A high-entropy halide solid electrolyte, its preparation method and application

By constructing a high-entropy halide solid electrolyte using a high-entropy strategy, the problems of ion transport and interfacial stability in halide electrolytes were solved, achieving high ionic conductivity and a wide electrochemical stability window, thereby improving the cycle stability and safety of the battery.

CN123120842APending Publication Date: 2026-11-17CHINA ELECTRONIC TECH GRP CORP NO 18 RES INST
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611131987.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-07-29
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing halide solid electrolytes have low room temperature ionic conductivity, which makes it difficult to meet the ion transport requirements under high-rate conditions. They are easily reduced by lithium metal anodes, leading to an increase in interface impedance. They are also sensitive to environmental humidity, affecting storage and battery assembly.

Method used

A high-entropy halide solid electrolyte was prepared by constructing a stable framework with indium and yttrium, introducing moderate lattice distortion with erbium, and enhancing electrochemical stability with hafnium and zirconium. The synergistic effect of the components was optimized by mechanochemical treatment and thermal treatment, resulting in high ionic conductivity, a wide electrochemical stability window, and excellent structural stability.

Benefits of technology

It significantly improves room temperature ionic conductivity, broadens the electrochemical stability window, improves interfacial compatibility with lithium metal anodes, and enhances the cycle stability and safety of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123120842A_ABST
    Figure CN123120842A_ABST
Patent Text Reader

Abstract

This invention provides a high-entropy halide solid electrolyte, its preparation method, and its application. The general chemical formula of the electrolyte is Li. 3− x In a Y b Er c Hf d Zr e Cl6, where: 0 < x ≤ 0.5, a + b + c + d + e = 1, 0
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of electrochemical energy storage technology, and in particular to a high-entropy halide solid electrolyte, its preparation method, and its application. Background Technology

[0002] In recent years, the rapid development of the new energy vehicle industry has placed higher demands on the energy density and safety of electrochemical energy storage devices. Traditional lithium-ion batteries use organic liquid electrolytes, which have inherent defects such as flammability, leakage, and a narrow electrochemical stability window, making it difficult to meet the needs of next-generation high-energy-density power batteries. Against this backdrop, all-solid-state batteries (ASSBs), which use non-flammable inorganic solid electrolytes to replace traditional organic electrolytes, are considered an important technological path to achieve next-generation high-energy-density energy storage systems because they can fundamentally solve the aforementioned safety problems and are compatible with high-voltage cathode materials and lithium metal anodes.

[0003] Among numerous solid-state electrolyte systems, halide solid-state electrolytes (such as Li3InCl6 and Li3YCl6) have attracted much attention due to their excellent oxidation stability against high-voltage cathode materials (such as high-nickel ternary cathodes), good deformability (densification can be achieved through cold pressing), and considerable ionic conductivity. However, the overall performance of these materials is still far from meeting the requirements for practical application: their room-temperature ionic conductivity is typically about an order of magnitude lower than that of sulfide electrolytes, making it difficult to meet the ion transport requirements under high-rate operating conditions; they are easily reduced when in contact with lithium metal anodes, leading to a continuous increase in interfacial impedance, which severely restricts the cycle life of the battery; some halide systems are highly sensitive to environmental humidity and are prone to hygroscopic hydrolysis, bringing additional processing burdens to the storage, transportation, and battery assembly of the materials.

[0004] Addressing the performance bottlenecks of halide solid electrolytes, the high-entropy strategy, with its unique structural control advantages, has become a highly promising modification direction in materials science in recent years. This strategy introduces multiple principal cations, utilizing the high configurational entropy effect to stabilize the crystal framework while inducing significant lattice distortion. This not only promises to reduce the lithium-ion migration barrier and improve room-temperature ionic conductivity but also effectively broadens the electrochemical stability window, providing a new approach to solving the rate capability, interface, and stability challenges of existing halide electrolytes.

[0005] However, research on high-entropy modification in the field of halide electrolytes is still in its early exploratory stage: on the one hand, the selection of elements for multiple cations lacks systematic theoretical guidance, and the ratio design is largely blind; on the other hand, traditional doping processes are difficult to adapt to high-entropy systems, and are prone to causing impurity phase precipitation or disrupting lattice continuity, which in turn leads to a decrease in ionic conductivity instead of an increase. Summary of the Invention

[0006] The purpose of this invention is to provide a high-entropy halide solid electrolyte, its preparation method, and its application, so as to solve the problems in the background art.

[0007] The technical solution adopted in this invention is: a high-entropy halide solid electrolyte, wherein the general chemical formula of the electrolyte is Li. 3−x In a Y b Er c Hf d Zr e Cl6, where: 0 < x ≤ 0.5, a + b + c + d + e = 1, 0 <b+c+d+e≤0.5。

[0008] Furthermore, 0.2≤x≤5, 0<b+c+d+e≤0.3.

[0009] Furthermore, the configurational entropy of the electrolyte is ≥2R, where R is an ideal gas state function.

[0010] The technical solution of the present invention also includes: a method for preparing the above-mentioned high-entropy halide solid electrolyte, which includes the following steps:

[0011] According to the stoichiometric ratio of high-entropy halide solid electrolytes, raw materials containing lithium, indium, yttrium, erbium, hafnium, and zirconium are taken and subjected to mechanochemical treatment to obtain precursor powder;

[0012] The precursor powder was heat-treated to obtain a sintered product;

[0013] The sintered product is subjected to crushing and dispersion treatment to obtain the high-entropy halide solid electrolyte.

[0014] Furthermore, the mechanochemical treatment involves pulverizing and mixing the raw material using zirconium oxide grinding balls with a diameter of 5mm to 10mm, and the mass ratio of the zirconium oxide grinding balls to the raw material being (20 to 30): 1.

[0015] Furthermore, the zirconium oxide grinding balls are used to pulverize and mix the raw materials at a speed of 300~550 rpm for 25h~45h.

[0016] Furthermore, the heating rate of the heat treatment is 1℃ / min to 5℃ / min, the heat treatment temperature is 200℃ to 550℃, and the holding time is 3h to 7h.

[0017] Furthermore, the handling of the raw materials and the heat treatment are carried out in an inert atmosphere, which is an argon atmosphere.

[0018] Furthermore, the raw materials include LiCl, InCl3, YCl3, ErCl3, HfCl4, and ZrCl4.

[0019] The technical solution of the present invention also includes: the application of the above-mentioned high-entropy halide solid electrolyte in all-solid-state lithium batteries.

[0020] The beneficial effects of this invention are as follows: through a high-entropy strategy of multi-cation synergistic doping, namely, using indium and yttrium to construct a stable framework, erbium to introduce appropriate lattice distortion to optimize ion transport, and hafnium and zirconium to ensure electrochemical stability and moisture resistance, the components complement each other in multiple dimensions such as structural stability, ion conductivity and electrochemical stability, and together construct a high-entropy halide solid electrolyte with high ionic conductivity, wide electrochemical stability window and excellent structural stability. Attached Figure Description

[0021] Appendix Figure 1 These are SEM images of the electrolytes obtained in Example 1 and Comparative Example 1 of this invention;

[0022] Appendix Figure 2 These are the AC impedance spectra of the electrolytes obtained in Example 1 and Comparative Example 1 of the present invention;

[0023] Appendix Figure 3 The results are the cycle performance test results of the all-solid-state mold battery assembled using the electrolytes obtained in Example 1 and Comparative Example 1 of this invention at a rate of 0.1C.

[0024] Appendix Figure 4 The results are the cycle performance test results of the all-solid-state mold battery assembled using the electrolytes obtained in Example 1 and Comparative Example 1 of this invention at a rate of 0.1C. Detailed Implementation

[0025] To better illustrate the objectives, complete technical approach, and advantages of this invention, the following detailed description will be provided in conjunction with specific embodiments. However, the embodiments described below are only a part of the embodiments of this invention and do not include all embodiments. Other embodiments that can be obtained by those skilled in the art without creative effort based on the embodiments of this invention are all within the protection scope of this invention.

[0026] In the embodiments described below, unless otherwise specified, the conventional methods used are all technical means recognized or commonly used by those skilled in the art, and the instruments, reagents, consumables, etc. used in the embodiments of the present invention can be obtained through legitimate commercial channels.

[0027] This invention provides a high-entropy halide solid electrolyte with the general chemical formula Li. 3−x In a Yb Er c Hf d Zr e Cl₆, where: 0<x≤0.5, a+b+c+d+e=1, 0<b+c+d+e≤0.5. Under the framework of this general chemical formula, the constituent elements are synergistically configured according to their respective structural and electrochemical functions, jointly constructing the complete performance system of the electrolyte.

[0028] Specifically: indium and yttrium form the main lattice structure of the electrolyte, and the ionic radii of the two are similar (Y 3+ is about 0.90Å, In 3+ is about 0.80Å), which enables yttrium to introduce configurational entropy to improve structural stability while maintaining the structural integrity of the halide host lattice; meanwhile, as a light rare earth element with relatively abundant reserves, the introduction of yttrium is conducive to reducing the dependence of the material system on a single scattered element (indium), and improves the industrial accessibility of the electrolyte and the process compatibility of large-scale preparation.

[0029] Erbium is introduced as a lattice strain regulating component, and its ionic radius (Er 3+ is about 0.890Å) is between In 3+ and Y 3+ , which can introduce moderate lattice distortion on the premise of not damaging the structural stability of the halide host lattice, is conducive to widening the lithium ion transmission channel and reducing the migration energy barrier, thereby improving the ionic conductivity. Moreover, compared with lanthanide elements with large radii such as La or Nd, Er³⁺ has a milder disturbance to the structure of the halide host lattice, which is conducive to maintaining structural integrity while introducing lattice distortion. In addition, different from lanthanide elements with multiple valence states such as Ce or Tb, Er exists stably only in the +3 valence state in the chloride system, which can effectively avoid the increase of electronic conductivity and interfacial side reactions caused by valence change.

[0030] At the same time, hafnium and zirconium are introduced into the system as electrochemical stabilizers. Both of them exist in the high +4 valence state, which can enhance the covalency of metal-chlorine bonds, significantly improve the oxidation and reduction stability of the electrolyte, thereby broadening the electrochemical stability window and improving the interfacial compatibility with cathode and anode materials; meanwhile, Hf 4+ and Zr 4+ The high charge density of exerts a strong electrostatic constraint on Cl - , which can fundamentally weaken the displacement ability of water molecules to chloride ions, thereby improving the structural integrity and electrochemical stability of the electrolyte in a humid environment.

[0031] Furthermore, erbium has different electronegativity and electronic configurations from hafnium and zirconium. Their synergistic effect changes the electron cloud density distribution around chlorine atoms, increasing the overlap of electron clouds between the metal and chlorine. This helps to regulate the covalent nature of the metal-chlorine bond, thereby improving the reduction stability of the electrolyte for lithium metal anodes. Hafnium and zirconium have highly similar chemical properties (and similar ionic radii), and their synergistic introduction can further enhance the high valence state stabilization effect, which is better than the individual doping of a single component.

[0032] In summary, this invention employs a high-entropy strategy of multi-cation synergistic doping, namely, using indium and yttrium to construct a stable framework, erbium to introduce appropriate lattice distortion to optimize ion transport, and hafnium and zirconium to ensure electrochemical stability and moisture resistance. The components complement each other in multiple dimensions such as structural stability, ion conductivity, and electrochemical stability, jointly constructing a high-entropy halide solid electrolyte with high ionic conductivity, a wide electrochemical stability window, and excellent structural stability.

[0033] Through systematic research and exploration, this invention has determined the preferred composition range of this high-entropy halide solid electrolyte: 0.2 ≤ x ≤ 5, 0 < b + c + d + e ≤ 0.3. Specifically, when the chemical formula of the electrolyte is Li... 2.8 In 0.7 Y 0.05 Er 0.05 Hf 0.1 Zr 0.1 In the Cl6 configuration, the corresponding lithium-ion vacancy concentration is 0.2, the total doping amount of multi-component cations is 0.3, and the configurational entropy of the system is 2.02R (>1.5R), where R is the ideal gas state function. Under this composition, the high valence state effect of hafnium and zirconium, and the size mismatch effect of yttrium and erbium, work synergistically to maintain the stability of the InCl6 bulk lattice structure while jointly constructing a high-entropy lattice distortion and charge compensation mechanism. This achieves an optimal balance among the three key performance indicators: ionic conductivity, electrochemical stability window, and interfacial stability.

[0034] The structural advantages resulting from the aforementioned compositional optimization are directly reflected in the comprehensive improvement of electrochemical performance. The electrolyte exhibits a room-temperature ionic conductivity of 1.48 mS / cm, a significantly broadened electrochemical stability window, markedly enhanced thermodynamic stability, and significantly improved interfacial compatibility with the lithium metal anode. The all-solid-state battery assembled based on this electrolyte maintains a capacity retention of 88.1% after 200 cycles at 0.2C, demonstrating excellent cycle stability. This fully demonstrates that the high-entropy halide solid-state electrolyte provided by this invention has promising application prospects in energy storage systems that combine high energy density and high safety.

[0035] Another aspect of the present invention provides a method for preparing the above-mentioned high-entropy halide solid electrolyte, which specifically includes the following steps:

[0036] S1. Raw materials containing lithium, indium, yttrium, erbium, hafnium, and zirconium are taken according to the stoichiometric ratio of high-entropy halide solid electrolytes and subjected to mechanochemical treatment to obtain precursor powder.

[0037] In this step, the raw materials are the chlorides of each metal element, specifically LiCl, InCl3, YCl3, ErCl3, HfCl4, and ZrCl4. The weighing of the raw materials should be carried out in an inert atmosphere, which is an argon atmosphere.

[0038] In this step, the preferred mechanical chemical treatment is to use zirconium oxide grinding balls to pulverize and mix the raw materials, with the zirconium oxide being ZrO2.

[0039] After the raw materials are weighed, they are first placed in a mortar and manually ground for 20 minutes. Then, the zirconium oxide grinding balls and the manually ground raw materials are transferred together to a ball mill jar and sealed (this operation should also be carried out in an inert atmosphere). When performing mechanochemical treatment: the diameter of the zirconium oxide grinding balls is preferably 5mm~10mm, and the mass ratio of zirconium oxide grinding balls to raw materials is preferably (20~30):1.

[0040] The selection of the above-mentioned ball milling parameters plays a crucial role in obtaining high-performance products: the optimal range of the mass ratio of zirconium oxide grinding balls to raw materials can provide the best mechanical energy input required to drive the solid-state reaction, which is key to achieving lattice distortion, atomic interdiffusion, and the formation of high-entropy solid solutions; too low energy will lead to incomplete reaction, while too high energy may introduce impurity phases; the combination of zirconium oxide grinding ball sizes of 5mm to 10mm takes into account the strong impact and crushing effect of large balls on raw material agglomerates and the fine grinding and uniform mixing effect of small balls on raw material powder. The two work together to ensure that the raw materials can achieve a highly uniform mixing and activation state at both the macroscopic and microscopic scales, laying the foundation for obtaining high-entropy solid solution products with pure phases and high crystallinity in subsequent heat treatment steps.

[0041] The preferred ball milling speed for pulverizing and mixing the raw materials using zirconium oxide grinding balls is 300~550 rpm, and the preferred time is 25h~45h. This parameter range is determined based on a systematic consideration of the mechanochemical energy input threshold: under these conditions, the ball milling process can provide the mechanical energy input required to drive the atomic-level uniform interdiffusion of multiple cations (Y, Er, Hf, Zr) in the InCl6 lattice and induce appropriate lattice distortion. Simultaneously, the aforementioned speed and time range effectively avoids problems such as localized overheating, uncontrollable phase transitions, and impurity introduction caused by excessively high speeds or excessively long milling times, ensuring that the obtained precursor powder is in a suitable amorphous or microcrystalline mixed state, providing a uniform and highly active reaction precursor for the formation of high-entropy solid solutions in subsequent heat treatment steps.

[0042] S2. The precursor powder is heat-treated to obtain a sintered product.

[0043] In this step, the precursor powder is transferred to a quartz tube, sealed, and placed in a muffle furnace. It is then heated to a set temperature at a certain heating rate in an inert atmosphere and held at that temperature for sintering.

[0044] Preferably, the inert atmosphere is argon; the heating rate of the heat treatment is 1℃ / min to 5℃ / min, the heat treatment temperature is 200℃ to 550℃, and the holding time is 3h to 7h. The determination of this parameter range is based on a "mild crystallization" strategy specifically developed for the multi-element doped high-entropy system of this invention; slow heating can effectively eliminate the internal stress introduced by ball milling and avoid local thermal runaway caused by excessively rapid heating; while the specific medium-low temperature sintering window can effectively avoid the risks of halogen volatilization and impurity phase formation under high temperature conditions, while promoting the full crystallization of the high-entropy solid solution and eliminating grain boundary defects.

[0045] The parameters in the above process steps have a good synergistic matching relationship. This synergistic effect constructs a low-energy-barrier lithium-ion transport channel at the micro level and endows the material with extremely high phase purity at the macro level, thereby achieving a simultaneous leap in ionic conductivity and electrochemical stability. The obtained technical effect is significantly better than that of conventional process parameters.

[0046] S3. The sintered product is crushed and dispersed to obtain a high-entropy halide solid electrolyte with a suitable particle size distribution.

[0047] Another aspect of the present invention provides the application of the above-mentioned high-entropy halide solid electrolyte in all-solid-state lithium batteries.

[0048] The following are specific embodiments and comparative examples of the present invention.

[0049] Example 1

[0050] (1) Weigh 1.1869g LiCl, 1.5483g InCl3, 0.0976g YCl3, 0.1368g ErCl3, 0.3203g HfCl4 and 0.233g ZrCl4 powder into a mortar and grind manually for 20 minutes. Then pour the powder into a ball mill jar containing ZrO2 grinding balls. The ratio of the mass of ZrO2 grinding balls to the total mass of the raw material powder is 20:1. After sealing the ball mill jar, ball milling is performed.

[0051] After ball milling at 200 rpm for 30 min, the speed was increased to 500 rpm and ball milled for 42 h to obtain precursor powder.

[0052] (2) After transferring the precursor powder into a quartz tube and sealing it, place it in a muffle furnace and heat it to 260°C at a heating rate of 2°C / min, and sinter it at this temperature for 5 hours.

[0053] (3) After sintering is completed and the temperature is lowered, the sintered product is ground and dispersed to obtain the high-entropy halide solid electrolyte Li. 2.8 In 0.7 Y 0.05 Er 0.05 Hf 0.1 Zr 0.1 Cl6.

[0054] Comparative Example 1

[0055] (1) Weigh 1.2717g LiCl and 2.2118g InCl3 powder and pour them into a mortar. Grind manually for 20 minutes and then pour them into a ball mill jar containing ZrO2 grinding balls. The ratio of the mass of ZrO2 grinding balls to the total mass of the raw material powder is 20:1. After sealing the ball mill jar, ball milling is performed.

[0056] After ball milling at 200 rpm for 30 min, the speed was increased to 500 rpm and ball milled for another 30 h to obtain precursor powder.

[0057] (2) After transferring the precursor powder into a quartz tube and sealing it, place it in a muffle furnace and heat it to 260°C at a heating rate of 2°C / min, and sinter it at this temperature for 5 hours.

[0058] (3) After sintering is completed and the temperature is lowered, the sintered product is ground and dispersed to obtain the unmodified halide solid electrolyte Li3InCl6.

[0059] Characterization and Testing

[0060] (1) The electrolyte powders obtained in Example 1 and Comparative Example 1 were pressed into tablets, and the microstructure of the electrolyte tablets and electrolyte powders obtained in Example 1 and Comparative Example 1 was characterized by scanning electron microscopy (SEM). The characterization results are shown in Appendix 1. Figure 1 . Figure 1 In the image: (a) and (b) are SEM images of the surface of the electrolyte sheet obtained in Example 1, (c) is an SEM image of the electrolyte powder obtained in Example 1, (d) and (e) are SEM images of the surface of the electrolyte sheet obtained in Comparative Example 1, and (f) is an SEM image of the electrolyte powder obtained in Comparative Example 1.

[0061] The tableting method is as follows: place the electrolyte powder in a mold with a diameter of 10 mm, place the mold on the worktable of the powder tableting machine, apply a pressure of about 3t to the mold, hold for 3 minutes, and then remove the pressed electrolyte tablet from the mold to obtain the desired electrolyte tablet.

[0062] From the appendix Figure 1 It can be seen that, in terms of surface morphology, both the electrolyte sheets obtained in Example 1 and Comparative Example 1 exhibit certain microscopic undulations, but the electrolyte sheet obtained in Example 1 is more dense and uniform than that obtained in Comparative Example 1. Regarding powder morphology, the electrolyte powder obtained in Comparative Example 1 exhibits a relatively regular blocky or near-blocky structure, with relatively uniform particle morphology and significant agglomeration, which may lead to localized blockage of lithium-ion conduction channels. In contrast, the electrolyte powder obtained in Example 1 exhibits richer morphological characteristics, with a relatively uniform particle size distribution and a certain degree of porosity or loose structure. This unique morphology provides more favorable conditions for lithium-ion conduction: on the one hand, uniform particle size can reduce path differences during lithium-ion transport; on the other hand, the loose porous structure helps increase the contact area between the electrolyte and the electrode, promoting rapid lithium-ion migration, reducing interfacial impedance, and thus optimizing lithium-ion conduction performance.

[0063] (2) The ionic conductivity of the electrolytes obtained in Example 1 and Comparative Example 1 was tested using an electrochemical workstation. The test results are shown in Appendix. Figure 2 .

[0064] Analysis Appendix Figure 2 It can be seen that the electrolyte obtained in Example 1 has an ionic conductivity of 1.48 mS / cm at 25°C, while the electrolyte obtained in Comparative Example 1 has an ionic conductivity of 0.96 mS / cm at 25°C.

[0065] (3) The electrolytes obtained in Example 1 and Comparative Example 1 were assembled into all-solid-state mold batteries, and their electrochemical performance was tested.

[0066] The battery assembly method is as follows: Approximately 60 mg of the halide solid electrolyte powder prepared in Example 1 is placed into a mold with a diameter of 10 mm and pressed for 2 min under a pressure of approximately 2.5 t. Then, approximately 60 mg of sulfide solid electrolyte powder (Li6PS5Cl composition) is spread on top and pressed again for 2 min under a pressure of approximately 2.7 t to obtain a bilayer composite electrolyte sheet. Commercial NCM83 (LiNi) is weighed according to a weight ratio of 70:30:3. 0.83 Co 0.12 Mn 0.05O2), the halide solid electrolyte powder prepared in Example 1, and vapor-grown carbon fiber were transferred to a mortar and manually ground for 20 minutes to ensure uniform mixing, thus obtaining the positive electrode composite material. Approximately 4 mg of the positive electrode composite material was evenly spread on the halide solid electrolyte side of the bilayer composite electrolyte sheet and pressed under 3t pressure for 3 minutes. Subsequently, an indium foil with a diameter of 10 mm and a thickness of 10 μm and a lithium foil with a diameter of 10 mm and a thickness of 100 μm were sequentially placed on the sulfide solid electrolyte side of the bilayer composite electrolyte sheet. The halide solid electrolyte of Comparative Example 1 was assembled into a battery using the same method.

[0067] The electrochemical performance testing method is as follows: At room temperature, the fabricated all-solid-state mold battery was charged and discharged at rates of 0.1C and 0.2C, respectively. The test results are shown in the appendix. Figures 3-4 .

[0068] From the appendix Figure 3 It can be seen that the all-solid-state mold battery assembled using the electrolyte prepared in Example 1 of the present invention has an initial discharge specific capacity of 163.9 mAh / g at 0.1C rate, a first-cycle coulombic efficiency of 95.7%, and a specific capacity of 123.3 mAh / g after 200 cycles, with a capacity retention rate of 75.2%. In contrast, the all-solid-state mold battery assembled using the electrolyte prepared in Comparative Example 1 has an initial discharge specific capacity of only 134.8 mAh / g at 0.1C rate, a first-cycle coulombic efficiency of 92.2%, and a discharge specific capacity of only 89.1 mAh / g after 139 cycles, with a capacity retention rate of only 66.1%.

[0069] From the appendix Figure 4 It can be seen that the all-solid-state mold battery assembled using the electrolyte prepared in Example 1 of the present invention has an initial discharge specific capacity of 115.9 mAh / g at 0.2C, an initial coulombic efficiency of 88.1%, and a specific capacity of 102.1 mAh / g after 200 cycles, with a capacity retention rate of 88.1%. In contrast, the LIC-based solid-state battery has an initial discharge specific capacity of only 79.3 mAh / g at 0.2C, an initial coulombic efficiency of 95.5%, and a discharge specific capacity of only 52.7 mAh / g after 123 cycles, with a capacity retention rate of only 66.5%.

[0070] It should be understood that the specific embodiments described above are merely illustrative or explanatory of the principles of the invention and do not constitute a limitation thereof. Therefore, any modifications, equivalent substitutions, improvements, etc., made without departing from the spirit and scope of the invention should be included within the protection scope of the invention. Furthermore, the appended claims are intended to cover all variations and modifications falling within the scope and boundaries of the claims, or equivalent forms of such scope and boundaries.

Claims

1. A high-entropy halide solid electrolyte, characterized in that, The general chemical formula of the electrolyte is Li 3− x In a Y b Er c Hf d Zr e Cl6, where: 0 < x ≤ 0.5, a + b + c + d + e = 1, 0 <b+c+d+e≤0.5。 2. The high-entropy halide solid electrolyte according to claim 1, characterized in that, 0.2≤x≤5, 0<b+c+d+e≤0.

3.

3. The high-entropy halide solid electrolyte according to claim 1 or 2, characterized in that, The configurational entropy of the electrolyte is greater than 1.5R, where R is the state function of an ideal gas.

4. A method for preparing the high-entropy halide solid electrolyte according to any one of claims 1-3, characterized in that, Including the following steps: According to the stoichiometric ratio of high-entropy halide solid electrolytes, raw materials containing lithium, indium, yttrium, erbium, hafnium, and zirconium are taken and subjected to mechanochemical treatment to obtain precursor powder; The precursor powder was heat-treated to obtain a sintered product; The sintered product is subjected to crushing and dispersion treatment to obtain the high-entropy halide solid electrolyte.

5. The method for preparing high-entropy halide solid electrolytes according to claim 4, characterized in that, The mechanochemical treatment involves pulverizing and mixing the raw material using zirconium oxide grinding balls with a diameter of 5mm to 10mm and a mass ratio of zirconium oxide grinding balls to the raw material of (20 to 30):

1.

6. The method for preparing high-entropy halide solid electrolytes according to claim 5, characterized in that, The raw material is pulverized and mixed using the zirconium oxide grinding balls at a speed of 300~550 rpm for 25h~45h.

7. The method for preparing high-entropy halide solid electrolytes according to claim 4, characterized in that, The heating rate of the heat treatment is 1℃ / min to 5℃ / min, the heat treatment temperature is 200℃ to 550℃, and the holding time is 3h to 7h.

8. The method for preparing high-entropy halide solid electrolytes according to claim 4, characterized in that, The raw material handling and heat treatment are carried out in an inert atmosphere, namely an argon atmosphere.

9. The method for preparing high-entropy halide solid electrolytes according to any one of claims 4-8, characterized in that, The raw materials include LiCl, InCl3, YCl3, ErCl3, HfCl4, and ZrCl4.

10. The application of the high-entropy halide solid electrolyte according to any one of claims 1-3 in all-solid-state lithium batteries.