An oxide solid electrolyte ceramic sheet, its preparation method, and a solid-state battery

By controlling the particle size and particle size distribution of oxide solid electrolytes, and by adopting a compounding process and optimizing the sintering process, the problems of insufficient grain boundary impedance and density of oxide solid electrolyte ceramic sheets were solved, thereby improving ionic conductivity and mechanical strength.

CN123120847APending Publication Date: 2026-11-17DONGFENG MOTOR GRP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611447611.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-17
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing oxide solid electrolyte ceramic sheets suffer from problems such as excessive grain boundary impedance or insufficient density during the preparation process, which limits the improvement of ionic conductivity.

Method used

By adjusting the particle size and particle size distribution of the oxide solid electrolyte, and using a compounding process, the particle size ranges of the first and second oxide solid electrolytes are controlled to be D1

Benefits of technology

This study achieved high density and low grain boundary impedance in oxide solid electrolyte ceramic sheets, which improved the overall ionic conductivity and enhanced mechanical strength and electrochemical stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123120847A_ABST
    Figure CN123120847A_ABST
Patent Text Reader

Abstract

This invention belongs to the field of solid-state battery technology, and relates to an oxide solid-state electrolyte ceramic sheet, its preparation method, and a solid-state battery. The oxide solid-state electrolyte ceramic sheet comprises a first oxide solid-state electrolyte and a second oxide solid-state electrolyte; wherein: the first oxide solid-state electrolyte has a Dv... 50 D1, the Dv of the second oxide solid electrolyte 50 For D2, D1 < D2 ≤ 5 μm, the Dv of the first oxide solid electrolyte is... 90 D3, the Dv of the second oxide solid electrolyte 90 The particle size distribution is D4; D3 < D4 ≤ 10 μm. This invention improves the total ionic conductivity by controlling the particle size and distribution of oxide solid electrolytes, thereby achieving synergistic optimization of the number of grain boundaries and porosity in the microstructure of the resulting oxide solid electrolyte ceramic sheets.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of solid-state battery technology, and relates to an oxide solid electrolyte ceramic sheet, its preparation method, and a solid-state battery. Background Technology

[0002] With the rapid development of new energy vehicles and portable electronic devices, the demand for energy storage devices with high energy density and high safety is increasing. Solid-state batteries, because they eliminate flammable and leaky organic liquid electrolytes and use non-flammable solid electrolytes, are considered one of the most promising next-generation battery technologies. Among the many solid electrolyte systems, oxide solid electrolytes have become a research hotspot due to their high ionic conductivity, wide electrochemical window, and good air stability.

[0003] Oxide solid electrolytes typically require high-temperature sintering to form dense ceramic sheets before they can be used as electrolyte separators in batteries. The ion conductivity of oxide electrolyte ceramic sheets depends not only on the intrinsic structure of the material but also on the degree of micro-density, grain size, and number of grain boundaries. Current manufacturing processes often involve direct pressing and sintering of single-size powders, resulting in ceramic sheets with high grain boundary impedance or insufficient density, thus limiting further improvements in room-temperature ion conductivity. Alternatively, sintering aids can be introduced to weaken the grain boundary impedance between oxide electrolytes, thereby improving the overall ion conductivity of the ceramic sheet. However, excessive addition can reduce the effective conductivity ratio of the oxide electrolyte and affect the phase composition, mechanical properties, and electrochemical stability of the ceramic sheet. Summary of the Invention

[0004] This invention aims to solve the technical problem that existing oxide solid electrolyte ceramics without sintering aids cannot simultaneously achieve high density and low grain boundary resistance, resulting in low ionic conductivity. Based on this, this invention provides an oxide solid electrolyte ceramic sheet, its preparation method, and a solid-state battery.

[0005] The technical solution provided by this invention is as follows: In a first aspect, the present invention provides an oxide solid electrolyte ceramic sheet, wherein the material of the oxide solid electrolyte ceramic sheet includes a first oxide solid electrolyte and a second oxide solid electrolyte; in: The first oxide solid electrolyte has a Dv50 of D1, and the second oxide solid electrolyte has a Dv50 of D2, where D1 < D2 ≤ 5 μm. The first oxide solid electrolyte has a Dv90 of D3, and the second oxide solid electrolyte has a Dv90 of D4; D3 < D4 ≤ 10 μm.

[0006] In conjunction with the first aspect of the invention, in a specific embodiment of the invention, D1 < D2 ≤ 3 μm; and / or, D3<D4≤5μm.

[0007] In conjunction with the first aspect of the present invention, in a specific embodiment of the present invention, the mass ratio of the first oxide solid electrolyte and the second oxide solid electrolyte is (0.11~0.67):1.

[0008] In conjunction with the first aspect of the present invention, in a specific embodiment of the present invention, the first oxide solid electrolyte and the second oxide solid electrolyte are respectively selected from at least one of NASICON type oxide solid electrolyte, garnet type oxide solid electrolyte or perovskite type oxide solid electrolyte.

[0009] Secondly, the present invention provides a method for preparing an oxide solid electrolyte ceramic sheet, comprising the following preparation steps: The first oxide solid electrolyte and the second oxide solid electrolyte are mixed with additives and granulated to obtain a molded powder. The molding powder is pressed into shape to obtain an oxide solid electrolyte preform. The oxide solid electrolyte preform is debinded and sintered to obtain an oxide solid electrolyte ceramic sheet; in: The material of the oxide solid electrolyte ceramic sheet includes a first oxide solid electrolyte and a second oxide solid electrolyte; The first oxide solid electrolyte has a Dv50 of D1, and the second oxide solid electrolyte has a Dv50 of D2; D1 < D2 ≤ 5 μm. The first oxide solid electrolyte has a Dv90 of D3, and the second oxide solid electrolyte has a Dv90 of D4; D3 < D4 ≤ 10 μm.

[0010] In conjunction with the second aspect of the present invention, in a specific embodiment of the present invention, the pressing pressure is 50 MPa to 400 MPa; and / or, The temperature for discharging the adhesive is 200℃~600℃; and / or, The sintering heating rate is 1℃ / min to 5℃ / min; and / or, The heat preservation time is 1 hour to 12 hours.

[0011] In conjunction with the second aspect of the present invention, in a specific embodiment of the present invention, if the oxide solid electrolyte is a perovskite type oxide solid electrolyte, the sintering temperature is 800℃~1300℃.

[0012] In conjunction with the second aspect of the present invention, in a specific embodiment of the present invention, if the oxide solid electrolyte is a NASICON type oxide solid electrolyte, the sintering temperature is 800℃~1100℃.

[0013] In conjunction with the second aspect of the present invention, in a specific embodiment of the present invention, if the oxide solid electrolyte is a garnet-type oxide solid electrolyte, the sintering temperature is 1050℃~1250℃.

[0014] Thirdly, the present invention provides a solid-state battery comprising the aforementioned oxide solid electrolyte ceramic sheet.

[0015] Compared with the prior art, the present invention has at least the following beneficial effects: This invention addresses two problems in existing processes: excessively fine powder leading to excessive grain boundary impedance and excessively coarse powder leading to insufficient ceramic density. By controlling the particle size and distribution of oxide solid electrolytes, this invention achieves synergistic optimization of the number of grain boundaries and porosity in the microstructure of the resulting oxide solid electrolyte ceramic sheet, thereby improving its total ionic conductivity.

[0016] The oxide solid electrolyte ceramic sheet prepared by this invention has high sintering density, low grain boundary impedance, and good structural uniformity, making it suitable for applications such as electrolyte layers in all-solid-state batteries, composite electrode frameworks, and other applications requiring ceramic sheets with high ionic conductivity. Compared with directly using a single ultrafine powder or a single coarse powder, this invention is more advantageous in obtaining oxide solid electrolyte ceramic sheets that possess both high ionic conductivity and high mechanical strength.

[0017] The process of this invention is simple, mainly using conventional ball milling, sieving, tableting, and sintering equipment. The process has good repeatability, is easy to scale up, and has good prospects for engineering applications. Furthermore, this invention is not limited to a specific oxide electrolyte system and has good applicability to various oxide solid electrolyte materials. Attached Figure Description

[0018] To more clearly illustrate the technical solutions in the embodiments of the present invention, the accompanying drawings used in the description of the embodiments will be briefly introduced below. Obviously, the accompanying drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.

[0019] Figure 1 This is a normal distribution diagram of the particle size of the LATP first oxide solid electrolyte provided in Example 1 of the present invention; Figure 2 This is a normal particle size distribution diagram of the LATP second oxide solid electrolyte provided in Example 1 of the present invention; Figure 3 EIS impedance diagram of the ceramic sheet prepared in Example 1; Figure 4 The image shows the EIS impedance diagram of the ceramic sheet prepared in Comparative Example 1. Detailed Implementation

[0020] To make the objectives, technical solutions, and advantages of this invention clearer, the technical solutions of this invention will be clearly and completely described below in conjunction with the embodiments of this invention. Obviously, the described embodiments are only some, not all, of the embodiments of this invention. Based on the embodiments of this invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of this invention.

[0021] The abbreviations involved in this invention have the following meanings: LLZO is lithium lanthanum zirconium oxide; LATP is lithium aluminum titanium phosphate; NASICON type oxide solid electrolyte is sodium superionic conductor type oxide solid electrolyte; Dv50 is the particle size corresponding to a cumulative volume percentage of 50% in the sample; Dv90 is the particle size corresponding to a cumulative volume percentage of 90% in the sample.

[0022] Oxide solid electrolytes possess high chemical stability, a wide electrochemical window, and good mechanical strength, making them promising candidates for application in all-solid-state lithium batteries. However, the ion conductivity of oxide electrolyte ceramic sheets depends not only on the material's structure but also on the degree of micro-density, grain size, and number of grain boundaries. Current manufacturing processes typically involve direct pressing and sintering of single-size powders, often resulting in ceramic sheets with high grain boundary impedance or insufficient density, thus limiting further improvements in room-temperature ionic conductivity. Alternatively, sintering aids can be introduced to weaken the grain boundary impedance between oxide ceramic electrolytes, thereby improving the overall ionic conductivity of the ceramic sheet. Existing sintering aids include lithium phosphate (Li3PO4), boron oxide (B2O3), and lithium tetrafluoroborate (LiBF4).

[0023] For example, methods for manufacturing composite oxide powders, solid electrolytes, and lithium-ion secondary batteries often employ a single powder refinement strategy without proposing preparation processes that combine coarse and fine powders, optimize particle size distribution, or optimize particle size windows. For ceramic sheets, ionic conductivity is not solely determined by powder fineness but is simultaneously influenced by porosity, grain size, grain boundary number, and grain boundary impedance. These preparation processes fail to establish a balance between increasing density and reducing grain boundary impedance, thus making it difficult to address the problem of excessive grain boundaries after sintering fine powder.

[0024] For example, lithium-ion conductive solid electrolytes, their manufacturing methods, and all-solid-state batteries rely on the addition of Li3BO3 sintering aids to improve interparticle contact. Essentially, this involves introducing a low-melting-point or easily softened second phase to fill the voids between LLZO particles, rather than optimizing the ceramic sheet microstructure by controlling the particle size and distribution of the oxide electrolyte powder itself. While this can improve particle contact to some extent, it does not resolve the inherent contradiction between excessively fine oxide electrolyte powder particles leading to increased grain boundaries and excessively coarse particles resulting in residual porosity.

[0025] In a first aspect, the present invention provides an oxide solid electrolyte ceramic sheet, wherein the material of the oxide solid electrolyte ceramic sheet includes a first oxide solid electrolyte and a second oxide solid electrolyte; wherein: the Dv50 of the first oxide solid electrolyte is D1, the Dv50 of the second oxide solid electrolyte is D2, D1 < D2 ≤ 5 μm, the Dv90 of the first oxide solid electrolyte is D3, the Dv90 of the second oxide solid electrolyte is D4, and D3 < D4 ≤ 10 μm. Dv90 reflects the upper limit of the size of large particles in the solid electrolyte powder and is a key parameter for controlling the tail end of the particle size distribution. Excessively large particles will become abnormally large seeds during sintering, forming coarse grains, cracks, and pores. Controlling Dv90 can eliminate these large particles and ensure a uniform microstructure after sintering. Dv50 represents the median particle size, reflecting the main size characteristics of the powder. The smaller the Dv50, the larger the specific surface area and the higher the surface energy of the powder, the stronger the sintering driving force, and the more densification can be achieved at lower temperatures or in a shorter time, which is beneficial for obtaining high-density ceramic sheets.

[0026] The ionic conductivity of oxide ceramic sheets is determined by the coupling of the ionic conductivity of the oxide electrolyte itself and the grain boundary impedance, and the density of the ceramic sheet directly affects the magnitude of the grain boundary impedance. Particle size control of sintered ceramic sheet powder can effectively reduce the formation of porosity within the ceramic sheet, thereby increasing ceramic density, reducing grain boundary impedance, and improving overall ionic conductivity.

[0027] In some specific embodiments of the present invention, D1 < D2 ≤ 3 μm. Compared to the range of D1 < D2 ≤ 5 μm, a smaller Dv50 (D1 < D2 ≤ 3 μm) during ceramic sintering is more conducive to the compactness of the ceramic sheet.

[0028] In some specific embodiments of the present invention, D3 < D4 ≤ 5 μm. Large-particle oxide solid electrolytes are prone to causing density inhomogeneity and microcracks during hydrostatic or dry pressing; compared to 10 μm, the upper limit of Dv90 is controlled within 5 μm, which can improve the uniformity of green body density and reduce the risk of sintering cracking.

[0029] In some specific embodiments of the present invention, the mass ratio of the first oxide solid electrolyte and the second oxide solid electrolyte is (0.11~0.67):1. Using this mass ratio to compound the first oxide solid electrolyte and the second oxide solid electrolyte makes the process repeatable and instructive.

[0030] Preferably, the mass ratio of the first oxide solid electrolyte and the second oxide solid electrolyte is (0.25~0.67):1.

[0031] In some specific embodiments of the present invention, the first oxide solid electrolyte and the second oxide solid electrolyte are respectively selected from at least one of NASICON type oxide solid electrolyte, garnet type oxide solid electrolyte or perovskite type oxide solid electrolyte.

[0032] Secondly, the present invention provides a method for preparing an oxide solid electrolyte ceramic sheet, comprising the following preparation steps: The first oxide solid electrolyte and the second oxide solid electrolyte are mixed with additives and granulated to obtain a molded powder. The molding powder is pressed into shape to obtain an oxide solid electrolyte preform. The oxide solid electrolyte preform is debinded and sintered to obtain an oxide solid electrolyte ceramic sheet; in: The material of the oxide solid electrolyte ceramic sheet includes a first oxide solid electrolyte and a second oxide solid electrolyte; The first oxide solid electrolyte has a Dv50 of D1, and the second oxide solid electrolyte has a Dv50 of D2; D1 < D2 ≤ 5 μm. The first oxide solid electrolyte has a Dv90 of D3, and the second oxide solid electrolyte has a Dv90 of D4; D3 < D4 ≤ 10 μm. The essence of particle size blending, i.e., bimodal or multimodal distribution, is to utilize small particles to fill the gaps between large particles, increasing the green body packing density, thereby optimizing sintering behavior and final performance. Furthermore, a single-particle-size system requires a highly consistent Dv50, while a blended system, through the complementarity of large and small particles, has greater tolerance to fluctuations in a single particle size.

[0033] In some specific embodiments of the present invention, the additives include one or more of organic binders, dispersants, or granulation media.

[0034] More specifically, a method for preparing an oxide electrolyte ceramic sheet includes the following steps: S1. Preparation of raw materials for oxide solid electrolyte: Prepare raw materials, including lithium source, aluminum source, titanium source and phosphate source, configured to form a solid electrolyte with the general formula Li. 1.3 Al0.3 Ti 1.7 (PO4)3 compound; the raw materials are thoroughly ball-milled and mixed, and then sintered in air at 800℃~1000℃ to obtain a bulk; the bulk is crushed to obtain an oxide solid electrolyte.

[0035] S2. Particle size control: The obtained oxide solid electrolyte is subjected to ball milling, air jet milling, grinding or sieving and classification to obtain oxide electrolyte within the target particle size range.

[0036] S3. Granulation and molding: The oxide solid electrolyte with controlled particle size is added to an organic binder, dispersant or granulation medium and mixed to obtain a molding powder with good flowability.

[0037] S4. Debinding and Sintering: The formed green blank is subjected to low-temperature debinding treatment and then sintered at high temperature to obtain oxide solid electrolyte ceramic sheets.

[0038] S5. Post-processing of ceramic sheets: After sintering, the oxide solid electrolyte ceramic sheets are taken out by natural cooling or programmed cooling, and then subjected to surface grinding, polishing or cutting to obtain electrolyte ceramic sheets with uniform thickness and flat surface.

[0039] In some specific embodiments of the present invention, in step S1, the lithium source is a compound that can provide lithium ions, including one or more of lithium oxide, lithium hydroxide, lithium carbonate, lithium phosphate, lithium hydrogen phosphate, and lithium nitrate.

[0040] In some specific embodiments of the present invention, in step S1, the aluminum source is a compound that can provide aluminum ions, including one or more of aluminum hydroxide, aluminum oxide, and aluminum phosphate.

[0041] In some specific embodiments of the present invention, in step S1, the titanium source is a compound that can provide titanium ions, including one or more of titanium dioxide and titanium phosphate.

[0042] In some specific embodiments of the present invention, in step S1, the phosphoric acid source is a compound that can provide phosphate ions, including one or more of phosphoric acid, ammonium phosphate, diammonium hydrogen phosphate, and ammonium dihydrogen phosphate.

[0043] Preferably, the lithium source is lithium carbonate, lithium oxide, and lithium nitrate; the aluminum source is aluminum oxide and aluminum hydroxide; the titanium source is titanium dioxide; and the phosphoric acid source is diammonium hydrogen phosphate and diammonium dihydrogen phosphate.

[0044] In some specific embodiments of the present invention, in step S2, the principle for controlling the particle size of the oxide solid electrolyte is to avoid excessively small particle size leading to an excessive number of grain boundaries and increased grain boundary impedance after sintering, while avoiding excessively large powder particle size leading to insufficient compaction, residual pores, and decreased density.

[0045] Preferably, the controlled particle size Dv50 is not higher than 3 μm, more preferably not higher than 2 μm; and the controlled particle size Dv90 is not higher than 10 μm, more preferably not higher than 5 μm. During the sintering process of the electrolyte ceramic sheet, large voids and obvious grain boundaries are more likely to form around the 10 μm large particle powder, so a smaller particle size of the second oxide solid electrolyte powder is selected; for the first oxide solid electrolyte powder, a smaller particle size is more conducive to filling the voids between large particles, which is beneficial to improving the density of the ceramic.

[0046] More preferably, the oxide electrolyte can be divided into a first oxide solid electrolyte and a second oxide solid electrolyte, wherein the Dv of the first oxide solid electrolyte is... 50 The Dv of the second oxide solid electrolyte is 0.2~1μm. 50 The particle size is 1~5μm, and then compounded according to a certain mass ratio to improve the stacking efficiency during the tableting process and the density of the ceramic after sintering.

[0047] In step S3, the binder can be one or more of polyvinyl alcohol, polyethylene glycol, and polyvinylpyrrolidone; the preferred addition amount is 0.5wt% to 5wt% by mass. Then, the oxide electrolyte preform is obtained by molding, dry pressing, cold isostatic pressing, or casting followed by stamping.

[0048] In some specific embodiments of the present invention, the preferred tableting pressure is 50MPa to 400MPa.

[0049] More preferably, the tableting pressure is 100MPa~300MPa to increase the initial packing density of the preform.

[0050] In some specific embodiments of the present invention, in step S4, the effective necking and densification between particles are promoted by controlling the heating rate, sintering temperature and holding time during the sintering process, while suppressing abnormal grain growth.

[0051] In some specific embodiments of the present invention, in step S4, the pressing pressure is 50MPa~400MPa.

[0052] In some specific embodiments of the present invention, in step S4, the temperature for removing the adhesive is 200℃~600℃. Removing the adhesive at this temperature allows the organic binder to fully decompose and volatilize, resulting in a denser final ceramic sheet.

[0053] In some specific embodiments of the present invention, in step S4, the heating rate of the sintering is 1℃ / min to 5℃ / min.

[0054] In some specific embodiments of the present invention, in step S4, the heat preservation time is 1h to 12h.

[0055] In some specific embodiments of the present invention, in step S4, the thickness of the oxide solid electrolyte ceramic sheet is 1.5~2mm.

[0056] In some specific embodiments of the present invention, in step S4, if the oxide solid electrolyte is a perovskite-type oxide solid electrolyte, the sintering temperature is 800℃~1300℃. This temperature is beneficial for a dense ceramic structure.

[0057] In some specific embodiments of the present invention, in step S4, if the oxide solid electrolyte is a NASICON-type oxide solid electrolyte, the sintering temperature is 800℃~1100℃. This temperature is beneficial for a dense ceramic structure.

[0058] In some specific embodiments of the present invention, in step S4, if the oxide solid electrolyte is a garnet-type oxide solid electrolyte, the sintering temperature is 1050℃~1250℃. This temperature is beneficial for a dense ceramic structure.

[0059] In some specific embodiments of the present invention, in step S5, hot pressing, surface modification, or interface layer construction may be performed if necessary to reduce the interface impedance in subsequent battery assembly. Finally, the ionic conductivity of the ceramic sheet is tested using an electrochemical workstation.

[0060] Thirdly, the present invention provides a solid-state battery comprising the aforementioned oxide solid electrolyte ceramic sheet.

[0061] The embodiments of the present invention will be described in detail below with reference to examples. However, those skilled in the art will understand that the following examples are for illustrative purposes only and should not be considered as limiting the scope of the invention. Unless otherwise specified in the examples, conventional conditions or conditions recommended by the manufacturer are followed. Reagents or instruments whose manufacturers are not specified are all commercially available conventional products.

[0062] Example 1 S1. Prepare raw materials: Weigh lithium carbonate, aluminum oxide, titanium dioxide, and diammonium hydrogen phosphate according to a molar ratio of 13:3:34:60. The raw materials are prepared to form a compound with the general formula Li. 1.3 Al 0.3 Ti 1.7 The compound of (PO4)3 (LATP); the raw materials are thoroughly ball-milled and mixed, and then sintered in air at 900°C to obtain a block; the block is then pulverized to obtain a powder.

[0063] S2. A first oxide solid electrolyte was prepared by ball milling with 5 mm ball milling beads for 4 hours. The median particle size of the first oxide solid electrolyte was D1=0.73μm and D3=1.53μm. A second oxide solid electrolyte was prepared by ball milling with 10 mm ball milling beads for 2 hours. The median particle size of the second oxide solid electrolyte was D2=2.02μm and D4=8.16μm. The mass ratio of the first oxide solid electrolyte to the second oxide solid electrolyte was selected as 0.43:1 for mixing.

[0064] S3. Weigh the first oxide solid electrolyte and the second oxide solid electrolyte from step S2 at a mass ratio of 0.43:1, add 1 wt% polyvinyl alcohol, mix evenly, and then cold press under 300 MPa pressure to obtain the oxide solid electrolyte preform.

[0065] S4. The oxide solid electrolyte preform obtained in step S3 is heated to 600°C at a heating rate of 5°C / min and held for 2 hours; then heated to 850°C at a heating rate of 5°C / min and held for 6 hours to obtain the oxide solid electrolyte ceramic sheet.

[0066] S5. The surface of the oxide solid electrolyte ceramic sheet obtained in step S4 is polished. The polishing process involves first using 400-grit sandpaper for initial grinding to remove the oxide layer and uneven areas on the sintered surface. Each pass of sandpaper is changed until the scratches are aligned. Then, 1200-grit, 2000-grit, and 2500-grit sandpaper are used sequentially to remove the scratches from the previous pass, reducing surface roughness and obtaining an electrolyte ceramic sheet with uniform thickness and a smooth surface. Next, an ion sputtering system is used. The ion sputtering process involves creating a vacuum in the ion sputtering system, controlling the gas flow rate, ensuring a current of 10 mA, maintaining this current for 200 seconds, and then completing single-sided gold plating. The ceramic sheet is then flipped over, and the process is repeated to plate gold on both sides. Finally, the ionic conductivity is measured using an electrochemical workstation and found to be 9.58 × 10⁻⁶. -4 The particle size statistics of the second oxide solid electrolyte and the first oxide solid electrolyte of LATP (S / cm) are shown in Tables 1 and 2.

[0067] Table 1. Particle size statistics of LATP primary oxide solid electrolyte.

[0068] Depend on Figure 1 Table 1 shows that when the cumulative percentage content (%) of LATP primary oxide solid electrolyte particles is 10.0%, 50.0%, and 90.0%, the corresponding average particle sizes are 0.30, 0.73, and 1.53 μm, respectively, with D1 being approximately 0.73 μm. Meanwhile, the coefficient of variation (CV[%]) decreases with increasing particle size, being 0.84, 0.66, and 0.34, respectively.

[0069] Table 2. Particle size statistics of LATP secondary oxide solid electrolyte.

[0070] Depend on Figure 2 Table 2 shows that when the cumulative percentage content (%) of LATP secondary oxide solid electrolyte particles is 10.0%, 50.0%, and 90.0%, the corresponding average particle sizes are 0.62, 2.02, and 8.16 μm, respectively, and D2 is approximately 2.02 μm. Meanwhile, the coefficient of variation (CV[%]) decreases with increasing particle size, being 2.55, 0.08, and 1.54, respectively.

[0071] Depend on Figure 3 As shown, the EIS impedance diagram of the ceramic sheet in Example 1; by Figure 4 As shown, the EIS impedance diagram of the ceramic sheet in Comparative Example 1 is presented. The formula for calculating ionic conductivity is: σ = 1 / R b , where R b This is the impedance value. (From...) Figure 3 , Figure 4 It can be seen that, according to the ionic conductivity formula, the ceramic sheet prepared by the dual-particle-size normal distribution powder compounding process in Example 1 has a better ionic conductivity than the ceramic sheet prepared by the single normal distribution powder in Comparative Example 1; thus proving the advantage of the particle size compounding process of the present invention.

[0072] Example 2 The preparation methods of Example 2 and Example 1 are roughly the same, except that in step S2, the mass ratio of the first oxide solid electrolyte to the second oxide solid electrolyte is 0.25:1, and the ionic conductivity values ​​of the oxide solid electrolyte ceramic sheet are shown in Table 3.

[0073] Example 3 The preparation methods of Example 3 and Example 1 are roughly the same, except that in step S2, the mass ratio of the first oxide solid electrolyte to the second oxide solid electrolyte is 0.67:1, and the ionic conductivity values ​​of the oxide solid electrolyte ceramic sheet are shown in Table 3.

[0074] Example 4 The preparation methods of Example 4 and Example 1 are roughly the same, except that in step S2, the mass ratio of the first oxide solid electrolyte to the second oxide solid electrolyte is 0.11:1, and the ionic conductivity values ​​of the oxide solid electrolyte ceramic sheet are shown in Table 3.

[0075] Example 5 The preparation methods of Example 5 and Example 1 are roughly the same, except that in step S2, the D1 of the first oxide solid electrolyte is 1 μm, the D2 of the second oxide solid electrolyte is 5 μm, and the ionic conductivity values ​​of the oxide solid electrolyte ceramic sheet are shown in Table 3.

[0076] Example 6 The preparation methods of Example 6 and Example 1 are roughly the same, except that in step S2, the D1 of the first oxide solid electrolyte is 0.2 μm, the D2 of the second oxide solid electrolyte is 1 μm, and the ionic conductivity values ​​of the oxide solid electrolyte ceramic sheet are shown in Table 3.

[0077] Comparative Example 1 The preparation methods of Comparative Example 1 and Example 1 are roughly the same, except that in step S2, only the D1 of the first oxide solid electrolyte is 0.73 μm. The ionic conductivity values ​​of the oxide solid electrolyte ceramic sheet are shown in Table 3.

[0078] Comparative Example 2 The preparation methods of Comparative Example 2 and Example 1 are roughly the same, except that in step S2, only the D2 of the second oxide solid electrolyte is 2.02 μm. The ionic conductivity values ​​of the oxide solid electrolyte ceramic sheet are shown in Table 3.

[0079] Comparative Example 3 The preparation methods of Comparative Example 3 and Example 1 are roughly the same, except that in step S2, the D1 of the first oxide solid electrolyte is 2 μm, the D2 of the second oxide solid electrolyte is 6 μm, and the ionic conductivity values ​​of the oxide solid electrolyte ceramic sheet are shown in Table 3.

[0080] Comparative Example 4: The preparation methods of Comparative Example 4 and Example 1 are roughly the same, except that in step S2, the mass ratio of the first oxide solid electrolyte to the second oxide solid electrolyte is 2.23:1, and the ionic conductivity values ​​of the oxide solid electrolyte ceramic sheet are shown in Table 3.

[0081] The performance of the oxide solid electrolyte ceramic sheets prepared in the embodiments and comparative examples of the present invention was tested using the following methods: Ionic conductivity testing method: Electrochemical impedance spectroscopy (EIS) was used. The ceramic sheet was sanded smooth on both sides (1.5mm~2mm thickness), and Au or Pt electrodes were symmetrically sputtered on both sides. It was then placed in a spring-loaded fixture of an electrochemical workstation. An AC perturbation of 10mV~50mV was applied, and the volume resistance Rb was obtained by high-frequency semicircular fitting of the Nyquist plot. This Rb was then substituted into σ=L / (Rb×A) to calculate the ionic conductivity (where L is the ceramic sheet thickness and A is the electrode area on the ceramic sheet surface).

[0082] Fine powder particle size analysis: The powder was dispersed in an inert medium such as ultrapure water (ratio of 1g powder to 100ml ultrapure water), and sonicated for 2-5 minutes to break up any agglomerates, thus obtaining a suspension. After the instrument preheated for 20 minutes, the background was measured using a pure medium as the background to subtract the background. The suspension was added dropwise to the circulating sample cell, and the shading ratio was controlled at 5%-15%. The circulation was started to maintain uniform suspension. After the shading ratio stabilized, three consecutive measurements were taken and the average was recorded. Dv10, Dv50, Dv90, and the distribution width were recorded.

[0083] Table 3 Performance data of ceramic sheets prepared in the examples and comparative examples

[0084] As shown in Tables 1 to 3, this invention effectively improves the ionic conductivity of oxide ceramic sheets through a particle size blending process. Specifically, by using LATP first oxide solid electrolyte with D1=0.73μm and D3=1.53μm and LATP second oxide solid electrolyte with D2=2.02μm and D4=8.16μm, blended at a mass ratio of 0.43:1, the ionic conductivity of the prepared ceramic sheets can reach 9.58×10⁻⁶. -4 S / cm. Compared to Comparative Examples 1 and 2, which used single-powder sintering, the improved ionic conductivity of the examples effectively demonstrates the effect of particle size blending on improving the ionic conductivity of ceramic sheets. Compared to Comparative Example 3, which used larger particle sizes, it is demonstrated that using smaller particle sizes is more conducive to achieving ceramic sheet densification and improving electrochemical performance. Compared to Comparative Example 4 with different mass ratios, it is demonstrated that the powder mass ratio in the range of (0.11~0.67):1 is more advantageous.

[0085] In summary, this invention solves two problems in existing processes by controlling the particle size and distribution of oxide solid electrolytes: excessively fine powder leading to excessive grain boundary impedance and excessively coarse powder leading to insufficient ceramic density. This allows the resulting oxide solid electrolyte ceramic sheets to achieve synergistic optimization of grain boundary quantity and porosity in their microstructure, thereby improving their total ionic conductivity.

[0086] In the description of this specification, the references to terms such as "one embodiment / mode," "some embodiments / modes," "example," "specific example," or "some examples," etc., indicate that a specific feature, structure, material, or characteristic described in connection with that embodiment / mode or example is included in at least one embodiment / mode or example of the present invention. In this specification, the illustrative expressions of the above terms do not necessarily refer to the same embodiment / mode or example. Moreover, the specific features, structures, materials, or characteristics described may be combined in any suitable manner in one or more embodiments / modes or examples. Furthermore, without contradiction, those skilled in the art can combine and integrate the different embodiments / modes or examples described in this specification, as well as the features of different embodiments / modes or examples.

[0087] It should be noted that in this invention, relational terms such as "first" and "second" are used merely to distinguish one entity or operation from another, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Furthermore, the terms "comprising," "including," or any other variations thereof are intended to cover non-exclusive inclusion, such that a process, method, article, or apparatus that comprises a list of elements includes not only those elements but also other elements not expressly listed, or elements inherent to such a process, method, article, or apparatus. Without further limitations, an element defined by the phrase "comprising one..." does not exclude the presence of other identical elements in the process, method, article, or apparatus that includes said element. In this invention, "a plurality of" means at least two, such as two, three, etc., unless otherwise expressly specified.

[0088] The above description is merely a specific embodiment of the present invention, enabling those skilled in the art to understand or implement the invention. Various modifications to these embodiments will be readily apparent to those skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the invention. Therefore, the present invention is not to be limited to the embodiments shown herein, but is to be accorded the widest scope consistent with the principles and novel features of the invention herein.

Claims

1. An oxide solid electrolyte ceramic sheet, characterized in that, The material of the oxide solid electrolyte ceramic sheet includes a first oxide solid electrolyte and a second oxide solid electrolyte; in: Dv of the first oxide solid electrolyte 50 D1, the Dv of the second oxide solid electrolyte 50 For D2, D1 < D2 ≤ 5μm, Dv of the first oxide solid electrolyte 90 D3, the Dv of the second oxide solid electrolyte 90 D4; D3 < D4 ≤ 10 μm.

2. The oxide solid electrolyte ceramic sheet as described in claim 1, wherein D1 < D2 ≤ 3 μm; and / or, D3<D4≤5μm.

3. The oxide solid electrolyte ceramic sheet as described in claim 1, characterized in that, The mass ratio of the first oxide solid electrolyte to the second oxide solid electrolyte is (0.11~0.67):

1.

4. The oxide solid electrolyte ceramic sheet as described in claim 1, characterized in that, The first oxide solid electrolyte and the second oxide solid electrolyte are each selected from at least one of NASICON type oxide solid electrolyte, garnet type oxide solid electrolyte or perovskite type oxide solid electrolyte.

5. A method for preparing an oxide solid electrolyte ceramic sheet, characterized in that, The preparation steps include the following: The first oxide solid electrolyte and the second oxide solid electrolyte are mixed with additives and granulated to obtain a molded powder. The molding powder is pressed into shape to obtain an oxide solid electrolyte preform. The oxide solid electrolyte preform is debinded and sintered to obtain an oxide solid electrolyte ceramic sheet; in: The material of the oxide solid electrolyte ceramic sheet includes a first oxide solid electrolyte and a second oxide solid electrolyte; Dv of the first oxide solid electrolyte 50 D1, the Dv of the second oxide solid electrolyte 50 D2; D1 < D2 ≤ 5μm, Dv of the first oxide solid electrolyte 90 D3, the Dv of the second oxide solid electrolyte 90 D4; D3 < D4 ≤ 10 μm.

6. The method for preparing the oxide solid electrolyte ceramic sheet as described in claim 5, characterized in that, The pressing pressure is 50 MPa to 400 MPa; and / or, The temperature for discharging the adhesive is 200℃~600℃; and / or, The sintering heating rate is 1℃ / min to 5℃ / min; and / or, The heat preservation time is 1 hour to 12 hours.

7. The method for preparing the oxide solid electrolyte ceramic sheet as described in claim 5, characterized in that, If the oxide solid electrolyte is a perovskite type oxide solid electrolyte, the sintering temperature is 800℃~1300℃.

8. The method for preparing the oxide solid electrolyte ceramic sheet as described in claim 5, characterized in that, If the oxide solid electrolyte is a NASICON type oxide solid electrolyte, the sintering temperature is 800℃~1100℃.

9. The method for preparing the oxide solid electrolyte ceramic sheet as described in claim 5, characterized in that, If the oxide solid electrolyte is a garnet-type oxide solid electrolyte, the sintering temperature is 1050℃~1250℃.

10. A solid-state battery, characterized in that, Includes the oxide solid electrolyte ceramic sheet as described in any one of claims 1 to 4.