A composite solid electrolyte, its preparation method and application
By combining a three-dimensional porous conductive framework with a sulfide solid electrolyte, a continuous electron transport network is constructed, which solves the problem of electronic insulation of the sulfide solid electrolyte, realizes efficient ion-electron dual conduction, and improves the electronic conductivity and cycle stability of the battery.
Patent Information
- Application Number
- CN202611396014.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-09
- Publication Date
- 2026-11-17
AI Technical Summary
Existing sulfide solid electrolyte electronic insulating materials cannot construct effective electron transport pathways, resulting in unmet requirements for rapid electron conduction in the electrode system. At the same time, disordered doping of conductive agents easily leads to the formation of local conductive agglomerates and interfacial voids, affecting the rate performance and cycle stability of the battery.
By employing a three-dimensional porous conductive framework and a sulfide solid electrolyte composite structure, a continuous and interconnected electron transport network is constructed through methods such as vapor deposition, sol-gel method, in-situ growth method or electrodeposition method, while maintaining the continuity of ion transport channels, thus achieving dual ion-electron conduction.
It effectively reduces the system's contact resistance and interfacial impedance, improves electronic conductivity, simplifies electrode fabrication processes, avoids side reactions of conductive agents, and enhances the rate performance and long-term cycle stability of sulfide-based all-solid-state batteries.
Smart Images

Figure CN123120845A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of solid-state battery technology, and in particular to a composite solid-state electrolyte, its preparation method, and its application. Background Technology
[0002] Sulfide solid electrolytes, with their excellent ionic conductivity, good flexibility, and superior interfacial contact properties, have become one of the preferred core electrolyte materials for all-solid-state batteries, effectively avoiding the safety hazards of leakage and explosion associated with traditional liquid electrolytes. However, due to the limited ion-conducting capacity and poor interfacial contact of the positive and negative electrode materials, solid electrolytes are usually introduced into the positive and negative electrode sheets to improve ion transport performance. But sulfide solid electrolytes themselves are electronically insulating materials with extremely poor electronic conductivity. A single sulfide solid electrolyte cannot construct an effective electron transport pathway, making it difficult to meet the operational requirements of rapid electron conduction in the electrode system.
[0003] To improve electrode conductivity and adapt to battery charge-discharge kinetics, the conductive network of the electrode is typically optimized by directly incorporating conductive agents. However, the conventional process of simply blending conductive agents with sulfide solid electrolytes and positive and negative electrode active materials only achieves disordered dispersion of conductive particles, failing to construct a continuous and stable three-dimensional conductive network. This results in high contact resistance between particles and fragmented conductive pathways, making it difficult to effectively improve the overall electronic conductivity of the electrode. Furthermore, disordered doping of conductive agents easily leads to defects such as localized conductive agglomerates and interfacial voids within the electrode. This not only fails to provide conductivity gains but also disrupts the tight contact structure between the sulfide electrolyte and the active material, increasing interfacial impedance and further degrading the overall electron transport performance of the electrode and the electrochemical kinetics of the battery. In addition, direct contact between the conductive agent and the sulfide electrolyte easily triggers interfacial side reactions, generating an insulating interfacial layer, which exacerbates the degradation of the conductive network and restricts the rate performance and cycle stability of sulfide-based all-solid-state batteries.
[0004] In the prior art, attempts have been made to improve the electronic conductivity of solid electrolytes through coating. For example, patent application CN121172052A discloses a graphene-coated solid electrolyte. However, this core-shell structure only improves electron transport on the surface of the solid electrolyte; the bulk phase remains electronically insulating, thus the overall electron transport pathway is still blocked. Furthermore, patent application CN121964800A discloses a method for synthesizing carbon-containing solid electrolytes, which adds a carbon-containing precursor to give the solid electrolyte better electronic and ionic conductivity. However, this method cannot control the distribution of carbon and electrolyte, and the uniform distribution of carbon in the electrolyte can damage the grain boundaries during synthesis, leading to a decrease in ionic conductivity.
[0005] Therefore, there is an urgent need to develop a composite solid electrolyte material that can both ensure the excellent ionic conductivity of sulfide solid electrolytes and construct an efficient electron transport pathway. Summary of the Invention
[0006] The purpose of this invention is to provide a composite solid electrolyte, its preparation method, and its application. Through the composite structure design of a three-dimensional porous conductive framework and a sulfide solid electrolyte, a continuous, three-dimensional interconnected electron transport network is constructed inside the sulfide solid electrolyte, while maintaining the continuity of the ion transport channels, thus realizing the dual conduction function of ions and electrons.
[0007] To achieve the above objectives, the present invention provides a composite solid electrolyte, comprising a three-dimensional conductive framework and a sulfide solid electrolyte filled within the three-dimensional conductive framework, wherein the three-dimensional conductive framework accounts for m% of the mass percentage of the composite solid electrolyte. The electronic conductivity of the three-dimensional conductive framework is , The electronic conductivity of the composite solid electrolyte is , The composite solid electrolyte satisfies .
[0008] Take 1g of three-dimensional conductive framework powder, place it in the mold of a powder conductivity meter, apply a pressure of 20MPa, and test its powder conductivity. Similarly, take 1g of composite solid electrolyte powder, place it in the mold of a powder conductivity meter, apply a pressure of 20MPa, and test its powder conductivity. .
[0009] Preferably, the conductive material of the three-dimensional conductive framework is one or more of carbon nanotubes, carbon nanofibers, graphene, flake graphite, porous carbon, aerogel, silver nanowires, porous silver, porous nickel, TiO2, TiN, MoS2, Ti3C2, MOF, and MXene.
[0010] Preferably, the raw materials for the sulfide solid electrolyte are Li3PS4, Li8P2S9, Li6PS5Cl, Li6PS5Br, Li6PS5I, and Li6PS5Cl. 0.5 Br 0.5 Li 5.5 PS 4.5 Cl 1.5 Li 6-x PS 5-x Cl 1+x Li 10 GeP2S 12 Li4SnS4, Li 9.54 Si 1.74 P1.44 S 11.7 Cl 0.3 Li 6+x M x P 1-x S 5x One or more of the following; The Li 6-x PS 5-x Cl 1+x middle ; The Li 6+x M x P 1-x S 5x middle M is selected from one or more of Si, Ge, and Sn.
[0011] The present invention also provides a method for preparing a composite solid electrolyte, including one of the following methods: vapor deposition, sol-gel method, in-situ growth method, electrodeposition method, and emulsion method.
[0012] Preferably, it includes the following steps: S1. Preparation of three-dimensional conductive framework: The conductive material is added to the solvent, along with a dispersant and a spheroidizing agent. After ultrasonic dispersion and stirring, the mixture is spray-dried to obtain a three-dimensional porous conductive framework. S2. Preparation of composite solid electrolyte: The raw materials of sulfide solid electrolyte are mixed with the three-dimensional porous conductive framework obtained in S1, an organic solvent is added, the mixture is ball-milled and dried, and then sintered under a protective atmosphere to obtain the composite solid electrolyte.
[0013] Preferably, in S2, the raw material for the sulfide solid electrolyte is one or more of lithium sulfide, lithium chloride, and phosphorus pentasulfide mixed in stoichiometric proportions.
[0014] This invention also provides an application of a composite solid electrolyte in the preparation of solid-state batteries.
[0015] Preferably, the solid-state battery includes a positive electrode, an electrolyte sheet, and a negative electrode, wherein the negative electrode contains the composite solid electrolyte and does not contain any other conductive agents.
[0016] Preferably, the other conductive agent is one or more of carbon nanotubes, conductive carbon black, carbon nanofibers, graphene, flake graphite, Ketjen black, and porous carbon.
[0017] Preferably, the preparation of the solid-state battery includes the following steps: LiNi 0.8 Co 0.1 Mn 0.1O2: The composite solid electrolyte: vapor-grown carbon fiber (VGCF): hydrogenated styrene-butadiene block copolymer (SEBS): xylene is uniformly mixed in a ratio of 85:10:3:2:100 to form a slurry and uniformly coated on carbon-coated aluminum foil. The slurry is then dried in an oven at 60°C to obtain the positive electrode sheet. Micron-sized silicon, the composite solid electrolyte, VGCF, SEBS, and xylene were uniformly mixed in a ratio of 80:15:3:2:100 to form a slurry, which was then uniformly coated onto a carbon-coated copper foil and dried in an oven at 60°C to obtain a negative electrode sheet. Take 100mg of Li6PS5Cl powder and place it in a solid-state battery mold with a diameter of 10mm, and compact it with a pressure of 1t; then place the positive electrode sheet on one side of the mold and compact it with a pressure of 2t; finally place the negative electrode sheet on the other side of the mold and compact it with a pressure of 1t; finally, compact the entire mold with a pressure of 1t to obtain a solid-state battery.
[0018] Therefore, the present invention employs the above-mentioned composite solid electrolyte, its preparation method, and its application, and the beneficial effects are as follows: (1) The present invention adopts a structural design of a three-dimensional porous conductive framework and a sulfide solid electrolyte composite, which abandons the traditional simple physical mixing modification method. Through the three-dimensional cross-linked porous conductive framework, a continuous and structurally stable high-speed electron transport path is constructed inside the electrode, which reduces the contact resistance and interface impedance of the system, improves the electronic conductivity of the composite system, and effectively makes up for the shortcomings of electronic insulation of sulfide solid electrolyte.
[0019] (2) In this invention, the sulfide solid electrolyte is continuously distributed in a three-dimensional porous conductive framework, and both the conductive electron network and the conductive ion network maintain continuity and high efficiency, realizing the synergistic effect of dual ion-electron conduction. The regular three-dimensional porous framework structure can accurately adapt to the electrolyte distribution, avoid defects such as conductive agent agglomeration and interface voids, and ensure close interfacial contact between the sulfide electrolyte and the active material.
[0020] (3) The present invention modulates the electronic conductivity of the three-dimensional porous conductive framework and the composite solid electrolyte (i.e., satisfies 0.02≤ A ratio ≤0.5 ensures optimal rate performance and cycle stability of the electrode. A ratio that is too low will block ion / electron transport, leading to decreased rate performance and cycle stability; a ratio that is too high will cause localized micro-short circuits and side reactions, also resulting in decreased rate performance and cycle stability.
[0021] (4) When the composite solid electrolyte of the present invention is applied to the negative electrode, no other conductive agent needs to be added, which simplifies the electrode preparation process. At the same time, it avoids the interfacial side reaction between the conductive agent and the sulfide electrolyte, suppresses the formation of the insulating interfacial layer, and significantly improves the rate performance and long-term cycle stability of the sulfide-based all-solid-state battery.
[0022] The technical solution of the present invention will be further described in detail below through embodiments. Detailed Implementation
[0023] The technical solution of the present invention will be further described below through embodiments.
[0024] Unless otherwise defined, the technical or scientific terms used in this invention shall have the ordinary meaning as understood by one of ordinary skill in the art to which this invention pertains.
[0025] Example 1 A composite solid electrolyte, wherein the conductive material of the three-dimensional conductive framework is carbon nanotubes, and the raw material of the sulfide solid electrolyte is Li6PS5Cl.
[0026] Its preparation method is as follows: (1) Synthesis of a three-dimensional conductive framework: 1.0 g of carbon nanotubes were added to water, along with 0.15 g of PVP (polyvinylpyrrolidone) and 0.3 g of silicone oil as dispersant and spheroidizing agent, respectively. The mixture was sonicated at 60 °C with simultaneous stirring for 2 hours to ensure thorough entanglement and dispersion of the carbon nanotubes. The dispersion was then spray-dried (at 150 °C) to obtain a three-dimensional conductive framework.
[0027] (2) Synthesis of composite solid electrolytes: 1.0 g of lithium sulfide (Li₂S), 0.97 g of lithium chloride (LiCl), and 0.37 g of phosphorus pentasulfide (P₂S₅) were thoroughly ground and mixed according to stoichiometric ratio to obtain raw material Li₆PS₅Cl. 100 mL of xylene was added as a solvent, along with a three-dimensional conductive framework with a mass percentage m = 0.10. The mixture was thoroughly ball-milled until homogeneous and dried. Then, it was sintered at 450 °C for 4 hours under a nitrogen atmosphere to obtain a composite solid electrolyte.
[0028] The electronic conductivity of the three-dimensional conductive framework in this embodiment was tested. =2741.5 S / cm, electronic conductivity of composite solid electrolyte =14.0 S / cm, =0.05.
[0029] Example 2 A composite solid electrolyte, wherein the conductive material of the three-dimensional conductive framework is porous carbon, and the raw material of the sulfide solid electrolyte is Li3PS4.
[0030] Its preparation method is as follows: (1) Synthesis of a three-dimensional conductive framework: 1.0 g of porous carbon was added to water, along with 0.2 g of PVP and 0.5 g of silicone oil as dispersant and spheroidizing agent, respectively. The mixture was ultrasonicated at 60 °C with simultaneous stirring for 2 hours to ensure thorough entanglement and dispersion of the porous carbon. The dispersion was then spray-dried (at 100 °C) to obtain a three-dimensional conductive framework.
[0031] (2) Synthesis of composite solid electrolytes: 1.0 g of Li₂S and 1.61 g of P₂S₅ were thoroughly ground and mixed according to the stoichiometric ratio to obtain raw material Li₃PS₄. 100 mL of xylene was added as a solvent, along with a three-dimensional conductive framework with a mass percentage m = 0.20. The mixture was ball-milled thoroughly until homogeneous and then dried. Finally, it was sintered at 450 °C for 4 hours under a nitrogen atmosphere to obtain a composite solid electrolyte.
[0032] The electronic conductivity of the three-dimensional conductive framework in this embodiment was tested. =36.9 S / cm, electronic conductivity of composite solid electrolyte =1.3S / cm, =0.18.
[0033] Example 3 A composite solid electrolyte, wherein the conductive material of the three-dimensional conductive framework is porous silver, and the raw material of the sulfide solid electrolyte is Li4SnS4.
[0034] Its preparation method is as follows: (1) Synthesis of a three-dimensional conductive framework: 1.0 g of porous silver was added to water, along with 0.1 g of PVP and 1.0 g of silicone oil as a dispersant and a spheroidizing agent, respectively. The mixture was sonicated at 60 °C with simultaneous stirring for 2 hours to ensure the porous silver was fully entangled and dispersed. The dispersion was then spray-dried (at 150 °C) to obtain a three-dimensional conductive framework.
[0035] (2) Synthesis of composite solid electrolytes: 1.0 g Li₂S and 1.64 g tin disulfide (SnS₂) were thoroughly ground and mixed according to stoichiometric ratio to obtain raw material Li₄SnS₄. 100 mL of xylene was added as a solvent, along with a three-dimensional conductive framework with a mass percentage m = 0.30. The mixture was ball-milled thoroughly until homogeneous and then dried. Finally, it was sintered at 450 °C for 4 hours under a nitrogen atmosphere to obtain a composite solid electrolyte.
[0036] The electronic conductivity of the three-dimensional conductive framework in this embodiment was tested. =75928.1 S / cm, electronic conductivity of composite solid electrolyte =736.0 S / cm, =0.03.
[0037] Example 4 A composite solid electrolyte, wherein the conductive material of the three-dimensional conductive framework is carbon nanotubes, and the raw material of the sulfide solid electrolyte is Li6PS5Cl.
[0038] Its preparation method is as follows: (1) Synthesis of a three-dimensional conductive framework: 1.0 g of carbon nanotubes were added to water, along with 0.15 g of PVP and 0.3 g of silicone oil as dispersant and spheroidizing agent, respectively. The mixture was sonicated at 60 °C with simultaneous stirring for 2 hours to ensure thorough entanglement and dispersion of the carbon nanotubes. The dispersion was then spray-dried (at 150 °C) to obtain a three-dimensional conductive framework.
[0039] (2) Synthesis of composite solid electrolytes: 1.0 g Li₂S, 0.97 g LiCl, and 0.37 g P₂S₅ were thoroughly ground and mixed according to stoichiometric ratio to obtain raw material Li₆PS₅Cl. 100 mL of xylene was added as a solvent, along with a three-dimensional conductive framework with a mass percentage m = 0.02. The mixture was ball-milled thoroughly until homogeneous and then dried. Finally, it was sintered at 450 °C for 4 hours under a nitrogen atmosphere to obtain a composite solid electrolyte.
[0040] The electronic conductivity of the three-dimensional conductive framework in this embodiment was tested. =2741.5 S / cm, electronic conductivity of composite solid electrolyte =1.5S / cm, =0.03.
[0041] Example 5 A composite solid electrolyte, wherein the conductive material of the three-dimensional conductive framework is carbon nanotubes, and the raw material of the sulfide solid electrolyte is Li6PS5Cl.
[0042] Its preparation method is as follows: (1) Synthesis of a three-dimensional conductive framework: 1.0 g of carbon nanotubes were added to water, along with 0.15 g of PVP and 0.3 g of silicone oil as dispersant and spheroidizing agent, respectively. The mixture was sonicated at 60 °C with simultaneous stirring for 2 hours to ensure thorough entanglement and dispersion of the carbon nanotubes. The dispersion was then spray-dried (at 150 °C) to obtain a three-dimensional conductive framework.
[0043] (2) Synthesis of composite solid electrolytes: 1.0 g Li₂S, 0.97 g LiCl, and 0.37 g P₂S₅ were thoroughly ground and mixed according to stoichiometric ratio to obtain raw material Li₆PS₅Cl. 100 mL of xylene was added as a solvent, along with a three-dimensional conductive framework with a mass percentage m = 0.30. The mixture was ball-milled thoroughly until homogeneous and then dried. Finally, it was sintered at 450 °C for 4 hours under a nitrogen atmosphere to obtain a composite solid electrolyte.
[0044] The electronic conductivity of the three-dimensional conductive framework in this embodiment was tested. =2741.5 S / cm, electronic conductivity of composite solid electrolyte =93.6S / cm, =0.11.
[0045] Example 6 A composite solid electrolyte, wherein the conductive material of the three-dimensional conductive framework is flake graphite, and the raw material of the sulfide solid electrolyte is Li6PS5Cl.
[0046] Its preparation method is as follows: (1) Synthesis of a three-dimensional conductive framework: 1.0 g of flake graphite was added to water, along with 0.4 g of PVP and 0.6 g of silicone oil as dispersant and spheroidizing agent, respectively. The mixture was sonicated at 60 °C with simultaneous stirring for 2 hours to ensure thorough entanglement and dispersion of the flake graphite. The dispersion was then spray-dried (at 150 °C) to obtain a three-dimensional conductive framework.
[0047] (2) Synthesis of composite solid electrolytes: 1.0 g Li₂S, 0.97 g LiCl, and 0.37 g P₂S₅ were thoroughly ground and mixed according to stoichiometric ratio to obtain raw material Li₆PS₅Cl. 100 mL of xylene was added as a solvent, along with a three-dimensional conductive framework with a mass percentage m = 0.28. The mixture was ball-milled thoroughly until homogeneous and then dried. Finally, it was sintered at 450 °C for 4 hours under a nitrogen atmosphere to obtain a composite solid electrolyte.
[0048] The electronic conductivity of the three-dimensional conductive framework in this embodiment was tested. =1.0 S / cm, electronic conductivity of composite solid electrolyte =0.1S / cm, =0.36.
[0049] Example 7 A composite solid electrolyte, wherein the conductive material of the three-dimensional conductive framework is porous silver, and the raw material of the sulfide solid electrolyte is Li6PS5Cl.
[0050] Its preparation method is as follows: (1) Synthesis of a three-dimensional conductive framework: 1.0 g of porous silver was added to water, along with 0.2 g of PVP and 0.8 g of silicone oil as dispersant and spheroidizing agent, respectively. The mixture was sonicated at 60 °C with simultaneous stirring for 2 hours to ensure thorough entanglement and dispersion of the porous silver. The dispersion was then spray-dried (at 100 °C) to obtain a three-dimensional conductive framework.
[0051] (2) Synthesis of composite solid electrolytes: 1.0 g Li₂S, 0.97 g LiCl, and 0.37 g P₂S₅ were thoroughly ground and mixed according to stoichiometric ratio to obtain raw material Li₆PS₅Cl. 100 mL of xylene was added as a solvent, along with a three-dimensional conductive framework with a mass percentage m = 0.10. The mixture was ball-milled until homogeneous and dried. Then, it was sintered at 450 °C for 4 hours under a nitrogen atmosphere to obtain a composite solid electrolyte.
[0052] The electronic conductivity of the three-dimensional conductive framework in this embodiment was tested. =99996.8 S / cm, electronic conductivity of composite solid electrolyte =973.2S / cm, =0.10.
[0053] Example 8 A composite solid electrolyte, wherein the conductive material of the three-dimensional conductive framework is porous carbon, and the raw material of the sulfide solid electrolyte is Li6PS5Cl.
[0054] Its preparation method is as follows: (1) Synthesis of a three-dimensional conductive framework: 1.0 g of porous carbon was added to water, along with 0.1 g of PVP and 0.3 g of silicone oil as dispersant and spheroidizing agent, respectively. The mixture was ultrasonicated at 60 °C with simultaneous stirring for 2 hours to ensure thorough entanglement and dispersion of the porous carbon. The dispersion was then spray-dried (at 200 °C) to obtain a three-dimensional conductive framework.
[0055] (2) Synthesis of composite solid electrolytes: 1.0 g Li₂S, 0.97 g LiCl, and 0.37 g P₂S₅ were thoroughly ground and mixed according to stoichiometric ratio to obtain raw material Li₆PS₅Cl. 100 mL of xylene was added as a solvent, along with a three-dimensional conductive framework with a mass percentage m = 0.10. The mixture was ball-milled until homogeneous and dried. Then, it was sintered at 450 °C for 4 hours under a nitrogen atmosphere to obtain a composite solid electrolyte.
[0056] The electronic conductivity of the three-dimensional conductive framework in this embodiment was tested. =21.4 S / cm, electronic conductivity of composite solid electrolyte =0.1S / cm, =0.05.
[0057] Example 9 A composite solid electrolyte, wherein the conductive material of the three-dimensional conductive framework is porous nickel, and the raw material of the sulfide solid electrolyte is Li6PS5Cl.
[0058] Its preparation method is as follows: (1) Synthesis of a three-dimensional conductive framework: 1.0 g of porous nickel was added to water, along with 0.5 g of PVP and 0.5 g of silicone oil as dispersant and spheroidizing agent, respectively. The mixture was ultrasonicated at 60 °C with simultaneous stirring for 2 hours to ensure thorough entanglement and dispersion of the porous nickel. The dispersion was then spray-dried (at 150 °C) to obtain a three-dimensional conductive framework.
[0059] (2) Synthesis of composite solid electrolytes: 1.0 g Li₂S, 0.97 g LiCl, and 0.37 g P₂S₅ were thoroughly ground and mixed according to stoichiometric ratio to obtain raw material Li₆PS₅Cl. 100 mL of xylene was added as a solvent, along with a three-dimensional conductive framework with a mass percentage m = 0.24. The mixture was ball-milled thoroughly until homogeneous and then dried. Finally, it was sintered at 450 °C for 4 hours under a nitrogen atmosphere to obtain a composite solid electrolyte.
[0060] The electronic conductivity of the three-dimensional conductive framework in this embodiment was tested. =84567.0 S / cm, electronic conductivity of the composite solid electrolyte =1000.3S / cm, =0.05.
[0061] Example 10 A composite solid electrolyte, wherein the conductive material of the three-dimensional conductive framework is carbon nanotubes, and the raw material of the sulfide solid electrolyte is Li6PS5Cl.
[0062] Its preparation method is as follows: (1) Synthesis of a three-dimensional conductive framework: 1.0 g of carbon nanotubes were added to water, along with 0.1 g of PVP and 0.45 g of silicone oil as dispersant and spheroidizing agent, respectively. The mixture was sonicated at 60 °C with simultaneous stirring for 2 hours to ensure thorough entanglement and dispersion of the carbon nanotubes. The dispersion was then spray-dried (at 100 °C) to obtain a three-dimensional conductive framework.
[0063] (2) Synthesis of composite solid electrolytes: 1.0 g Li₂S, 0.97 g LiCl, and 0.37 g P₂S₅ were thoroughly ground and mixed according to stoichiometric ratio to obtain raw material Li₆PS₅Cl. 100 mL of xylene was added as a solvent, along with a three-dimensional conductive framework with a mass percentage m = 0.03. The mixture was ball-milled until homogeneous and dried. Then, it was sintered at 450 °C for 4 hours under a nitrogen atmosphere to obtain a composite solid electrolyte.
[0064] The electronic conductivity of the three-dimensional conductive framework in this embodiment was tested. =2953.2 S / cm, electronic conductivity of composite solid electrolyte =1.8S / cm, =0.02.
[0065] Example 11 A composite solid electrolyte, wherein the conductive material of the three-dimensional conductive framework is carbon nanotubes, and the raw material of the sulfide solid electrolyte is Li6PS5Cl.
[0066] Its preparation method is as follows: (1) Synthesis of a three-dimensional conductive framework: 1.0 g of carbon nanotubes were added to water, along with 0.05 g of PVP and 0.2 g of silicone oil as dispersant and spheroidizing agent, respectively. The mixture was sonicated at 60 °C with simultaneous stirring for 2 hours to ensure thorough winding and dispersion of the carbon nanotubes. The dispersion was then spray-dried (at 100 °C) to obtain a three-dimensional conductive framework.
[0067] (2) Synthesis of composite solid electrolytes: 1.0 g Li₂S, 0.97 g LiCl, and 0.37 g P₂S₅ were thoroughly ground and mixed according to stoichiometric ratio to obtain raw material Li₆PS₅Cl. 100 mL of xylene was added as a solvent, along with a three-dimensional conductive framework with a mass percentage m = 0.19. The mixture was ball-milled thoroughly until homogeneous and then dried. Finally, it was sintered at 450 °C for 4 hours under a nitrogen atmosphere to obtain a composite solid electrolyte.
[0068] The electronic conductivity of the three-dimensional conductive framework in this embodiment was tested. =1938.2 S / cm, electronic conductivity of composite solid electrolyte =184.3 S / cm, =0.50.
[0069] Comparative Example 1 A composite solid electrolyte, wherein the conductive material of the three-dimensional conductive framework is carbon nanotubes, and the raw material of the sulfide solid electrolyte is Li6PS5Cl.
[0070] Its preparation method is as follows: (1) Synthesis of a three-dimensional conductive framework: 1.0 g of carbon nanotubes were added to water, along with 0.15 g of PVP and 0.30 g of silicone oil as dispersant and spheroidizing agent, respectively. The mixture was sonicated at 60 °C with simultaneous stirring for 2 hours to ensure thorough entanglement and dispersion of the carbon nanotubes. The dispersion was then spray-dried (at 150 °C) to obtain a three-dimensional conductive framework.
[0071] (2) Synthesis of composite solid electrolytes: 1.0 g Li₂S, 0.97 g LiCl, and 0.37 g P₂S₅ were thoroughly ground and mixed according to stoichiometric ratio to obtain raw material Li₆PS₅Cl. 100 mL of xylene was added as a solvent, along with a three-dimensional conductive framework with a mass percentage m = 0.07. The mixture was ball-milled thoroughly until homogeneous and then dried. Finally, it was sintered at 450 °C for 4 hours under a nitrogen atmosphere to obtain a composite solid electrolyte.
[0072] The electronic conductivity of this comparative three-dimensional conductive framework was tested. =2741.5 S / cm, electronic conductivity of composite solid electrolyte =14.0 S / cm, =0.07.
[0073] Comparative Example 2 A composite solid electrolyte, wherein the conductive material of the three-dimensional conductive framework is carbon nanotubes, and the raw material of the sulfide solid electrolyte is Li6PS5Cl.
[0074] Its preparation method is as follows: (1) Synthesis of a three-dimensional conductive framework: 1.0 g of carbon nanotubes were added to water, along with 0.50 g of PVP and 0.50 g of silicone oil as dispersant and spheroidizing agent, respectively. The mixture was sonicated at 60 °C with simultaneous stirring for 2 hours to ensure thorough winding and dispersion of the carbon nanotubes. The dispersion was then spray-dried (at 100 °C) to obtain a three-dimensional conductive framework.
[0075] (2) Synthesis of composite solid electrolytes: 1.0 g Li₂S, 0.97 g LiCl, and 0.37 g P₂S₅ were thoroughly ground and mixed according to stoichiometric ratio to obtain raw material Li₆PS₅Cl. 100 mL of xylene was added as a solvent, along with a three-dimensional conductive framework with a mass percentage m = 0.39. The mixture was ball-milled thoroughly until homogeneous and then dried. Finally, it was sintered at 450 °C for 4 hours under a nitrogen atmosphere to obtain a composite solid electrolyte.
[0076] The electronic conductivity of this comparative three-dimensional conductive framework was tested. =1948.0 S / cm, electronic conductivity of composite solid electrolyte =24.1S / cm, =0.03.
[0077] Comparative Example 3 A composite solid electrolyte, wherein the conductive material of the three-dimensional conductive framework is carbon nanotubes, and the raw material of the sulfide solid electrolyte is Li6PS5Cl.
[0078] Its preparation method is as follows: (1) Synthesis of a three-dimensional conductive framework: 1.0 g of carbon nanotubes were added to water, along with 0.40 g of PVP and 0.20 g of silicone oil as dispersant and spheroidizing agent, respectively. The mixture was sonicated at 60 °C with simultaneous stirring for 2 hours to ensure thorough entanglement and dispersion of the carbon nanotubes. The dispersion was then spray-dried (at 100 °C) to obtain a three-dimensional conductive framework.
[0079] (2) Synthesis of composite solid electrolytes: 1.0 g Li₂S, 0.97 g LiCl, and 0.37 g P₂S₅ were thoroughly ground and mixed according to stoichiometric ratio to obtain raw material Li₆PS₅Cl. 100 mL of xylene was added as a solvent, along with a three-dimensional conductive framework with a mass percentage m = 0.30. The mixture was ball-milled thoroughly until homogeneous and then dried. Finally, it was sintered at 450 °C for 4 hours under a nitrogen atmosphere to obtain a composite solid electrolyte.
[0080] The electronic conductivity of this comparative three-dimensional conductive framework was tested. =0.8S / cm, electronic conductivity of composite solid electrolyte =0.1S / cm, =0.42.
[0081] Comparative Example 4 A composite solid electrolyte, wherein the conductive material of the three-dimensional conductive framework is carbon nanotubes, and the raw material of the sulfide solid electrolyte is Li6PS5Cl.
[0082] Its preparation method is as follows: (1) Synthesis of a three-dimensional conductive framework: 1.0 g of carbon nanotubes were added to water, along with 0.10 g of PVP and 0.25 g of silicone oil as dispersant and spheroidizing agent, respectively. The mixture was sonicated at 60 °C with simultaneous stirring for 2 hours to ensure thorough entanglement and dispersion of the carbon nanotubes. The dispersion was then spray-dried (at 150 °C) to obtain a three-dimensional conductive framework.
[0083] (2) Synthesis of composite solid electrolytes: 1.0 g Li₂S, 0.97 g LiCl, and 0.37 g P₂S₅ were thoroughly ground and mixed according to stoichiometric ratio to obtain raw material Li₆PS₅Cl. 100 mL of xylene was added as a solvent, along with a three-dimensional conductive framework with a mass percentage m = 0.10. The mixture was ball-milled until homogeneous and dried. Then, it was sintered at 450 °C for 4 hours under a nitrogen atmosphere to obtain a composite solid electrolyte.
[0084] The electronic conductivity of this comparative three-dimensional conductive framework was tested. =110482 S / cm, electronic conductivity of composite solid electrolyte =283.2S / cm, =0.03.
[0085] Comparative Example 5 A composite solid electrolyte, wherein the conductive material of the three-dimensional conductive framework is carbon nanotubes, and the raw material of the sulfide solid electrolyte is Li6PS5Cl.
[0086] Its preparation method is as follows: (1) Synthesis of a three-dimensional conductive framework: 1.0 g of carbon nanotubes were added to water, along with 0.20 g of PVP and 0.10 g of silicone oil as dispersant and spheroidizing agent, respectively. The mixture was sonicated at 60 °C with simultaneous stirring for 2 hours to ensure thorough entanglement and dispersion of the carbon nanotubes. The dispersion was then spray-dried (at 200 °C) to obtain a three-dimensional conductive framework.
[0087] (2) Synthesis of composite solid electrolytes: 1.0 g Li₂S, 0.97 g LiCl, and 0.37 g P₂S₅ were thoroughly ground and mixed according to stoichiometric ratio to obtain raw material Li₆PS₅Cl. 100 mL of xylene was added as a solvent, along with a three-dimensional conductive framework with a mass percentage m = 0.10. The mixture was ball-milled until homogeneous and dried. Then, it was sintered at 450 °C for 4 hours under a nitrogen atmosphere to obtain a composite solid electrolyte.
[0088] The electronic conductivity of this comparative three-dimensional conductive framework was tested. =10.6 S / cm, electronic conductivity of composite solid electrolyte =0.04S / cm, =0.04.
[0089] Comparative Example 6 A composite solid electrolyte, wherein the conductive material of the three-dimensional conductive framework is carbon nanotubes, and the raw material of the sulfide solid electrolyte is Li6PS5Cl.
[0090] Its preparation method is as follows: (1) Synthesis of a three-dimensional conductive framework: 1.0 g of carbon nanotubes were added to water, along with 0.15 g of PVP and 0.05 g of silicone oil as dispersant and spheroidizing agent, respectively. The mixture was sonicated at 60 °C with simultaneous stirring for 2 hours to ensure thorough winding and dispersion of the carbon nanotubes. The dispersion was then spray-dried (at 180 °C) to obtain a three-dimensional conductive framework.
[0091] (2) Synthesis of composite solid electrolytes: 1.0 g Li₂S, 0.97 g LiCl, and 0.37 g P₂S₅ were thoroughly ground and mixed according to stoichiometric ratio to obtain raw material Li₆PS₅Cl. 100 mL of xylene was added as a solvent, along with a three-dimensional conductive framework with a mass percentage m = 0.30. The mixture was ball-milled thoroughly until homogeneous and then dried. Finally, it was sintered at 450 °C for 4 hours under a nitrogen atmosphere to obtain a composite solid electrolyte.
[0092] The electronic conductivity of this comparative three-dimensional conductive framework was tested. =8941.8 S / cm, electronic conductivity of the composite solid electrolyte =1089.3S / cm, =0.41.
[0093] Comparative Example 7 A composite solid electrolyte, wherein the conductive material of the three-dimensional conductive framework is carbon nanotubes, and the raw material of the sulfide solid electrolyte is Li6PS5Cl.
[0094] Its preparation method is as follows: (1) Synthesis of a three-dimensional conductive framework: 1.0 g of carbon nanotubes were added to water, along with 0.40 g of PVP and 1.00 g of silicone oil as dispersant and spheroidizing agent, respectively. The mixture was sonicated at 60 °C with simultaneous stirring for 2 hours to ensure thorough entanglement and dispersion of the carbon nanotubes. The dispersion was then spray-dried (at 100 °C) to obtain a three-dimensional conductive framework.
[0095] (2) Synthesis of composite solid electrolytes: 1.0 g Li₂S, 0.97 g LiCl, and 0.37 g P₂S₅ were thoroughly ground and mixed according to stoichiometric ratio to obtain raw material Li₆PS₅Cl. 100 mL of xylene was added as a solvent, along with a three-dimensional conductive framework with a mass percentage m = 0.10. The mixture was ball-milled until homogeneous and dried. Then, it was sintered at 450 °C for 4 hours under a nitrogen atmosphere to obtain a composite solid electrolyte.
[0096] The electronic conductivity of this comparative three-dimensional conductive framework was tested. =1883.9 S / cm, electronic conductivity of composite solid electrolyte =2.1S / cm, =0.01.
[0097] Comparative Example 8 A composite solid electrolyte, wherein the conductive material of the three-dimensional conductive framework is carbon nanotubes, and the raw material of the sulfide solid electrolyte is Li6PS5Cl.
[0098] Its preparation method is as follows: (1) Synthesis of a three-dimensional conductive framework: 1.0 g of carbon nanotubes were added to water, along with 0.30 g of PVP and 0.70 g of silicone oil as dispersant and spheroidizing agent, respectively. The mixture was sonicated at 60 °C with simultaneous stirring for 2 hours to ensure thorough entanglement and dispersion of the carbon nanotubes. The dispersion was then spray-dried (at 120 °C) to obtain a three-dimensional conductive framework.
[0099] (2) Synthesis of composite solid electrolytes: 1.0 g Li₂S, 0.97 g LiCl, and 0.37 g P₂S₅ were thoroughly ground and mixed according to stoichiometric ratio to obtain raw material Li₆PS₅Cl. 100 mL of xylene was added as a solvent, along with a three-dimensional conductive framework with a mass percentage m = 0.10. The mixture was ball-milled until homogeneous and dried. Then, it was sintered at 450 °C for 4 hours under a nitrogen atmosphere to obtain a composite solid electrolyte.
[0100] The electronic conductivity of this comparative three-dimensional conductive framework was tested. =1436.4 S / cm, electronic conductivity of the composite solid electrolyte =98.3S / cm, =0.68.
[0101] Comparative Example 9 According to the component ratio of Example 1, carbon nanotubes and Li6PS5Cl were simply physically mixed, rather than through a three-dimensional framework composite method.
[0102] Comparative Example 10 No carbon nanotubes were added; only Li6PS5Cl was used. The remaining steps were the same as in Example 1.
[0103] Test Solid-state batteries were prepared using composite solid-state electrolytes from Examples 1-11 and Comparative Examples 1-10, respectively, and the preparation methods are as follows: LiNi 0.8 Co 0.1 Mn 0.1O2: composite solid electrolyte: VGCF: SEBS: xylene are uniformly mixed in a ratio of 85:10:3:2:100 to form a slurry, which is then uniformly coated onto carbon-coated aluminum foil and dried in an oven at 60°C to obtain the positive electrode sheet. Micron-sized silicon, the composite solid electrolyte, VGCF, SEBS, and xylene were uniformly mixed in a ratio of 80:15:3:2:100 to form a slurry, which was then uniformly coated onto a carbon-coated copper foil and dried in an oven at 60°C to obtain a negative electrode sheet. Take 100mg of Li6PS5Cl powder and place it in a solid-state battery mold with a diameter of 10mm, and compact it with a pressure of 1t; then place the positive electrode sheet on one side of the mold and compact it with a pressure of 2t; finally place the negative electrode sheet on the other side of the mold and compact it with a pressure of 1t; finally, compact the entire mold with a pressure of 1t to obtain a solid-state battery.
[0104] To measure the 0.1C capacity (mAh / g) of a solid-state battery: charge at a constant current of 0.1C to 4.2V, then at a constant voltage of 4.2V to 0.05C, and let stand for 10 minutes; discharge at 0.1C to 2.5V, and record the discharge capacity as the 0.1C capacity. To measure the 1C capacity (mAh / g) of a solid-state battery: charge it at a constant current of 1C to 4.2V, then at a constant voltage of 4.2V to 0.05C, and let it rest for 10 minutes; discharge it at 1C to 2.5V, and record the discharge capacity as the 1C capacity. Calculate the 1C / 0.1C capacity retention rate of a solid-state battery: Record the ratio of the 1C capacity to the 0.1C capacity as the 1C / 0.1C capacity retention rate; The capacity retention rate of a solid-state battery after 200 cycles was measured as follows: The battery was charged at a constant current of 1C to 4.2V, then charged at a constant voltage of 4.2V to 0.05C, and left to rest for 10 minutes; finally, it was discharged at 1C to 2.5V. This constitutes one cycle. The ratio of the discharge capacity of the 200th cycle to that of the 1st cycle was recorded as the capacity retention rate after 200 cycles.
[0105] The measurement results are shown in Table 1.
[0106] Table 1. Capacity retention at 1C, 0.1C, and 1C / 0.1C, and capacity retention after 200 cycles.
[0107] As shown in Table 1, Examples 1 to 3 fully satisfy the requirements. The porous framework maximizes electronic conductivity, and the sulfide solid electrolyte maximizes ionic conductivity, resulting in all-solid-state batteries with optimal specific capacity, 1C / 0.1C capacity retention, and 200-cycle capacity retention performance. Examples 4-5, 6-7, 8-9, and 10-11 represent the boundary values. Their specific capacity utilization, 1C / 0.1C capacity retention, and 200-cycle capacity retention are slightly worse than those of Examples 1-3, but are still at a relatively high level. Comparative Examples 1 to 8 show that the performance of the porous framework and sulfide solid electrolyte exceeds the upper and lower limits, and the specific capacity, 1C / 0.1C capacity retention and 200-cycle capacity retention are poor. Comparative Example 9 simply mixed carbon nanotubes and sulfide solid electrolyte according to the raw material ratio of Example 1, which could not improve the bulk electronic conductivity of the sulfide solid electrolyte, and the specific capacity, 1C / 0.1C capacity retention and 200-cycle capacity retention were even worse. Furthermore, when carbon nanotubes were not added, Comparative Example 10 exhibited the worst performance in terms of specific capacity, 1C / 0.1C capacity retention, and 200-cycle capacity retention.
[0108] Therefore, the present invention adopts the above-mentioned composite solid electrolyte and its preparation method and application. Through the composite structure design of a three-dimensional porous conductive framework and a sulfide solid electrolyte, a continuous, three-dimensional interconnected electron transport network is constructed inside the sulfide solid electrolyte, while maintaining the continuity of the ion transport channel, thus realizing the dual conduction function of ions and electrons.
[0109] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention and not to limit them. Although the present invention has been described in detail with reference to preferred embodiments, those skilled in the art should understand that modifications or equivalent substitutions can still be made to the technical solutions of the present invention, and these modifications or equivalent substitutions cannot cause the modified technical solutions to deviate from the spirit and scope of the technical solutions of the present invention.
Claims
1. A composite solid electrolyte, characterized in that: The composite solid electrolyte comprises a three-dimensional conductive framework and a sulfide solid electrolyte filled within the three-dimensional conductive framework, wherein the three-dimensional conductive framework accounts for m% of the mass of the composite solid electrolyte. The electronic conductivity of the three-dimensional conductive framework is , The electronic conductivity of the composite solid electrolyte is , The composite solid electrolyte satisfies .
2. The composite solid electrolyte according to claim 1, characterized in that: The conductive material of the three-dimensional conductive framework is one or more of the following: carbon nanotubes, carbon nanofibers, graphene, flake graphite, porous carbon, aerogel, silver nanowires, porous silver, porous nickel, TiO2, TiN, MoS2, Ti3C2, MOF, and MXene.
3. The composite solid electrolyte according to claim 1, characterized in that: The raw materials for the sulfide solid electrolyte are Li3PS4, Li8P2S9, Li6PS5Cl, Li6PS5Br, Li6PS5I, and Li6PS5Cl. 0.5 Br 0.5 Li 5.5 PS 4.5 Cl 1.5 Li 6- x PS 5-x Cl 1+x Li 10 GeP2S 12 Li4SnS4, Li 9.54 Si 1.74 P 1.44 S 11.7 Cl 0.3 Li 6+x M x P 1-x S 5x One or more of the following; The Li 6-x PS 5-x Cl 1+x middle ; The Li 6+x M x P 1-x S 5x middle M is selected from one or more of Si, Ge, and Sn.
4. A method for preparing a composite solid electrolyte as described in any one of claims 1 to 3, characterized in that: This includes one of the following methods: vapor deposition, sol-gel method, in-situ growth method, electrodeposition method, and emulsion method.
5. The method for preparing a composite solid electrolyte according to claim 4, characterized in that, Includes the following steps: S1. Preparation of three-dimensional conductive framework: The conductive material is added to the solvent, along with a dispersant and a spheroidizing agent. After ultrasonic dispersion and stirring, the mixture is spray-dried to obtain a three-dimensional porous conductive framework. S2. Preparation of composite solid electrolyte: The raw materials of sulfide solid electrolyte are mixed with the three-dimensional porous conductive framework obtained in S1, an organic solvent is added, the mixture is ball-milled and dried, and then sintered under a protective atmosphere to obtain the composite solid electrolyte.
6. The method for preparing a composite solid electrolyte according to claim 5, characterized in that, In S2, the raw materials for the sulfide solid electrolyte are one or more of lithium sulfide, lithium chloride, and phosphorus pentasulfide mixed in stoichiometric proportions.
7. The application of a composite solid electrolyte as described in any one of claims 1 to 3 in the preparation of a solid-state battery.
8. The application according to claim 7, characterized in that: The solid-state battery includes a positive electrode, an electrolyte sheet, and a negative electrode. The negative electrode contains the composite solid electrolyte and does not contain any other conductive agents.
9. The application according to claim 8, characterized in that: The other conductive agents are one or more of the following: carbon nanotubes, conductive carbon black, carbon nanofibers, graphene, flake graphite, Ketjen black, and porous carbon.
Citation Information
Patent Citations
Composite positive plate, preparation method thereof and all-solid-state lithium ion battery
CN121172052A
Sulfide electrolyte material and preparation method thereof, positive plate, secondary battery, battery assembly and electric equipment
CN121964800A