Solid electrolytes and their preparation methods, positive electrode plates, batteries
By covalently bonding a polysiloxane graft layer to the surface of a solid electrolyte matrix, which contains hydrophobic and lithium-ion-conducting functional groups, the problem of sulfide and halide solid electrolytes being susceptible to moisture corrosion in air is solved, achieving a balance between high ionic conductivity and air stability.
Patent Information
- Application Number
- CN202611602595.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-10-16
- Publication Date
- 2026-11-17
AI Technical Summary
Existing sulfide and halide solid electrolytes are susceptible to moisture corrosion in air, leading to structural degradation, decreased conductivity, and release of corrosive gases. Furthermore, existing carbon coatings cannot effectively promote lithium-ion transport, thus affecting battery performance.
A polysiloxane graft layer is covalently bonded to the surface of a solid electrolyte substrate. The polysiloxane graft layer contains hydrophobic and lithium-ion conductive functional groups, forming a stable interface that combines hydrophobicity and ion conductivity, thereby improving the water stability of the air environment and reducing the interfacial impedance.
While maintaining high ionic conductivity, it effectively blocks water vapor, improves the air environment stability of solid electrolytes and reduces interface impedance, ensuring the continuity of lithium-ion transport.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] This application relates to the field of battery technology, and in particular to a solid electrolyte and its preparation method, a positive electrode, and a battery. Background Technology
[0002] All-solid-state lithium batteries are widely regarded as the core direction of next-generation electrochemical energy storage due to their high energy density and inherent safety (no risk of liquid electrolyte leakage), especially in fields such as electric vehicles, aerospace, and large-scale energy storage systems, where they have disruptive potential.
[0003] Sulfide solid electrolytes can reach 10 at room temperature -3 Sulfide solid electrolytes have attracted much attention due to their high lithium-ion conductivity at the S / cm level, but their intrinsic electrochemical window is narrow, requiring interface engineering to match high-voltage cathodes. In contrast, halide solid electrolytes (such as Li3InCl6 and Li2ZrCl6) have a wide electrochemical window and are well compatible with high-voltage cathodes. Therefore, both sulfide solid electrolytes and halide solid electrolytes have become hot research materials.
[0004] However, poor environmental stability is a common bottleneck restricting the industrialization of these two types of electrolytes. Specifically, sulfide solid electrolytes are extremely sensitive to moisture, releasing toxic H2S gas violently upon contact with water; while halide solid electrolytes (especially chloride systems), although having slightly better intrinsic stability, still face the problem of hygroscopic hydrolysis. Under normal air conditions (relative humidity > 10%), moisture corrosion will trigger the following chain of failures:
[0005] 1) Structural degradation: Water molecules embed into the crystal lattice or replace halogen sites, generating amorphous phases, hydrates, or halide oxides (such as InOCl) impurities, which destroy the integrity of the crystal;
[0006] 2) Sharp drop in conductivity: Structural collapse leads to the blockage of lithium-ion transport channels, resulting in an order-of-magnitude decrease in room temperature ionic conductivity;
[0007] 3) Corrosive gas release: Sulfides release H2S, while chlorinated halides easily release HCl gas during high-temperature treatment or high-voltage charging and discharging after water absorption, which corrodes equipment and components;
[0008] 4) Stringent processing window: The entire process from synthesis to cell assembly is forced to be carried out in an inert atmosphere with extremely low dew points (sulfides usually need to be <-60℃, halides need to be <-60℃), which greatly increases manufacturing costs and increases the process complexity of large-scale production.
[0009] To address the aforementioned technical problems, existing technologies improve the hydrophobic properties of halide solid electrolytes by carbon coating the surface of the electrolyte. While carbon coating provides some physical barrier and hydrophobicity, its primary function is electron conduction, and it does not promote lithium-ion transport. In fact, the carbon coating on the surface may even hinder lithium-ion passage, thereby affecting the ionic conductivity of the halide solid electrolyte.
[0010] Therefore, how to construct a multifunctional protective layer that can effectively block water vapor without affecting lithium-ion transport while maintaining high ionic conductivity is a technical challenge that halide solid electrolytes and sulfide solid electrolytes need to solve. Summary of the Invention
[0011] This application provides a solid electrolyte and its preparation method, a positive electrode, and a battery; the hydrophobic functional groups and lithium-ion conductive functional groups on the solid electrolyte matrix can respectively improve the hydrophobicity and ionic conductivity of the solid electrolyte matrix.
[0012] In a first aspect, this application provides a solid electrolyte, including a solid electrolyte matrix and a polysiloxane graft layer located on at least a portion of the surface of the solid electrolyte matrix, wherein the solid electrolyte matrix and the polysiloxane graft layer are interconnected by -MO-Si-, and M includes at least one of a metal element and P.
[0013] The polysiloxane graft layer includes hydrophobic functional groups and lithium-ion conductive functional groups; the solid electrolyte matrix includes a halide solid electrolyte and / or a sulfide solid electrolyte.
[0014] The hydrophobic functional group is derived from a hydrophobic functional group precursor, which includes at least one of 1H,1H,2H,2H-perfluorooctyltrimethoxysilane, 1H,1H,2H,2H-perfluorodecyltriethoxysilane, n-octyltrimethoxysilane, n-dodecyltrimethoxysilane, and n-octadecyltrimethoxysilane.
[0015] The lithium-ion-conducting functional group is derived from a lithium-ion-conducting functional group precursor, which includes at least one of 2-[methoxy(polyethoxy)6-9propyl]trimethoxysilane, succinate-functionalized silane, and cyclic carbonate-functionalized silane.
[0016] In the solid electrolyte described above, the polysiloxane graft layer comprises a -Si-O-Si- main chain, the carbon atoms in the hydrophobic functional group are connected to silicon atoms on the -Si-O-Si- main chain, and the carbon atoms in the lithium-ion-conducting functional group are connected to silicon atoms on the -Si-O-Si- main chain.
[0017] The solid electrolyte as described above, wherein the chemical formula of the halide solid electrolyte includes Li a M'D x Wherein, 1≤a≤3, 4≤x≤6, M' includes at least one of In, Zr, Y, Sc, Er, Yb, and Ho, and D includes at least one of F, Cl, Br, and I;
[0018] And / or, the chemical formula of the sulfide solid electrolyte includes Li 6-y PS 5-y A 1+y A includes at least one of Cl, Br, I, and F, and 0 ≤ y < 1.
[0019] In the solid electrolyte described above, the thickness of the polysiloxane graft layer is 3-16 nm.
[0020] The solid electrolyte as described above is prepared by a method comprising the following steps:
[0021] In an inert atmosphere, a solid electrolyte matrix, a hydrophobic functional group precursor, and a lithium-ion functional group precursor are dispersed in a nonpolar solvent and stirred to react. The solid electrolyte is obtained by washing with the nonpolar solvent and vacuum drying, wherein the water content in the nonpolar solvent is less than 20 ppm by mass.
[0022] Secondly, this application provides a method for preparing the solid electrolyte as described above, comprising:
[0023] In an inert atmosphere, a solid electrolyte matrix, a hydrophobic functional group precursor, and a lithium-ion-conducting functional group precursor are dispersed in a nonpolar solvent and reacted with stirring; the solid electrolyte is obtained by washing with a nonpolar solvent and vacuum drying.
[0024] The hydrophobic functional group precursor includes at least one of 1H,1H,2H,2H-perfluorooctyltrimethoxysilane, 1H,1H,2H,2H-perfluorodecyltriethoxysilane, n-octyltrimethoxysilane, n-dodecyltrimethoxysilane, and n-octadecyltrimethoxysilane.
[0025] The lithium-ion functional group precursor includes at least one of 2-[methoxy(polyethoxy)6-9propyl]trimethoxysilane, succinate-functionalized silane, and cyclic carbonate-functionalized silane.
[0026] The preparation method described above, wherein the step of dispersing the solid electrolyte matrix, the hydrophobic functional group precursor, and the lithium-ion functional group precursor in a nonpolar solvent specifically includes: first dispersing the hydrophobic functional group precursor and the lithium-ion functional group precursor in a nonpolar solvent, mixing them to form a precursor solution, and then adding the solid electrolyte matrix to the precursor solution under stirring to form a suspension.
[0027] In the preparation method described above, the temperature of the stirring reaction is 45℃-60℃, and the stirring reaction time is 0.5-4h.
[0028] In the preparation method described above, the molar ratio of the hydrophobic functional group precursor to the lithium-ion-conducting functional group precursor is (0.5-5):1.
[0029] And / or, the total mass fraction of the hydrophobic functional group precursor and the lithium-ion functional group precursor in the precursor solution is 0.1-1%;
[0030] And / or, the solid content of the suspension is 1.96%-10%.
[0031] In the preparation method described above, the number of washing cycles is 3-5.
[0032] And / or, the vacuum drying temperature is 60-120℃, and the vacuum drying time is 2-6h.
[0033] Thirdly, this application provides a positive electrode sheet, wherein the positive electrode sheet includes the above-mentioned solid electrolyte.
[0034] Fourthly, this application provides a battery, wherein the battery includes the above-described positive electrode.
[0035] This application provides a solid electrolyte and its preparation method, positive electrode, and battery. By covalently bonding a polysiloxane graft layer to the surface of a solid electrolyte substrate, and making the polysiloxane graft layer simultaneously include hydrophobic functional groups and lithium-ion conductive functional groups, a stable interface with both hydrophobicity and ion conductivity can be constructed on the surface of halide solid electrolytes and / or sulfide solid electrolytes, thereby improving the water stability of the solid electrolyte in the air environment and reducing the risk of increased interface impedance. Detailed Implementation
[0036] To enable those skilled in the art to better understand the solutions of this invention, the following provides a more detailed description of this application. The specific embodiments listed below are merely descriptions of the principles and features of this invention; the examples are only for explaining the invention and are not intended to limit its scope. Based on the embodiments of this invention, all other embodiments obtained by those skilled in the art without inventive effort are within the scope of protection of this invention.
[0037] All-solid-state lithium battery technology involves solid electrolyte materials, electrode composites, cell assembly, and storage and transportation processing, and is particularly suitable for electric vehicles, energy storage devices, and high-safety power systems. Halide and sulfide solid electrolytes are often used as key ion transport media in these batteries due to their high ionic conductivity and good electrochemical compatibility.
[0038] In existing solutions, to mitigate the sensitivity of halide and sulfide solid electrolytes to moisture in the air, two main technical approaches are typically employed: bulk modification and surface coating. Bulk modification often involves altering the internal composition of the material through elemental doping or composite addition to improve stability; surface coating, on the other hand, forms a protective layer on the outer layer of the particles to prevent moisture from contacting the electrolyte matrix, thereby reducing the risk of hygroscopic decomposition.
[0039] However, bulk modification often requires stringent process conditions and can easily interfere with the original crystal structure and ion migration channels of the solid electrolyte, leading to impaired intrinsic conductivity. While surface coating can improve hydrophobicity to some extent, existing coatings mostly focus on physical barriers and lack synergistic support for lithium-ion transport, which can easily cause increased interfacial impedance and may fail during subsequent processing or cycling due to unstable bonding.
[0040] The aforementioned defects directly lead to a difficulty in achieving both air stability and ion conduction performance.
[0041] In view of this, this application covalently bonds a polysiloxane graft layer on the surface of a solid electrolyte substrate, so that the polysiloxane graft layer includes both hydrophobic functional groups and lithium-ion conductive functional groups, thereby achieving a balance between hydrophobicity and ion conductivity.
[0042] In a first aspect, this application provides a solid electrolyte, including a solid electrolyte matrix and a polysiloxane graft layer located on at least a portion of the surface of the solid electrolyte matrix, wherein the solid electrolyte matrix and the polysiloxane graft layer are interconnected by -MO-Si-, and M includes at least one of a metal element and P.
[0043] The polysiloxane graft layer includes hydrophobic functional groups and lithium-ion conducting functional groups; the hydrophobic functional groups include substituted or unsubstituted C6-C18 alkanes, wherein the substituents include halogens;
[0044] The lithium-ion-conducting functional group includes at least one of the following: a group containing a polyethylene glycol segment, a succinic acid group, and a cyclic carbonate group, wherein the group containing a polyethylene glycol segment includes -(O-CH2-CH2). n - where n is an integer between 6 and 9;
[0045] Solid electrolyte matrices include halide solid electrolytes and / or sulfide solid electrolytes;
[0046] The hydrophobic functional group is derived from a hydrophobic functional group precursor, which includes at least one of 1H,1H,2H,2H-perfluorooctyltrimethoxysilane, 1H,1H,2H,2H-perfluorodecyltriethoxysilane, n-octyltrimethoxysilane, n-dodecyltrimethoxysilane, and n-octadecyltrimethoxysilane.
[0047] The lithium-ion functional group is derived from a lithium-ion functional group precursor, which includes at least one of 2-[methoxy(polyethoxy)6-9propyl]trimethoxysilane, succinate-functionalized silane, and cyclic carbonate-functionalized silane.
[0048] This application constructs a stable interface with both hydrophobicity and ion conductivity on the surface of halide solid electrolytes and / or sulfide solid electrolytes by covalently bonding a polysiloxane graft layer to the surface of a solid electrolyte substrate, and by including both hydrophobic and lithium-ion conductive functional groups in the polysiloxane graft layer. This improves the water stability of the solid electrolyte in the air environment and reduces the risk of increased interfacial impedance.
[0049] Specifically, in this application, the solid electrolyte does not improve environmental adaptability by altering the bulk composition of the matrix. Instead, while maintaining the intrinsic ion conduction framework of the solid electrolyte matrix largely undisturbed, a functionalized polysiloxane graft layer chemically anchored to the matrix is constructed on the surface of the solid electrolyte matrix. The solid electrolyte matrix can be a halide solid electrolyte, a sulfide solid electrolyte, or a mixture of both.
[0050] The polysiloxane graft layer contains both hydrophobic and lithium-ion-conducting functional groups. This layer can cover the surface of a solid electrolyte substrate while preventing a significant increase in the diffusion path of lithium ions across the interface. By combining hydrophobic and lithium-ion-conducting units within the polysiloxane graft layer, hydrophobicity and ion transport are synergistically achieved at the same interface.
[0051] For the specific composition of the hydrophobic functional group, one possible embodiment may use substituted or unsubstituted C6-C18 alkanes, wherein the substituent is a halogen. The C-halogen bond in the halogen-substituted carbon chain has high bond energy and low segment polarizability, forming a low surface energy orientation layer on the surface after grafting. This inhibits the wetting and spreading of water molecules on the particle surface, thereby slowing down the adsorption and penetration of water vapor from the air to the matrix interface. For example, a semi-fluorocarbon chain can also be used to balance hydrophobicity, material cost, and processing compatibility. Furthermore, long-chain alkyl groups can also be used as hydrophobic functional groups; after surface orientation, long-chain alkyl groups can also form a dense organic barrier.
[0052] For the specific composition of the lithium-ion-conducting functional group, one possible embodiment may employ a group containing oligoethylene glycol segments. Multiple ether oxygen atoms in the oligoethylene glycol segments can reversibly coordinate with lithium ions, forming continuous or semi-continuous solvated migration sites locally in the polysiloxane graft layer. Lithium ions can then be transported across the interface via jumps between adjacent coordination sites. For example, a lithium-ion-conducting functional group containing succinic anhydride groups may also be used. The nitrile groups in the succinic anhydride groups have strong dipole moments and can interact polarly with lithium ions, promoting deassociation and directional migration of lithium ions within the polysiloxane graft layer. Furthermore, a functional group containing cyclic carbonate groups may also be used, utilizing the coordination environment formed by its polar carbonyl group and cyclic structure to assist the migration of lithium ions from the lithium salt or interface. One or more of the above lithium-ion-conducting functional groups may be selected, or two or three may be used in combination. For example, when oligoethylene glycol segments coexist with succinic acid groups, the former provides flexible coordination links and the latter provides polar attraction sites, enabling the formation of various types of migration nodes at the nanoscale; when oligoethylene glycol segments coexist with cyclic carbonate groups, both segment mobility and local high polarity environments can be taken into account.
[0053] In one possible embodiment, the hydrophobic functional group is derived from 1H,1H,2H,2H-perfluorooctyltrimethoxysilane and / or 1H,1H,2H,2H-perfluorodecyltriethoxysilane. These molecules contain perfluorocarbon chains with high bond energies and low segment polarizability. After grafting, they form a low surface energy orientation layer on the surface, inhibiting the wetting and spreading of water molecules on the particle surface, thereby slowing down the adsorption and penetration of water vapor from the air to the matrix interface. The hydrophobic functional group can also be derived from at least one of n-octyltrimethoxysilane, n-dodecyltrimethoxysilane, and n-octadecyltrimethoxysilane. The long-chain alkyl groups contained in these molecules act as hydrophobic functional groups, and their surface orientation can also form a dense organic barrier. Compared to fluorinated segments, long-chain alkyl systems are more readily available and, in some cases, exhibit higher compatibility with the organic components of the electrode composite system. Perfluorocarbon chains and long-chain alkyl groups can be used alone or in combination in a predetermined ratio. The hydrophobic functional groups do not exist as migratable additives, but are fixed in the grafted layer, so that the low surface energy groups are located near the gas-solid interface for a long time, thereby maintaining a stable water-blocking boundary.
[0054] In one possible embodiment, the lithium-ion-conducting functional group is derived from 2-[methoxy(polyethoxy)6-9propyl]trimethoxysilane, whose molecule contains a short PEG chain composed of 6-9 ethoxy (-CH2CH2O-) units. The lone pair electrons on the ether oxygen atom can undergo Lewis acid-base coordination with lithium ions, and promote lithium ion transport along the PEG chain through local chain movement. Functionalized silanes are generally prepared by using a basic alkoxysilane as the silane parent, and by covalently grafting the target organic functional segment onto the silane side chain through silicon-hydroaddition or nucleophilic substitution reactions. One end of the molecule retains a hydrolyzable alkoxysilane group, which, after hydrolysis, can condense with hydroxyl groups on the surface of inorganic particles to form Si-O-Si bonds, achieving covalent anchoring of the silane on the particle surface; the other end exposes an active functional group; the lithium-ion-conducting functional group can also be derived from succinicornitrile-functionalized silanes, whose molecular side chains are covalently linked to succinicornitrile functional segments containing -CN cyano groups. The nitrogen atom in the cyano group (-CN) possesses a lone pair of electrons, which can act as a Lewis base site to coordinate and dissociate with lithium ions. As the organic segments of the silane side chain undergo localized thermal motion, lithium ions can continuously transition and transfer between adjacent cyano sites, thus constructing a lithium-ion transport pathway at the solid electrolyte interface and reducing interfacial impedance. Lithium-conducting functional groups can also originate from cyclic carbonate-functionalized silanes, whose molecular side chains are covalently bonded with cyclic carbonate groups. The oxygen atom of the carbonyl group (C=O) on the cyclic carbonate ring possesses a lone pair of electrons, which can generate Lewis acid-base coordination with lithium ions. Relying on the localized motion of the flexible alkyl spacer segments of the side chain, lithium ions can undergo relay-style transitions and transfer between different cyclic carbonate sites, promoting lithium salt dissociation and improving interfacial lithium-ion conductivity.
[0055] The polysiloxane graft layer is fixed to the surface of the solid electrolyte matrix via -MO-Si-, where M includes at least one metal element and P. The hydrophobic functional groups construct a low surface energy boundary, weakening the adsorption, aggregation, and inward diffusion of water molecules on the surface. Simultaneously, the lithium-ion-conducting functional groups provide migration sites for lithium ions across the surface layer through ether-oxygen coordination, nitrile polar interactions, or cyclic carbonate coordination environments. This process achieves the coupling of "hydrophobic barrier-ion channel" within the same polysiloxane graft layer, ensuring that surface protection does not come at the cost of completely blocking ion movement, but rather retains lithium-ion mobility while limiting water vapor intrusion. Since the modification is mainly limited to the surface layer of the solid electrolyte matrix and does not directly reconstruct the matrix crystal framework, it has minimal interference with the original rapid ion conduction network of halide or sulfide solid electrolytes. Because the polysiloxane graft layer and the matrix are covalently bonded, overall desorption is difficult to occur during subsequent mixing, tableting, and cycling, thus ensuring the continuity of the air stability improvement effect throughout the processing.
[0056] In one possible implementation, the polysiloxane graft layer includes a -Si-O-Si- main chain, where carbon atoms in the hydrophobic functional groups are connected to silicon atoms on the -Si-O-Si- main chain, and carbon atoms in the lithium-ion functional groups are connected to silicon atoms on the -Si-O-Si- main chain.
[0057] The polysiloxane grafted layer in this application uses a polysiloxane network as an organic-inorganic hybrid framework to form a continuous cross-linked layer that is firmly bonded to the surface of a solid electrolyte matrix.
[0058] After hydrophobic functional groups are connected to the main chain silicon atoms through Si-C covalent bonds, they can preferentially align with the external environment as low surface energy side groups, thereby weakening the wetting and penetration of water molecules on the surface.
[0059] The lithium-ion-conducting functional groups, after being covalently attached to the main chain silicon atoms via Si-C bonds, can provide lithium-ion coordination sites and migration channels within the polysiloxane graft layer. By simultaneously constructing hydrophobic and lithium-ion-conducting side groups within the same polysiloxane network, ion migration continuity can be maintained while suppressing moisture absorption. This allows the polysiloxane graft layer to both block moisture contact and provide a low-resistance transport interface for lithium ions, thus achieving a balance between air stability, interfacial bonding stability, and ionic conductivity.
[0060] In one possible implementation, the chemical formula of the halide solid electrolyte includes Li a M'D x Where 1≤a≤3, 4≤x≤6, M' includes at least one of In, Zr, Y, Sc, Er, Yb, and Ho, and D includes at least one of F, Cl, Br, and I.
[0061] The solid electrolyte matrix can be a halide system, Li a M'D x , where a and x represent the stoichiometry of lithium and metal halide framework, respectively; M' is selected from at least one of In, Zr, Y, Sc, Er, Yb, and Ho, which can regulate the crystal field environment and anion site distribution, thereby providing stable and reactive surface sites for subsequent polysiloxane graft layers; D is selected from at least one of F, Cl, Br, and I, which enables halide anions to participate in the formation of a stable lattice while also taking into account electrochemical window and processing adaptability.
[0062] It is understandable that 1≤a≤3, for example, a range of values between 1, 2, 3, or any two of them.
[0063] It is understandable that 4≤x≤6, for example, a range of values between 4, 5, 6, or any two of them.
[0064] In one possible implementation, the chemical formula of the sulfide solid electrolyte includes Li 6-y PS 5-y A 1+y A includes at least one of Cl, Br, I, and F, and 0 ≤ y < 1.
[0065] It is understandable that 0 ≤ y < 1, such as 0, 0.2, 0.4, 0.6, 0.8, 0.9 or any two of these ranges.
[0066] In one possible implementation, the thickness of the polysiloxane graft layer is 3-16 nm.
[0067] Understandably, the thickness of the polysiloxane graft layer is 3-16 nm, for example, 3 nm, 4 nm, 5 nm, 6 nm, 7 nm, 8 nm, 9 nm, 10 nm, 11 nm, 12 nm, 13 nm, 14 nm, 15 nm, 16 nm or any two of these ranges.
[0068] This application controls the thickness of the polysiloxane graft layer within the nanoscale range of 3-16 nm. If the thickness is less than 3 nm, the polysiloxane graft layer is difficult to form a continuous and effective hydrophobic barrier, allowing moisture to easily penetrate and contact the substrate, thus reducing air stability. If the thickness is too thick, such as exceeding 16 nm, the path for lithium ions to cross the surface becomes longer, increasing the interfacial resistance and weakening the intrinsic ion conduction performance. By controlling the polysiloxane graft layer within the 3-16 nm range, a sufficiently dense moisture-proof layer can be formed on the surface by the hydrophobic functional groups, while not significantly hindering the participation of lithium-ion functional groups in ion migration, thus achieving both moisture protection and ion transport.
[0069] In one possible implementation, the solid electrolyte is prepared by a method comprising the following steps:
[0070] In an inert atmosphere, a solid electrolyte matrix, a hydrophobic functional group precursor, and a lithium-ion functional group precursor are dispersed in a nonpolar solvent and stirred to react. The solid electrolyte is obtained by washing with the nonpolar solvent and vacuum drying, wherein the water content in the nonpolar solvent is less than 20 ppm by mass.
[0071] Secondly, this application provides a method for preparing a solid electrolyte, comprising:
[0072] In an inert atmosphere, a solid electrolyte matrix, a hydrophobic functional group precursor, and a lithium-ion functional group precursor are dispersed in a nonpolar solvent and stirred to react. The solid electrolyte is obtained by washing with a nonpolar solvent and vacuum drying, wherein the water content in the nonpolar solvent is less than 20 ppm.
[0073] The hydrophobic functional group precursor includes at least one of 1H,1H,2H,2H-perfluorooctyltrimethoxysilane, 1H,1H,2H,2H-perfluorodecyltriethoxysilane, n-octyltrimethoxysilane, n-dodecyltrimethoxysilane, and n-octadecyltrimethoxysilane.
[0074] The lithium-ion functional group precursor includes at least one of 2-[methoxy(polyethoxy)6-9propyl]trimethoxysilane, succinate-functionalized silane, and cyclic carbonate-functionalized silane.
[0075] Typically, during routine synthesis, storage, or extremely short-duration operations, halide electrolyte matrix powders exhibit surface halogen ions (such as Cl-). - Inevitably, it will undergo hydrolysis with trace amounts of water molecules in the environment, generating trace amounts of surface metal hydroxyl groups (M-OH) or physically adsorbed water, and P-OH exists on the surface of the sulfide electrolyte matrix powder. Although these sites are harmful, they happen to be the reactive centers in this application. This application disperses the solid electrolyte matrix powder to be modified, a hydrophobic functional group precursor, and a lithium-ion functional group precursor in a nonpolar solvent. One end of the hydrophobic functional group precursor and the lithium-ion functional group precursor molecule has an anchoring group that can undergo a condensation reaction with M-OH (or P-OH). The most typical anchoring group is silanoxy (-Si(OR)3, R is CH3 or C2H5). The Si-OR group undergoes hydrolysis to generate Si-OH, which, when it encounters M-OH (or P-OH) on the surface of the solid electrolyte matrix, immediately undergoes dehydration condensation with M-OH (or P-OH) to form a stable -MO-Si- covalent bond, where M includes at least one of a metal element and P. This reaction firmly anchors hydrophobic functional group precursors and lithium-ion functional group precursor molecules to the surface of a solid electrolyte matrix in the form of a chemical monolayer.
[0076] After surface anchoring, trace amounts of moisture in the reaction system, along with heating, further promote the lateral condensation reaction between unreacted Si-OH or Si-OR groups on adjacent anchored molecules, generating -Si-O-Si-siloxane bridge bonds. This process connects the originally dispersed single-point anchored molecules, forming a continuous, dense polysiloxane nanofilm with a three-dimensional network structure. During this crosslinking process, the hydrophobic and lithium-ion functional groups in the hydrophobic and lithium-ion functional group precursors are covalently embedded into the polysiloxane nanofilm, thereby forming the polysiloxane graft layer of this application.
[0077] In one possible implementation, the nonpolar solvent includes at least one of anhydrous toluene, n-hexane, cyclohexane, and n-heptane. It should be understood that the above examples are merely illustrative and not limiting.
[0078] In one possible implementation, the step of dispersing the solid electrolyte matrix, the hydrophobic functional group precursor, and the lithium-ion functional group precursor in a nonpolar solvent specifically includes: first dispersing the hydrophobic functional group precursor and the lithium-ion functional group precursor in a nonpolar solvent, mixing them to form a precursor solution, and then adding the solid electrolyte matrix to the precursor solution under stirring to form a suspension.
[0079] Hydrophobic and lithium-ion-conducting functional group precursors are first prepared into a precursor solution in a nonpolar solvent, and then contacted with a solid electrolyte matrix to ensure uniform mixing. This more uniform dispersion of the two precursors facilitates adsorption, condensation, or other covalent bonding reactions on the surface of the solid electrolyte matrix, thereby constructing a polysiloxane graft layer containing both hydrophobic and lithium-ion-conducting functional groups. By preparing the precursor solution first and adding it to the solid electrolyte matrix under stirring, the surface reaction proceeds more uniformly, resulting in a continuous and stable surface layer. This layer provides moisture barrier properties while maintaining the local coordination environment required for lithium-ion migration, thus synergistically achieving a balance between air stability and ion conductivity with the solid electrolyte matrix.
[0080] In one possible implementation, the temperature of the stirring reaction is 45℃-60℃, and the stirring reaction time is 0.5-4h.
[0081] It is understood that the temperature of the stirring reaction is 45℃-60℃, for example, 45℃, 47℃, 50℃, 52℃, 55℃, 57℃, 60℃ or any two of these ranges.
[0082] It is understood that the stirring reaction time is 0.5-4h, for example, 0.5h, 1h, 1.5h, 2h, 2.5h, 3h, 3.5h, 4h or any two of these ranges.
[0083] The aforementioned temperature is used to control the reaction rate between the hydrophobic functional group precursor, the lithium-ion functional group precursor and the active sites on the surface of the solid electrolyte matrix. If the temperature is too low, the grafting reaction will be insufficient, and if the temperature is too high, it may cause side reactions of the precursor or have an adverse effect on the surface of the sulfide or halide solid electrolyte matrix. Therefore, limiting it within the above range can enable the hydrophobic functional group and the lithium-ion functional group to form a stable polysiloxane graft layer simultaneously. The time is used to control the surface coverage and the densification process of the polysiloxane graft layer. If the reaction time is insufficient, the surface bonding density will be low, and if it is too long, it may lead to increased self-polymerization or agglomeration in the solution, so as to obtain a more uniform surface modification.
[0084] In one possible implementation, the molar ratio of the hydrophobic functional group precursor to the lithium-ion functional group precursor is (0.5-5):1.
[0085] It is understandable that the molar ratio of the hydrophobic functional group precursor to the lithium-ion functional group precursor is (0.5-5):1, for example, 0.5:1, 1:1, 2:1, 3:1, 4:1, 5:1 or any value between the two.
[0086] By controlling the molar ratio within the range of 0.5:1 to 5:1, a relatively stable mixed precursor solution can be formed in a nonpolar solvent by combining hydrophobic functional group precursors and lithium-ion conductive functional group precursors. Upon contact with the solid electrolyte matrix, surface grafting and condensation occur simultaneously, forming a polysiloxane graft layer that serves as both a hydrophobic barrier and lithium-ion conductive sites. If the ratio is too low, the hydrophobic component coverage is insufficient; if the ratio is too high, the density of the lithium-ion conductive component decreases. Therefore, this range allows for a balanced adjustment of the surface functional distribution.
[0087] In one possible implementation, the total mass fraction of the hydrophobic functional group precursor and the lithium-ion functional group precursor in the precursor solution is 0.1-1%.
[0088] By limiting the total mass fraction of hydrophobic functional group precursors and lithium-ion conducting functional group precursors in the precursor solution, the thickness of the polysiloxane graft layer on the solid electrolyte matrix can be controlled. When this range is too low, the hydrophobic and lithium-ion conducting functional groups do not cover the substrate sufficiently, and cannot effectively block water vapor for a long time, resulting in a deterioration in the performance of the solid electrolyte after contact with water. When this range is too high, the thickness of the polysiloxane graft layer will increase. Although it can effectively block water vapor, the hydrophobic functional groups on the surface will hinder the passage of lithium ions, thereby affecting the ionic conductivity of the solid electrolyte.
[0089] In one possible implementation, the solid content of the suspension is 1.96%-10%.
[0090] By limiting the solid content of the suspension, the dispersion state of the solid electrolyte matrix in the suspension can be controlled, avoiding agglomeration and ensuring that the hydrophobic functional group precursor and the lithium-ion conducting functional group precursor are uniformly anchored on the surface of the solid electrolyte matrix. At the same time, by controlling the local concentration of the hydrophobic functional group precursor and the lithium-ion conducting functional group precursor on the surface of the solid electrolyte matrix, the anchoring amount of the hydrophobic functional group precursor and the lithium-ion conducting functional group precursor and the thickness of the polysiloxane graft layer can be precisely controlled, thereby improving the repeatability of the modification process.
[0091] In one possible implementation, the washing is performed 3-5 times.
[0092] Understandably, the number of washes is 3-5 times, such as 3, 4, 5 times or any range between two of these.
[0093] The purpose of washing is to remove all unreacted or physically adsorbed free hydrophobic functional group precursors and lithium-ion functional group precursors and their oligomers from the particle surface, ensuring the accuracy of subsequent testing and applications.
[0094] In one possible implementation, the vacuum drying temperature is 60-120°C, and the vacuum drying time is 2-6 hours.
[0095] It is understood that the temperature for vacuum drying is 60-120℃, such as 60℃, 70℃, 80℃, 90℃, 100℃, 110℃, 120℃ or any two of these ranges.
[0096] It is understandable that the vacuum drying time is 2-6 hours, for example, 2 hours, 3 hours, 4 hours, 5 hours, 6 hours or any two of these ranges.
[0097] Thirdly, this application provides a positive electrode sheet, which includes the aforementioned solid electrolyte.
[0098] Fourthly, this application provides a battery, which includes the aforementioned positive electrode plate.
[0099] The technical solution of this application and how the technical solution of this application solves the above-mentioned technical problems are described in detail below with specific embodiments. The following specific embodiments can be combined with each other, and the same or similar concepts or processes may not be described again in some embodiments.
[0100] Example 1
[0101] The preparation method of the solid electrolyte in this embodiment is as follows:
[0102] S1: In a glove box filled with high-purity inert gas (with the mass content of H2O and O2 in the glove box controlled to be less than 0.1 ppm), the hydrophobic functional group precursor: 1H,1H,2H,2H-perfluorooctyltrimethoxysilane and the lithium-ion functional group precursor: 2-[methoxy(polyethoxy)7propyl]trimethoxysilane (the average number of polyethoxy chain segments is 7) are mixed at a molar ratio of 1.5:1 to obtain a mixed precursor. 0.2 g of this mixed precursor is weighed and dissolved in 100 mL of anhydrous toluene, a nonpolar solvent, wherein the mass content of water in the anhydrous toluene is less than 20 ppm. The solution is stirred thoroughly to prepare a precursor solution with a total mass fraction of approximately 0.2 wt%.
[0103] S2: Weigh 10g of Li3InCl6 powder as the solid electrolyte matrix and slowly add it to the above precursor solution under stirring to form a uniform suspension with a solid content of 9.26%. Place the sealed reaction vessel in an oil bath and heat it to 55°C, and continue stirring at this temperature for 3 hours.
[0104] S3: After the reaction was complete, the suspension was transferred to a centrifuge tube under argon protection and centrifuged at 7000 rpm for 5 minutes. The supernatant was then discarded. 80 mL of anhydrous toluene (a nonpolar solvent with a water content of less than 20 ppm) was added for washing. The mixture was then ultrasonically dispersed for 2 minutes and centrifuged again. This dispersion-centrifugation washing process was repeated four times. Finally, the mixture was vacuum dried at 120°C for 4 hours to obtain the solid electrolyte.
[0105] Example 2
[0106] The preparation method of the solid electrolyte in this embodiment is basically the same as that in Example 1, except that in step S1, the hydrophobic functional group precursor is n-octadecyltrimethoxysilane to obtain the solid electrolyte.
[0107] Example 3
[0108] This embodiment is basically the same as Embodiment 1, except that: in step S1, the lithium-ion-conducting functional group precursor is mononitrile trimethoxysilane (CAS: 2526-62-7), and the molar ratio of the hydrophobic functional group precursor to the lithium-ion-conducting functional group precursor is 2:1. In steps S1 and S3, the nonpolar solvent is anhydrous n-heptane, resulting in a solid electrolyte.
[0109] In step S2: the oil bath heating temperature is 60℃, and the stirring reaction time is 2 hours.
[0110] Example 4
[0111] The preparation method of the solid electrolyte in this embodiment is basically the same as that in Example 1, except that in step S2, the solid electrolyte matrix is Li6PS5Cl, and a solid electrolyte is obtained.
[0112] Example 5
[0113] The preparation method of the solid electrolyte in this embodiment is basically the same as that in Example 1, except that in step S1, 0.05g of mixed precursor is weighed and stirred thoroughly to prepare a precursor solution with a total mass fraction of 0.05wt%, thereby obtaining the solid electrolyte.
[0114] Example 6
[0115] The preparation method of the solid electrolyte in this embodiment is basically the same as that in Example 1, except that in step S1, 1.2g of mixed precursor is weighed and stirred thoroughly to prepare a precursor solution with a total mass fraction of 1.2wt%, thereby obtaining the solid electrolyte.
[0116] Example 7
[0117] The preparation method of the solid electrolyte in this embodiment is basically the same as that in Example 1, except that in step S1, the hydrophobic functional group precursor and the lithium-ion functional group precursor are mixed in a molar ratio of 5:1.
[0118] In step S2: the mixture is heated to 45°C in an oil bath and stirred continuously at this temperature for 4 hours to obtain a solid electrolyte.
[0119] Example 8
[0120] The preparation method of the solid electrolyte in this embodiment is basically the same as that in Example 1, except that: in step S1, the hydrophobic functional group precursor and the lithium-ion functional group precursor are mixed at a molar ratio of 0.5:1; and in step S2, the oil bath heating temperature is 60°C, and the stirring reaction time is 0.5 hours. A solid electrolyte is then obtained.
[0121] Example 9
[0122] The preparation method of the solid electrolyte in this embodiment is basically the same as that in Example 1, except that in step S1, the hydrophobic functional group precursor and the lithium-ion functional group precursor are mixed at a molar ratio of 0.1:1 to obtain the solid electrolyte.
[0123] Example 10
[0124] The preparation method of the solid electrolyte in this embodiment is basically the same as that in Example 1, except that in step S1, the hydrophobic functional group precursor and the lithium-ion functional group precursor are mixed in a molar ratio of 6:1 to obtain the solid electrolyte.
[0125] Comparative Example 1
[0126] The preparation method of the solid electrolyte in this comparative example is basically the same as that in Example 1, except that: no lithium-ion functional group precursor is added in step S1, and 0.2g of hydrophobic functional group precursor is weighed to obtain the solid electrolyte.
[0127] Comparative Example 2
[0128] The preparation method of the solid electrolyte in this comparative example is basically the same as that in Example 1, except that: no hydrophobic functional group precursor is added in step S1, and 0.2g of lithium-ion functional group precursor is weighed to obtain the solid electrolyte.
[0129] Comparative Example 3
[0130] The solid electrolyte in this comparative example is Li3InCl6.
[0131] Comparative Example 4
[0132] The solid electrolyte in this comparative example is Li6PS5Cl.
[0133] The solid electrolytes prepared in the above embodiments and comparative examples were subjected to ionic conductivity tests, air stability tests, coating layer thickness tests, and contact angle tests. The test results are shown in Table 1.
[0134] Test method:
[0135] 1. Ionic conductivity testing method
[0136] The ionic conductivity of the solid electrolyte was tested using the electrochemical impedance spectroscopy (EIS): 150 mg of the solid electrolyte powder to be tested was weighed in a glove box with water and oxygen content both less than 1 ppm at room temperature. The powder was placed in an insulating mold with an inner diameter of 10 mm and pressed into an electrolyte sheet under a pressure of 300 MPa for 60 s. The thickness L of the sheet was measured. Carbon-coated aluminum foil was attached to both sides of the electrolyte sheet as ion blocking electrodes. The pressure was then increased again to 300 MPa to assemble a test cell. The electrochemical impedance spectroscopy was collected at 25℃±3℃ using an electrochemical workstation with a test frequency of 10 MHz and an AC perturbation amplitude of 10 mV. The electrolyte impedance R was obtained by fitting the impedance spectrum and calculated using the formula: Ionic conductivity = L / (R×S), where S is the electrode contact area.
[0137] 2. Air stability test method
[0138] All operations before tableting were performed in a glove box with water and oxygen content both less than 1 ppm. 300 mg of each solid electrolyte powder was weighed and placed in a mold with an inner diameter of 10 mm. The mixture was pressed into electrolyte sheets at 300 MPa for 60 seconds, and the thickness was measured. The sheets were then laid flat in a petri dish and exposed for 2 hours at a dew point of -20°C with a dew point fluctuation ≤3°C. After exposure, carbon-coated aluminum foil was attached to both sides of the solid electrolyte sheets as ion-blocking electrodes, and the sheets were again pressurized to 300 MPa to assemble the test cells. The ionic conductivity of each solid electrolyte after 2 hours of exposure at -20°C dew point was measured using AC impedance spectroscopy at 25°C ± 3°C. The ionic conductivity testing conditions and data processing methods were consistent with the aforementioned ionic conductivity testing method. The air stability of the solid electrolytes was characterized by comparing their ionic conductivity with that of the modified solid electrolyte. The assembly and testing of the halide electrolyte samples were performed in a glove box with water and oxygen content less than 1 ppm or using a sealed mold.
[0139] 3. Ionic conductivity retention rate
[0140] The retention rate of ionic conductivity of the modified solid electrolyte = ionic conductivity after exposure to dew point at -20℃ for 2 hours / ionic conductivity of the modified solid electrolyte.
[0141] The retention rate of ionic conductivity of the unmodified solid electrolyte in the comparative example = ionic conductivity after exposure to dew point at -20℃ for 2 hours / initial ionic conductivity of the solid electrolyte.
[0142] 4. Contact Angle Test Method
[0143] The static water contact angle test method was used to quantitatively evaluate the changes in the hydrophobic properties of solid electrolyte surfaces before and after modification. Before testing, 150 mg of unmodified and modified solid electrolyte powder were taken and pressed into dense, crack-free electrolyte sheets using a 10 mm standard mold under 2T pressure for 60 s in an inert atmosphere glove box with water and oxygen contents both <0.1 ppm. The entire sample preparation and transfer process was sealed to prevent moisture absorption and deterioration. A high-precision contact angle meter and a micro-syringe were used for the test. Ultrapure water with a resistivity of 18.2 MΩ·cm was selected as the test solution, and the droplet volume was controlled at 5 μL. The droplet was slowly released from a distance of 3 mm from the sample surface, and images were acquired after the droplet stabilized for 3 s. The static water contact angle was calculated using ellipse fitting or Young-Laplace fitting. Each sample was tested at least three times at different locations, and the arithmetic mean was taken. Unmodified halide solid electrolytes react rapidly with water, causing droplets to spread and wet instantly, failing to form stable droplets; their contact angle is defined as 0°. Modified electrolytes, with a hydrophobic modification layer constructed on their surface, exhibit a significantly improved contact angle. The difference in contact angle before and after modification quantitatively verifies the effectiveness of the hydrophobic modification layer and the degree of improvement in hydrophobic performance. The entire testing process is conducted in an ultra-low dew point dry environment or glove box, with uniform sample preparation pressure to eliminate interference from surface roughness and structural differences in the test results.
[0144] 4. Thickness testing method
[0145] The surface of solid electrolyte particles was observed using high-resolution transmission electron microscopy (HRTEM).
[0146] Table 1. Performance test results of solid electrolytes in the examples and comparative examples.
[0147]
[0148] As can be seen from Examples 1 and 5 in Table 1, in Example 5, when the amount of hydrophobic functional group precursor and lithium-ion functional group precursor added is small, although the modified solid electrolyte has excellent ionic conductivity, its ionic conductivity decreases significantly after exposure to the -20℃ dew point for 2 hours. As can be seen from Examples 1 and 6, in Example 6, when the amount of hydrophobic functional group precursor and lithium-ion functional group precursor added is large, although the ionic conductivity of the modified solid electrolyte does not decrease significantly after exposure to the -20℃ dew point for 2 hours, its modified ionic conductivity decreases. Therefore, it is necessary to control the local concentration of hydrophobic functional group precursor and lithium-ion functional group precursor on the surface of the solid electrolyte matrix, so as to accurately control the anchoring amount of hydrophobic functional group precursor and lithium-ion functional group precursor and the thickness of polysiloxane graft layer, thereby simultaneously improving the air stability and ionic conductivity of the solid electrolyte.
[0149] As can be seen from the embodiments of this application and Comparative Example 1, after adding the hydrophobic functional group precursor, the ionic conductivity of the electrolyte changes little after exposure to the -20°C dew point for 2 hours. However, Comparative Example 1, which did not add the lithium-ion functional group precursor, has poor ionic conductivity after modification. This indicates that adding only the hydrophobic functional group precursor can only improve the air stability of the solid electrolyte but has an inhibitory effect on the ionic conductivity.
[0150] As can be seen from the embodiments of this application and Comparative Example 2, the ionic conductivity after modification is not significantly changed by only adding a lithium-ion functional group precursor. However, compared with the embodiment, the ionic conductivity of Comparative Example 2, which did not add a hydrophobic functional group precursor, dropped sharply after being exposed to a dew point of -20°C for 2 hours. This indicates that although adding only a lithium-ion functional group precursor can maintain excellent ionic conductivity, its poor hydrophobicity will result in poor air stability of the solid electrolyte.
[0151] As can be seen from the embodiments of this application, Comparative Example 3 and Comparative Example 4, the ionic conductivity of the unmodified solid electrolyte drops sharply after exposure to a dew point of -20°C for 2 hours. It can also be seen that the modified solid electrolyte of this invention has excellent air stability while maintaining excellent ionic conductivity.
[0152] Finally, it should be noted that other embodiments of the invention will readily occur to those skilled in the art upon consideration of the specification and practice of the invention disclosed herein. This invention is intended to cover any variations, uses, or adaptations of the invention that follow the general principles of the invention and include common knowledge or customary techniques in the art not disclosed herein, and is not limited to the precise structures described above, and various modifications and changes can be made without departing from its scope. The scope of the invention is limited only by the appended claims.
Claims
1. A solid electrolyte, characterized in that, It includes a solid electrolyte matrix and a polysiloxane graft layer located on at least a portion of the surface of the solid electrolyte matrix, wherein the solid electrolyte matrix and the polysiloxane graft layer are interconnected by -MO-Si-, and M includes at least one of a metal element and P; The polysiloxane graft layer includes hydrophobic functional groups and lithium-ion conductive functional groups; the solid electrolyte matrix includes a halide solid electrolyte and / or a sulfide solid electrolyte. The hydrophobic functional group is derived from a hydrophobic functional group precursor, which includes at least one of 1H,1H,2H,2H-perfluorooctyltrimethoxysilane, 1H,1H,2H,2H-perfluorodecyltriethoxysilane, n-octyltrimethoxysilane, n-dodecyltrimethoxysilane, and n-octadecyltrimethoxysilane. The lithium-ion-conducting functional group is derived from a lithium-ion-conducting functional group precursor, which includes at least one of 2-[methoxy(polyethoxy)6-9propyl]trimethoxysilane, succinate-functionalized silane, and cyclic carbonate-functionalized silane.
2. The solid electrolyte according to claim 1, characterized in that, The polysiloxane grafted layer includes a -Si-O-Si- main chain, in which carbon atoms in the hydrophobic functional groups are connected to silicon atoms on the -Si-O-Si- main chain, and in which carbon atoms in the lithium-ion-conducting functional groups are connected to silicon atoms on the -Si-O-Si- main chain.
3. The solid electrolyte according to claim 1, characterized in that, The chemical formula of the halide solid electrolyte includes Li a M'D x Wherein, 1≤a≤3, 4≤x≤6, M' includes at least one of In, Zr, Y, Sc, Er, Yb, and Ho, and D includes at least one of F, Cl, Br, and I; And / or, the chemical formula of the sulfide solid electrolyte includes Li 6-y PS 5-y A 1+y A includes at least one of Cl, Br, I, and F, and 0 ≤ y < 1.
4. The solid electrolyte according to claim 1, characterized in that, The thickness of the polysiloxane graft layer is 3-16 nm.
5. The solid electrolyte according to any one of claims 1-4, characterized in that, The solid electrolyte is prepared by a method comprising the following steps: In an inert atmosphere, a solid electrolyte matrix, a hydrophobic functional group precursor, and a lithium-ion functional group precursor are dispersed in a nonpolar solvent and stirred to react. The solid electrolyte is obtained by washing with the nonpolar solvent and vacuum drying, wherein the water content in the nonpolar solvent is less than 20 ppm by mass.
6. A method for preparing a solid electrolyte according to any one of claims 1-5, characterized in that, include: In an inert atmosphere, a solid electrolyte matrix, a hydrophobic functional group precursor, and a lithium-ion functional group precursor are dispersed in a nonpolar solvent and stirred to react. The solid electrolyte is obtained by washing with a nonpolar solvent and vacuum drying, wherein the water content in the nonpolar solvent is less than 20 ppm by mass. The hydrophobic functional group precursor includes at least one of 1H,1H,2H,2H-perfluorooctyltrimethoxysilane, 1H,1H,2H,2H-perfluorodecyltriethoxysilane, n-octyltrimethoxysilane, n-dodecyltrimethoxysilane, and n-octadecyltrimethoxysilane. The lithium-ion functional group precursor includes at least one of 2-[methoxy(polyethoxy)6-9propyl]trimethoxysilane, succinate-functionalized silane, and cyclic carbonate-functionalized silane.
7. The preparation method according to claim 6, characterized in that, The specific steps of dispersing the solid electrolyte matrix, the hydrophobic functional group precursor, and the lithium-ion functional group precursor in a nonpolar solvent include: first, dispersing the hydrophobic functional group precursor and the lithium-ion functional group precursor in a nonpolar solvent, mixing them to form a precursor solution, and then adding the solid electrolyte matrix to the precursor solution under stirring to form a suspension.
8. The preparation method according to claim 7, characterized in that, The temperature of the stirring reaction is 45℃-60℃, and the stirring reaction time is 0.5-4h.
9. The preparation method according to claim 7, characterized in that, The molar ratio of the hydrophobic functional group precursor to the lithium-ion functional group precursor is (0.5-5):1; And / or, the total mass fraction of the hydrophobic functional group precursor and the lithium-ion functional group precursor in the precursor solution is 0.1-1%; And / or, the solid content of the suspension is 1.96%-10%.
10. The preparation method according to any one of claims 7-8, characterized in that, The washing is performed 3-5 times; And / or, the vacuum drying temperature is 60-120℃, and the vacuum drying time is 2-6h.
11. A positive electrode plate, characterized in that, The positive electrode comprises a solid electrolyte according to any one of claims 1-5.
12. A battery, characterized in that, The battery includes the positive electrode according to claim 11.