Wide potential window plasticized solid electrolyte and its preparation method and lithium / sodium battery

By mixing bis(fluorosulfonyl)imide alkali metal salts, electron-withdrawing organic compounds, and metal oxides, the challenges of high ionic conductivity, interfacial compatibility, and electrochemical stability window in solid electrolytes were solved, resulting in improved battery performance and safety.

CN123120858APending Publication Date: 2026-11-17NANJING UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611352250.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-02
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing solid electrolytes cannot simultaneously achieve high ionic conductivity, excellent interfacial compatibility, and a wide electrochemical stability window.

Method used

By mixing alkali metal salts of bis(fluorosulfonyl)imide, organic compounds with electron-withdrawing groups, and metal oxides, the melting point is lowered through eutectic reaction, the interfacial contact is optimized, a dense interfacial film is formed, and the ionic conductivity and electrochemical stability window are improved.

Benefits of technology

It achieves high ionic conductivity, excellent interfacial contact, and a wide electrochemical stability window, significantly improving the battery's cycle performance and safety while reducing manufacturing difficulty and cost.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123120858A_ABST
    Figure CN123120858A_ABST
Patent Text Reader

Abstract

This invention relates to the field of lithium / sodium battery technology, specifically to a wide-potential-window plasticized solid electrolyte and its preparation method, and a lithium / sodium battery. It is composed of a bis(fluorosulfonyl)imide binary alkali metal salt, an electron-withdrawing organic compound, and a metal oxide, with optional film-forming aids, through a heating process at 70-120°C. The organic compound has an affinity for alkali metal ions, while the metal oxide captures FSI⁻, synergistically enhancing ionic conductivity. The electrolyte exhibits excellent plasticity, allowing for tight wetting of the electrode to form a continuous ion pathway, resulting in the in-situ formation of a stable CEI film. The electrochemical window reaches -0.1 to 5.5V for lithium-based electrolytes and -0.1 to 5.1V for sodium-based electrolytes. It also possesses high room-temperature conductivity, a wide stability range, and intrinsic flame retardant properties, making it suitable for LFP, LCO, high-voltage LRMO, and NVP electrodes. It exhibits high capacity retention over long cycles, solving the problem of traditional solid electrolytes struggling to balance conductivity, interface, and voltage window.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of lithium / sodium battery technology, specifically to a wide potential window plasticized solid electrolyte and its preparation method, and a lithium / sodium battery. Background Technology

[0002] Driven by the ever-increasing demand for higher energy density and superior safety, solid-state batteries (SSBs) are becoming a revolutionary technological solution that is disrupting traditional lithium-ion batteries. Solid-state electrolytes (SSEs), as the core components that determine the overall performance of solid-state batteries, must simultaneously possess high ionic conductivity, excellent interfacial compatibility, and a wide electrochemical stability window. These are prerequisites for building high-efficiency solid-state batteries.

[0003] However, none of the solid electrolytes reported to date can simultaneously achieve the aforementioned key properties. For example, while sulfide solid electrolytes possess ultra-high ionic conductivity and excellent ductility, they suffer from inherent electrochemical instability with high-voltage cathodes; oxide solid electrolytes, despite having relatively wide electrochemical stability windows, generally face the problem of poor electrode-electrolyte interface compatibility; halide solid electrolytes exhibit outstanding oxidation stability, but their intrinsic incompatibility with lithium metal anodes remains a key bottleneck restricting their practical applications; meanwhile, polymer solid electrolytes, while exhibiting excellent interfacial compatibility, are limited by slow ion transport kinetics at room temperature.

[0004] Therefore, existing solid electrolytes have the problem of not being able to simultaneously achieve high ionic conductivity, tight interfacial contact, and a wide electrochemical window. Summary of the Invention

[0005] To address the aforementioned problems, this invention provides a wide-potential-window plasticized solid electrolyte, its preparation method, and a lithium / sodium battery. The solid electrolyte is composed of a bis(fluorosulfonyl)imide alkali metal salt, an organic compound with electron-withdrawing groups, and a metal oxide. The organic compound binds to the alkali metal ions in the salt, while the metal oxide binds to the anions in the salt. This synergistic effect improves the ionic conductivity of the solid electrolyte, optimizes the interfacial contact between the electrolyte and the electrolyzer, and broadens the electrochemical stability window, thereby solving the problem that existing solid electrolytes struggle to simultaneously achieve high ionic conductivity, tight interfacial contact, and a wide electrochemical window.

[0006] To achieve the above objectives, the present invention adopts the following technical solution: The first objective of this invention is to provide a wide potential window plasticized solid electrolyte, wherein the solid electrolyte is composed of a bis(fluorosulfonyl)imide alkali metal salt, an organic compound having an electron-withdrawing group, and a metal oxide; the electron-withdrawing group is a cyano or sulfonyl group; the mass ratio of the bis(fluorosulfonyl)imide alkali metal salt to the organic compound having an electron-withdrawing group is 1:0.05~2; and the mass ratio of the bis(fluorosulfonyl)imide alkali metal salt to the metal oxide is 1:0.05~0.3.

[0007] In a preferred embodiment of the present invention, the organic compound having an electron-withdrawing group is dimethylmalononitrile, dimethyl sulfone, cyclobutene sulfone, or 1,3-propenesulfonate lactone.

[0008] In a preferred embodiment of the present invention, the alkali metal salt of bisfluorosulfonylimide is lithium bisfluorosulfonylimide or sodium bisfluorosulfonylimide and the stabilizer is potassium bisfluorosulfonylimide or cesium bisfluorosulfonylimide. The mass ratio of lithium bisfluorosulfonylimide or sodium bisfluorosulfonylimide to the stabilizer is 1:0.59~1.7.

[0009] In a preferred embodiment of the present invention, the metal oxide is aluminum oxide, lithium oxide, titanium oxide, or cerium oxide.

[0010] In a preferred embodiment of the present invention, the solid electrolyte mixing process further includes a film-forming aid; the mass ratio of the alkali metal salt of bis(fluorosulfonyl)imide to the film-forming aid is 1:0.3~1.5.

[0011] In a preferred embodiment of the present invention, the film-forming aid is sodium carboxymethyl cellulose, polyvinylidene fluoride, polyacrylonitrile, or polyacrylic acid.

[0012] The second objective of this invention is to provide a method for preparing the above-mentioned wide potential window plasticized solid electrolyte, comprising the following steps: mixing a bis(fluorosulfonyl)imide alkali metal salt, an organic compound having an electron-withdrawing group, and a metal oxide, and heating the mixture at 70°C to 120°C to obtain a wide potential window plasticized solid electrolyte.

[0013] In a preferred embodiment of the present invention, the heating time is 1h to 3h.

[0014] A third objective of the present invention is to provide a lithium / sodium battery comprising a positive electrode, a negative electrode, a glass fiber separator, and an electrolyte, or comprising a positive electrode, a negative electrode, and an electrolyte, wherein the electrolyte is the wide potential window plasticized solid electrolyte described above.

[0015] In a preferred embodiment of the present invention, the electrochemical window of the wide potential window plasticized solid electrolyte is -0.1V to 5.5V.

[0016] Compared with the prior art, the beneficial effects of the present invention are: 1. This invention provides a wide-potential-window plasticized solid electrolyte, wherein the solid electrolyte is composed of a bis(fluorosulfonyl)imide alkali metal salt, an organic compound with electron-withdrawing groups, and a metal oxide. The organic compound has an affinity for alkali metal ions in the salt, and the metal oxide has an affinity for anions in the salt. This synergistic effect improves the ionic conductivity of the solid electrolyte, optimizes the interfacial contact between the electrolyte and the electrolyzer, and broadens the electrochemical stability window, thereby solving the problem that existing solid electrolytes cannot simultaneously achieve high ionic conductivity, tight interfacial contact, and a wide electrochemical window.

[0017] 2. In the DAILS solid electrolyte provided by this invention, KFSI acts as a structural stabilizer, effectively inhibiting system crystallization. The electron-withdrawing cyano group in the DMMN molecule exhibits an affinity for Li⁺, while the Lewis acidic aluminum active site of Al₂O₃ has the ability to bind FSI⁻. This localized ion affinity synergistically reconstructs the electronic structure, induces localized structural disorder, and accelerates the dissociation of lithium ions from the electrolyte matrix, thereby significantly improving the ionic conductivity of DAILS. Furthermore, it exhibits a significant deformation of 63.1% at 42.3 MPa, and T... g With a temperature as low as -34°C, it exhibits excellent cold-pressed fluidity. This mechanical property allows it to fully penetrate into the porous electrode under room temperature and pressure without heating and melting. P, S, and F are uniformly distributed in the LFP cathode, forming a three-dimensional continuous ion conduction network, thereby significantly reducing interfacial impedance. At the same time, it eliminates the dependence of solid-state batteries on continuous external pressure, significantly reducing the difficulty and cost of practical manufacturing.

[0018] 3. The DAILS electrochemical stability window provided by this invention is wide, ranging from -0.1V to 5.5V (vs. Li⁺ / Li), significantly wider than traditional sulfide, oxide, halide, and polymer systems. The preferential decomposition of FSI⁻ and DMMN can generate a dense CEI layer rich in LiF / Li₂CO₃ in situ. This allows the Li / DAILS / LRMO battery to maintain a capacity retention of 76.3% and an average coulombic efficiency of 99.3% after 400 cycles at 0.3C with a high cutoff voltage of 4.8V, achieving long-term stable cycling of the high-voltage lithium-rich cathode without any surface modification or coating treatment. Furthermore, DAILS is intrinsically non-flammable under direct ignition conditions, offering an inherent safety advantage compared to flammable liquid electrolytes, meeting the rigid safety requirements of high-energy-density power batteries.

[0019] 4. The DAINS solid electrolyte obtained by replacing LiFSI with NaFSI in this invention also achieves a synergistic improvement in ionic conductivity (0.07 mS·cm at room temperature). -1 ), T gWith an operating temperature as low as -7.5°C and an electrochemical window of -0.1V to 5.1V (vs. Na⁺ / Na), the Na / DAINS / NVP battery maintains a capacity retention of up to 95.8% and a coulombic efficiency of 99.9% after 250 cycles at 0.3C. Attached Figure Description

[0020] Figure 1 This is a schematic diagram of the synthesis of the DAILS solid electrolyte of the present invention.

[0021] Figure 2 This diagram illustrates the advantages of the DAILS solid electrolyte of this invention. Figure 2 Figure a shows the synergistic effect between DMMN / Al2O3 and LiFSI in enhancing lithium-ion conductivity; Figure b shows the excellent interfacial contact characteristics of plastic DAILS; and Figure c shows the excellent high-pressure stability of DAILS due to the dense and stable CEI.

[0022] Figure 3 This is a diagram showing the basic performance of the solid electrolyte of this invention. Figure 3 Figure a shows a comparison of the ionic conductivity of DAILS, DILS, AILS, and LS; Figure b shows the differential scanning calorimetry curve of DAILS; Figure c shows the stress-strain curve of DAILS; Figure d shows the cross-sectional electron microscope images of the solid electrolyte and the cathode; Figure e shows the corresponding EDS element mappings; Figure f shows the linear scanning voltammetry curve of DAILS; Figure g shows a comparison of the electrochemical stability windows of DAILS with traditional sulfide, oxide, halide, and polymer-based solid electrolytes; and Figure h shows the flammability test results of DAILS.

[0023] Figure 4 The graph shows the rate performance and cycle stability of the battery using DAILS solid electrolyte according to this invention. Figure 4 In the diagram, a represents the rate performance of the Li / DAILS / LFP battery, b represents the cycle stability of the Li / DAILS / LFP battery, c represents the rate performance of the Li / DAILS / LCO battery, d represents the cycle stability of the Li / DAILS / LCO battery, e represents the charge-discharge curve of the Li / DAILS / LRMO battery, and f represents the cycle stability of the Li / DAILS / LRMO battery.

[0024] Figure 5 This is a performance diagram of the DAINS solid electrolyte of the present invention. Figure 5Figure a shows a comparison of the ionic conductivity of DAINS, DINS, AINS, and NS; Figure b shows the XRD patterns of DAINS, DMMN, Al2O3, NaFSI, and KFSI; Figure c shows the differential scanning calorimetry curve of DAINS; Figure d shows the stress-strain curve of DAINS; Figure e shows the linear scanning voltammetry curve of DAILS; Figure f shows the galvanostatic cycling curve of the Na / DAINS / Na symmetric cell; Figure g shows the rate performance of the Na / DAINS / NVP cell; Figure h shows the cycle performance of the Na / DAINS / NVP cell; and Figure i shows the charge-discharge curve of the Na / DAINS / NVP cell.

[0025] Figure 6 This is a diagram showing the cyclic performance of the Li / MAILS / LFP of this invention.

[0026] Figure 7 This is a diagram showing the cyclic performance of the Li / BAILS / LFP of this invention.

[0027] Figure 8 This is a diagram showing the cycling performance of the Li / DCILS / LFP of the present invention.

[0028] Figure 9 This is a diagram showing the Li / MLCILS / LCO cycle performance of the present invention.

[0029] Figure 10 This is a graph showing the Li / MLPILS / LCO cycle performance of the present invention.

[0030] Figure 11 This is a graph showing the cycling performance of the Li / MLNILS / LFP of the present invention.

[0031] Figure 12 This is a diagram showing the Li / SAILS / LCO cycle performance of the present invention. Detailed Implementation

[0032] The technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.

[0033] It should be noted that the technical terms used in this invention are only for the purpose of describing specific embodiments and are not intended to limit the scope of protection of this invention. Unless otherwise specified, all raw materials, reagents, instruments and equipment used in the following embodiments of this invention can be purchased from the market or prepared by existing methods.

[0034] To date, no reported solid-state electrolyte can simultaneously achieve high ionic conductivity, excellent interfacial compatibility, and a wide electrochemical stability window. For example, while sulfide solid-state electrolytes possess ultra-high ionic conductivity and excellent ductility, they suffer from inherent electrochemical instability with high-voltage cathodes; oxide solid-state electrolytes, despite having relatively wide electrochemical stability windows, generally face poor electrode-electrolyte interfacial compatibility; halide solid-state electrolytes exhibit outstanding oxidation stability, but their intrinsic incompatibility with lithium metal anodes remains a key bottleneck restricting their practical application; meanwhile, polymer solid-state electrolytes, while exhibiting excellent interfacial compatibility, are limited by slow ion transport kinetics at room temperature. Given the inherent trade-offs among these core performance indicators, there is an urgent need to develop a novel solid-state electrolyte that can break through existing battery chemistry systems and technological paradigms. To overcome these inherent limitations, this invention rationally designs and synthesizes a novel wide-potential-window plasticized solid-state electrolyte, achieving optimal synergy between high ionic conductivity, excellent interfacial contact, and a wide electrochemical stability window.

[0035] First, this invention provides a wide potential window plasticized solid electrolyte, which is composed of a bis(fluorosulfonyl)imide alkali metal salt, an organic compound with an electron-withdrawing group, and a metal oxide. The electron-withdrawing group can be a cyano group, a sulfonyl group, etc.

[0036] It should be noted that this type of solid-state electrolysis lowers the melting point through the eutectic effect of lithium / sodium salts, thus eliminating the dependence on solvents found in traditional organic solid-state electrolytes; it improves ionic conductivity by attracting and dissociating positive and negative ions in lithium / sodium salts through organic compounds with electron-withdrawing groups and metal oxides with Lewis acid sites; it optimizes interfacial contact through the excellent plasticity of the materials; and it enhances the electrochemical stability window through the CEI / SEI formed by the trace decomposition of the materials. SEI refers to the solid electrolyte interfacial film.

[0037] The mass ratio of the bis(fluorosulfonyl)imide alkali metal salt to the organic compound with an electron-withdrawing group is 1:0.05~2. If the mass of the organic compound with the electron-withdrawing group exceeds the above range, the resulting substance will first become liquid and then solid as the mass increases, and the corresponding ionic conductivity will first increase and then decrease. If the mass ratio of the bis(fluorosulfonyl)imide alkali metal salt to the metal oxide is 1:0.05~0.3, and the mass of the metal oxide exceeds the above range, the ionic conductivity of the resulting substance will decrease as the mass increases.

[0038] The alkali metal salt of bisfluorosulfonylimide is lithium bisfluorosulfonylimide or sodium bisfluorosulfonylimide and a stabilizer, wherein the stabilizer is potassium bisfluorosulfonylimide or cesium bisfluorosulfonylimide, and the mass ratio of lithium bisfluorosulfonylimide or sodium bisfluorosulfonylimide to the stabilizer is 1:0.59~1.7.

[0039] The organic compound with the electron-withdrawing group is dimethylmalononitrile, dimethyl sulfone, cyclobutene sulfone, or 1,3-propenesulfonate lactone. The selection of the organic solid with the electron-withdrawing group must consider its high-pressure stability and compatibility with Li under low pressure.

[0040] The metal oxide is aluminum oxide, lithium oxide, titanium oxide, or cerium oxide.

[0041] The solid electrolyte mixing process also includes a film-forming aid. The mass ratio of the alkali metal bis(fluorosulfonyl)imide salt to the film-forming aid is 1:0.3~1.5. If the mass of the film-forming aid exceeds the above range, the ionic conductivity of the formed substance will decrease with increasing mass.

[0042] The film-forming aid is sodium carboxymethyl cellulose, polyvinylidene fluoride, polyacrylonitrile, or polyacrylic acid; its purpose is to enable the solid electrolyte to form a film on its own during application, thus eliminating the need for glass fiber assistance.

[0043] In a preferred embodiment of the present invention, the solid electrolyte is a DAILS solid electrolyte, such as... Figure 1 As shown, DAILS is obtained by strategically combining dimethylmalononitrile (DMMN), alumina (Al2O3), lithium bis(fluorosulfonyl)imide (LiFSI), and potassium bis(fluorosulfonyl)imide (KFSI). KFSI acts as a structural stabilizer, effectively inhibiting crystallization. The electron-withdrawing cyano group in the DMMN molecule exhibits an affinity for lithium ions (Li⁺), while the Lewis acid aluminum active site in Al2O3 binds to bis(fluorosulfonyl)imide anions (FSI⁻). This localized ion affinity synergistically reconstructs the electronic structure, induces localized structural disorder, and accelerates the dissociation of lithium ions from the electrolyte matrix, thereby significantly improving the ionic conductivity of DAILS. Figure 2 a). In addition, such as Figure 2 As shown in b, DAILS have a lower glass transition temperature (T). g Its excellent plasticity allows it to efficiently wet porous electrode structures during battery assembly, facilitating the formation of a three-dimensional conformal interface between the electrolyte and the electrode, effectively reducing interfacial impedance. More importantly, DAILS exhibits an extremely wide electrochemical stability window (-0.1V to 5.5V relative to Li⁺ / Li), thanks to the preferential decomposition of FSI⁻ anions and DMMN, resulting in the in-situ formation of a LiF / Li₂CO₃-rich cathode-electrolyte interface layer (CEI). Figure 2c). This dense and stable CEI layer enables long-term stable cycling of a 4.8V high-voltage lithium-rich manganese-based cathode without the need for additional surface modification or coating protection. Notably, replacing LiFSI with sodium bis(fluorosulfonyl)imide (NaFSI) also successfully prepared a novel DMMN / Al₂O₃-based sodium salt solid electrolyte (named DAINS) that optimizes both electrochemical and mechanical properties. The sodium vanadium phosphate cathode paired with this DAINS solid electrolyte exhibits significantly improved cycle stability and rate performance.

[0044] Secondly, this invention provides a method for preparing the above-mentioned wide potential window plasticized solid electrolyte, comprising the following steps: A wide potential window plasticized solid electrolyte was obtained by mixing a bis(fluorosulfonyl)imide alkali metal salt, an organic compound with an electron-withdrawing group, and a metal oxide, stirring and heating at 80°C for 2 hours, and then cooling.

[0045] Alternatively, a wide potential window plasticized solid electrolyte can be obtained by mixing a bis(fluorosulfonyl)imide alkali metal salt, an organic compound with an electron-withdrawing group, a metal oxide, and a film-forming aid, stirring and heating at 100°C for 2 hours, and then cooling.

[0046] The reaction mechanism involves Lewis acid-base interaction between bis(fluorosulfonyl)imide alkali metal salts, organic compounds, and metal oxides to form a homogeneous and excellent solid electrolyte.

[0047] Finally, the present invention provides a lithium / sodium battery, the lithium / sodium battery comprising a positive electrode, a negative electrode, a glass fiber separator and an electrolyte, wherein the electrolyte is the wide potential window plasticized solid electrolyte described above.

[0048] In the assembly process of lithium / sodium batteries, the solid electrolyte is heated to 80°C and then injected into a glass fiber separator, and assembly is carried out while it is still hot. The positive electrode is composed of an active material, carbon black, polyvinylidene fluoride, and N-methyl-2-pyrrolidone in a mass ratio of 7:2:1. The active material is lithium-rich manganese oxide (LRMO), lithium iron phosphate (LFP), or lithium cobalt oxide (LCO). Solid electrolytes with added film-forming aids do not require the assistance of a glass fiber separator and can be directly pressed into sheets for use.

[0049] The following specific examples will provide further explanation.

[0050] In this invention, lithium bis(fluorosulfonyl)imide is LiFSI, potassium bis(fluorosulfonyl)imide is KFSI, sodium bis(fluorosulfonyl)imide is NaFSI, dimethylmalononitrile is DMMN, dimethyl sulfone is MSM, cyclobutene sulfone is BDS, succinate is SN, alumina is Al2O3, lithium oxide is Li2O, cerium oxide is CeO2, sodium carboxymethyl cellulose is CMC, polyvinylidene fluoride is PVDF, and polyacrylonitrile is PAN.

[0051] Example 1 A method for preparing a wide potential window plasticized solid electrolyte, namely DAILS, includes the following steps: 0.37 g of LiFSI, 0.63 g of KFSI, 0.1 g of DMMN and 0.05 g of Al2O3 were mixed, stirred and heated at 80 °C for 2 h and then cooled to obtain DAILS solid electrolyte.

[0052] Example 2 A method for preparing a wide potential window plasticized solid electrolyte, namely DAINS, includes the following steps: 0.53 g of NaFSI, 0.47 g of KFSI, 0.2 g of DMMN and 0.05 g of Al2O3 were mixed, stirred and heated at 80 °C for 2 h and then cooled to obtain DAINS solid electrolyte.

[0053] Example 3 A method for preparing a wide potential window plasticized solid electrolyte, namely MAILS, includes the following steps: 0.37 g of LiFSI, 0.63 g of KFSI, 0.1 g of MSM and 0.05 g of Al2O3 were mixed, stirred and heated at 80 °C for 2 h and then cooled to obtain MAILS solid electrolyte.

[0054] Example 4 A method for preparing a wide potential window plasticized solid electrolyte, namely BAILS, includes the following steps: 0.37 g of LiFSI, 0.63 g of KFSI, 0.1 g of BDS and 0.05 g of Al2O3 were mixed, stirred and heated at 80 °C for 2 h and then cooled to obtain BAILS solid electrolyte.

[0055] Example 5 A method for preparing a wide potential window plasticized solid electrolyte, namely DCILS, includes the following steps: 0.37 g of LiFSI, 0.63 g of KFSI, 0.1 g of DMMN and 0.05 g of CeO2 were mixed, stirred and heated at 80 °C for 2 h and then cooled to obtain DCILS solid electrolyte.

[0056] Example 6 A method for preparing a wide potential window plasticized solid electrolyte, namely MLCILS, includes the following steps: 0.37 g of LiFSI, 0.63 g of KFSI, 2 g of MSM, 0.3 g of Li2O and 1.5 g of CMC were mixed, stirred and heated at 100 °C for 2 h and then cooled to obtain MLCILS solid electrolyte.

[0057] Example 7 A method for preparing a wide potential window plasticized solid electrolyte, namely MLPILS, includes the following steps: 0.37 g of LiFSI, 0.63 g of KFSI, 2 g of MSM, 0.3 g of Li2O and 1.2 g of PVDF were mixed, stirred and heated at 100 °C for 2 h and then cooled to obtain MLPILS solid electrolyte.

[0058] Example 8 A method for preparing a wide potential window plasticized solid electrolyte, namely MLNILS, includes the following steps: 0.37 g of LiFSI, 0.63 g of KFSI, 2 g of MSM, 0.3 g of Li2O and 0.3 g of PAN were mixed, stirred and heated at 100 °C for 2 h and then cooled to obtain MLNILS solid electrolyte.

[0059] Comparative Example 1 A method for preparing a DILS solid electrolyte includes the following steps: 0.37 g of LiFSI, 0.63 g of KFSI and 0.1 g of DMMN were mixed, stirred and heated at 80 °C for 2 h and then cooled to obtain DILS solid electrolyte.

[0060] Comparative Example 2 A method for preparing an AILS solid electrolyte includes the following steps: 0.37 g of LiFSI, 0.63 g of KFSI and 0.05 g of Al2O3 were mixed, stirred and heated at 80 °C for 2 h and then cooled to obtain the AILS solid electrolyte.

[0061] Comparative Example 3 A method for preparing an LS solid electrolyte includes the following steps: 0.37 g of LiFSI and 0.63 g of KFSI were mixed, stirred and heated at 120 °C for 2 h, and then cooled to obtain LS solid electrolyte.

[0062] Comparative Example 4 A method for preparing a DINS solid electrolyte includes the following steps: 0.53 g of NaFSI, 0.47 g of KFSI and 0.2 g of DMMN were mixed, stirred and heated at 80 °C for 2 h and then cooled to obtain DINS solid electrolyte.

[0063] Comparative Example 5 A method for preparing an AINS solid electrolyte includes the following steps: 0.53 g of NaFSI, 0.47 g of KFSI and 0.05 g of Al2O3 were mixed, stirred and heated at 80 °C for 2 h and then cooled to obtain the AINS solid electrolyte.

[0064] Comparative Example 6 A method for preparing an NS solid electrolyte includes the following steps: 0.53 g of NaFSI and 0.47 g of KFSI were mixed, stirred and heated at 120 °C for 2 h, and then cooled to obtain NS solid electrolyte.

[0065] Comparative Example 7 A method for preparing a SAILS solid electrolyte includes the following steps: 0.37 g of LiFSI, 0.63 g of KFSI, 0.1 g of SN and 0.05 g of Al2O3 were mixed, stirred and heated at 80 °C for 2 h and then cooled to obtain SAILS solid electrolyte.

[0066] The electrolytes prepared in the above embodiments and comparative examples were tested.

[0067] Figure 3 This is a diagram showing the basic performance of the solid electrolyte of this invention. Figure 3 Figure a shows a comparison of the ionic conductivity of DAILS, DILS, AILS, and LS; Figure b shows the differential scanning calorimetry curve of DAILS; Figure c shows the stress-strain curve of DAILS; Figure d shows the cross-sectional electron microscope images of the solid electrolyte and the cathode; Figure e shows the corresponding EDS element mappings; Figure f shows the linear scanning voltammetry curve of DAILS; Figure g shows a comparison of the electrochemical stability windows of DAILS with traditional sulfide, oxide, halide, and polymer-based solid electrolytes; and Figure h shows the flammability test results of DAILS.

[0068] First, the variation of DAILS ionic conductivity with temperature was studied using electrochemical impedance spectroscopy (EIS). For example... Figure 3 As shown in figure a, the ionic conductivity of DAILS can reach 0.2 mS·cm at room temperature. -1 To elucidate the specific contributions of each component to the high conductivity from a mechanistic perspective, this invention rationally designed and prepared three sets of control samples: a DMMN-based lithium salt solid electrolyte containing only DMMN, LiFSI, and KFSI (denoted as DILS); an Al2O3-based lithium salt solid electrolyte containing only Al2O3, LiFSI, and KFSI (denoted as AILS); and a basic lithium salt solid electrolyte composed only of LiFSI and KFSI (denoted as LS). Figure 3As can be clearly seen, DAILS exhibited the highest ionic conductivity among all samples, followed by DILS, AILS, and LS. This result confirms that both DMMN and Al2O3 play a positive role in ion transport, with DMMN contributing more significantly. Figure 3 As shown in b, the synergistic effect among the multiple components gives DAILS an extremely low glass transition temperature T. g The temperature was approximately -34℃, indicating extremely smooth ion migration within the system. Furthermore, the differential scanning calorimetry (DSC) curve showed a distinct melting endothermic peak (T0) at 51℃. m This confirms its intrinsic solid-state properties.

[0069] Thanks to T below room temperature g DAILS can achieve a significant deformation of 63.1% at a pressure of 42.3 MPa. Figure 3 c) It exhibits excellent deformability under quasi-static compressive loading. This good mechanical compliance allows it to penetrate tightly and fully into the porous electrode structure under pressure, thereby constructing a conformal, gapless electrode-electrolyte interface and effectively suppressing interfacial impedance caused by voids. Figure 3 As shown in d–3e, the energy dispersive X-ray spectroscopy (EDS) elemental distribution map shows that P, S, and F elements are uniformly distributed, confirming that DAILS has achieved full penetration inside the lithium iron phosphate (LFP) cathode. This close interfacial contact facilitates the construction of a continuous three-dimensional ion conduction network inside the composite electrode, thereby eliminating the dependence on continuous external pressure during battery operation and laying the foundation for the low-cost fabrication of practical solid-state batteries.

[0070] Linear sweep voltammetry (LSV) test Figure 3 f) indicates that DAILS operates at -0.1V to 5.5V (vs. Li + Within an extremely wide potential range, both oxidation and reduction currents of / Li are negligible, and its electrochemical stability window is significantly wider than that of traditional sulfide, oxide, halide, and polymer-based solid electrolytes. Figure 3 g). Furthermore, DAILS are intrinsically non-flammable when directly ignited ( Figure 3 (h), highlighting its outstanding safety features in high-performance solid-state batteries.

[0071] Next, the electrochemical performance was tested using a CR2032 coin cell. The positive electrode material used was lithium-rich manganese oxide (LRMO), lithium iron phosphate (LFP), or lithium cobalt oxide (LCO) as the active material, which was mixed with carbon black and polyvinylidene fluoride (PVDF) in N-methyl-2-pyrrolidone (NMP) at a mass ratio of 7:2:1. The resulting electrode was then further dried under vacuum at 90°C for 12 hours. The prepared solid electrolyte was heated to 80°C and then injected into a glass fiber separator, followed by conventional coin cell assembly while still hot. To evaluate cycle performance, the battery was cycled several times at a low current, followed by the remaining cycles at a high current. The assembly sequence of the battery was: positive electrode shell, aluminum foil, positive electrode sheet, glass fiber separator injected with solid electrolyte, negative electrode, gasket, spring sheet, and negative electrode shell.

[0072] Figure 4 The graph shows the rate performance and cycle stability of the battery using DAILS solid electrolyte according to this invention. Figure 4 In the diagram, a represents the rate performance of the Li / DAILS / LFP battery, b represents the cycle stability of the Li / DAILS / LFP battery, c represents the rate performance of the Li / DAILS / LCO battery, d represents the cycle stability of the Li / DAILS / LCO battery, e represents the charge-discharge curve of the Li / DAILS / LRMO battery, and f represents the cycle stability of the Li / DAILS / LRMO battery.

[0073] Benefiting from high ionic conductivity, excellent interfacial compatibility, and a wide electrochemical stability window, batteries using DAILS exhibit outstanding electrochemical performance. For example... Figure 4 As shown in a–4b, the all-solid-state Li / DAILS / LFP battery exhibits excellent rate performance and long cycle stability at room temperature. Tests were conducted at current densities ranging from 0.2C to 1C (1C = 160 mA·g). -1 The battery still releases 137.4 mAh·g at 1C. -1 The high discharge specific capacity, representing 85.1% of the low-rate (0.2C) capacity, indicates that Li⁺ can be efficiently transported in the composite solid electrolyte. Notably, the battery retains 90.2% of its capacity after 600 cycles at 0.5C, achieving a discharge specific capacity of 131.8 mAh·g⁻¹. -1 The average coulomb efficiency is 99.7%.

[0074] Figure 4 c–4d demonstrates the cycling and rate performance of the Li / DAILS / LCO battery. This battery completes 500 cycles at 0.5C and a high voltage range of 2.6V to 4.5V (1C = 160 mA·g). -1 The discharge specific capacity remains at 150.0 mAh·g. -1The capacity retention rate was 84.7%; 200.0 mAh·g was released at 0.2C, 0.4C, 0.6C, 0.8C and 1C rates, respectively. -1 186.3mAh·g -1 171.6mAh·g -1 156.4 mAh·g -1 and 151.9mAh·g -1 The specific capacity recovers to 190.7 mAh·g when the temperature returns to 0.2C. -1 .

[0075] like Figure 4 As shown in e–4f, the all-solid-state Li / DAILS / LRMO battery achieved stable cycle performance (1C=300mA·g) within the voltage range of 0.3C and 2–4.8V. -1 The initial discharge specific capacity is 194.1 mAh·g. -1 After 400 cycles, the capacity retention rate was 76.3%, and the average coulombic efficiency reached 99.3%. The high coulombic efficiency confirms the excellent compatibility between DAILS and the 4.8V lithium-rich manganese-based cathode.

[0076] Then, to verify its applicability in sodium-ion batteries, this invention replaced LiFSI with NaFSI and successfully prepared DAINS electrolyte. Simultaneously, three sets of control samples were rationally prepared: DINS (DMMN-based sodium salt solid electrolyte, composed of DMMN, NaFSI, and KFSI); AINS (Al2O3-based sodium salt solid electrolyte, composed of Al2O3, NaFSI, and KFSI); and NS (basic sodium salt solid electrolyte, containing only NaFSI and KFSI).

[0077] Figure 5 This is a performance diagram of the DAINS solid electrolyte of the present invention. Figure 5 Figure a shows a comparison of the ionic conductivity of DAINS, DINS, AINS, and NS; Figure b shows the XRD patterns of DAINS, DMMN, Al2O3, NaFSI, and KFSI; Figure c shows the differential scanning calorimetry curve of DAINS; Figure d shows the stress-strain curve of DAINS; Figure e shows the linear scanning voltammetry curve of DAILS; Figure f shows the galvanostatic cycling curve of the Na / DAINS / Na symmetric cell; Figure g shows the rate performance of the Na / DAINS / NVP cell; Figure h shows the cycle performance of the Na / DAINS / NVP cell; and Figure i shows the charge-discharge curve of the Na / DAINS / NVP cell.

[0078] like Figure 5 As shown in figure a, DAINS exhibits the highest ionic conductivity at room temperature, reaching 0.07 mS·cm.-1 The concentrations of DMMN and Al₂O₃ were higher than those of DINS, AINS, and NS, respectively. This result confirms that both DMMN and Al₂O₃ promote Na⁺ transport, consistent with the pattern observed in lithium-based systems. Figure 5 The XRD pattern of b shows that, compared to the crystalline DMMN, Al2O3, NaFSI, and KFSI, DAINS exhibits a distinctly amorphous structure. DSC analysis ( Figure 5 c) This further indicates its glass transition temperature T g The temperature range is as low as -7.5℃. The amorphous structure and low Tg significantly enhance the ionic conductivity of DAINS. In addition to ionic conductivity, its mechanical properties were also characterized in this study. Despite its high melting point (50℃), Figure 5 c) DAINS still achieved a significant deformation of 64.8% under a pressure of 16.6 MPa. Figure 5 d), exhibiting excellent plasticity and interface compatibility. Figure 5 The linear sweep voltammetry curves in e indicate that DAINS has a wide electrochemical stability window, ranging from -0.1V to 5.1V (vs. Na). + / Na).

[0079] Benefiting from improved ionic conductivity, optimized interfacial compatibility, and a wide electrochemical stability window, batteries equipped with DAINS solid-state electrolytes exhibit excellent electrochemical performance. For example... Figure 5 As shown in f, a symmetrical cell using DAINS is used at 0.04 mA·cm⁻¹. -2 At the given current density, the polarization showed almost no significant increase over nearly 500 hours. Meanwhile, the sodium vanadium phosphate (NVP) cathode, matched with DAINS, exhibited significantly improved cycle stability and rate performance. For example... Figure 5 As shown in g, the Na / DAINS / NVP battery operates at rates of 0.2C, 0.4C, 0.6C, 0.8C, and 1C (1C = 117 mA·g). -1 ), releasing 104.4 mAh·g respectively. -1 99.7mAh·g -1 96.0mAh·g -1 89.3mAh·g -1 and 85.7mAh·g -1 The specific capacity; when returned to 0.2C, the capacity can recover to 104.0 mAh·g. -1 . Figure 5 The h-5i shows that the battery has an initial discharge capacity of 102.1 mAh·g at 0.3C. -1 After 250 cycles, the capacity retention rate was 95.8%, and the average coulombic efficiency reached 99.9%.

[0080] Example 3 uses a MAILS solid electrolyte formed by mixing LiFSI, KFSI, MSM, and Al2O3 as an example. Figure 6 This is a graph showing the Li / MAILS / LFP cycle performance of the present invention. (See diagram below.) Figure 6 As shown, the all-solid-state Li / MAILS / LFP battery exhibits excellent long-term cycle stability at 30℃. After 200 cycles at 2C, the capacity retention is 89.7%, and the discharge specific capacity reaches 122.6 mAh·g. - ¹.

[0081] Example 4 uses BAILS solid electrolyte formed by mixing LiFSI, KFSI, BDS, and Al2O3 as an example. Figure 7 This is a graph showing the Li / BAILS / LFP cycle performance of the present invention. (See diagram below.) Figure 7 As shown, the all-solid-state Li / BAILS / LFP battery exhibits excellent long-term cycle stability at 30℃. After 200 cycles at 2C, the capacity retention is 98.9%, and the discharge specific capacity reaches 121.5 mAh·g. - ¹.

[0082] Example 5 uses a DCILS solid electrolyte formed by mixing LiFSI, KFSI, DMMN, and CeO2. Figure 8 This is a graph showing the Li / DCILS / LFP cycle performance of the present invention. (See diagram below.) Figure 8 As shown, the all-solid-state Li / DCILS / LFP battery exhibits excellent long-term cycle stability at 30℃. After 200 cycles at 2C, the capacity retention is 94.1%, and the discharge specific capacity reaches 133.8 mAh·g. - ¹.

[0083] Taking the MLCILS solid electrolyte formed by mixing LiFSI, KFSI, MSM, Li2O and CMC as an example (Example 6), this self-supporting solid electrolyte membrane can help improve electrochemical performance. Figure 9 This is a graph showing the Li / MLCILS / LCO cycle performance of this invention. (See diagram below.) Figure 9 As shown, the all-solid-state Li / MLCILS / LCO battery exhibits excellent long-term cycling stability at room temperature. After 100 cycles at 1C, the capacity retention is 90.3%, and the discharge specific capacity reaches 145.4 mAh·g. - ¹.

[0084] Taking the MLPILS solid electrolyte formed by mixing LiFSI, KFSI, MSM, Li2O and PVDF as an example (Example 7), this self-supporting solid electrolyte membrane can help improve electrochemical performance. Figure 10 This is a graph showing the Li / MLPILS / LCO cycle performance of this invention. (See diagram below.) Figure 10As shown, the all-solid-state Li / MLPILS / LCO battery exhibits excellent long-term cycling stability at room temperature. After 100 cycles at 2C, the capacity retention is 100.0%, and the discharge specific capacity reaches 150.1 mAh·g⁻¹. - ¹.

[0085] Taking the MLNILS solid electrolyte formed by mixing LiFSI, KFSI, MSM, Li2O and PAN as an example (Example 8), this self-supporting solid electrolyte membrane can help improve electrochemical performance. Figure 11 This is a graph showing the cycling performance of the Li / MLNILS / LFP of this invention. (See diagram below.) Figure 11 As shown, the all-solid-state Li / MLNILS / LFP battery exhibits excellent long-term cycling stability at room temperature. After 50 cycles at 2C, the capacity retention is 100.0%, and the discharge specific capacity reaches 134.6 mAh·g⁻¹. - ¹.

[0086] Comparative Example 7 uses a SAILS solid electrolyte formed by mixing LiFSI, KFSI, SN, and Al2O3. Figure 12 This is a graph showing the Li / SAILS / LCO cycle performance of this invention. (See diagram below.) Figure 12 As shown, the coulombic efficiency of the all-solid-state Li / SAILS / LCO battery at room temperature is less than 90%, which may be related to the reaction between SN and Li. This indicates that the selection of electron-withdrawing organic solids should not be limited to their affinity for Li, but should also take into account their stability with Li and their stability under high voltage.

[0087] It should be noted that when numerical ranges are involved in this invention, it should be understood that both endpoints of each numerical range, as well as any value between the two endpoints, can be selected. Since the steps and methods used are the same as in the embodiments, preferred embodiments are described here to avoid redundancy. Although preferred embodiments of this invention have been described, those skilled in the art, once they understand the basic inventive concept, can make other changes and modifications to these embodiments. Therefore, the appended scope of protection is intended to be interpreted as including the preferred embodiments and all changes and modifications falling within the scope of this invention.

[0088] Obviously, those skilled in the art can make various modifications and variations to this invention without departing from its spirit and scope. Therefore, if these modifications and variations fall within the scope of protection of this invention and its equivalents, this invention also intends to include these modifications and variations.

Claims

1. A wide potential window plasticized solid electrolyte, characterized in that, The solid electrolyte is composed of a mixture of bis(fluorosulfonyl)imide alkali metal salt, an organic compound with an electron-withdrawing group, and a metal oxide; the electron-withdrawing group is cyano or sulfonyl; the mass ratio of bis(fluorosulfonyl)imide alkali metal salt to the organic compound with an electron-withdrawing group is 1:0.05~2; the mass ratio of bis(fluorosulfonyl)imide alkali metal salt to the metal oxide is 1:0.05~0.

3.

2. The wide potential window plasticized solid electrolyte according to claim 1, characterized in that, Organic compounds with electron-withdrawing groups include dimethylmalononitrile, dimethyl sulfone, cyclobutene sulfone, or 1,3-propenesulfonate lactone.

3. The wide potential window plasticized solid electrolyte according to claim 1, characterized in that, The alkali metal salt of bisfluorosulfonylimide is lithium bisfluorosulfonylimide or sodium bisfluorosulfonylimide and a stabilizer, wherein the stabilizer is potassium bisfluorosulfonylimide or cesium bisfluorosulfonylimide, and the mass ratio of lithium bisfluorosulfonylimide or sodium bisfluorosulfonylimide to the stabilizer is 1:0.59~1.

7.

4. The wide potential window plasticized solid electrolyte according to claim 1, characterized in that, The metal oxide is aluminum oxide, lithium oxide, titanium oxide, or cerium oxide.

5. The wide potential window plasticized solid electrolyte according to claim 1, characterized in that, The solid electrolyte mixing process also includes a film-forming aid; the mass ratio of the alkali metal salt of bis(fluorosulfonyl)imide to the film-forming aid is 1:0.3~1.

5.

6. The wide potential window plasticized solid electrolyte according to claim 1, characterized in that, The film-forming aids are sodium carboxymethyl cellulose, polyvinylidene fluoride, polyacrylonitrile, or polyacrylic acid.

7. A method for preparing a wide potential window plasticized solid electrolyte according to any one of claims 1 to 6, characterized in that, Includes the following steps: A wide-potential-window plasticized solid electrolyte is obtained by mixing a bis(fluorosulfonyl)imide alkali metal salt, an organic compound with an electron-withdrawing group, and a metal oxide, and heating the mixture at 70°C to 120°C.

8. The method for preparing a wide potential window plasticized solid electrolyte according to claim 7, characterized in that, Heating time is 1 to 3 hours.

9. A lithium / sodium battery, characterized in that, The lithium / sodium battery includes a positive electrode, a negative electrode, a glass fiber separator, and an electrolyte, or includes a positive electrode, a negative electrode, and an electrolyte, wherein the electrolyte is a wide potential window plasticized solid electrolyte as described in any one of claims 1 to 6.

10. The lithium / sodium battery according to claim 9, characterized in that, The electrochemical window of the wide potential window plasticized solid electrolyte is -0.1V to 5.5V.