A PDOL-based polymer electrolyte for lithium batteries, its preparation method and application
By introducing a fluorinated composite solvent and a three-dimensional crosslinking agent into a PDOL-based electrolyte, and employing a three-step liquid-liquid stepwise mixing and stepped temperature polymerization process, a stable polymer network is constructed. This solves the problems of low oxidation potential and poor compatibility of PDOL-based electrolytes with graphite anodes, achieving high voltage stability and long cycle life in lithium batteries.
Patent Information
- Application Number
- CN202611266290.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-20
- Publication Date
- 2026-11-17
AI Technical Summary
Traditional PDOL-based electrolytes have low oxidation potential (<4.0V), are prone to DOL solvent co-intercalation into graphite, and have poor polymerization uniformity, making them unsuitable for the high-voltage operating window of high-nickel NCM811 ternary cathode materials, and also have insufficient compatibility with graphite anodes.
A composite lithium salt, mainly composed of 1,3-dioxolane (DOL) as the monomer and lithium difluorooxalate borate (LiDFOB), was constructed using a fluorinated composite solvent and a three-dimensional crosslinking agent to form a stable polymer network. The three-dimensional polymer network was formed through a three-step liquid-liquid stepwise mixing process and stepped temperature polymerization, thus optimizing the electrolyte system.
The oxidation potential of the electrolyte was increased to 4.5 V, which enhanced the compatibility of the graphite anode, improved the cycle stability and high voltage oxidation resistance of the battery, and achieved a cycle capacity retention rate of 92.53%.
Smart Images

Figure CN123120855A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of solid electrolyte technology for lithium batteries, and particularly to a PDOL-based polymer electrolyte for lithium batteries, its preparation method, and its application. Background Technology
[0002] With the rapid development of the global energy structure, there is an unprecedented and urgent demand for high-energy-density energy storage technologies. High-nickel NCM811 ternary cathodes, with their ultra-high specific capacity, have become the core cathode material for high-energy-density lithium-ion batteries. While traditional liquid electrolyte lithium batteries possess relatively high ionic conductivity (10⁻⁶),… -2 While exhibiting conductivity at the S / cm level, it poses serious safety hazards. Traditional solid polymer electrolytes based on PEO suffer from severe room temperature crystallization and low ionic conductivity (below 10). -5 The S / cm value only allows for use at high temperatures above 60℃, making it unsuitable for applications requiring power batteries at room temperature. While existing ether-based 1,3-dioxolane (DOL)-based liquid electrolytes exhibit excellent compatibility with lithium metal anodes, their oxidation potential is less than 4.0V, making it difficult to match the high-voltage operating window of NCM811. This significantly limits the application of DOL-based electrolytes in high-nickel systems.
[0003] While DOL ring-opening polymerization yields poly(1,3-dioxolane) (PDOL)-based gel electrolytes, which can optimize electrode interface contact by leveraging the advantages of in-situ molding, the unmodified conventional PDOL system has two technical shortcomings: First, pure PDOL molecular chains have high regularity and are prone to crystallization, resulting in poor stability in the high-voltage NCM811 system; second, free DOL solvent in the PDOL matrix is highly susceptible to intercalation behavior between graphite layers along with lithium ions, thus destroying the graphite sheet structure.
[0004] In existing technologies, in-situ copolymerization can effectively disrupt the regular arrangement of polyether chains and reduce PDOL room temperature crystallization. Patent CN115745798A utilizes the copolymerization of polydioxopentane dimethacrylate and vinyl ethylene carbonate to prepare an all-solid-state electrolyte, relying on double bond copolymerization to improve crystallization defects. The introduction of fluorine-containing additives can preferentially decompose and generate a flexible, Li-rich SEI during the graphite lithium intercalation stage, weakening the solvation coordination ability of DOL and significantly reducing the amount of ether molecules carried by Li. +Embedding graphite sheets reduces graphite layer peeling and repeated SEI damage and regeneration. Patent CN118919833A employs a combination of various glycidyl ethers and fluorinated boron compounds to construct a flame-retardant PDOL system, relying on fluorinated boron additives to improve cycle stability, enhance flame-retardant properties, and reduce the risk of electrolyte ignition upon heating. However, existing PDOL modification schemes only optimize from the single dimension of the polymer skeleton, without simultaneously considering high-voltage oxidation resistance and graphite anode compatibility. Therefore, it is necessary to systematically improve these issues through electrolyte crosslinking system design, interface control, and process optimization.
[0005] Based on this, the present invention designs a PDOL-based polymer electrolyte for lithium batteries, its preparation method and application. Summary of the Invention
[0006] This invention provides a PDOL-based polymer electrolyte for lithium batteries, its preparation method, and its application. The purpose is to solve the problems of low oxidation potential (<4.0V), easy DOL solvent co-intercalation into graphite, and poor polymerization uniformity of traditional PDOL-based electrolytes.
[0007] To achieve the above objectives, embodiments of the present invention provide a PDOL-based polymer electrolyte for lithium batteries, its preparation method, and its application. The present invention achieves certain improvements through component synergistic optimization and process improvement: using 1,3-dioxolane (DOL) as the polymerizing monomer, a composite lithium salt mainly composed of lithium difluorooxalate borate, combined with a fluorinated composite solvent and a three-dimensional crosslinking agent, a stable polymer network is constructed; a three-step liquid-liquid stepwise mixing process is adopted to effectively avoid the rapid polymerization defect caused by excessively high local concentration of solid initiator, and to achieve homogenization of the precursor solution; at the same time, a three-step stepped temperature polymerization is used to prepare the electrolyte: by standing at room temperature for 12~24h, the fluorinated monomer is preferentially copolymerized to form a two-dimensional stacked polymer chain, and then a three-dimensional polymer network is formed by two-step stepped heating in situ polymerization at 40~60℃ / 24~48h, which effectively avoids the combination of crosslinking agent and fluorinated comonomer, improves the degree of polymerization of the electrolyte system, and forms a crosslinked electrolyte in situ inside the battery. The polymer electrolyte of this invention is stably adapted to 4.35V high-voltage cycling of NCM811 cathode; the Gr-NCM811 battery retains 92.53% of its capacity at 0.5C 25℃ / 100 cycles. The process of this invention is fully compatible with existing liquid lithium battery production lines, is simple, uses readily available raw materials, and operates under mild reaction conditions.
[0008] One aspect of the present invention provides a PDOL-based polymer electrolyte for lithium batteries, comprising a mixture of polymer monomers, a composite lithium salt, a fluorinated composite solvent, and a crosslinking agent; The polymer monomer mixture includes 1,3-dioxolane (DOL) and glycidyl 2,2,3,3-tetrafluoropropyl ether (TFPO). The composite lithium salt includes lithium difluorooxalate borate (LiDFOB). The fluorinated composite solvent includes fluoroethylene carbonate (FEC). The crosslinking agent includes isocyanuric acid (R,R,R)-triglycidyl ester ((R,R,R)-TGIC) and / or isocyanuric acid (S,S,S)-triglycidyl ester ((S,S,S)-TGIC).
[0009] Preferably, the composite lithium salt further includes lithium bis(trifluoromethanesulfonyl)imide (LiTFSI) and / or lithium bis(fluorosulfonyl)imide (LiFSI).
[0010] Preferably, the fluorinated composite solvent further includes at least one of vinylene carbonate (VC), ethyl methyl carbonate (EMC), and fluoroethyl methyl carbonate (FEMC).
[0011] An embodiment of the present invention also provides a method for preparing the above-described PDOL-based polymer electrolyte for lithium batteries, comprising the following steps: S1: Under an inert atmosphere, the polymer monomer mixture is mixed with a crosslinking agent and stirred until completely dissolved to obtain a first mixed solution; S2: Under an inert atmosphere, the composite lithium salt is dissolved in a fluorine-containing composite solvent and stirred until completely dissolved to obtain a second mixed solution; S3: Under an inert atmosphere, the second mixed solution is added to the first mixed solution and stirred until homogeneous to obtain a precursor solution; S4: Perform step temperature polymerization on the precursor solution to obtain the PDOL-based in-situ crosslinked polymer electrolyte.
[0012] Preferably, in step S1, the volume ratio of 1,3-dioxolane to glycidyl 2,2,3,3-tetrafluoropropyl ether in the monomer mixture is (5:3) to (5:1); the crosslinking agent accounts for 0.0001 to 8 wt% of the monomer mixture. More preferably, it is 0.001 wt%, 0.1 wt%, 0.5 wt%, 1 wt%, 2 wt%, ..., 5 wt%, 6 wt%.
[0013] Preferably, in step S2, the molar concentration of the composite lithium salt is 1.0-2.0 mol / L; and the volume of the fluorinated composite solvent is 30%~50%. More preferably, it is 30 vol%, 40 vol%, 50 vol%, etc.
[0014] Preferably, in step S3, the stirring speed is 200-400 rad / min, and the stirring time is 5-30 min. More preferably, it is 5 min, 10 min, 15 min, 20 min, 25 min, or 30 min. The stirring process should end when the solution is completely clear, and excessive stirring for a long time should be avoided; excessive stirring can easily cause premature prepolymerization of the system, which is not conducive to the wetting, spreading, and uniform dispersion of the electrolyte in the subsequent liquid injection process.
[0015] Preferably, in step S4, the stepped temperature polymerization process includes: standing at room temperature for 12-24 hours; standing at a constant temperature of 45°C for 12-24 hours; and standing at a constant temperature of 60°C for 12-24 hours. More preferably, it includes 12h, 24h, 36h, 48h, etc. The thermal polymerization time can be flexibly adjusted according to the amount of initiator added in the system. If the polymerization time is too long, the excess active cations will continuously induce deep cross-linking, resulting in excessively high polymer cross-linking density and hindered chain segment movement, which will cause a significant increase in the electrolyte's bulk impedance. At the same time, the excess active components are prone to inducing continuous side reactions at the electrode interface, damaging the stability of the interfacial film. Conversely, if the polymerization time is insufficient, the monomer cross-linking reaction will be incomplete, the polymer's three-dimensional network structure will be incomplete, and a large amount of unreacted free DOL will remain in the system. Free DOL is prone to solvent decomposition, graphite co-intercalation, and other side reactions during high-voltage charging and discharging, ultimately deteriorating the electrochemical stability of the polymer electrolyte.
[0016] Another aspect of the embodiments of the present invention provides the application of the above-described PDOL-based polymer electrolyte or the PDOL-based polymer electrolyte prepared by the above-described preparation method in solid-state batteries.
[0017] Another aspect of the present invention provides a lithium battery comprising a positive electrode, a graphite negative electrode, a separator, and the PDOL-based polymer electrolyte described above or the PDOL-based polymer electrolyte prepared by the above preparation method.
[0018] The above-described solution of the present invention has the following beneficial effects: (1) The PDOL-based polymer electrolyte of the present invention has the advantages of high voltage stability and good graphite anode compatibility, as well as simple preparation process, readily available raw materials and mild reaction conditions. It solves the problems of low oxidation potential (<4.0V), easy DOL solvent co-intercalation into graphite and poor polymerization uniformity of traditional PDOL-based electrolytes.
[0019] (2) This invention employs a three-step method to prepare the polymer electrolyte precursor solution, combined with a three-step stepped temperature polymerization process. First, the polymer monomer components are premixed with the crosslinking agent solution to achieve uniform dispersion of the materials; then, the lithium salt and initiator are added to an organic solvent for pre-dissolution and preparation to obtain a mixed solution, ensuring uniform dispersion of the lithium salt and initiator in the solvent system; finally, the two pre-prepared solutions are mixed and blended to obtain a homogeneous precursor solution. The polymerization stage uses stepped temperature control, which, compared to directly adding a solid initiator, avoids the problem of local high concentration, inhibits rapid polymerization, and improves the overall uniformity of the precursor solution.
[0020] (3) By adding fluorinated comonomers, this invention, on the one hand, disrupts the regular structure of PDOL chain segments, reduces the tendency to crystallize, and improves the room temperature ion conductivity; on the other hand, the fluorinated functional groups endow the polymer with oxidation resistance. During cycling, the fluorinated monomers participate in the formation of the SEI film on the graphite anode, generating a highly stable LiF-rich passivation layer, which blocks the insertion of DOL solvent into the graphite sheets and avoids solvent co-intercalation damaging the anode. At the same time, a fluorinated composite solvent is selected. The strong electron-withdrawing inductive effect of fluorine atoms raises the HOMO energy level of the solvation system, increasing the oxidation potential of the electrolyte to 4.5 V. Moreover, the fluorinated solvent preferentially decomposes on the positive and negative electrode surfaces, constructing a dense SEI and CEI film, which isolates the active oxygen generated by the positive electrode under high voltage and prevents its oxidative corrosion of the electrolyte.
[0021] (4) The present invention also adds a crosslinking agent to construct a spatial network polymer skeleton, which can not only disrupt the regular arrangement of polymers, reduce crystallinity, and improve ionic conductivity, but also anchor PDOL segments through covalent bonds, inhibit the breaking of ether oxygen bonds and polymer depolymerization under high voltage, reduce free DOL monomers, eliminate oxidative active sites, and optimize high voltage electrochemical stability. The introduced multifunctional lithium salt additive has a triple function of lithium source supply, polymerization initiation and interfacial film formation: the dissociated lithium ions provide a stable lithium source for the electrolyte and ensure the normal migration of lithium ions during charging and discharging; under specific conditions, it generates active cations, initiates crosslinking polymerization, and assists in the formation of a stable three-dimensional network structure; at the same time, it undergoes redox decomposition at the positive and negative electrode interfaces, participates in the in-situ construction of SEI / CEI films, forms a dense, stable and low impedance interfacial protective layer, inhibits side reactions, alleviates electrolyte decomposition loss, and improves interfacial stability and cycle life. Attached Figure Description
[0022] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the drawings used in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.
[0023] Figure 1These are comparative images showing the macroscopic morphology of the precursor solutions prepared in Examples 1-6 and Comparative Examples 1-2 of this invention after polymerization.
[0024] Figure 2 The graph shows the cycle performance test results of the button batteries assembled in Examples 1-3 and Comparative Example 3 of this invention.
[0025] Figure 3 The graph shows the cycle performance test results of the button batteries assembled in Examples 1, 4-6 of this invention.
[0026] Figure 4 The graph shows the cycle performance test results of the button batteries assembled in Embodiment 1 and Comparative Examples 1 and 2 of the present invention.
[0027] Figure 5 The graph shows the cycle performance test results of the button batteries assembled in Embodiment 1 and Comparative Examples 4, 5, and 6 of this invention. Detailed Implementation
[0028] To make the technical problems, technical solutions and advantages of the present invention clearer, a detailed description will be given below in conjunction with the accompanying drawings and specific embodiments.
[0029] Unless otherwise defined, all technical terms used herein have the same meaning as commonly understood by those skilled in the art. The technical terms used herein are for the purpose of describing particular embodiments only and are not intended to limit the scope of the invention.
[0030] Unless otherwise specified, all raw materials, reagents, instruments and equipment used in this invention can be purchased from the market or prepared by existing methods.
[0031] This invention addresses existing problems by providing a PDOL-based polymer electrolyte for lithium batteries, its preparation method, and its application.
[0032] The following description is provided through specific embodiments and comparative examples.
[0033] Example 1 This embodiment provides a method for preparing a PDOL-based polymer electrolyte for lithium batteries, comprising the following steps: (1) Take 0.5 mL of DOL monomer and 0.1 mL of TFPO, add 5 wt% of isocyanuric acid (R,R,R)-triglycidyl ester, place in a 10 mL vial, stir at room temperature for 10 min to obtain a homogeneous and transparent first mixed solution.
[0034] (2) Take 1.2 M LiDFOB and 0.8 M LiTFSI and slowly add them to a composite solvent consisting of 0.2 mL FEC and 0.2 mL FEMC. Then add 10 μL VC and stir at room temperature for 15 min until the lithium salt is completely dissolved to obtain a clear second mixed solution.
[0035] (3) Under stirring conditions, the second mixed solution is slowly transferred to the first mixed solution using a pipette, and stirred continuously at a speed of 400 rad / min until a homogeneous and transparent mixed solution is formed, thus obtaining the precursor solution.
[0036] (4) The precursor solution was allowed to stand at room temperature for 12-24 hours to allow 1,3-dioxolane (DOL) and the fluorinated monomer TFPO to preferentially undergo ring-opening copolymerization at room temperature, generating long chains of fluorinated polymers with a two-dimensional stacked structure. Subsequently, the precursor solution was transferred to a step-controlled temperature polymerization program at 40-60 °C for deep polymerization. In the low-temperature prepolymerization stage, the solution was kept at 45 °C for 12 hours to initiate the binding of trace crosslinking agents with the terminal hydroxyl groups of the polymer long chains by low-temperature heating, gradually constructing a three-dimensional polymer network structure. This process can effectively suppress the side reactions of the crosslinking agent and the fluorinated comonomer, and achieve the homogenization of the network structure by controlling the crosslinking rate. Afterward, the temperature was raised to 60 °C and kept at 60 °C for 24 hours to carry out high-temperature deep crosslinking, which promoted the complete ring-opening of residual DOL and the completion of the double crosslinking copolymerization reaction, thereby significantly improving the overall polymerization conversion rate of the electrolyte system, and finally obtaining the PDOL-based polymer electrolyte.
[0037]
[0038] ,in, .
[0039] The NCM811 positive electrode, ceramic-coated composite separator, and graphite negative electrode are assembled into a battery cell in sequence. The PDOL-based polymer electrolyte is then injected into the battery casing and sealed.
[0040] The assembled battery was first left to stand at room temperature (25℃±2℃) for 12 hours to allow the PDOL-based polymer electrolyte to fully wet the electrodes and separator. The battery was then placed in a 45℃ oven for 24 hours and then transferred to a 60℃ oven for 12 hours to allow the PDOL-based polymer electrolyte to solidify in situ inside the battery, thus obtaining a lithium battery containing the PDOL-based polymer electrolyte.
[0041] Example 2 The only difference between this embodiment and Example 1 is that the amount of isocyanuric acid (R,R,R)-triglycidyl ester used is 4 wt% of the polymer monomer mass, while the other components, proportions and preparation methods are the same as in Example 1.
[0042] Example 3 The only difference between this embodiment and Example 1 is that the amount of isocyanuric acid (R,R,R)-triglycidyl ester used is 6 wt% of the polymer monomer mass, while the other components, proportions and preparation methods are the same as in Example 1.
[0043] Example 4 The only difference between this embodiment and Example 1 is that the concentration of LiDFOB in the second mixed solution is 0.6 M, while the other components, proportions, and preparation methods are the same as in Example 1.
[0044] Example 5 The only difference between this embodiment and Example 1 is that the concentration of LiDFOB in the second mixed solution is 0.8 M, while the other components, proportions, and preparation methods are the same as in Example 1.
[0045] Example 6 The only difference between this embodiment and Example 1 is that the concentration of LiDFOB in the second mixed solution is 1.0 M, while the other components, proportions, and preparation methods are the same as in Example 1.
[0046] Comparative Example 1 The difference between this comparative example and Example 1 is that in the second mixed solution, FEMC is replaced with an equal volume of EMC, while the remaining components, proportions, and preparation methods are the same as in Example 1.
[0047] Comparative Example 2 The difference between this comparative example and Comparative Example 1 is that TFPO is not added to the first mixed solution, while the other components, proportions, and preparation methods are the same as those in Comparative Example 1.
[0048] Comparative Example 3 The difference between this comparative example and Example 1 is that TGIC is not added to the first mixed solution, while the remaining components, proportions, and preparation methods are the same as in Example 1.
[0049] Comparative Example 4 The difference between this comparative example and Example 1 is that the total concentration of lithium salt in the second mixed solution is changed to 2.0 M, specifically 1.5 M LiDFOB and 0.5 M LiTFSI. The other components, proportions and preparation methods are the same as in Example 1.
[0050] Comparative Example 5 The difference between this comparative example and Comparative Example 4 is that LiTFSI is replaced with an equimolar amount of LiFSI, while the other components, proportions, and preparation methods are the same as those in Comparative Example 4.
[0051] Comparative Example 6 The difference between this comparative example and Example 1 is that the TFPO is replaced with an equal volume of 1,4-bis(2',3'-epoxypropyl)perfluorobutane (PFBDGE), while the other components, proportions and preparation methods are the same as in Example 1.
[0052] Performance Testing and Result Analysis The positive and negative electrode materials were separately fed into a homogenizing device to prepare electrode slurries. The positive electrode slurry was prepared by mixing NCM811 ternary positive electrode material, Super P conductive agent, and PVDF binder at a mass ratio of 18:1:1, and then thoroughly stirred before use. An automatic coating machine was used to uniformly coat the prepared positive electrode slurry onto the surface of an aluminum current collector, with a coating thickness controlled at 100 μm and a coating rate of 15 mm·s. -1 After coating, the positive electrode sheet is dried in a vacuum oven at 90 ℃ for 10~12 h, and then cut into circular electrode sheets with a diameter of 12 mm. The mass of the electrode sheets and the blank aluminum foil are weighed to calculate the actual loading of active material in the electrode.
[0053] The preparation process of the negative electrode slurry is the same as that of the positive electrode slurry. The slurry is uniformly coated on the surface of the copper foil current collector, and the coating thickness is controlled to be 75 μm.
[0054] The obtained positive and negative electrode sheets, CR2032 button battery casing, and separator were placed together in a 50 ℃ vacuum drying oven for 2 h for pretreatment and drying. Then, they were quickly transferred to an argon glove box with water and oxygen content both below 0.1 ppm. Battery assembly was completed inside the glove box. During the assembly process, the polymer electrolyte prepared in the above examples and comparative examples was injected. By adjusting the amount of positive and negative electrode materials, the final positive and negative electrode capacity ratio (N / P ratio) of the battery cell was controlled between 1.05 and 1.09.
[0055] After the battery assembly was completed, it was first allowed to stand at room temperature for 12 hours, and then placed in a 60 °C constant temperature oven for heat treatment polymerization for 12 hours. After the samples cooled naturally to room temperature, the electrochemical performance of the batteries assembled in each example and comparative example was tested. For systems that require further control of the degree of polymerization, the heat treatment time can be extended to 12-24 hours to ensure that the in-situ polymerization reaction is fully completed.
[0056] Test conditions: The charge-discharge cycle performance of the button cell was tested using the Blue Battery Test System. The charge-discharge voltage range was 2.8 V to 4.35 V. After activation at a current density of 0.1 C for 3 cycles, the cycle test was carried out at a current density of 0.5 C and 25°C.
[0057] Figure 1 The images show the macroscopic morphology of the precursor solutions after polymerization in Examples 1-6 and Comparative Examples 1 and 2. The results show that Comparative Example 3 (without crosslinking agent) and Comparative Example 2 (without TFPO) both exhibit a fluid, semi-gel state, indicating that they cannot form a stable solid electrolyte and therefore cannot be molded. In contrast, the samples in Examples 1-3 all formed self-supporting solid polymer networks, demonstrating the crucial role of the copolymerization of DOL and TFPO and the crosslinking agent in network construction.
[0058] Figure 2 The results show the effect of crosslinking agent content on battery cycle performance. Compared with Comparative Example 3 (which had almost no capacity output), the batteries in Examples 1-3 all exhibited good cycle stability. As the crosslinking agent content increased from 4 wt% to 6 wt%, the battery capacity initially increased and then decreased. This indicates that an appropriate amount of crosslinking agent (e.g., 5 wt%) can construct an optimal three-dimensional network, effectively binding free DOLs and suppressing side reactions, while excessive crosslinking agent will increase lithium-ion transport resistance.
[0059] Figure 3 The results show the effect of lithium salt concentration on battery cycle performance. When the LiDFOB concentration (i.e., initiator / lithium salt concentration) increased from 0.6 M in Example 4 to 1.2 M in Example 1, the battery capacity retention significantly improved. Sufficient LiDFOB effectively initiated deep polymerization and cross-linking of monomers, reducing residual monomers and thus greatly improving cycle stability.
[0060] Figure 4 The results show the effect of fluorinated monomers and solvents on cycling performance. Example 1, which contains both TFPO and FEMC, exhibits significantly better cycling stability and capacity retention than Comparative Example 1 (without FEMC) and Comparative Example 2 (without TFPO). This demonstrates the synergistic effect of the fluorinated comonomer TFPO and the fluorinated composite solvent, which together construct a stable LiF-rich interfacial film and enhance the antioxidant capacity of the PDOL-based polymer electrolyte.
[0061] like Figure 5 As shown, the capacity of Comparative Example 4 (total lithium salt concentration 2.0 M) was inferior to that of Example 1, demonstrating that excessive lithium salt and initiator can degrade performance due to excessive polymerization and restricted chain segment movement. The cycle life of Comparative Example 5 (using LiFSI instead of LiTFSI) was significantly shortened, indicating that LiFSI has poor interfacial stability in this system. The performance of Comparative Example 6 (using PFBDGE instead of TFPO) was significantly reduced, demonstrating that TFPO monomers with specific structures (containing ether oxygen segments) have irreplaceable advantages in constructing efficient ion transport channels and moderately crosslinked networks. The bi-epoxy long perfluorinated chain structure of Comparative Example 6 is prone to excessive crosslinking, increasing ion transport resistance.
[0062] The comparison results of the above embodiments and comparative examples fully demonstrate that the present invention has successfully prepared a PDOL-based solid electrolyte with high voltage stability, excellent graphite anode compatibility and long cycle life through the synergistic optimization of components (TFPO, LiDFOB, chiral TGIC, FEMC / FEC) and a step-temperature controlled polymerization process.
[0063] The above description represents the preferred embodiments of the present invention. It should be noted that those skilled in the art can make various improvements and modifications without departing from the principles of the present invention, and these improvements and modifications should also be considered within the scope of protection of the present invention.
Claims
1. A PDOL-based polymer electrolyte for lithium batteries, characterized in that, Includes polymer monomer mixtures, complex lithium salts, fluorinated complex solvents, and crosslinking agents; The polymer monomer mixture includes 1,3-dioxolane and glycidyl 2,2,3,3-tetrafluoropropyl ether; The composite lithium salt includes lithium difluorooxalate borate; The fluorinated composite solvent includes fluoroethylene carbonate; The crosslinking agent includes isocyanuric acid (R,R,R)-triglycidyl ester and / or isocyanuric acid (S,S,S)-triglycidyl ester.
2. The PDOL-based polymer electrolyte for lithium batteries according to claim 1, characterized in that, The composite lithium salt also includes lithium bis(trifluoromethanesulfonyl)imide and / or lithium bis(fluorosulfonyl)imide.
3. The PDOL-based polymer electrolyte for lithium batteries according to claim 1, characterized in that, The fluorinated composite solvent also includes at least one of vinylene carbonate, ethyl methyl carbonate, and fluoroethyl methyl carbonate.
4. A method for preparing a PDOL-based polymer electrolyte for lithium batteries as described in any one of claims 1-3, characterized in that, Includes the following steps: S1: Under an inert atmosphere, the polymer monomer mixture is mixed with a crosslinking agent and stirred until completely dissolved to obtain a first mixed solution; S2: Under an inert atmosphere, the composite lithium salt is dissolved in a fluorine-containing composite solvent and stirred until completely dissolved to obtain a second mixed solution; S3: Under an inert atmosphere, the second mixed solution is added to the first mixed solution and stirred until homogeneous to obtain a precursor solution; S4: Perform step temperature polymerization on the precursor solution to obtain the PDOL-based in-situ crosslinked polymer electrolyte.
5. The preparation method according to claim 4, characterized in that, In step S1, the volume ratio of 1,3-dioxolane to glycidyl 2,2,3,3-tetrafluoropropyl ether in the polymer monomer mixture is (5:3) to (5:1); the mass of the crosslinking agent accounts for 0.0001 to 8 wt% of the mass of the polymer monomer mixture.
6. The preparation method according to claim 4, characterized in that, In step S2, the molar concentration of the composite lithium salt is 1.0-2.0 mol / L; the volume of the fluorinated composite solvent is 30%-50%.
7. The preparation method according to claim 4, characterized in that, In step S3, the stirring speed is 200~400 rad / min and the stirring time is 5~30 min.
8. The preparation method according to claim 4, characterized in that, In step S4, the stepped temperature polymerization process includes: standing at room temperature for 12-24 hours; standing at a constant temperature of 45°C for 12-24 hours; and standing at a constant temperature of 60°C for 12-24 hours.
9. The application of the PDOL-based polymer electrolyte as described in any one of claims 1-3 or the PDOL-based polymer electrolyte prepared by the preparation method described in any one of claims 4-8 in solid-state batteries.
10. A lithium battery, characterized in that, The PDOL-based polymer electrolyte includes a positive electrode, a graphite negative electrode, a separator, and the PDOL-based polymer electrolyte as described in any one of claims 1-3 or prepared by the preparation method described in any one of claims 4-8.
Citation Information
Patent Citations
Polydioxopentyl three-dimensional cross-linked polymer electrolyte as well as preparation method and application thereof
CN115745798A
In-situ preparation and application of flame-retardant PDOL-based polymer solid electrolyte
CN118919833A