Bifunctional Amorphous Halogen Oxide Solid Electrolytes Synthesized with Water of Crystallization Assist, Methods and Applications
By using a water-based crystallization-assisted synthesis method, a bifunctional amorphous halide oxide solid electrolyte with a long-range disordered and completely amorphous sodium halide oxide network structure was prepared. This solved the problem of insufficient amorphization of sodium-based halide/halide oxide solid electrolytes and realized an all-solid-state sodium-ion battery with high ionic conductivity and high energy density.
Patent Information
- Application Number
- CN202611295509.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-25
- Publication Date
- 2026-11-17
AI Technical Summary
The insufficient amorphization of existing sodium-based halide/halogen oxide solid electrolytes results in low ionic conductivity. Traditional solid electrolytes do not contribute capacity in composite cathodes, limiting the energy density of all-solid-state sodium-ion batteries.
A bifunctional amorphous halide oxide solid electrolyte was prepared by using a water-of-crystallization-assisted synthesis method with sodium carbonate containing water of crystallization and variable-valence metal chlorides as raw materials. Through mechanochemical treatment, a long-range disordered and completely amorphous sodium halide oxide network structure was formed, and variable-valence metal elements were introduced into it to form redox active sites.
It significantly improves room temperature ionic conductivity, reduces residual crystalline impurities, enhances battery energy density and cycle stability, reduces multiple solid-solid interface side reactions, and simplifies the all-solid-state battery structure.
Smart Images

Figure CN123120843A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of solid electrolyte technology, specifically relating to a bifunctional amorphous halide oxide solid electrolyte synthesized with the aid of water of crystallization, its method, and its application. Background Technology
[0002] Sodium-ion batteries, due to the abundance, low cost, and wide distribution of sodium resources, are considered a crucial technological route for large-scale energy storage, low-cost energy storage, and next-generation electrochemical energy storage systems. However, traditional sodium-ion batteries typically use organic liquid electrolytes, which pose risks such as flammability, leakage, thermal runaway, and increased interfacial side reactions under high voltage or long-cycle conditions, limiting their further application in high-safety, high-energy-density energy storage systems. Therefore, replacing liquid electrolytes with solid-state electrolytes and constructing all-solid-state sodium-ion batteries is an important development direction for improving intrinsic battery safety, expanding the operating temperature range, and enhancing cycle stability. Solid-state electrolytes are the core functional materials in all-solid-state batteries, and existing solid-state electrolytes mainly include polymer, oxide, sulfide, and halide systems. Polymer electrolytes typically exhibit good processability and flexibility, but their low room-temperature ionic conductivity makes them unsuitable for high-rate batteries. Oxide electrolytes offer good electrochemical and air stability, but often require high-temperature sintering and are brittle with poor interfacial contact. Sulfide electrolytes possess high ionic conductivity and good compactability, but are prone to reacting with moisture and potentially releasing harmful gases; furthermore, their high-voltage stability and interfacial compatibility remain insufficient. In contrast, halide solid-state electrolytes generally combine a wide electrochemical window, good mechanical compactability, and good interfacial compatibility with high-voltage cathodes, thus attracting widespread attention in recent years.
[0003] Halide solid electrolytes typically consist of alkali metal ions, a metal center, and halide anions. Their ion transport behavior is closely related to the anion framework stacking mode, the coordination environment of the metal center, the concentration of alkali metal vacancies, and the degree of local structural disorder. For lithium-based halide systems, numerous studies have shown that they can achieve high room-temperature ionic conductivity and exhibit good application potential on the high-voltage cathode side. However, Na... + Due to their larger radius, diffusion in ordered crystalline halide frameworks is often subject to stronger spatial confinement and higher migration barriers, making it difficult for many sodium-based halide solid electrolytes to meet the room temperature ionic conductivity requirements for practical applications.
[0004] Amorphization is considered an important approach to improve the ion transport capacity of halide solid electrolytes. Compared to long-range ordered crystalline structures, amorphous structures have higher local coordination disorder and a more flexible anionic framework, which can weaken the binding effect between alkali metal ions and surrounding anions to a certain extent, widen ion migration channels, lower ion migration energy barriers, and reduce the adverse effects of grain boundaries on ion transport. Existing research shows that by cation substitution, introduction of anions such as oxygen / nitrogen, multi-anion structure design, or multiphase regulation, local coordination distortion and long-range order disruption can be induced in halide systems, thereby increasing the amorphous phase content and improving ionic conductivity. However, existing modification strategies usually only reduce the crystallinity of the material or partially amorphize it, and may still leave unreacted crystalline precursors or generate new crystalline secondary phases, resulting in discontinuous ion transport paths, inhomogeneous material composition, and limited improvement in conductivity. Secondly, amorphization methods that rely on heterovalent metal doping or the addition of multiphase components usually have a narrow composition window. Excessive introduction of control components may induce the re-precipitation of crystalline phases or local phase separation.
[0005] On the other hand, traditional solid electrolytes are typically designed as electronically insulating and electrochemically inert ion conductors. In all-solid-state battery composite cathodes, a high proportion of solid electrolyte is usually required as the cathode electrolyte to establish a continuous ion transport network. However, this solid electrolyte portion itself does not contribute to capacity; it acts as an inactive component in the electrode, reducing the proportion of active material and limiting the battery's mass energy density and volumetric energy density. Simultaneously, traditional composite cathodes generally consist of multiple components, including cathode active materials, solid electrolytes, and conductive agents, resulting in numerous solid-solid interfaces. Inhomogeneous multiphase contact can easily lead to interfacial side reactions, uneven local current distribution, and continuous impedance growth. To address this issue, recent years have seen the emergence of redox-active solid electrolytes or active halide cathode electrolytes. These designs introduce variable-valence metal centers into the solid electrolyte framework, enabling reversible redox activity while maintaining ion transport capabilities, thereby reducing "dead weight" and increasing the overall capacity contribution of the electrode.
[0006] While active solid-state electrolytes offer a novel approach to addressing the high proportion of inactive components in traditional composite cathodes, current research primarily focuses on crystalline or non-crystalline forms and their application in conjunction with traditional cathode active materials to form composite cathodes. These systems still suffer from complex multi-component solid-solid interfaces and interfacial side reactions. Therefore, there is an urgent need to develop a sodium-based halide oxide solid-state electrolyte that combines high sodium-ion conductivity, a completely amorphous structure, low impurity phase residue, and redox activity. This would enable it not only to function as an ion transport medium but also to participate in electrochemical reactions as a capacity-contributing component. Simultaneously, directly compositing it with a carbon matrix to construct an all-solid-state battery without traditional cathode active materials holds promise for reducing multiple solid-solid interfaces, lowering interfacial impedance and side reactions, and increasing the proportion of effective active components in the electrode. This would provide new material systems and structural design ideas for high-safety, high-energy-density all-solid-state sodium-ion batteries. Summary of the Invention
[0007] The purpose of this invention is to provide a bifunctional amorphous halide oxide solid electrolyte synthesized with crystal water assistance, as well as a method and application, to solve the technical problems of insufficient amorphization of existing sodium-based halide / halogen oxide solid electrolytes leading to low ionic conductivity, and the limitation of energy density caused by the non-contribution of capacity by traditional solid electrolytes in composite cathodes.
[0008] To achieve the above objectives, the present invention employs the following technical solution: This invention discloses a bifunctional amorphous halide oxide solid electrolyte synthesized with the aid of water of crystallization, comprising the following steps: The solid electrolyte is obtained by mechanical and chemical treatment using sodium carbonate containing water of crystallization and variable-valence metal chloride as raw materials. The solid electrolyte contains Na, O, Cl and at least one variable-valence metal element, and exhibits a long-range disordered, completely amorphous network structure. The at least one variable-valence metal element is distributed in the completely amorphous network structure and forms redox active sites, giving the solid electrolyte both ionic conductivity and intrinsic electrochemical activity. The completely amorphous network structure is generated by in-situ structural induction of the water of crystallization in the sodium carbonate containing water of crystallization, and there are no residual crystalline impurities in the solid electrolyte.
[0009] Furthermore, the sodium carbonate containing water of crystallization is at least one of sodium carbonate monohydrate and sodium carbonate decahydrate; the variable valence metal element is at least one of Nb, V and W.
[0010] Furthermore, the variable-valence metal chloride is at least one of niobium pentachloride, vanadium trichloride, and tungsten pentachloride.
[0011] Furthermore, the at least one variable-valence metal element is uniformly dispersed in the fully amorphous network structure and participates in reversible redox reactions during charging and discharging, enabling the solid electrolyte to independently contribute capacity in the all-solid-state battery.
[0012] This invention also discloses a method for synthesizing a bifunctional amorphous halide oxide solid electrolyte with the assistance of water of crystallization, comprising the following steps: Sodium carbonate containing water of crystallization is mixed with a variable-valence metal chloride to obtain a precursor mixture; The precursor mixture is subjected to mechanochemical treatment, which causes the sodium carbonate containing water of crystallization to undergo a mechanochemical reaction and structural reconstruction with the variable valence metal chloride, resulting in a bifunctional amorphous halide oxide solid electrolyte.
[0013] Furthermore, the mechanochemical treatment is a mechanical ball milling treatment; The molar ratio of sodium carbonate containing water of crystallization to variable valence metal chloride is 1:(1~5).
[0014] Furthermore, the ball milling speed of the mechanical ball milling process is 300 rpm to 500 rpm, the ball milling time is 1 h to 12 h, and the ball-to-material ratio is (20 to 60): 1.
[0015] Furthermore, the mechanochemical treatment is carried out under an inert atmosphere or sealed conditions.
[0016] This invention also discloses the application of the above-mentioned bifunctional amorphous halide oxide solid electrolyte synthesized with crystal water assistance in the preparation of all-solid-state sodium-ion batteries, wherein the positive electrode of the all-solid-state sodium-ion battery is prepared by mixing the bifunctional amorphous halide oxide solid electrolyte with a conductive agent. The bifunctional amorphous halide oxide solid electrolyte serves as an active solid electrolyte in the positive electrode, simultaneously providing sodium ion transport channels and contributing to redox capacity.
[0017] Furthermore, the conductive agent includes at least one of conductive carbon black, Super P, acetylene black, Ketjen black, carbon nanotubes, carbon fibers, vapor-grown carbon fibers, graphene, and reduced graphene oxide.
[0018] Compared with the prior art, the present invention has the following beneficial effects: This invention discloses a bifunctional amorphous halide oxide solid electrolyte synthesized with water of crystallization assistance. Using sodium carbonate containing water of crystallization and variable-valence metal chlorides as raw materials, the in-situ structural induction effect of water of crystallization during mechanochemical processing induces coordination reconstruction between Na, O, Cl, and the variable-valence metal elements, effectively reducing the amorphization energy barrier and suppressing the formation of crystalline impurities. This results in a long-range disordered, fully amorphous sodium halide oxide network structure, avoiding the problem of residual crystalline impurities such as Nb₂O₅ due to incomplete solid-phase reactions in traditional anhydrous systems. This ensures the continuity and uniformity of the ion transport path, resulting in an order-of-magnitude increase in room-temperature ionic conductivity compared to anhydrous synthesis systems. Furthermore, the water of crystallization promotes the amorphous structure of the solid electrolyte, exhibiting long-range disorder and short-range order, breaking the periodic lattice constraints of crystalline states and forming a rich, isotropic three-dimensional sodium ion transport network. This effectively reduces the energy barrier for sodium ion migration and significantly improves room-temperature ionic conductivity. Furthermore, the selected metal elements exhibit redox activity, enabling them to participate in electrochemical reactions as capacity-contributing components. This overcomes the drawback of traditional solid-state electrolytes, which only transport ions and do not contribute capacity, thereby improving the energy density of solid-state batteries. Simultaneously, the variable-valence metal elements are uniformly distributed in the amorphous framework and form redox active sites, allowing the resulting solid-state electrolyte to break through the limitation of traditional solid-state electrolytes acting only as inert ion conductors. It possesses both ion conductivity and intrinsic electrochemical activity, enabling it to independently contribute capacity in all-solid-state batteries. This allows it to be directly combined with conductive agents to construct all-solid-state battery cathodes without traditional cathode active materials. This fundamentally eliminates the side reactions and impedance deterioration problems induced by multiple solid-solid interfaces of cathode active materials / solid electrolytes / conductive agents in traditional composite cathodes, increasing the effective proportion of capacity-contributing components in the electrode and improving the energy density and cycle stability of all-solid-state sodium-ion batteries.
[0019] Furthermore, the bifunctional amorphous halide oxide solid electrolyte of this invention can be directly composited with a carbon matrix to construct an all-solid-state battery cathode without traditional cathode active materials. This further reduces multiple solid-solid interfaces and non-capacity-contributing components in the composite cathode, improving ion transport continuity, capacity contribution, and battery energy density. It can also be directly composited with a conductive agent to construct an active cathode, possessing both sodium ion transport and reversible redox capacity contribution functions, without the need for additional matching with traditional cathode materials. This structure reduces the multiple solid-solid interfaces between cathode materials / solid electrolytes / conductive agents in traditional composite cathodes, lowering the risk of poor interface contact and side reaction accumulation, thereby optimizing the electrode structure and ion / electron co-transport pathway of all-solid-state sodium-ion batteries. This active cathode can operate stably within a wide voltage window of 1.4-4.1 V, exhibiting excellent cycle stability and electrochemical performance comparable to existing cathode material systems, simplifying the solid-state battery structure. Attached Figure Description
[0020] Figure 1 The X-ray diffraction pattern of the bifunctional amorphous halide oxide solid electrolyte prepared in Example 2 of this invention; Figure 2 The X-ray diffraction patterns of the solid electrolytes obtained in Example 1 and Comparative Examples 1 and 2 are shown. Figure 3 The results of synchrotron radiation PDF tests on the solid electrolytes obtained in Example 1 and Comparative Examples 1 and 2 are shown. Figure 4 The X-ray diffraction patterns of the bifunctional amorphous halide oxide solid electrolytes obtained in Examples 3 and 4 are shown. Figure 5 The X-ray diffraction pattern of the bifunctional amorphous halide oxide solid electrolyte obtained in Example 5; Figure 6 The results show the ionic conductivity of the solid electrolytes obtained in Example 1 and Comparative Examples 1 and 2. Figure 7 The results of the rate test of the all-solid-state ion battery obtained in Example 1 are shown. Figure 8 The results are for the 0.1C test of the all-solid-state ion battery obtained in Example 1. Figure 9 The results are for the 0.3C test of the all-solid-state ion battery obtained in Example 1. Figure 10 The images show TEM images of the solid electrolyte obtained in Example 1 and the corresponding TEM-EDS elemental distribution test results. Figure 11 The results are the electrochemical stability test results of the solid electrolyte obtained in Example 1; Figure 12 The results show the electrochemical stability of the solid electrolyte obtained in Comparative Example 1. Figure 13 The results show the electrochemical stability test results of the solid electrolyte obtained in Comparative Example 2. Detailed Implementation
[0021] To enable those skilled in the art to understand the features and effects of the present invention, the terms and expressions used in the specification and claims are explained and defined in general below. Unless otherwise specified, all technical and scientific terms used herein have the ordinary meaning understood by those skilled in the art regarding the present invention, and in case of conflict, the definitions in this specification shall prevail.
[0022] The theories or mechanisms described and disclosed herein, whether right or wrong, should not in any way limit the scope of the invention, that is, the contents of the invention can be implemented without being limited by any particular theory or mechanism.
[0023] In this document, all features defined by numerical ranges or percentage ranges, such as numerical values, quantities, contents, and concentrations, are for the sake of brevity and convenience only. Accordingly, descriptions of numerical ranges or percentage ranges should be considered as covering and specifically disclosing all possible sub-ranges and individual numerical values (including integers and fractions) within those ranges.
[0024] In this article, unless otherwise specified, “contains,” “includes,” “containing,” “has,” or similar terms cover the meanings of “composed of” and “mainly composed of,” for example, “A contains a” covers the meanings of “A contains a and others” and “A contains only a.”
[0025] For the sake of brevity, not all possible combinations of the technical features in each implementation scheme or embodiment are described herein. Therefore, as long as there is no contradiction in the combination of these technical features, the technical features in each implementation scheme or embodiment can be combined arbitrarily, and all possible combinations should be considered within the scope of this specification.
[0026] According to a first aspect of the present invention, a bifunctional amorphous halide oxide solid electrolyte synthesized with the aid of water of crystallization is provided. The solid electrolyte is synthesized by high-energy mechanical ball milling using sodium carbonate containing water of crystallization and a variable-valence metal chloride as raw materials, and has a long-range disordered, completely amorphous structure. The solid electrolyte contains Na, O, Cl and at least one variable-valence metal element. The Na and O are derived from sodium carbonate containing water of crystallization, and the Cl and the variable-valence metal element are derived from the variable-valence metal chloride. The water of crystallization in the sodium carbonate containing water of crystallization plays an in-situ structural induction role during the mechanochemical reaction, promoting coordination reconstruction among Na, O, Cl and variable valence metal elements, destroying the long-range ordered crystal structure of the raw materials, and inhibiting the residue of crystalline impurities, thereby forming a completely amorphous sodium halide oxide network structure; the variable valence metal elements are distributed in the completely amorphous sodium halide oxide network structure and form redox active sites, so that the solid electrolyte has both sodium ion conductivity and intrinsic electrochemical activity.
[0027] The aforementioned solid electrolyte is used as an active solid electrolyte in all-solid-state sodium-ion batteries to simultaneously provide sodium ion transport channels and redox capacity contributions.
[0028] Using the above technical solution, sodium carbonate containing water of crystallization can not only provide Na and O sources to the reaction system, but the water of crystallization can also participate in or induce local structural rearrangement during mechanochemical processing, reducing the energy barrier for forming amorphous sodium halide oxide network structures in solid-state reactions, increasing the degree of amorphization, and reducing or avoiding the problem of residual crystalline impurities that easily occur in anhydrous sodium carbonate systems. Variable-valence metal chlorides can simultaneously provide Cl and variable-valence metal elements to the reaction system. After the variable-valence metal elements are embedded in the amorphous sodium halide oxide framework, they form redox active sites, enabling the resulting solid electrolyte to not only act as an inert ion conductor, but also to possess both ion transport and capacity contribution functions.
[0029] Preferably, the sodium carbonate containing water of crystallization includes at least one of sodium carbonate monohydrate (Na2CO3•H2O) and sodium carbonate decahydrate (Na2CO3•10H2O).
[0030] Furthermore, the sodium carbonate containing water of crystallization is preferably sodium carbonate monohydrate, Na₂CO₃•H₂O. Using Na₂CO₃•H₂O as a raw material provides a moderate amount of water of crystallization, which is beneficial for its structural induction effect during mechanochemical processing, while also reducing the potential side reactions caused by excessive moisture.
[0031] Preferably, the variable valence metal element includes at least one of Nb, V, and W; the variable valence metal chloride includes at least one of niobium pentachloride (NbCl5), vanadium trichloride (VCl3), and tungsten chloride (WCl5).
[0032] Furthermore, the variable-valence metal chloride is preferably NbCl5. NbCl5 can simultaneously provide Cl and variable-valence Nb elements, and undergoes solid-phase reconstruction with sodium carbonate containing water of crystallization during mechanochemical processing to form an amorphous sodium halide oxide solid electrolyte containing Nb active sites.
[0033] Preferably, when the variable valence metal chloride is NbCl5, the resulting solid electrolyte is an amorphous halide oxide solid electrolyte of the Na-Nb-O-Cl system.
[0034] Preferably, the at least one variable-valence metal element is uniformly dispersed in the fully amorphous network structure and participates in reversible redox reactions during charging and discharging, enabling the solid electrolyte to independently contribute capacity in the all-solid-state battery.
[0035] In this way, the risk of structural inhomogeneity caused by local enrichment or phase separation of variable-valence metal elements can be reduced, and the compositional uniformity and reactivity distribution uniformity of solid electrolytes can be improved. At the same time, the participation of variable-valence metal elements in redox reactions can enable solid electrolytes to contribute to capacity in all-solid-state batteries, thereby reducing the energy density loss caused by traditional inert solid electrolytes as non-capacity contributing components.
[0036] The present invention also discloses that the solid electrolyte is used to form an all-solid-state sodium-ion battery cathode by combining with a carbon matrix, wherein the cathode does not contain conventional cathode active materials.
[0037] Furthermore, the conductive agent includes at least one of conductive carbon black, Super P, acetylene black, Ketjen black, carbon nanotubes, carbon fibers, vapor-grown carbon fibers (VGCF), graphene, and reduced graphene oxide.
[0038] In this way, the solid electrolyte can simultaneously undertake the functions of ion transport and capacity contribution after being combined with the carbon matrix, avoiding the complex solid-solid interface problems caused by the multiphase mixing of positive electrode active material, solid electrolyte and conductive agent in traditional composite cathodes, and reducing the adverse effects of redundancy of inactive components on energy density.
[0039] This invention also discloses a method for preparing the above-mentioned bifunctional amorphous halide oxide solid electrolyte synthesized with the aid of water of crystallization, comprising the following steps: Sodium carbonate containing water of crystallization is mixed with a variable-valence metal chloride to obtain a precursor mixture; The precursor mixture is subjected to mechanochemical treatment to cause sodium carbonate containing water of crystallization to undergo a mechanochemical reaction and structural reconstruction with variable valence metal chloride. By utilizing the in-situ structural induction effect of water of crystallization during the reaction process, a long-range disordered and completely amorphous bifunctional amorphous halide oxide solid electrolyte is obtained. The resulting solid electrolyte contains Na, O, Cl, and at least one variable-valence metal element, which is distributed in a completely amorphous sodium halide oxide network structure and forms redox active sites.
[0040] Through the aforementioned mechanochemical treatment, sodium carbonate containing crystal water can be brought into full contact and react with variable-valence metal chlorides under solid-state conditions. During ball milling, the crystal water induces local coordination environment rearrangement, promoting the reconstruction of structural units such as Na-O, MO, and M-Cl, thereby disrupting the crystalline structure in the raw material and forming a continuous amorphous network. Compared to systems using direct ball milling of anhydrous sodium carbonate and variable-valence metal chlorides, this invention is more advantageous in improving the degree of amorphization, suppressing residual crystalline impurities, and improving the sodium ion transport performance of the resulting solid electrolyte.
[0041] Furthermore, the sodium carbonate containing water of crystallization includes at least one of Na2CO3•H2O and Na2CO3•10H2O, preferably Na2CO3•H2O.
[0042] Furthermore, the variable valence metal chloride includes at least one of NbCl5, VCl3, and WCl5, preferably NbCl5.
[0043] Furthermore, the molar ratio of sodium carbonate containing water of crystallization to variable valence metal chloride can be adjusted according to the target sodium content, oxygen content, chlorine content, and variable valence metal content.
[0044] Furthermore, when the sodium carbonate containing water of crystallization is Na2CO3•H2O and the variable valence metal chloride is NbCl5, Na2CO3•H2O and NbCl5 are mixed and then subjected to high-energy ball milling to obtain a bifunctional amorphous halide oxide solid electrolyte of the Na-Nb-O-Cl system.
[0045] Furthermore, the mechanochemical treatment is a mechanical ball milling treatment.
[0046] Furthermore, the ball milling speed of the mechanical ball milling process is 300 rpm-500 rpm, the ball milling time is 1 h-12 h, and the ball-to-material ratio is (20-60):1.
[0047] Furthermore, the mechanical ball milling process is carried out under an inert atmosphere or sealed conditions to reduce the influence of external moisture and oxygen on the reaction system.
[0048] Furthermore, after ball milling, the milling jar is transferred to an inert atmosphere, opened, and the product is collected.
[0049] According to a third aspect of the present invention, an application is provided of the above-described bifunctional amorphous halide oxide solid electrolyte synthesized with the aid of crystallization water in an all-solid-state sodium-ion battery.
[0050] Furthermore, the positive electrode of the all-solid-state sodium-ion battery is prepared by mixing the bifunctional amorphous halide oxide solid electrolyte with a conductive agent.
[0051] Furthermore, the bifunctional amorphous halide oxide solid electrolyte serves as an active solid electrolyte in the positive electrode, simultaneously providing sodium ion transport channels and contributing to redox capacity.
[0052] Furthermore, the all-solid-state sodium-ion battery is an all-solid-state sodium-ion battery without traditional positive electrode active materials, and its operating voltage range is 1.4-4.1 V.
[0053] By employing the above application method, the bifunctional amorphous halide oxide solid electrolyte is no longer merely an inert ion conductor in the composite cathode, but rather a core functional component possessing both ion conduction and electrochemical activity. When combined with a carbon matrix, it can construct the cathode structure, thereby reducing the side reactions and impedance growth problems caused by multiple solid-solid interfaces between the solid electrolyte, cathode active material, and conductive agent in traditional composite cathodes. It also increases the effective proportion of capacity-contributing components in the electrode, which is beneficial for improving the capacity utilization and cycle stability of all-solid-state sodium-ion batteries.
[0054] The present invention will be further illustrated below with reference to specific embodiments. It should be understood that these embodiments are for illustrative purposes only and are not intended to limit the scope of the invention. Furthermore, it should be understood that after reading the teachings of this invention, those skilled in the art can make various alterations or modifications to the invention, and these equivalent forms also fall within the scope defined by the appended claims.
[0055] The following examples use instruments and equipment conventional in the art. Experimental methods in the following examples, unless otherwise specified, are generally performed under conventional conditions or as recommended by the manufacturer. All raw materials used in the following examples are conventional commercially available products with specifications conventional in the art. In this specification and the following examples, unless otherwise specified, "%" refers to weight percentage, "parts" refers to parts by weight, and "ratio" refers to weight proportion.
[0056] This invention involves mixing sodium carbonate containing water of crystallization with a variable-valence metal chloride to obtain a precursor mixture. The sodium carbonate containing water of crystallization provides Na, O, and water of crystallization, while the variable-valence metal chloride provides Cl and a variable-valence metal element. The precursor mixture is subjected to mechanochemical treatment to cause mechanochemical reconstruction of the sodium carbonate containing water of crystallization and the variable-valence metal chloride. The in-situ structural induction effect of water of crystallization during the reaction process promotes the formation of an amorphous network, resulting in a bifunctional amorphous halide oxide solid electrolyte synthesized with water of crystallization assistance. The obtained solid electrolyte has a long-range disordered, completely amorphous sodium halide oxide network structure, containing Na, O, Cl, and at least one variable-valence metal element. The variable-valence metal element is distributed in the amorphous sodium halide oxide network structure and forms redox active sites.
[0057] The bifunctional amorphous halide oxide solid electrolyte of the present invention has a wide operating voltage window and can simultaneously provide sodium ion transport channels and capacity contribution in all-solid-state sodium-ion batteries. It can be directly combined with conductive agents to construct an active cathode without traditional cathode active materials, thereby reducing multiple solid-solid interfaces, reducing the risk of interfacial side reactions and impedance growth, and improving the structural stability and cycle stability of the battery.
[0058] Example 1 A method for synthesizing a bifunctional amorphous halide oxide solid electrolyte with crystallization water assistance, comprising the following steps: Step 1: Preparation of precursor mixture Sodium carbonate containing water of crystallization (Na2CO3•H2O) was mixed with an active metal chloride (NbCl5) to obtain a precursor mixture; wherein the molar ratio of Na2CO3•H2O to NbCl5 was 1:2. Step 2: Preparation of solid electrolyte In a glove box (H2O < 0.01 ppm, O2 < 0.01 ppm), the precursor mixture obtained in step 1 was placed into a ball mill jar, followed by the addition of grinding beads. The ball mill jar was then vacuum-sealed and placed in a ball mill for mechanical ball milling. The grinding beads had a diameter of 5 mm and were made of ZrO2. The ball-to-material ratio was 40:1. The ball milling speed was 400 rpm, and the ball milling time was 8 h. During the mechanical ball milling process, the ball milling was paused for 5 minutes after each 5-minute pause. After the mechanical ball milling process was completed, the ball mill jar was opened in the glove box, and the product was collected to obtain a bifunctional amorphous halide oxide solid electrolyte, denoted as NHNOC-12.
[0059] Example 2 The difference between this embodiment and Embodiment 1 is that: In step 2, the ball milling time is adjusted to 1.0h, 1.5h, 2.0h, 4.0h, 6.0h, 8.0h, 10h, and 12h respectively; the remaining steps and conditions are the same.
[0060] Example 3 The difference between this embodiment and Embodiment 1 is that: In step 1, the active metal chloride of the raw material is vanadium chloride (VCl3), and the remaining steps and conditions are the same. The resulting bifunctional amorphous halide oxide solid electrolyte is denoted as NHVOC-12.
[0061] Example 4 The difference between this embodiment and Embodiment 1 is that: In step 1, the active metal chloride of the raw material is tungsten pentachloride (WCl5), and the other steps and conditions are the same. The resulting bifunctional amorphous halide oxide solid electrolyte is denoted as NHWOC-12.
[0062] Example 5 The difference between this embodiment and Embodiment 1 is that: In step S1, the raw material is sodium carbonate (Na2CO3•10H2O) containing water of crystallization, wherein the molar ratio of Na2CO3•10H2O to NbCl5 is 1:2; The remaining steps and conditions are the same, and the resulting bifunctional amorphous halide oxide solid electrolyte is denoted as NHNOC10-12.
[0063] Comparative Example 1 The difference between this comparative example and Example 1 is that: In step S1, the raw material used is sodium carbonate (Na2CO3) that does not contain water of crystallization. The remaining steps and conditions are the same, and the resulting bifunctional amorphous halide oxide solid electrolyte is denoted as NANOC-12.
[0064] Comparative Example 2 The difference between this comparative example and Example 1 is that: In step S1, the raw material used is anhydrous sodium carbonate (Na2CO3), wherein the molar ratio of Na2CO3 to NbCl5 is 2:3, in order to eliminate the amorphization effect caused by different oxygen contents; The remaining steps and conditions are the same, and the resulting bifunctional amorphous halide oxide solid electrolyte is denoted as NANOC-23.
[0065] Application Example 1 Preparation of zirconium-based solid electrolyte interlayer In a glove box (H2O < 0.01 ppm, O2 < 0.01 ppm), raw materials were weighed at a ZrCl4 to Na2CO3 molar ratio of 1:2 and placed in a ball mill jar. Then, ZrO2 grinding beads with a diameter of 5 mm were added, with a ball-to-material ratio of 30:1. After vacuum sealing, the ball mill jar was placed in a ball mill for mechanical ball milling at a speed of 400 rpm for 8 hours. During the ball milling process, an intermittent mode of 10 minutes of ball milling followed by 5 minutes of rest was adopted. After the high-energy ball milling process, the ball mill jar was opened in the glove box and the product was collected to obtain a zirconium-based solid electrolyte, denoted as NZCO. This solid electrolyte is used only as a sandwich material for assembling all-solid-state batteries.
[0066] S(11) Preparation of composite cathode materials Using the NHNOC-12 prepared in Example 1 as the target solid electrolyte, a composite cathode material was prepared. Specifically, the target solid electrolyte and VGCF were mixed at a mass ratio of 90:10 and then placed in a ball mill for simple mixing. The ball mill beads had a diameter of 5 mm and were made of ZrO2; the ball-to-material ratio was 20:1; the ball milling speed was 100 rpm; and the ball milling time was 1 hour. During the mechanical ball milling process, the ball milling was paused for 5 minutes, followed by a 5-minute rest period, to obtain the composite cathode material.
[0067] S(12) Assemble an all-solid-state ion battery Using the prepared NZCO as the interlayer, the composite cathode material obtained in step S(11) above is the cathode, Na 15 Sn4 is used as the negative electrode in the assembly of an all-solid-state ion battery. Specifically, 50 mg of NZCO solid electrolyte is weighed and placed in a battery mold, and a pressure of 200 MPa is applied. Then, 8 mg of composite positive electrode material and 50 mg of Na3PS4 are added to both sides of the inert zirconium-based solid electrolyte, and the mixture is spread evenly with a spatula, and a pressure of 200 MPa is applied. Finally, 40 mg of Na3PS4 is added to the Na3PS4 side. 15 The Sn4 negative electrode was flattened with a spatula, and finally a pressure of 300 MPa was applied. After standing for 2 hours, an all-solid-state ion battery was obtained.
[0068] Test Example 1 X-ray diffraction tests were performed on the solid electrolyte obtained in Example 2, and the results are shown in [reference needed]. Figure 1 ; X-ray diffraction and PDF tests were performed on the solid electrolytes obtained in Example 1 and Comparative Examples 1 and 2. The results are shown in [reference needed]. Figure 2 and Figure 3 ; X-ray diffraction tests were performed on the solid electrolytes obtained in Examples 3 and 4. The results are shown in [reference needed]. Figure 4 ; X-ray diffraction tests were performed on the solid electrolyte obtained in Example 5, and the results are shown in [reference needed]. Figure 5 ; according to Figure 1 It is known that the solid electrolyte prepared from sodium carbonate (Na2CO3•H2O) containing water of crystallization, even with a ball milling time of only 1 h, exhibits a broad and diffuse peak in the XRD pattern within the range of 10-80°. This result indicates that during mechanochemical treatment, water of crystallization can play an in-situ structure-inducing role, promoting the rapid destruction and local coordination reconstruction of the long-range ordered crystal structure in the precursor, thereby effectively promoting the formation of amorphous sodium halide oxide structures.
[0069] according to Figure 2 and Figure 3It is evident that the solid electrolyte NHNOC-12, prepared from sodium carbonate containing water of crystallization (Na2CO3•H2O), exhibits significantly different structural characteristics compared to NANOC-12 and NANOC-23, prepared by ball milling anhydrous sodium carbonate and NbCl5. XRD results show that NANOC-12 and NANOC-23 contain obvious Nb2O5 crystalline oxide diffraction peaks, indicating that the anhydrous system readily generates crystalline impurities during mechanochemical reactions; while NHNOC-12 did not show obvious crystalline impurity peaks and primarily exhibited amorphous characteristics. Further PDF analysis reveals that NHNOC-12 exhibits a long-range disordered structure, indicating that water of crystallization plays an in-situ structural induction role during ball milling, promoting amorphous reconstruction.
[0070] from Figure 4 As can be seen, both vanadium-based and tungsten-based solid electrolytes exhibit amorphous structures, which further proves the universality of water of crystallization promoting amorphous reconstruction.
[0071] Test Example 2 (1) Ionic conductivity test The solid electrolytes obtained in Examples 1 and 2, and Comparative Examples 1 and 2 were tested using cold pressing technology.
[0072] The specific testing method is as follows: In a glove box (H2O < 0.01 ppm, O2 < 0.01 ppm), 200 mg of the target solid electrolyte was weighed and then poured into a solid battery mold (10 mm in diameter). A pressure of 200 MPa was then applied for cold pressing, and the pressure was held for 2 minutes. Subsequently, the sample was tested using a Bio-Logic VMP3 electrochemical workstation at 25°C (room temperature) within a frequency range of 1 Hz to 7 MHz.
[0073] The ionic conductivity test results of the solid electrolytes obtained in Example 1 and Comparative Examples 1 and 2 are shown in [reference]. Figure 6 ; Combination Figure 6 It can be seen that different precursors have a significant impact on the ion conduction performance of the resulting solid electrolyte.
[0074] Figure 6 The results show that the room temperature ionic conductivity of NHNOC-12, NANOC-12, and NANOC-23 obtained in Example 1 and Comparative Examples 1 and 2 are 0.57 mS / cm. -1 0.10 mS cm -1 and 0.15 mS cm -1 This indicates that the sodium ion transport capacity of the water-assisted synthesis materials is significantly improved, with NHNOC-12 exhibiting the best ion-conducting performance among the three.
[0075] (2) Electrochemical testing The all-solid-state sodium-ion battery obtained in the application example was subjected to electrochemical performance testing on the Blue Electric testing system. The test temperature was 25 °C, the voltage window was 1.4–4.1 V, and the areal loading was 7.8 mg cm⁻¹. -2 The test results can be found in [link / reference]. Figures 7-9 .in, Figure 7 The results are from the rate performance test. Figure 8 and Figure 9 The results are from long-cycle tests at 0.1C and 0.3C, respectively.
[0076] Depend on Figure 7 It can be seen that as the current rate gradually increases from 0.05C to 1.0C, the battery's discharge specific capacity decreases in a stepwise manner; when the rate decreases again, the capacity can recover accordingly, indicating that this all-solid-state battery has a certain rate response capability and reversible capacity recovery capability. Figure 8 It can be seen that under 0.1C cycling conditions, the battery experiences a certain capacity decay in the early stages before gradually stabilizing. After 160 cycles, the capacity retention rate is 84.08%, and the coulombic efficiency remains close to 100%. Figure 9 It can be seen that at a higher rate of 0.3C, the battery can still maintain stable charge-discharge behavior after long cycles, with a capacity retention of 75.80% after 560 cycles, and the coulombic efficiency also remains stable. The above results indicate that although the material may undergo activation, interface reconstruction, or structural adjustment processes in the initial cycling stage, leading to some capacity decay, its capacity decay slows down in subsequent cycles, exhibiting good cycling stability and high charge-discharge reversibility.
[0077] Test Example 3 TEM and TEM-EDS testing TEM and elemental mapping tests were performed on the NHNOC-12 obtained in the examples. The test results are shown in [link to relevant documentation]. Figure 10 . Figure 10 The left side shows a TEM image of NHNOC-12, and the right side shows the surface distribution maps of Na, Nb, O, and Cl elements. Figure 10 It can be seen that NHNOC-12 exhibits an irregular particle morphology formed by nanoparticle aggregation. The distribution profiles of Na, Nb, O, and Cl elements are basically consistent with the particle morphology of the TEM matrix, and the signals of each element are continuously distributed throughout the entire particle region. No obvious independent element enrichment regions detached from the matrix were observed, nor were there any significant agglomeration, clustering, or local absence of single elements. These results indicate that Na, Nb, O, and Cl elements can be relatively uniformly distributed within the particles of the NHNOC-12 sample.
[0078] Test Example 4 Linear Scan Voltammetry (LSV) Test: Linear Scan Voltammetry (LSV) Test: Using Na 15 The electrochemical stability of the solid electrolytes obtained in Example 1 (NHNOC-12), Comparative Example 1 (NANOC-12), and Comparative Example 2 (NANOC-23) was evaluated using the Sn4|Na3PS4|SE|SE+VGCF battery structure. The conductive agent used was vapor-grown carbon fiber (VGCF). Battery assembly was performed in an argon-filled glove box (H2O, O2 < 0.01 ppm). The specific steps were as follows: First, 50 mg of SE powder was placed in a PEEK mold and pressed into a sheet under 0.5 tons of pressure. SE and VGCF were manually mixed at a mass ratio of 10:1. 6 mg of the mixture was uniformly coated onto one side of the electrolyte sheet. 50 mg of Na3PS4 powder was coated onto the other side of the electrolyte sheet, and it was pressed into shape under 2.0 tons of pressure. Finally, 40 mg of Na3PS4 powder was added to the Na3PS4 powder side. 15 Sn4 powder was pressed at 4.0 tons of pressure and held at that pressure for 3 minutes to serve as the counter electrode. LSV testing was performed using an MTZ-35 analyzer (Bio-Logic) at 25°C with a scan rate of 0.1 mV s⁻¹, scanning from open circuit voltage to 6 V and 0 V, respectively.
[0079] Test results are available Figure 11 , Figure 12 and Figure 13 NHNOC-12 and NANOC-23 exhibit significant anodic currents starting at approximately 4.25 V, while the anodic current initiation potential of NANOC-12 is approximately 4.30 V, indicating that the three materials possess similar high-potential oxidation stability. Based on the current initiation potential determined by the tangent method, the low-potential reaction initiation potentials of NHNOC-12, NANOC-12, and NANOC-23 are all approximately 2.35 V, while the high-potential oxidation reaction initiation potentials are approximately 4.25, 4.30, and 4.25 V, respectively. Since the working electrode is composed of a solid electrolyte and VGCF composite, and these materials possess certain redox activities, the low-potential cathode current may simultaneously encompass intrinsic reduction of Nb centers, interface reconstruction, and possible reductive decomposition processes. Therefore, approximately 2.35 V should more accurately be described as the cathode electrochemical reaction initiation potential and cannot be directly equated to the irreversible reductive decomposition potential. In contrast, the sustained anodic current appearing at approximately 4.25–4.30 V can be used to characterize the initiation boundary of the high-potential oxidation reaction of the materials. Overall, the electrochemical reaction potential ranges of the three electrolytes are quite similar. Among them, NHNOC-12 prepared with the aid of water of crystallization maintains a high ionic conductivity, and its high-potential oxidation initiation potential is not significantly lower than that of the anhydrous control sample.
[0080] The above content is only for illustrating the technical concept of the present invention and should not be construed as limiting the scope of protection of the present invention. Any modifications made to the technical solution based on the technical concept proposed in this invention shall fall within the scope of protection of the claims of this invention.
Claims
1. A bifunctional amorphous halide oxide solid electrolyte synthesized with water of crystallization assistance, characterized in that, Includes the following steps: The solid electrolyte is obtained by mechanical and chemical treatment using sodium carbonate containing water of crystallization and variable-valence metal chloride as raw materials. The solid electrolyte contains Na, O, Cl and at least one variable-valence metal element, and exhibits a long-range disordered, completely amorphous network structure. The at least one variable-valence metal element is distributed in the completely amorphous network structure and forms redox active sites, giving the solid electrolyte both ionic conductivity and intrinsic electrochemical activity. The completely amorphous network structure is generated by in-situ structural induction of the water of crystallization in the sodium carbonate containing water of crystallization, and there are no residual crystalline impurities in the solid electrolyte.
2. The bifunctional amorphous halide oxide solid electrolyte synthesized with crystallization water assistance according to claim 1, characterized in that, The sodium carbonate containing water of crystallization is at least one of sodium carbonate monohydrate and sodium carbonate decahydrate; the variable valence metal element is at least one of Nb, V and W.
3. The bifunctional amorphous halide oxide solid electrolyte synthesized with crystallization water assistance according to claim 1, characterized in that, The variable-valence metal chloride is at least one of niobium pentachloride, vanadium trichloride, and tungsten pentachloride.
4. The bifunctional amorphous halide oxide solid electrolyte synthesized with crystallization water assistance according to claim 1, characterized in that, The at least one variable-valence metal element is uniformly dispersed in the fully amorphous network structure and participates in reversible redox reactions during charging and discharging, enabling the solid electrolyte to independently contribute to the capacity of the all-solid-state battery.
5. A method for synthesizing a bifunctional amorphous halide oxide solid electrolyte with crystallization water assistance as described in any one of claims 1 to 4, characterized in that, Includes the following steps: Sodium carbonate containing water of crystallization is mixed with a variable-valence metal chloride to obtain a precursor mixture; The precursor mixture is subjected to mechanochemical treatment, which causes the sodium carbonate containing water of crystallization to undergo a mechanochemical reaction and structural reconstruction with the variable valence metal chloride, resulting in a bifunctional amorphous halide oxide solid electrolyte.
6. The method for synthesizing a bifunctional amorphous halide oxide solid electrolyte with crystallization water assistance according to claim 5, characterized in that, The mechanochemical treatment is a mechanical ball milling treatment; The molar ratio of sodium carbonate containing water of crystallization to variable valence metal chloride is 1:(1~5).
7. A method for synthesizing a bifunctional amorphous halide oxide solid electrolyte with crystallization water assistance according to claim 5, characterized in that, The ball milling process is performed at a speed of 300 rpm to 500 rpm, a milling time of 1 h to 12 h, and a ball-to-material ratio of (20 to 60):
1.
8. The method for synthesizing a bifunctional amorphous halide oxide solid electrolyte with crystallization water assistance according to claim 7, characterized in that, The mechanochemical treatment is carried out under an inert atmosphere or sealed conditions.
9. The application of the bifunctional amorphous halide oxide solid electrolyte synthesized with crystallization water assistance as described in any one of claims 1 to 4 in the preparation of an all-solid-state sodium-ion battery, characterized in that, The positive electrode of the all-solid-state sodium-ion battery is prepared by mixing the bifunctional amorphous halide oxide solid electrolyte with a conductive agent. The bifunctional amorphous halide oxide solid electrolyte serves as an active solid electrolyte in the positive electrode, simultaneously providing sodium ion transport channels and contributing to redox capacity.
10. The application of the bifunctional amorphous halide oxide solid electrolyte synthesized with crystallization water assistance according to claim 9 in the preparation of all-solid-state sodium-ion batteries, characterized in that, The conductive agent includes at least one of conductive carbon black, Super P, acetylene black, Ketjen black, carbon nanotubes, carbon fibers, vapor-grown carbon fibers, graphene, and reduced graphene oxide.