Solid electrolyte composition, solid electrolyte, secondary battery, electrical equipment

By using fluorinated aromatic nitrile compounds and fluorinated aromatic ether compounds to form an anion-dominant aggregate solvation structure in a solid electrolyte, the stability and safety issues of traditional electrolytes under high voltage are solved, achieving stable cycling and safe performance of the battery under high voltage.

CN123120856APending Publication Date: 2026-11-17EVE ENERGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611289578.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-24
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Traditional liquid electrolytes struggle to balance high-voltage stability and safety at high voltages. Existing solid electrolytes are prone to oxidation and decomposition at the high-voltage cathode interface, and interface desolvation is difficult, making it hard to meet the requirements of high-voltage long-cycle operation.

Method used

Fluorinated aromatic nitrile compounds are used as hydrogen bond donors and fluorinated aromatic ether compounds or fluorinated aromatic sulfide compounds are used as diluents to form an anion-dominant aggregate solvation structure, which regulates the coordination environment of lithium ions, promotes the entry of lithium salt anions into the inner solvation sheath, forms a stable interface film rich in fluorides, and combines with a cross-linked polymer network to form a solid electrolyte with high mechanical strength.

Benefits of technology

It achieves high voltage stability and low interfacial impedance, and the electrolyte does not ignite or explode under extreme conditions, thus improving the synergistic effect of electrochemical performance and safety performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123120856A_ABST
    Figure CN123120856A_ABST
Patent Text Reader

Abstract

This application discloses a solid electrolyte composition, a solid electrolyte, a secondary battery, and an electrical device, relating to the field of batteries. The solid electrolyte composition includes: a polymer monomer, a diluent, and a eutectic solvent. The eutectic solvent includes lithium salts and fluorinated aromatic nitrile compounds, and the diluent includes fluorinated aromatic ether compounds or fluorinated aromatic sulfides. In this application, the fluorinated aromatic nitrile compounds act as hydrogen bond donors, working in conjunction with the fluorinated aromatic ether compounds or fluorinated aromatic sulfides as diluents to achieve a synergistic improvement in electrochemical performance and safety performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application relates to the field of batteries, specifically to a solid electrolyte composition, a solid electrolyte, a secondary battery, and an electrical device. Background Technology

[0002] The development of lithium-ion batteries towards higher voltages places higher demands on the oxidation stability of electrolytes. Traditional liquid electrolytes struggle to balance high-voltage stability and safety. While eutectic solvents possess non-flammability and good ion transport properties, the hydrogen bond donors (alcohols, amides, or carboxylic acids) in existing systems are prone to oxidative decomposition at the high-voltage cathode interface. Furthermore, their strong coordination with lithium ions makes interface desolvation difficult, hindering the achievement of high-voltage, long-cycle requirements.

[0003] Therefore, how to provide a solid electrolyte system that combines excellent cycle performance and safety performance has become an urgent problem to be solved in this field. Summary of the Invention

[0004] This application provides a solid electrolyte composition, a solid electrolyte, a secondary battery, and an electrical device, which aims to balance battery cycle performance and safety performance.

[0005] This application provides a solid electrolyte composition comprising: a polymer monomer, a diluent, and a eutectic solvent, wherein the eutectic solvent comprises lithium salts and fluorinated aromatic nitrile compounds, and the diluent comprises fluorinated aromatic ether compounds or fluorinated aromatic sulfides.

[0006] Optionally, in some embodiments of this application, the fluorinated aromatic nitrile compound includes compounds as shown in Formula I: Formula I; Wherein, R1 is selected from fluorinated C1-C6 alkyl, fluorinated C1-C6 alkoxy or fluorinated C1-C6 alkylthio. R2, R3, R4, and R5 are each independently selected from -H, -F, substituted or unsubstituted C1-C6 alkyl groups.

[0007] Optionally, in some embodiments of this application, the general structural formula of the fluorinated aromatic nitrile compound is C8H. 3- n F 4+n N, where n is selected from 0, 1, or 2.

[0008] Optionally, in some embodiments of this application, the diluent comprises a compound represented by Formula II: Formula II; Where X is selected from O or S; R6 is selected from unsubstituted or fluorinated C1-C6 alkyl groups; The R7, the R8, the R9, the R 10 The R 11 Selected from -H, -F, unsubstituted or fluorinated C1 to C6 alkyl groups.

[0009] Optionally, in some embodiments of this application, R6 is selected from methyl or trifluoromethyl.

[0010] Optionally, in some embodiments of this application, the molar ratio of the lithium salt to the fluorinated aromatic nitrile compound ranges from 1:5 to 1:2.

[0011] Optionally, in some embodiments of this application, the mass percentage of the diluent is in the range of 10% to 30% based on the total mass of the solid electrolyte composition being 100%.

[0012] Optionally, in some embodiments of this application, the solid electrolyte composition further includes a crosslinking agent and an initiator; Based on the total mass of the solid electrolyte composition being 100%, the mass percentage of the polymer monomer ranges from 15% to 30%. The mass ratio of the crosslinking agent to the polymer monomer ranges from 1:100 to 3:100; The mass ratio of the initiator to the polymer monomer ranges from 3:500 to 1:100.

[0013] Accordingly, this application also provides a solid electrolyte, which is formed by curing the aforementioned solid electrolyte composition.

[0014] Accordingly, this application also provides a secondary battery, including the solid electrolyte as described above.

[0015] In addition, this application also provides an electrical device, including a solid electrolyte as described above or a secondary battery as described above.

[0016] In this application, fluorinated aromatic nitrile compounds act as hydrogen bond donors, while fluorinated aromatic ether compounds or fluorinated aromatic sulfides act as diluents, forming an anion-dominated aggregate solvation structure that effectively regulates the coordination environment of lithium ions. This solvation structure promotes the entry of lithium salt anions into the inner solvation sheath of lithium ions, preferentially decomposing at the electrode interface to form a stable interface film rich in fluorides, thus achieving both high voltage stability and low interfacial impedance. Simultaneously, this solid electrolyte composition exhibits good thermal stability after curing, remaining non-flammable and non-explosive under extreme conditions such as thermal abuse, needle penetration, and extrusion, achieving a synergistic improvement in electrochemical performance and safety performance. Attached Figure Description

[0017] Figure 1 This is a room temperature cycling curve provided by an exemplary embodiment of this application; Figure 2 This is a 45°C cycling curve provided in one exemplary embodiment of this application. Detailed Implementation

[0018] The technical solutions in the embodiments of this application will be clearly and completely described below. Obviously, the described embodiments are only some embodiments of this application, and not all embodiments. Based on the embodiments in this application, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of this application.

[0019] This application provides a solid electrolyte composition, a solid electrolyte, a secondary battery, and an electrical device, which aims to balance battery cycle performance and safety performance.

[0020] This application provides a solid electrolyte composition comprising: a polymer monomer, a diluent, and a eutectic solvent, wherein the eutectic solvent includes lithium salts and fluorinated aromatic nitrile compounds, and the diluent includes fluorinated aromatic ether compounds or fluorinated aromatic sulfide compounds.

[0021] In this application, fluorinated aromatic nitrile compounds act as hydrogen bond donors, while fluorinated aromatic ether compounds or fluorinated aromatic sulfides act as diluents, forming an anion-dominated aggregate solvation structure that effectively regulates the coordination environment of lithium ions. This solvation structure promotes the entry of lithium salt anions into the inner solvation sheath of lithium ions, preferentially decomposing at the electrode interface to form a stable interface film rich in fluorides, thus achieving both high voltage stability and low interfacial impedance. Simultaneously, this solid electrolyte composition exhibits good thermal stability after curing, remaining non-flammable and non-explosive under extreme conditions such as thermal abuse, needle penetration, and extrusion, achieving a synergistic improvement in electrochemical performance and safety performance.

[0022] In some examples, the lithium salt includes at least one of lithium bis(trifluoromethanesulfonyl)imide (LiTFSI), lithium bis(fluorosulfonyl)imide (LiFSI), lithium difluorooxalateborate (LiDFOB), and lithium bis(oxalateborate)borate (LiBOB).

[0023] In some embodiments of this application, the fluorinated aromatic nitrile compounds include compounds as shown in Formula I: Formula I; Wherein, R1 is selected from fluorinated C1~C6 alkyl, fluorinated C1~C6 alkoxy or fluorinated C1~C6 alkylthio. R2, R3, R4, and R5 are each independently selected from -H, -F, substituted or unsubstituted C1 to C6 alkyl groups.

[0024] It is understandable that in the fluorinated aromatic nitrile compounds shown in Formula I, R1 is selected from fluoroalkyl, fluoroalkoxy, or fluoroalkylthio groups, which have strong electron-withdrawing effects. When R1 is trifluoromethyl, the compound, as a hydrogen bond donor, can form hydrogen bond interactions with lithium salt anions of suitable strength, promoting efficient dissociation of lithium salts while avoiding excessive aggregation of ion pairs due to overly strong hydrogen bond interactions. When R1 is trifluoromethoxy, the strong electron-withdrawing effect of trifluoromethoxy further reduces the highest occupied molecular orbital energy level of the donor molecule, improving the antioxidant stability of the donor at the high-voltage cathode interface. At the same time, the oxygen atom in trifluoromethoxy can coordinate with lithium ions, further optimizing the solvation structure of lithium ions. The cyano group, as a strong electron-withdrawing and coordinating group, can effectively anchor lithium salt anions and regulate the coordination environment of lithium ions. By adjusting the number and position of fluorine substitutions at R2 to R5 positions on the benzene ring, the molecular polarity, hydrogen bond donor capacity, and antioxidant stability of the hydrogen bond donor can be controlled. Through structural design and functional group regulation of the aforementioned fluorinated aromatic nitrile compounds, these compounds can form hydrogen bonds of suitable strength with lithium salt anions in a eutectic solvent system, promoting efficient dissociation of lithium salts and releasing free lithium ions, while avoiding the adverse effects of excessive ion pair aggregation. The synergistic effect of substituents such as cyano and trifluoromethoxy effectively lowers the highest occupied molecular orbital energy level of the donor molecule, giving it excellent antioxidant stability at the high-voltage cathode interface, thereby suppressing the oxidative decomposition side reactions of the electrolyte under high voltage. This stability is directly reflected in the battery's ability to adapt to high-voltage systems of 4.55V and above and maintain long-term cycle stability. In addition, the precise regulation of the number and position of fluorine substitutions on the benzene ring further optimizes the molecular polarity and donor capability of the fluorinated aromatic nitrile compounds, giving the eutectic solvent suitable viscosity and ion transport characteristics, thus balancing the excellent safety performance, high voltage adaptability, and long-term cycle stability of the solid electrolyte.

[0025] In some embodiments of this application, the general structural formula of the fluorinated aromatic nitrile compound is C8H. 3-n F 4+n N, where n is selected from 0, 1, or 2.

[0026] It is understandable that the general structural formula of fluorinated aromatic nitrile compounds is C8H. 3-n F 4+nWhen n=0, the donor exhibits lower viscosity and higher ion mobility, which is beneficial for improving rate performance; when n=1 or 2, the donor has higher fluorine content and stronger antioxidant capacity, which is beneficial for improving high-voltage cycling stability. Fluorinated aromatic nitrile compounds within this general formula range exhibit excellent intermolecular compatibility with fluorinated aromatic ether compounds or fluorinated aromatic sulfide diluents, forming stable and homogeneous eutectic solvent systems. Each specific compound within this general formula range can form stable eutectic solvents with lithium salts and diluents, and the solid electrolyte formed after curing exhibits excellent safety performance and electrochemical stability.

[0027] In some embodiments of this application, the diluent includes the compound represented by Formula II: Formula II; Where X is selected from O or S; R6 is selected from unsubstituted or fluorinated C1-C6 alkyl groups; R7, R8, R9, R 10 R 11 Selected from -H, -F, unsubstituted or fluorinated C1 to C6 alkyl groups.

[0028] Understandably, in the diluent shown in Formula II, the strong electron-withdrawing effect of the fluorinated benzene ring reduces the electron cloud density on the ether oxygen or thioether groups, thereby weakening the coordination between lithium ions and the diluent. This allows more anions to enter the inner solvation sheath of the lithium ion, forming an anion-dominated aggregate solvation structure. Simultaneously, substituents at specific positions in the diluent molecule provide steric hindrance, preventing the diluent molecule from approaching the lithium ion excessively, forcing more anions to participate in the coordination of the lithium ion, further strengthening the anion-dominated solvation structure. This anion-dominated solvation structure preferentially reduces and decomposes at the negative electrode interface, forming a dense solid electrolyte interface film rich in fluorides, significantly improving interface stability and lithium ion transport efficiency. The diluent can also effectively reduce the viscosity of the eutectic solvent, improving the wettability of the solid electrolyte composition to the electrode and separator, and enhancing injection efficiency and interface contact quality. When X is sulfur, the higher polarizability and weaker electronegativity of sulfur atoms further weaken the coordination between lithium ions and the diluent, which is conducive to forming a more anion-dominated solvation structure.

[0029] In some embodiments of this application, R6 is selected from methyl and trifluoromethyl.

[0030] Understandably, when R6 is methyl, the electron-donating effect of the methyl group synergistically combines with the electron-withdrawing effect of the fluorine substituent on the benzene ring, giving the diluent suitable polarity and moderate coordination ability. This effectively reduces the system viscosity without excessively competing for lithium-ion coordination sites. When R6 is trifluoromethyl, the strong electron-withdrawing effect of trifluoromethyl further lowers the highest occupied molecular orbital energy level of the diluent molecule, enhancing its antioxidant capacity under high voltage conditions. Simultaneously, the steric hindrance effect of trifluoromethyl is more significant, more effectively preventing diluent molecules from entering the inner solvation sheath of lithium ions and encouraging more anions to participate in coordination. When R6 is trifluoromethyl, the diluent exhibits superior antioxidant stability at the positive electrode interface and can form a more fluoride-rich interfacial film at the negative electrode interface.

[0031] In some embodiments of this application, the molar ratio of lithium salt to fluorinated aromatic nitrile compound ranges from 1:5 to 1:2.

[0032] Understandably, controlling the molar ratio of lithium salt to fluorinated aromatic nitrile compound within the range of 1:5 to 1:2 allows for suitable hydrogen bonding interactions between the lithium salt and the fluorinated aromatic nitrile compound, promoting complete dissociation of the lithium salt and release of free lithium ions, while preventing excessive viscosity and hindered ion migration due to an excess of the fluorinated aromatic nitrile compound. At this molar ratio, the solvation structure of lithium ions in the eutectic solvent is optimized, allowing anions to enter the inner solvation sheath of lithium ions and form aggregate structures conducive to interfacial film formation.

[0033] In some embodiments of this application, the mass percentage of the diluent is in the range of 10% to 30% based on the total mass of the solid electrolyte composition being 100%.

[0034] Understandably, with the total mass of the solid electrolyte composition being 100%, controlling the diluent's mass percentage within the range of 10% to 30% allows for a balance between the diluent's viscosity-regulating effect and the network-building effect of the polymer monomers. The addition of the diluent effectively reduces the viscosity of the solid electrolyte composition, improving its wettability to the electrodes and separator, enabling the solid electrolyte composition to uniformly fill the cell interior. Simultaneously, the fluorine-containing component in the diluent participates in regulating the solvation structure of lithium ions, promoting the entry of more anions into the inner solvation sheath. Within this proportion range, the polymer monomers can form a sufficient cross-linked network to encapsulate and confine the eutectic solvent within it.

[0035] In some embodiments of this application, the solid electrolyte composition further includes a crosslinking agent and an initiator; the mass percentage of polymer monomers is in the range of 15% to 30% based on the total mass of the solid electrolyte composition of 100%; the mass ratio of crosslinking agent to polymer monomers is in the range of 1:100 to 3:100; and the mass ratio of initiator to polymer monomers is in the range of 3:500 to 1:100.

[0036] Understandably, controlling the polymer monomer mass percentage within the range of 15% to 30% allows the solid electrolyte composition to form a continuous and dense three-dimensional cross-linked polymer network after curing. This network effectively encapsulates the eutectic solvent, ensuring both rapid lithium-ion transport channels and providing the electrolyte with sufficient mechanical strength to inhibit lithium dendrite growth. Controlling the cross-linking agent to polymer monomer mass ratio within the range of 1:100 to 3:100 maintains an appropriate cross-linking density, avoiding both insufficient cross-linking leading to a loose polymer network and insufficient mechanical strength, and excessive cross-linking leading to increased system brittleness and obstructed ion transport channels. Controlling the initiator to polymer monomer mass ratio within the range of 3:500 to 1:100 allows the free radical polymerization reaction to proceed at an appropriate rate, ensuring full conversion of the polymer monomer and cross-linking agent, thus improving the battery's safety and electrochemical performance.

[0037] In some embodiments of this application, the method for preparing a solid electrolyte composition includes: performing a first mixing treatment on a diluent and a eutectic solvent to obtain a first mixture; mixing a crosslinking agent, a polymer monomer, and the first mixture to obtain a second mixture; and mixing an initiator with the second mixture to obtain a solid electrolyte composition.

[0038] Understandably, the stepwise mixing method involves first mixing the diluent with the eutectic solvent to ensure thorough dispersion of the diluent and achieve molecular-level mixing with the solvent's components. The addition of the diluent allows for immediate regulation of the eutectic solvent's viscosity and the solvation environment for lithium ions. Then, the crosslinking agent, polymer monomer, and initiator are added sequentially, avoiding problems such as uneven local concentrations, premature polymerization, or localized overheating and decomposition of the initiator that might occur with simultaneous addition of components. This stepwise mixing method ensures uniform dispersion of the solid electrolyte composition and maintains system stability, providing crucial support for subsequent in-situ thermosetting to form a structurally homogeneous solid electrolyte.

[0039] In some embodiments of this application, the conditions for the first mixing process include: The first mixing temperature ranges from 50℃ to 120℃; The first mixing time ranges from 1 hour to 6 hours.

[0040] Understandably, controlling the first mixing temperature within the range of 50°C to 120°C provides sufficient thermal energy to promote hydrogen bonding interactions and molecular rearrangement between the lithium salt and the fluorinated aromatic nitrile compounds, resulting in a clear and transparent homogeneous liquid, while avoiding component decomposition or side reactions caused by excessively high temperatures. Controlling the first mixing time within the range of 1 hour to 6 hours ensures thorough homogenization of the components and complete formation of the hydrogen bond network, while avoiding inefficiency caused by excessively long mixing times. The eutectic solvent formed under these mixing conditions exhibits excellent homogeneous stability and ion transport properties.

[0041] Accordingly, this application also provides a solid electrolyte, which is formed by curing the aforementioned solid electrolyte composition.

[0042] Understandably, the solid electrolyte formed by in-situ thermosetting of this solid electrolyte composition possesses both high ionic conductivity and high mechanical strength. Fluorinated aromatic nitrile compounds in the eutectic solvent synergistically interact with fluorinated aromatic ether compounds or fluorinated aromatic sulfide diluents to form an anion-dominant aggregate solvation structure. This structure preferentially reduces at the negative electrode interface to form a dense, fluoride-rich solid electrolyte interfacial film, endowing the electrolyte with excellent interfacial stability and high voltage adaptability. The cross-linked polymer network effectively confines the eutectic solvent within it, improving lithium-ion transport and providing sufficient mechanical strength to suppress lithium dendrite growth.

[0043] Accordingly, this application also provides a secondary battery, including the solid electrolyte as described above.

[0044] Understandably, secondary batteries incorporating this solid-state electrolyte can be adapted to high-voltage cathode materials, achieving high energy density output. The good thermal stability and excellent interfacial stability of the solid-state electrolyte endow the battery with superior safety performance, preventing fire and explosion under extreme conditions such as thermal abuse, nail penetration, and compression. The anion-dominated solvation structure and fluoride-rich interfacial film in the solid-state electrolyte ensure that the electrode / electrolyte interface remains stable during long-term cycling, with slow increase in interfacial impedance. This allows the battery to maintain high capacity retention and low expansion rate during both room-temperature and high-temperature cycling.

[0045] In addition, this application also provides an electrical device, including a solid electrolyte as described above or a secondary battery as described above.

[0046] Understandably, electrical devices incorporating this solid-state electrolyte or secondary battery offer a combination of high safety, high energy density, and long lifespan. The high voltage adaptability of solid-state electrolytes allows devices to store more energy in a smaller size and weight, meeting long-duration power requirements. The thermal stability of solid-state electrolytes significantly reduces safety risks during use, transportation, and storage, improving device reliability and user safety. Excellent cycle stability ensures sufficient power supply even after prolonged use, extending device lifespan. This type of electrical device is particularly suitable for applications with high requirements for energy density, safety, and lifespan.

[0047] Example 1 The solid electrolyte composition was prepared according to the following steps: Step 1: Lithium bis(trifluoromethanesulfonyl)imide (LiTFSI) and fluorinated aromatic nitrile compound 4-fluoro-2-trifluoromethylbenzonitrile (FTFBN, CAS No. 194853-86-6) are mixed at a molar ratio of 1:4. Diluent 2-methyl-4-fluoroanisole (TFBn, CAS No. 399-54-2) is added, and the mixture is stirred at 80°C for 4 hours to obtain a clear and transparent first mixture; wherein the mass ratio of diluent to eutectic solvent is 1:4.

[0048] Step 2: Add the polymer monomer polyethylene glycol methyl ether methacrylate (PEGMA) and the crosslinking agent polyethylene glycol diacrylate (PEGDA) to the first mixture to obtain the second mixture; the mass ratio of crosslinking agent to polymer monomer is 1:50; Step 3: Mix the second mixture with the initiator azobisisobutyronitrile (AIBN) to obtain a solid electrolyte composition, wherein, based on the total mass of the solid electrolyte composition being 100%, the mass percentage of polymer monomers is 25%, the mass percentage of diluent is 25%, the mass ratio of initiator to polymer monomers is 1:125, and the balance is a eutectic solvent.

[0049] Follow these steps to assemble the pouch battery: Step 4: The positive electrode, negative electrode, and separator of the battery are wound into a core in the conventional way, but not sealed first. The solid electrolyte composition is injected into the battery casing by vacuum injection. The negative electrode contains a composite negative electrode active material of graphite and silicon carbon. The separator is a composite separator with polyethylene as the base film and coated with an alumina ceramic layer and a polyvinylidene fluoride adhesive layer on its surface.

[0050] Step 5: After liquid injection, the battery is placed in an oven or heating device and heated at 85°C for 4 hours in an argon atmosphere at a pressure of 300MPa. After thermosetting, the battery is finally encapsulated, followed by formation, molding, and capacity testing to form the battery.

[0051] Example 2 The difference between this embodiment and Example 1 is that in step 1, 3,4-difluoro-2-trifluoromethylbenzonitrile (DFTFBN, CAS No. 1803809-94-0) is used as a fluorinated aromatic nitrile compound to replace 4-fluoro-2-trifluoromethylbenzonitrile (FTFBN).

[0052] Example 3 The difference between this embodiment and Embodiment 1 is that in step 1, 3,4,5-trifluoro-2-trifluoromethylbenzonitrile (TFTFBN) is used as a fluorinated aromatic nitrile compound to replace 4-fluoro-2-trifluoromethylbenzonitrile (FTFBN).

[0053] Example 4 The difference between this embodiment and Example 1 is that in step 1, 6-fluoro-2-trifluoromethylbenzonitrile (iso1-FTFBN, CAS No. 133116-83-3) is used as a fluorinated aromatic nitrile compound to replace 4-fluoro-2-trifluoromethylbenzonitrile (FTFBN).

[0054] Example 5 The difference between this embodiment and Example 1 is that in step 1, 3,5-difluoro-2-trifluoromethylbenzonitrile (3,5-DFTFBN, CAS No. 1806397-97-6) is used as a fluorinated aromatic nitrile compound to replace 4-fluoro-2-trifluoromethylbenzonitrile (FTFBN).

[0055] Example 6 The difference between this embodiment and Embodiment 1 is that in step 1, 3,4,6-trifluoro-2-trifluoromethylbenzonitrile (3,4,6-Tri-FTFBN) is used as a fluorinated aromatic nitrile compound to replace 4-fluoro-2-trifluoromethylbenzonitrile (FTFBN).

[0056] Example 7 The difference between this embodiment and Example 1 is that in step 1, 4-fluoro-2-trifluoromethoxybenzonitrile (FOTFBN, CAS No. 1323966-32-0) is used as a fluorinated aromatic nitrile compound to replace 4-fluoro-2-trifluoromethylbenzonitrile (FTFBN).

[0057] Example 8 The difference between this embodiment and Embodiment 1 is that in step 1, 3-methyl-4-fluoroanisole (iso-1-TFBn, CAS No. 2338-54-7) is used as a diluent instead of 2-methyl-4-fluoroanisole (TFBn).

[0058] Example 9 The difference between this embodiment and Embodiment 1 is that in step 1, 2-trifluoromethyl-4-fluoroanisole (CAS No. 1214360-06-1) is used as a diluent instead of 2-methyl-4-fluoroanisole (TFBn).

[0059] Example 10 The difference between this embodiment and Embodiment 1 is that 2-ethyl-4-fluoroanisole (CAS No. 1369865-70-2) is used as a diluent in step 1 instead of 2-methyl-4-fluoroanisole (TFBn).

[0060] Example 11 The difference between this embodiment and Example 1 is that the molar ratio of lithium salt bis(trifluoromethanesulfonyl)imide (LiTFSI) to fluorinated aromatic nitrile compound 4-fluoro-2-trifluoromethylbenzonitrile (FTFBN) in step 1 is 1:2.

[0061] Example 12 The difference between this embodiment and Example 1 is that the molar ratio of lithium salt lithium bis(trifluoromethanesulfonyl)imide (LiTFSI) to fluorinated aromatic nitrile compound 4-fluoro-2-trifluoromethylbenzonitrile (FTFBN) in step 1 is 1:5.

[0062] Example 13 The difference between this embodiment and Example 1 is that in step 1, the diluent 2-methyl-4-fluoroanisole (TFBn) accounts for 10% of the total mass of the solid electrolyte composition, and in step 2, the polymer monomer polyethylene glycol methyl ether methacrylate (PEGMA) accounts for 15% of the total mass of the solid electrolyte composition, the crosslinking agent polyethylene glycol diacrylate (PEGDA) accounts for 1% of the mass of the polymer monomer, and the initiator azobisisobutyronitrile (AIBN) accounts for 0.6% of the mass of the polymer monomer.

[0063] Example 14 The difference between this embodiment and Example 1 is that in step 1, the diluent 2-methyl-4-fluoroanisole (TFBn) accounts for 30% of the total mass of the solid electrolyte composition, and in step 2, the polymer monomer polyethylene glycol methyl ether methacrylate (PEGMA) accounts for 30% of the total mass of the solid electrolyte composition, the crosslinking agent polyethylene glycol diacrylate (PEGDA) accounts for 3% of the mass of the polymer monomer, and the initiator azobisisobutyronitrile (AIBN) accounts for 1% of the mass of the polymer monomer.

[0064] Comparative Examples 1 to 2 Comparative Example 1 The difference between this comparative example and Example 1 is that, in step 1, succinic anionylene is used as the hydrogen bond donor instead of 4-fluoro-2-trifluoromethylbenzonitrile (FTFBN), and fluoroethylene carbonate (FEC) is used as the diluent instead of 2-methyl-4-fluoroanisole (TFBn). The diluent accounts for 8% of the total mass of the solid electrolyte composition. The molar ratio of lithium bis(trifluoromethanesulfonyl)imide (LiTFSI) to the fluorinated aromatic nitrile compound is 2:3. The polymer monomer polyethylene glycol methyl ether methacrylate (PEGMA) accounts for 10% of the total mass of the solid electrolyte composition. The crosslinking agent polyethylene glycol diacrylate (PEGDA) accounts for 0.8% of the polymer monomer mass, and the initiator azobisisobutyronitrile (AIBN) accounts for 0.5% of the polymer monomer mass.

[0065] Comparative Example 2 The difference between this comparative example and Example 1 is that, in step 1, succinic anionylene is used as the hydrogen bond donor instead of 4-fluoro-2-trifluoromethylbenzonitrile (FTFBN), and fluoroethylene carbonate (FEC) is used as the diluent instead of 2-methyl-4-fluoroanisole (TFBn). The diluent accounts for 35% of the total mass of the solid electrolyte composition. The molar ratio of lithium bis(trifluoromethanesulfonyl)imide (LiTFSI) to the fluorinated aromatic nitrile compound is 2:11. The polymer monomer polyethylene glycol methyl ether methacrylate (PEGMA) accounts for 45% of the total mass of the solid electrolyte composition. The crosslinking agent polyethylene glycol diacrylate (PEGDA) accounts for 0.5% of the polymer monomer mass, and the initiator azobisisobutyronitrile (AIBN) accounts for 0.3% of the polymer monomer mass.

[0066] Battery testing methods: Room temperature cycling performance: a) In the first week at 25℃±2℃, charge at a constant current of 0.2C to 4.55V, then charge at a constant voltage of 4.55V to 0.02C, and let stand for 10 minutes; then discharge at a constant current of 0.2C to 3V. b) During weeks 2-99, charge at a constant current of 2.2C to 4.22V; charge at a constant current of 1.65C to 4.24V; charge at a constant current of 1.4C to 4.30V, then charge at a constant voltage of 4.30V to 1.0C; charge at a constant current of 1.0C to 4.55V, then charge at a constant voltage of 4.55V to 0.1C cutoff; let stand for 10 minutes; discharge at a constant current of 1.0C to 3.00V. c) In the 100th week, charge at a constant current of 0.2C to 4.55V, then charge at a constant voltage of 4.55V to 0.02C, and let stand for 10 minutes; then discharge at a constant current of 0.2C to 3V. d) Starting from week 101, every week 1-99, charge at a constant current of 2.2C to 4.22V; charge at a constant current of 1.65C to 4.24V; charge at a constant current of 1.4C to 4.30V, then charge at a constant voltage of 4.30V to 1.0C; charge at a constant current of 1.0C to 4.55V, then charge at a constant voltage of 4.55V to 0.1C cutoff; let stand for 10 minutes; discharge at a constant current of 1.0C to 3.00V. e) Starting from week 101, every 100th week, charge at a constant current of 0.2C to 4.55V, then charge at a constant voltage of 4.55V to 0.02C, let stand for 10 minutes; then discharge at a constant current of 0.2C to 3V. f) The total cycle is 1000 times.

[0067] Room temperature cycling expansion rate: Under conditions of 25℃±2℃, the battery is charged to 4.55V at a constant current and constant voltage of 0.2C and then placed flat on the panel of a PPG thickness tester. A force of 500g is applied to the battery to perform a full-charge thickness test, which is recorded as the initial thickness T0. After 1000 cycles, the battery cell is cycled again using the same method to perform a full-charge thickness test after 1000 cycles, which is recorded as T. x The cyclic expansion rate is calculated as T. x / T0-1.

[0068] Figure 1 This is the ambient temperature cycling curve for Example 1.

[0069] 45℃ Cyclic Performance Test: a) Under conditions of 45℃±2℃, in the first week, charge at a constant current of 0.2C to 4.55V, then charge at a constant voltage of 4.55V to 0.02C, and let stand for 10 minutes; then discharge at a constant current of 0.2C to 3V. b) During weeks 2-99, charge at a constant current of 2.2C to 4.22V; charge at a constant current of 1.65C to 4.24V; charge at a constant current of 1.4C to 4.30V, then charge at a constant voltage of 4.30V to 1.0C; charge at a constant current of 1.0C to 4.55V, then charge at a constant voltage of 4.55V to 0.1C cutoff; let stand for 10 minutes; discharge at a constant current of 1.0C to 3.00V. c) In the 100th week, charge at a constant current of 0.2C to 4.55V, then charge at a constant voltage of 4.55V to 0.02C, and let stand for 10 minutes; then discharge at a constant current of 0.2C to 3V. d) Starting from week 101, every week 1-99, charge at a constant current of 2.2C to 4.22V; charge at a constant current of 1.65C to 4.24V; charge at a constant current of 1.4C to 4.30V, then charge at a constant voltage of 4.30V to 1.0C; charge at a constant current of 1.0C to 4.55V, then charge at a constant voltage of 4.55V to 0.1C cutoff; let stand for 10 minutes; discharge at a constant current of 1.0C to 3.00V. e) Starting from week 101, every 100th week, charge at a constant current of 0.2C to 4.55V, then charge at a constant voltage of 4.55V to 0.02C, let stand for 10 minutes; then discharge at a constant current of 0.2C to 3V. f) A total of 500 cycles.

[0070] Figure 2 The 45°C cycling curve is from Example 1.

[0071] 45℃ Cyclic Expansion Rate: The battery is charged to 4.55V at a constant current and constant voltage of 0.2C at 45℃±2℃. It is then placed flat on the panel of a PPG thickness tester. A force of 500g is applied to the battery for a full-charge thickness test, recorded as the initial thickness T0. After 500 cycles in the 45℃ cycling chamber, the battery is removed from the chamber, and the same method is used to perform another 500 cycles for a full-charge thickness test, recorded as Tx. The cyclic expansion rate is calculated as Tx / T0-1.

[0072] Thermal abuse test: At 25℃±3℃, 10 battery samples were charged at a constant current of 0.5C to 4.55V, and then charged at a constant voltage of 4.55V to 0.05C cutoff, and left to stand for 10 minutes. The batteries were then placed in a test chamber, which was heated at a rate of 5±2℃ / min. When the temperature inside the chamber reached 130±2℃, it was kept constant for 60 minutes. The batteries were observed to see if they caught fire or exploded. If there was no fire or explosion, the result was 10 / 10.

[0073] Triangular bar compression test: At 25℃±3℃, 10 battery samples were charged at a constant current of 0.5C to 4.55V, then charged at a constant voltage of 4.55V to 0.05C cutoff, and left to stand for 10 minutes. The batteries were fixed on the test bench, and the compression speed was 3kN±10N / min. A compression force of 1.5kN±10N was applied to the batteries using a triangular bar. The test was stopped once the compression force reached its maximum value. Observe whether the batteries catch fire or explode. If there is no fire or explosion, the result is 10 / 10.

[0074] Needle prick test: a) Ten battery samples were tested after being charged at a constant current of 0.5C to the cutoff point of 0.05C; b) Using a stainless steel needle with a diameter of 3.0±0.5mm, quickly puncture the center of the battery cell at a speed of 150mm / s in a direction perpendicular to the cell surface. Leave the needle on the cell for at least 0.5 hours until it cools down, then remove it. The tip of the stainless steel needle should have a V-shaped taper (32°). Continue to observe for 6 hours after removing the needle. Observe whether the battery catches fire or explodes. If there is no fire or explosion, the result is 10 / 10.

[0075] The differences between the solid electrolyte compositions of the embodiments in this application and those of the comparative examples are detailed in Table 1.

[0076] Table 1

[0077] The battery test results of the embodiments and comparative examples of this application are detailed in Table 2.

[0078] Table 2

[0079] According to Examples 1 to 14 and Comparative Examples 1 to 2 of this application, the solid electrolyte system of this application, composed of fluorinated aromatic nitrile compounds as hydrogen bond donors and fluorinated aromatic ether compounds as diluents, exhibits significantly better safety performance than the system using succinic anion as a hydrogen bond donor and fluoroethylene carbonate as a diluent. The anion-dominant aggregate solvation structure formed by the synergistic interaction of fluorinated aromatic nitrile compounds and fluorinated aromatic ether compounds forms a dense interface film rich in fluorides upon decomposition at the electrode interface. This interface film possesses excellent thermal and mechanical stability, resulting in a significantly higher throughput under extreme conditions such as thermal abuse, needle penetration, and compression compared to the batteries in the comparative examples. Regarding cycle performance, the room-temperature cycle capacity retention rate and high-temperature cycle capacity retention rate of the batteries in this application are significantly higher than those in the comparative examples, and the cell expansion rate is significantly lower than that in the comparative examples. The directional hydrogen bonding between the cyano group of fluorinated aromatic nitrile compounds and the lithium salt anion effectively promotes the dissociation of the lithium salt. Simultaneously, the electron-withdrawing and steric hindrance effects of fluorinated aromatic ethers guide the anion into the lithium-ion inner solvation sheath, forming an aggregate structure conducive to interfacial stability. This solvation structure and the fluoride-rich interfacial film together suppress side reactions at the electrode / electrolyte interface, reduce structural degradation and gas production during cycling, and endow the solid electrolyte with excellent long-term cycling stability and dimensional stability.

[0080] According to Examples 1 to 7 of this application, when the number of fluorine substituents on the benzene ring of the fluorinated aromatic nitrile compound increases or the substitution mode of the fluorine substituents changes, the electrochemical stability window of the solid electrolyte widens accordingly, and the high-voltage cycling stability is further improved. The introduction of fluorine substituents on the benzene ring enhances the antioxidant capacity of the fluorinated aromatic nitrile compound, making it more stable at the high-voltage cathode interface, thereby improving the cycle retention rate of the solid electrolyte at high voltage. All examples showed excellent pass rates in safety performance tests, indicating that adjusting the degree of fluorine substitution does not negatively affect the intrinsic safety of the solid electrolyte, and the synergistic effect between the fluorinated aromatic nitrile compound and the fluorinated aromatic ether compound can be effectively exerted under different fluorine substitution modes.

[0081] According to Examples 1 and 8 to 10 of this application, the solid electrolyte maintains excellent electrochemical and safety performance even when the position and type of substituents on the benzene ring of the diluent change. In fluorinated aromatic ether compounds, the electron-withdrawing effect of the fluorinated benzene ring and the steric hindrance effect of the alkyl substituents jointly regulate the coordination environment of lithium ions. Fluorine and alkyl substituents at different positions can form effective intermolecular synergistic effects with fluorinated aromatic nitrile compounds, promoting the entry of anions into the inner solvation sheath of lithium ions to form an anion-dominated aggregate structure. Changes in the position of the substituents do not impair the ability to form this solvation structure or the ability to construct the interfacial film, indicating that compounds within the general formula range of fluorinated aromatic ether compounds can effectively function as active diluents.

[0082] According to Examples 1 and 11 to 14 of this application, under the condition that the types of fluorinated aromatic nitrile compounds and diluents remain consistent, when the molar ratio of lithium salt to fluorinated aromatic nitrile compounds is adjusted within the range of 1:5 to 1:2, the mass percentage of diluent is adjusted within the range of 10% to 30%, the mass percentage of polymer monomer is adjusted within the range of 15% to 30%, the mass ratio of crosslinking agent to polymer monomer is adjusted within the range of 1% to 3%, and the mass ratio of initiator to polymer monomer is adjusted within the range of 0.6% to 1%, the overall electrochemical performance and safety performance of the solid electrolyte can be maintained at an excellent level. Variations in the proportions of each component within the above ranges do not disrupt the homogeneous stability of the eutectic solvent, the formation of the anion-dominated solvation structure, the crosslinking density of the polymer network, or the structural integrity of the electrode interface film. Within this range, the ratio of lithium salt to fluorinated aromatic nitrile compounds maintains suitable hydrogen bond interaction strength; the mass percentage of diluent within this range balances the dual functions of viscosity reduction and solvation regulation; and the mass ratio of polymer monomers, crosslinking agents, and initiators to polymer monomers within this range ensures effective encapsulation and confinement of the crosslinked network within the eutectic solvent. This solid-state electrolyte system exhibits a wide process window and good formulation tolerance; variations in the proportions of each component within a certain range do not lead to significant performance degradation, which is beneficial for formulation adjustment and quality control in industrial production.

[0083] The foregoing has provided a detailed description of a solid electrolyte composition, solid electrolyte, secondary battery, and electrical device provided in the embodiments of this application. Specific examples have been used to illustrate the principles and implementation methods of this application. The descriptions of the above embodiments are only for the purpose of helping to understand the methods and core ideas of this application. At the same time, for those skilled in the art, there will be changes in the specific implementation methods and application scope based on the ideas of this application. Therefore, the content of this specification should not be construed as a limitation of this application.

Claims

1. A solid electrolyte composition, characterized in that, include: The polymer monomer, diluent, and eutectic solvent, wherein the eutectic solvent includes lithium salts and fluorinated aromatic nitrile compounds, and the diluent includes fluorinated aromatic ether compounds or fluorinated aromatic sulfides.

2. The solid electrolyte composition according to claim 1, characterized in that, The fluorinated aromatic nitrile compounds include compounds as shown in Formula I: Equation I; Wherein, R1 is selected from fluorinated C1-C6 alkyl, fluorinated C1-C6 alkoxy or fluorinated C1-C6 alkylthio. R2, R3, R4, and R5 are each independently selected from -H, -F, substituted or unsubstituted C1-C6 alkyl groups.

3. The solid electrolyte composition according to claim 1, characterized in that, The general structural formula of the fluorinated aromatic nitrile compound is C8H. 3-n F 4+n N, where n is selected from 0, 1, or 2.

4. The solid electrolyte composition according to claim 1, characterized in that, The diluent includes the compound represented by Formula II: Formula II; Where X is selected from O or S; R6 is selected from unsubstituted or fluorinated C1-C6 alkyl groups; The R7, the R8, the R9, the R 10 The R 11 Selected from -H, -F, unsubstituted or fluorinated C1 to C6 alkyl groups.

5. The solid electrolyte composition according to claim 4, characterized in that, R6 is selected from methyl or trifluoromethyl.

6. The solid electrolyte composition according to claim 1, characterized in that, The molar ratio of the lithium salt to the fluorinated aromatic nitrile compound ranges from 1:5 to 1:

2.

7. The solid electrolyte composition according to claim 1, characterized in that, The mass percentage of the diluent, based on the total mass of the solid electrolyte composition being 100%, ranges from 10% to 30%.

8. The solid electrolyte composition according to claim 1, characterized in that, The solid electrolyte composition further includes a crosslinking agent and an initiator; Based on the total mass of the solid electrolyte composition being 100%, the mass percentage of the polymer monomer ranges from 15% to 30%. The mass ratio of the crosslinking agent to the polymer monomer ranges from 1:100 to 3:100; The mass ratio of the initiator to the polymer monomer ranges from 3:500 to 1:

100.

9. A solid electrolyte, characterized in that, The solid electrolyte is formed by curing the solid electrolyte composition as described in any one of claims 1 to 8.

10. A secondary battery, characterized in that, Includes the solid electrolyte as described in claim 9.

11. An electrical appliance, characterized in that, This includes the solid electrolyte as described in claim 9 or the secondary battery as described in claim 10.