One in that: in step S1, 1000 wt% of anhydrous acetonitrile and PVDF-HFP polymer matrix are added and stirred to dissolve. Other steps and conditions are the same as in Specific Implementation Method One.
[0069] Specific Implementation Method Eight: This implementation method differs from Specific Implementation Method One in that: in step S3, the system is first vacuum dried at 60°C for 8 hours to remove most of the DMF in the system, and then the temperature is raised to 80°C and vacuum dried for another 4 hours. Other steps and conditions are the same as in Specific Implementation Method One.
[0070] Specific Implementation Method Nine: This implementation method differs from Specific Implementation Method One in that: in step S5, LiNi is added. 0.8 Co 0.1 Mn 0.1 O2, carbon black, and PVDF are ground together, and other steps and conditions are the same as in Specific Implementation Method 1.
[0071] Comparative Example 1: Preparation of a PVDF-HFP-based polymer solid electrolyte with added lithium salt. The specific steps include:
[0072] S1: Under a protective atmosphere, 750 wt% of N,N-dimethylformamide and a certain amount of PVDF-HFP polymer matrix were added to a container and stirred to dissolve. The stirring temperature was 60 ℃ and the stirring time was 1 h to obtain solution A.
[0073] S2: Add 100% by weight of lithium bis(trifluoromethanesulfonylimide) of the PVDF-HFP polymer matrix to solution A and stir at 60 °C for 8 h to obtain a uniform and transparent solution B.
[0074] S3: After degassing solution B, use a scraper to evenly coat it onto the surface of a clean glass plate to form a wet film of uniform thickness.
[0075] The wet membrane was dried at 60°C for 12 h to obtain a PVDF-HFP based solid electrolyte membrane.
[0076] Use plastic tweezers to peel the dried PVDF-HFP-based solid electrolyte membrane out of the mold, and then use a professional cutting tool to cut it into a circular electrolyte membrane with a diameter of 19mm.
[0077] LiFePO4, carbon black, and PVDF were weighed in a mass ratio of 8:1:1, N-methylpyrrolidone was added, and the mixture was ground to obtain an electrode slurry.
[0078] Electrode paste was uniformly coated onto aluminum foil current collector using a scraping method, with a thickness of 100 μm set for the scraping process.
[0079] The coated current collector is dried at high temperature under vacuum to obtain the positive electrode sheet. The drying temperature is set to 80℃ and the drying time is 24 h.
[0080] Finally, the dried electrode sheets are cut into round pieces with a diameter of 12 mm for later use.
[0081] Prepare a lithium metal anode, and assemble the above-mentioned PVDF-HFP based solid electrolyte membrane, the above-mentioned LiFePO4 positive electrode sheet and the lithium metal anode to obtain a solid-state lithium metal battery.
[0082] To further illustrate the present invention, the following detailed description, in conjunction with specific embodiments, provides a PI / PVDF-HFP composite solid electrolyte, its preparation method, and its applications.
[0083] Example 1
[0084] Preparation of PI / PVDF-HFP composite solid electrolyte membrane: First, under a protective atmosphere, 4 mL of N,N-dimethylformamide and 0.45 g of PVDF-HFP polymer matrix with a weight average molecular weight of 450,000 were added to a container and stirred to dissolve. The stirring temperature was 60℃ and the stirring time was 1 h, yielding solution A. Then, 0.02 g of lithium difluorooxalateborate, 0.45 g of lithium bis(trifluoromethanesulfonyl)imide, and 0.10 g of Li... 1.3 Al 0.3 Ti 1.7 (PO4)3 was added to solution A and stirred at 60°C for 8 h to obtain a uniform and transparent solution B. Finally, solution B was degassed and cast into a PI porous membrane with a porosity of 80% and a thickness of 20 μm, and dried at 60°C for 12 h to obtain a PI / PVDF-HFP composite solid electrolyte membrane.
[0085] Application of PI / PVDF-HFP composite solid electrolyte membrane in solid lithium metal batteries: The obtained PI / PVDF-HFP composite solid electrolyte membrane, lithium iron phosphate cathode sheet, and lithium sheet are assembled into a solid lithium metal battery.
[0086] Use plastic tweezers to peel the dried PI / PVDF-HFP composite solid electrolyte membrane out of the mold, and then use a professional cutting tool to cut it into round pieces with a diameter of 19 mm for later use.
[0087] Weigh 1.60 g LiFePO4, 0.20 g carbon black, and 0.20 g PVDF, add 5 mL N-methylpyrrolidone, and grind to obtain an electrode slurry. Coat the slurry evenly onto an aluminum foil current collector using a blade coating method, with a coating thickness of 100 μm. Dry the coated current collector at 80℃ under vacuum for 24 h to obtain the positive electrode sheet. Finally, cut the dried electrode sheet into 12 mm diameter discs for later use.
[0088] Prepare a lithium metal anode, and assemble the above-mentioned PVDF-HFP based solid electrolyte membrane, the above-mentioned LiFePO4 positive electrode sheet and the lithium metal anode to obtain a solid-state lithium metal battery.
[0089] Example 2: Unlike Example 1, Li 1.3 Al 0.3 Ti 1.7 The amount of (PO4)3 added was 0.16 g, and the other steps and parameters were the same as in Example 1.
[0090] Example 3: Unlike Example 1, 0.10 g of Li was added. 6.4 La3Zr 1.4 Ta 0.6 O 12 The other steps and parameters are the same as in Example 1.
[0091] Example 4: Unlike Example 1, 0.03 g of lithium difluorooxalate borate was added to solution A. All other steps and parameters were the same as in Example 1.
[0092] Example 5: Unlike Example 1, 0.02 g of lithium nitrate was added to solution A. All other steps and parameters were the same as in Example 1.
[0093] Example 6: Unlike Example 1, solution B was degassed and then cast into a PI porous membrane with a porosity of 70% and a thickness of 16 μm. All other steps and parameters were the same as in Example 1.
[0094] Example 7: Unlike Example 1, 4.5 mL of anhydrous acetonitrile and PVDF-HFP polymer matrix were added and stirred to dissolve. All other steps and parameters were the same as in Example 1.
[0095] Example 8: Unlike Example 1, the B solution was degassed and then cast into a PI porous membrane. It was first vacuum dried at 60 °C for 8 h to remove most of the DMF in the system. Then the temperature was raised to 80 °C and vacuum dried for another 4 h. The other steps and parameters were the same as in Example 1.
[0096] Example 9: Unlike Example 1, 1.60 g of LiNi was weighed. 0.8 Co 0.1 Mn 0.1 O2, 0.20 g carbon black and 0.20 g PVDF, 5 mL N-methylpyrrolidone were added and the mixture was ground. Other steps and parameters were the same as in Example 1.
[0097] Comparative Example 1
[0098] Preparation of PVDF-HFP based solid electrolyte membrane: First, under a protective atmosphere, 4 mL of N,N-dimethylformamide and 0.45 g of PVDF-HFP polymer matrix were added to a container and stirred to dissolve. The stirring temperature was 60℃ and the stirring time was 1 h, resulting in solution A. Then, 0.45 g of lithium bis(trifluoromethanesulfonylimide) was added to solution A and stirred at 60℃ for 8 h to obtain a uniform and transparent solution B. Finally, after degassing solution B, it was uniformly coated onto the surface of a clean glass plate using a doctor blade to form a wet film of uniform thickness. The wet film was dried at 60℃ for 12 h to obtain the PVDF-HFP based solid electrolyte membrane.
[0099] Application of PVDF-HFP based solid electrolyte membrane in solid lithium metal batteries: The obtained PVDF-HFP based solid electrolyte membrane, lithium iron phosphate cathode, and lithium sheet are assembled into a solid lithium metal battery.
[0100] Use plastic tweezers to peel the dried PVDF-HFP-based solid electrolyte membrane out of the mold, and then use a professional cutting tool to cut it into round pieces with a diameter of 19 mm for later use.
[0101] Weigh 1.60 g LiFePO4, 0.20 g carbon black, and 0.20 g PVDF, add 5 mL N-methylpyrrolidone, and grind to obtain an electrode slurry. Coat the slurry evenly onto an aluminum foil current collector using a blade coating method, with a coating thickness of 100 μm. Dry the coated current collector at 80℃ under vacuum for 24 h to obtain the positive electrode sheet. Finally, cut the dried electrode sheet into 12 mm diameter discs for later use.
[0102] Prepare a lithium metal anode, and assemble the above-mentioned PVDF-HFP based solid electrolyte membrane, the above-mentioned LiFePO4 positive electrode sheet and the lithium metal anode to obtain a solid-state lithium metal battery.
[0103] After the battery assembly is completed and activated, its electrochemical performance is tested.
[0104] (1) Ionic conductivity test: The PI / PVDF-HFP composite solid electrolyte membrane (used as an example) and the PVDF-HFP-based solid electrolyte membrane (used as a comparative example) were sandwiched between two stainless steel circular sheets and assembled into CR 2032 button cells in a glove box. The cells were tested using AC impedance spectroscopy (EIS) on a Chenhua CHI760 electrochemical workstation. The obtained data were then fitted to obtain the final required impedance data, and the ionic conductivity was calculated from this data.
[0105] (2) Rate and Cyclic Performance Testing: Cyclic and rate performance tests were conducted on the full cells assembled in the examples and comparative examples using a testing system (model CT3002A) from Wuhan Landian Electronics Co., Ltd. The charge / discharge cutoff voltages of the full cells assembled with LiFePO4 as the positive electrode were 3.8 V and 2.5 V, respectively; the charge / discharge cutoff voltages of the full cells assembled with NCM811 as the positive electrode were 4.2 V and 3.0 V, respectively. The test temperature was 30 °C. Before long-cycle testing, the full cells were activated for 3 cycles at a current density of 0.1 C, followed by cycle testing at a current density of 0.5 C. Rate performance testing involved 5 cycles at current densities of 0.2 C, 0.5 C, 1 C, 2 C, and a recovery current density of 0.2 C.
[0106] The thermal stability, mechanical properties, and electrochemical performance of the assembled batteries of Example 1 and Comparative Example 1 are compared in Table 1. Table 1 Performance of Example 1 and Comparative Example 1 performance Example 1 Comparative Example 1 Thermogravimetric analysis The temperatures corresponding to 5%, 10%, and 15% weight loss of the samples were 186.78 °C, 234.52 °C, and 270.14 °C, respectively, with a residual weight of 22.64%. The temperatures corresponding to 5%, 10%, and 15% weight loss of the samples were 194.35 °C, 240.11 °C, and 274.15 °C, respectively, with a residual weight of 21.04%. Maximum tensile strength 6.7 MPa 4.6 MPa Electrochemical window 5.03 V 4.91 V Ionic conductivity <![CDATA[1.64 x10 -4 S cm -1 ]]> <![CDATA[0.91 x10 -4 S cm -1 ]]> Lithium-ion transference number 0.567 0.205 Lithium symmetric battery <![CDATA[current density 0.2 mA cm -2 , stable cycling exceeds 800 h.]]> <![CDATA[Current density 0.2 mA cm -2 , stable cycling exceeds 550 h.]]> Ratio performance <![CDATA[The discharge specific capacities of the full cell at 0.2 C, 0.5 C, 1.0 C and 2.0 C are 158.7, 144.8, 107.8 and 84.76 mAh g -1 . When the current density is changed from 1.0 C to 0.2 C, the discharge specific capacity recovers to 160.4 mAh g -1 .]]> <![CDATA[The discharge specific capacities of the full cell at 0.2C, 0.5 C, 1.0 C and 2.0 C are 156, 138, 127 and 100 mAh g respectively -1 . When the current density is changed from 1.0 C to 0.2C, the discharge specific capacity recovers to 137 mAh g -1 .]]> LFP | Electrolyte | Li-based full cell <![CDATA[At a voltage of 2.8-3.6V, the initial discharge specific capacity at a current density of 0.5 C is 161.20 mAh g -1 , and the discharge specific capacity after 220 cycles is 134.30 mAh g -1 , with a capacity retention rate of 83.31%.]]> <![CDATA[At a voltage of 2.8-3.6V, the initial discharge specific capacity at a current density of 0.5 C is 142 mAh g -1 , and the discharge specific capacity after 100 cycles is 33 mAh g -1 , with a capacity retention rate of 23%.]]>
[0107] The PI / PVDF-HFP composite solid electrolyte membranes obtained in Examples 1 to 9 and the PVDF-HFP-based solid electrolyte membranes obtained in the comparative examples were assembled into stainless steel symmetric batteries. Electrochemical impedance spectroscopy tests and lithium-ion conductivity calculations were performed, and the results are shown in Table 2. Table 2. Lithium-ion conductivity of the examples and comparative examples type <![CDATA[Ionic conductivity / S cm -1 > Example 1 <![CDATA[1.64 × 10 -4 ]]> Example 2 <![CDATA[1.27 × 10 -4 ]]> Example 3 <![CDATA[1.81 × 10 -4 ]]> Example 4 <![CDATA[1.33 × 10 -4 ]]> Example 5 <![CDATA[1.25 × 10 -4 ]]> Example 6 <![CDATA[1.61 × 10 -4 ]]> Example 7 <![CDATA[1.38 × 10 -4 ]]> Example 8 <![CDATA[1.22 × 10 -4 ]]> Example 9 <![CDATA[1.18 × 10 -4 ]]> Comparative Example 1 <![CDATA[0.91 × 10 -4 ]]>
[0108] The foregoing has provided a detailed description of the PI / PVDF-HFP composite solid electrolyte, its preparation method, and its application. Specific examples have been used to illustrate the principles and specific implementation methods of the present invention. The descriptions of the above embodiments are only for the purpose of helping to understand the method and core technology of the present invention. At the same time, for those skilled in the art, there will be changes in the specific implementation methods and application scope based on the ideas of the present invention. Therefore, the content of this specification should not be construed as a limitation of the present invention.
Claims
1. A PI / PVDF-HFP composite solid electrolyte, characterized in that, It includes a PVDF-HFP polymer matrix, a porous PI membrane, a fast ion conductor filler, a lithium salt, and interface stabilizing additives.
2. The PI / PVDF-HFP composite solid electrolyte membrane as described in claim 1, characterized in that, The fast ion conductor filler includes Li 1.3 Al 0.3 Ti 1.7 (PO4)3, Li 1.5 A1 0.5 Ge 1.5 (PO4)3, Li 6.5 La3Zr 1.5 Nb 0.5 O 12 Li 6.4 La3Zr 1.4 Ta 0.6 O 12 Li7 La3 Zr2 O 12 Li 0.5 La 0.5 Any one of TiO3; preferably, the mass of the fast ion conductor filler is 5% to 100% of the mass of the PVDF-HFP polymer matrix; more preferably, the mass of the fast ion conductor filler is 20% to 50% of the mass of the PVDF-HFP polymer matrix.
3. The PI / PVDF-HFP composite solid electrolyte membrane as described in claims 1-2, characterized in that, The lithium salt is at least one of lithium bis(trifluoromethanesulfonyl)imide, lithium bis(fluorosulfonyl)imide, lithium hexafluorophosphate, lithium perchlorate, lithium tetrafluoroborate, lithium hexafluoroarsenate, lithium bis(oxalateborate), and lithium fluoroalkyl phosphate; preferably, the mass ratio of the lithium salt to the PVDF-HFP polymer matrix is 1:3 to 1:
1.
4. The PI / PVDF-HFP composite solid electrolyte membrane as described in claims 1-3, characterized in that, The interface stabilizing additive is at least one of vinyl ethylene carbonate, fluoroethylene carbonate, lithium bis(oxalato)borate, lithium difluorooxalato)borate, lithium nitrate, and lithium di(salicylic acid)borate; preferably, the additive is 0.1% to 5% of the total mass of the PVDF-HFP polymer matrix, lithium salt, and fast ion conductor filler.
5. The PI / PVDF-HFP composite solid electrolyte membrane as described in claims 1-4, characterized in that, The PI porous membrane has a porosity of 30% to 90% and a thickness of 5 μm to 150 μm; preferably, the PI porous membrane has a porosity of 50% to 80% and a thickness of 10 μm to 30 μm.
6. A method for preparing the PI / PVDF-HFP composite solid electrolyte membrane according to any one of claims 1 to 5, characterized in that, Includes the following steps: S1: Under a protective atmosphere, the first organic solvent and the PVDF-HFP polymer matrix are added to a container and stirred to dissolve, resulting in a homogeneous solution A; S2: Add the interface stabilizing additive, lithium salt and fast ion conductor filler to the solution A and stir to obtain a uniform and transparent solution B; S3: After degassing solution B, it is cast onto a PI porous membrane and dried to obtain a PI / PVDF-HFP composite solid electrolyte membrane.
7. The method for preparing the PI / PVDF-HFP composite solid electrolyte membrane according to claims 1-6, characterized in that, The first organic solvent is selected from any one of anhydrous acetonitrile, ethylene carbonate, N-methylpyrrolidone, N,N-dimethylformamide, acetone, tetrahydrofuran, dimethyl sulfoxide, and dichloroethane; preferably, the concentration of the PVDF-HFP polymer matrix in the first organic solvent is 0.05 g / mL to 1.00 g / mL.
8. The method for preparing the PI / PVDF-HFP composite solid electrolyte membrane according to claims 1-7, characterized in that, In step S1, the stirring temperature of the solution is 30℃~60℃ and the stirring time is more than 0.5h; in step S2, the stirring temperature of the solution is 30℃~60℃ and the stirring time is more than 0.5h; in step S3, the drying temperature is 30℃~80℃ and the drying time is 6h~25h.
9. The application of the PI / PVDF-HFP composite solid electrolyte membrane according to claims 1-8, characterized in that... Application of a PI / PVDF-HFP composite solid electrolyte in solid-state lithium metal batteries; A solid-state lithium metal battery, characterized in that it comprises a positive electrode, a lithium metal negative electrode, and a PI / PVDF-HFP composite solid electrolyte membrane as described in any one of claims 1 to 8.
10. A method for preparing a solid-state lithium metal battery, characterized in that, Includes the following steps: S4: Prepare the PI / PVDF-HFP composite solid electrolyte membrane using the preparation method of the PI / PVDF-HFP composite solid electrolyte membrane as described in claims 1 to 8, and then cut it into circular pieces with a diameter of 19 mm for later use; S5: Grind the positive electrode active material, conductive agent and binder, add the second organic solvent to obtain the electrode slurry, coat it evenly on the current collector by scraping, and dry the coated current collector at high temperature under vacuum to obtain the positive electrode sheet, and then cut the electrode sheet into a circular piece with a diameter of 12mm for later use. S6: Prepare a lithium metal negative electrode, and assemble the solid electrolyte membrane from step S4, the positive electrode sheet from step S5, and the lithium metal negative electrode to obtain a solid-state lithium metal battery.
11. The method for preparing a solid-state lithium metal battery according to claim 10, characterized in that, The conductive agent is selected from at least one of carbon black (Super P, acetylene black, Ketjen black), conductive graphite, carbon fiber, carbon nanotubes, graphene, and vapor-grown carbon fiber; the binder is selected from at least one of PVDF, PTFE, and SBR; the active material is selected from LiNi 0.8 Co 0.1 Mn 0.1 O2, LiNi 0.8 Co 0.15 Al 0.05 Any one of O2, LiFePO4, LiMnPO4, LiNiPO4, LiCoPO4, LiCoO2, and MoS2; preferably, the mass ratio of the active material, conductive agent, and binder in step S5 is 8:1:
1.
12. The method for preparing a solid-state lithium metal battery according to claim 10, characterized in that, In step S5, the thickness set for the scraping coating is 100 μm.
13. The method for preparing a solid-state lithium metal battery according to claim 10, characterized in that, In step S5, the vacuum drying temperature is set to 80℃ and the drying time is 24h.
14. The method for preparing a solid-state lithium metal battery according to claim 10, characterized in that, The second organic solvent is selected from any one of anhydrous acetonitrile, ethylene carbonate, N-methylpyrrolidone, N,N-dimethylformamide, acetone, tetrahydrofuran, dimethyl sulfoxide, and dichloroethane.
Citation Information
Patent Citations
Composite polymer solid electrolyte, preparation method thereof and solid-state lithium metal battery
CN121366940A
Solid electrolyte membrane as well as preparation method and application thereof
CN121642141A
Composite solid electrolyte membrane, preparation method and application thereof, and solid lithium metal battery
CN121839864A