A PVDF-based high-entropy lithium salt solid electrolyte, its preparation method and application
By designing a PVDF-based high-entropy lithium salt solid electrolyte and utilizing a multi-anion synergistic coordination structure and surface-modified fillers, the performance bottleneck of PVDF-based solid electrolytes was solved, achieving high lithium-ion transference number, stable interface, and long cycle life, thus improving the overall performance of lithium metal batteries.
Patent Information
- Application Number
- CN202611461297.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-20
- Publication Date
- 2026-11-17
AI Technical Summary
Existing PVDF-based solid electrolytes cannot simultaneously achieve high room temperature ionic conductivity, high lithium-ion transference number, stable lithium metal interface, excellent mechanical properties, and long cycle life, and traditional improvement methods have limitations.
A PVDF-based high-entropy lithium salt solid electrolyte is adopted. By synergistically combining the main lithium salt LiTFSI with four auxiliary lithium salts LiFSI, LiPF6, LiDFOB and LiNO3, a multi-anion synergistic coordination structure is formed. Combined with surface-modified inorganic fillers, the lithium salt composition design is optimized, the lithium ion transport path is improved and the interfacial side reactions are reduced.
It significantly improves the lithium-ion transference number, enhances interface stability and mechanical properties, extends battery cycle life, reduces ion transport activation energy, inhibits lithium dendrite growth, and improves battery safety and high energy density.
Smart Images

Figure CN123120862A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of battery material preparation technology, and particularly relates to the field of solid-state lithium metal battery preparation, specifically a PVDF-based high-entropy lithium salt solid electrolyte and its preparation method and application. Background Technology
[0002] With the rapid development of portable electronic devices, electric vehicles, and large-scale energy storage systems, the requirements for high energy density, high safety, long cycle life, and wide temperature range adaptability of suitable secondary batteries are constantly increasing. Lithium metal anodes, due to their extremely high theoretical specific capacity and low electrochemical potential, are considered important anode materials for constructing next-generation high-energy-density battery systems. However, in traditional liquid electrolyte systems, lithium metal anodes are prone to uneven deposition during repeated deposition / stripping, which can induce lithium dendrite growth. Lithium dendrites not only consume active lithium and electrolyte, leading to reduced coulombic efficiency and shortened cycle life, but may also puncture the separator, causing internal short circuits and posing serious safety hazards. Furthermore, traditional liquid electrolytes themselves have inherent safety risks such as leakage, volatilization, combustion, and explosion.
[0003] Replacing traditional liquid electrolytes with solid-state electrolytes is considered a crucial technological approach to improve the safety of lithium metal batteries and suppress lithium dendrite growth. Solid-state electrolytes typically possess excellent thermal stability and good mechanical strength, physically blocking lithium dendrite penetration while fundamentally eliminating problems such as leakage, volatilization, and combustion associated with liquid electrolytes. Based on their material composition, solid-state electrolytes mainly include inorganic solid-state electrolytes, polymer solid-state electrolytes, and organic / inorganic composite solid-state electrolytes. While inorganic solid-state electrolytes exhibit high bulk ionic conductivity, their brittleness and processing difficulties severely limit their practical applications. Organic / inorganic composite solid-state electrolytes suffer from inherent drawbacks such as poor compatibility between inorganic fillers and the polymer matrix, high ion transport barriers, and complex fabrication processes. In contrast, polymer solid-state electrolytes offer advantages such as good flexibility, strong film-forming properties, simple processing, and good contact with the electrode interface, making them more suitable for fabricating thin-film, flexible, and large-area battery modules.
[0004] Among various polymer solid electrolyte matrix materials, polyvinylidene fluoride (PVDF) is widely used in the construction of solid or quasi-solid electrolytes due to its high dielectric constant, good chemical stability, moderate mechanical properties, and excellent film-forming ability. The PVDF molecular chain contains a large number of polar C-F bonds, which facilitates lithium salt dissociation. Simultaneously, its good mechanical strength helps improve the dimensional stability and puncture resistance of the electrolyte film. Furthermore, PVDF-based electrolytes exhibit good interfacial adhesion with commonly used lithium battery positive and negative electrode materials, which helps reduce interfacial impedance caused by insufficient rigid contact in solid-state batteries.
[0005] However, existing PVDF-based solid electrolytes still have significant performance bottlenecks: First, the limited mobility of PVDF polymer segments results in insufficiently continuous ion transport channels at room temperature, leading to typically low room-temperature ionic conductivity of the electrolyte, which is insufficient to meet the demands of high-rate charge and discharge. Second, traditional PVDF-based solid electrolytes have low lithium-ion transference numbers and high anion migration ratios, which can easily cause concentration polarization during battery charge and discharge, resulting in uneven distribution of lithium ions on the surface of the lithium metal anode and accelerating lithium dendrite formation. Third, there are complex interactions between PVDF segments, lithium salt anions, and lithium ions; excessively strong local coordination may restrict the rapid migration of lithium ions and increase the ion migration barrier. In addition, the interfacial stability between PVDF-based solid electrolytes and lithium metal anodes still needs improvement. Interfacial side reactions continuously consume lithium salts and active lithium, leading to a continuous increase in interfacial impedance, ultimately affecting the cycle life and safety performance of the battery.
[0006] To address these shortcomings, existing technologies primarily employ methods such as inorganic filler composites, polymer structure modification, plasticizer introduction, and lithium salt concentration control. For example, by adding inorganic fillers such as Al2O3, SiO2, LLZO, and LLZTO, the mechanical strength, thermal stability, and local ion transport capacity of polymer electrolytes are improved; the structure of PVDF-based polymers is controlled through copolymerization, grafting, crosslinking, or blending to improve polymer chain mobility and film-forming properties; and plasticizers or ionic liquids are introduced to enhance the electrolyte's flexibility and room-temperature ionic conductivity.
[0007] The aforementioned improvement methods still have certain limitations. Inorganic fillers are prone to agglomeration in polymer matrices, causing interfacial defects and discontinuous ion transport paths, and may even reduce the uniformity and mechanical reliability of the electrolyte membrane. Although polymer molecular structure modification can improve chain segment movement, the synthesis steps are relatively complex, and the process stability and large-scale preparation are difficult. Simply increasing the lithium salt concentration or introducing a single auxiliary lithium salt often fails to simultaneously address lithium salt dissociation, ion transference number, interfacial film stability, and electrochemical window. While the addition of plasticizers or liquid components can improve ionic conductivity, it may also reduce the mechanical strength, thermal stability, and safety of the electrolyte.
[0008] Especially in lithium metal battery systems, the electrolyte not only needs to possess high bulk ionic conductivity but also needs to form a stable, dense solid electrolyte interface film with good lithium-ion conductivity on the surface of the lithium metal anode. In traditional single lithium salt systems, the types of anions and interfacial reaction pathways are relatively limited, resulting in a finite composition of the interface film, making it difficult to simultaneously meet the requirements of high mechanical stability, high ionic conductivity, and high chemical stability. Therefore, how to simultaneously regulate bulk ion transport behavior and electrode / electrolyte interface chemistry through electrolyte formulation design is key to improving the overall performance of PVDF-based solid electrolytes.
[0009] In summary, existing PVDF-based solid-state electrolytes still struggle to simultaneously achieve high room-temperature ionic conductivity, high lithium-ion transference number, stable lithium metal interface, excellent mechanical properties, and long cycle life. Therefore, there is an urgent need to develop a novel PVDF-based solid-state electrolyte system that, while maintaining the good film-forming properties and mechanical stability of PVDF, improves lithium-ion transport pathways, reduces interfacial side reactions, and suppresses lithium dendrite growth through rational lithium salt composition design and synergistic effects of multiple components, thereby meeting the application requirements of high-safety, high-energy-density lithium metal batteries. Summary of the Invention
[0010] To address the challenge of existing PVDF-based solid electrolytes simultaneously achieving high room-temperature ionic conductivity, high lithium-ion transference number, stable lithium metal interface, excellent mechanical properties, and long cycle life, this invention provides a PVDF-based high-entropy lithium salt solid electrolyte, its preparation method, and its applications.
[0011] This invention is achieved using the following technical solution: This invention provides a PVDF-based high-entropy lithium salt solid electrolyte, wherein the PVDF-based high-entropy lithium salt solid electrolyte has a thickness of 50–150 μm and comprises: PVDF polymer matrix, A high-entropy lithium salt system, dispersed in a PVDF polymer matrix, consists of a main lithium salt and four auxiliary lithium salts; The main lithium salt is lithium bis(trifluoromethanesulfonyl)imide (LiTFSI), and the auxiliary lithium salts are lithium bis(fluoromethanesulfonyl)imide (LiFSI), lithium hexafluorophosphate (LiPF6), lithium difluorooxalate borate (LiDFOB), and lithium nitrate (LiNO3). The molar ratio of the main lithium salt to each auxiliary lithium salt is (3~4):(0.2~0.3). In the high-entropy lithium salt system, the anions of the four auxiliary lithium salts form a multi-anion cooperative coordination structure in the PVDF matrix. The cooperative coordination structure makes the intensity of the PVDF β phase diffraction peak at 2θ≈20.2° in the XRD pattern of the PVDF-based high-entropy lithium salt solid electrolyte higher than that of the PVDF solid electrolyte containing only lithium bis(trifluoromethanesulfonyl)imide, and the lithium ion transference number of the PVDF-based high-entropy lithium salt solid electrolyte is ≥0.45.
[0012] Preferably, the ion transport activation energy of the PVDF-based high-entropy lithium salt solid electrolyte is ≤0.15eV.
[0013] The "high-entropy lithium salt system" described in this invention refers to a multi-anion lithium salt system composed of a main lithium salt and at least four auxiliary lithium salts, wherein the types and concentrations of anions in each auxiliary lithium salt are within a specific range. In this system, multiple anions form competitive coordination relationships in the PVDF matrix, so that the first solvation shell of the lithium ion simultaneously contains at least four different anions, thereby significantly increasing the configurational entropy of the lithium ion solvation structure and suppressing the formation of overly stable contact ion pairs between a single anion and the lithium ion.
[0014] In the high-entropy lithium salt system of this invention, the main lithium salt LiTFSI provides the basic lithium-ion concentration and ion conductivity; the auxiliary lithium salt LiFSI has a high degree of dissociation, which can promote further dissociation of the lithium salt in the PVDF matrix, while FSI... - Anions participate in interfacial reactions to form LiF-rich SEI components; PF6 of the co-lithium salt LiPF6 - Anions have a large molecular volume and low coordination ability, which can increase the diversity of anion species and increase the configuration entropy of solvation structures. Meanwhile, PF6... - At low concentrations, it does not participate in significant interfacial side reactions; DFOB of the auxiliary lithium salt LiDFOB - Anions are preferentially reduced on the lithium anode surface, forming a dense SEI layer containing borate and LiF; the NO3- of the auxiliary lithium salt LiNO3... - Anions are reduced to form Li3N on the surface of the lithium anode. Li3N has high lithium-ion conductivity, which can promote the rapid transport of lithium ions in the SEI layer.
[0015] The anions of the four auxiliary lithium salts mentioned above form a synergistic functional division of labor in the PVDF matrix, namely "dissociation promotion, configurational entropy increase, SEI densification, and interfacial ion conduction." This synergistic effect is not a simple superposition of multiple lithium salts, but is achieved through the competitive coordination relationship of each anion in the polar environment of PVDF. Specifically, the molar ratio of LiTFSI to the four auxiliary lithium salts is controlled within the range of (3~4):(0.2~0.3), so that the proportion of the total molar number of auxiliary lithium salts to the molar number of main lithium salts is within a specific window. This ensures that multiple anions can participate in the construction of the lithium-ion solvation structure, while avoiding excessive auxiliary lithium salts that would lead to anion aggregation and exacerbate interfacial side reactions.
[0016] This invention provides a method for preparing a PVDF-based high-entropy lithium salt solid electrolyte, comprising the following steps: S1. Take PVDF powder and vacuum dry it at 60~80℃ for 12~24 hours to remove the adsorbed moisture.
[0017] S2. Add the dried PVDF powder to an organic solvent, DMF (N,N-dimethylformamide). The organic solvent is mainly used to dissolve PVDF and disperse lithium salt. It is at least partially removed during the subsequent film-forming and drying process. Stir at 40~60℃ for 2~4 hours to obtain a PVDF polymer solution with a mass fraction of 8%~12%, calculated by mass ratio.
[0018] S3. Add the main lithium salt lithium bis(trifluoromethanesulfonyl)imide and four auxiliary lithium salts lithium bis(fluoromethanesulfonyl)imide (LiFSI), lithium hexafluorophosphate (LiPF6), lithium difluorooxalate borate (LiDFOB), and lithium nitrate (LiNO3) sequentially to the PVDF polymer solution. In the electrolyte precursor solution, the concentration of the main lithium salt LiTFSI is 1.2-1.6 mol / L, preferably 1.4 mol / L; the concentration of each auxiliary lithium salt is 0.08-0.12 mol / L; the four auxiliary lithium salts are added in the order of lithium bis(fluoromethanesulfonyl)imide, lithium hexafluorophosphate, lithium difluorooxalate borate, and lithium nitrate, with a stirring interval of 10-30 minutes between each addition. By utilizing the synergistic effects of different lithium salt anions in lithium salt dissociation, ion transport, polymer segment regulation, and interfacial film formation, and by controlling the ratio between the main lithium salt and various auxiliary lithium salts, different anions can form a synergistic effect in the PVDF matrix. This improves the lithium salt dissociation state, regulates the lithium ion coordination environment, improves the lithium ion transport path inside the electrolyte, enhances the lithium ion migration ability, and thus improves the lithium ion transport performance in the electrolyte membrane and enhances its interfacial stability with the lithium metal anode.
[0019] After adjusting the volume, stir at 25-40°C in the dark for 24-48 hours to obtain a homogeneous electrolyte precursor solution.
[0020] To improve the mechanical strength, lithium-ion transference number, and interfacial stability of the electrolyte, as an alternative, a surface-modified inorganic filler is added to the PVDF polymer solution before adding the main lithium salt and auxiliary lithium salt. The inorganic filler is selected from one or more of BaTiO3, LLZTO, LLZO, Al2O3, SiO2, and TiO2, and the amount of inorganic filler added is 1% to 30% of the PVDF powder. Preferably, the surface-modified inorganic filler is BaTiO3 particles surface-modified with a silane coupling agent. The surface-modified inorganic filler can improve the compatibility between the inorganic filler and the PVDF polymer matrix, reduce filler agglomeration, and form a composite interface between the filler surface, PVDF segments, and the high-entropy lithium salt system, thereby facilitating the construction of continuous lithium-ion transport channels.
[0021] S4. The electrolyte precursor solution is poured onto the substrate, coated or cast into a film, and dried. The drying process includes initial drying at 40~60℃ for 6~12 hours, followed by continued drying in a vacuum drying oven at 50~70℃ for 24~48 hours to remove residual solvent, thereby obtaining the PVDF-based high-entropy lithium salt solid electrolyte.
[0022] This method has a simple process flow, mild film-forming conditions, and readily available raw materials, making it suitable for laboratory preparation and further scale-up production.
[0023] This invention provides an application of a PVDF-based high-entropy lithium salt solid electrolyte in a lithium metal battery. The lithium metal battery includes a positive electrode, a negative electrode, and a PVDF-based high-entropy lithium salt solid electrolyte disposed between the positive and negative electrodes. The active material of the positive electrode is one of lithium transition metal oxides and lithium transition metal phosphates, preferably LiFePO4, LiCoO2, or LiNi. 0.8 Co 0.1 Mn 0.1 Any one of O2, with the negative electrode being a metallic lithium foil or a lithium-plated copper foil.
[0024] This lithium metal battery exhibits high cycle stability, good rate performance, superior interface stability, and improved safety performance.
[0025] Preferably, the PVDF-based high-entropy lithium salt solid electrolyte is at 0.2 mA·cm⁻¹ -2 The cycle life of the assembled lithium symmetric battery at the current density is ≥800 hours.
[0026] Compared with the prior art, the present invention has the following beneficial effects: (1) This invention achieves a high-entropy solvation structure by synergistically combining the main lithium salt LiTFSI with four auxiliary lithium salts: LiFSI, LiPF6, LiDFOB, and LiNO3, resulting in the simultaneous presence of at least five different anions in the PVDF matrix. This structure significantly increases the configurational entropy of the lithium-ion solvation shell and reduces the strong coordination between lithium ions and individual anions, thereby lowering the ion transport activation energy. Experiments show that the ion transport activation energy of Example 1 of this invention is only 0.13 eV, significantly lower than the 0.21 eV of Comparative Example 1, which contains only LiTFSI.
[0027] (2) The high-entropy lithium salt system of the present invention can induce the transformation of PVDF from α-crystalline phase to β-crystalline phase. XRD test shows that the intensity of the β-crystalline phase diffraction peak of the electrolyte membrane of Example 1 at 2θ≈20.2° is significantly enhanced compared with that of Comparative Example 1. The high content of β-crystalline phase endows the PVDF matrix with strong polarity and piezoelectric properties, which helps to guide the uniform deposition of lithium ions and inhibit the growth of lithium dendrites.
[0028] (3) This invention forms a composite SEI film containing LiF, Li3N, Li2O, borate, and organic lithium salts through the synergistic interfacial reaction of four auxiliary lithium salt anions on the lithium anode surface. The LiDFOB-derived borate component improves the SEI compactness, the LiNO3-derived Li3N component improves the lithium-ion conductivity of the SEI, the LiFSI-derived LiF component improves the mechanical strength of the SEI, and the introduction of LiPF6 increases the diversity of inorganic components in the SEI. This composite SEI film effectively suppresses the continuous side reactions between the electrolyte and metallic lithium, and slows down the growth of interfacial impedance.
[0029] (4) This invention improves the stability of the lithium symmetric battery at 0.2 mA·cm⁻¹ by simultaneously improving bulk ion transport and electrode / electrolyte interface stability. -2 The Li|LiFePO4 full cell maintains a high capacity retention rate after 1000 cycles at 1C rate, with stable cycling for over 1000 hours at current density. Its overall performance is superior to existing technologies. Attached Figure Description
[0030] Figure 1 This is the SEM image of Example 1.
[0031] Figure 2 This is the SEM image of Comparative Example 1.
[0032] Figure 3 A comparison of the XRD patterns of Example 1 and Comparative Example 1 shows that the diffraction peak of the β phase (20.2°) in the high-entropy electrolyte is significantly enhanced.
[0033] Figure 4 The Arrhenius curves for Example 1 and Comparative Example 1 show that the high-entropy electrolyte has a lower ion transport activation energy (0.13 eV vs. 0.21 eV).
[0034] Figure 5 This is a comparison graph showing the cycle performance of lithium symmetric batteries using Example 1 and Comparative Example 1.
[0035] Figure 6 This is a comparison chart of the discharge capacity of the Li|LiFePO4 full cells of Example 1 and Comparative Example 1 at a 1C rate.
[0036] Figure 7 The lithium-ion migration number diagram is for the lithium-symmetric battery used in Example 1.
[0037] Figure 8 The lithium-ion migration number diagram is used for the lithium symmetric battery of Comparative Example 1. Detailed Implementation
[0038] The specific embodiments of the present invention will be described in detail below.
[0039] Example 1 A method for preparing a PVDF-based high-entropy lithium salt solid electrolyte, such as... Figure 1 As shown, it includes the following steps: S1. Weigh 1.0 g of PVDF powder (Sigma-Aldrich) with a weight average molecular weight of 400,000 and dry it under vacuum at 70 °C for 24 hours.
[0040] S2. Add 9.0g of DMF solvent to the dried PVDF powder and stir in a 50℃ water bath for 3 hours to obtain a clear PVDF polymer solution with a mass fraction of 10%.
[0041] S3. Add 1.4 mol / L LiTFSI, 0.1 mol / L LiFSI, 0.1 mol / L LiPF6, 0.1 mol / L LiDFOB and 0.1 mol / L LiNO3 to the PVDF polymer solution, with the concentrations based on the volume of the prepared electrolyte precursor solution. Make up the volume and stir at 30°C in the dark for 36 hours to obtain a homogeneous electrolyte precursor solution.
[0042] S4. The electrolyte precursor solution was poured onto a flat glass plate, and the coating thickness was controlled to be 150 μm using a doctor blade. It was initially dried at 50 °C for 8 hours, and then transferred to a vacuum drying oven at 60 °C for 36 hours to obtain a PVDF-based high-entropy lithium salt solid electrolyte and a self-supporting electrolyte membrane with a thickness of 100 μm, denoted as HEPF-1.
[0043] Example 2 Except for the high-entropy lithium salt system, the rest is the same as in Example 1. In this example, in step S3, 1.2 mol / L LiTFSI, 0.08 mol / L LiFSI, 0.08 mol / L LiPF6, 0.08 mol / L LiDFOB and 0.08 mol / L LiNO3 are used, and the resulting product is denoted as HEPF-2.
[0044] Example 3 Except for the high-entropy lithium salt system, the rest is the same as in Example 1. In this example, in step S3, 1.6 mol / L LiTFSI, 0.12 mol / L LiFSI, 0.12 mol / L LiPF6, 0.12 mol / L LiDFOB and 0.12 mol / L LiNO3 are used, and the resulting product is denoted as HEPF-3.
[0045] Example 4 This embodiment contains modified barium titanate filler. Except for the addition of surface-modified inorganic filler in step S3, the rest is the same as in Example 1. In step S3, 5% of the mass of PVDF barium titanate (BaTiO3) submicron particles with a particle size of about 200 nm, which are surface-modified with silane coupling agent KH-550, are first added to the PVDF polymer solution. After ultrasonic dispersion for 1 hour, the main lithium salt and three auxiliary lithium salts are added in sequence. The subsequent steps are exactly the same as in Example 1. The resulting product is denoted as HEPF-1 / BT.
[0046] Example 5 In order to prioritize the formation of an optimal stable SEI film rich in various inorganic components on the surface of the lithium anode in situ, this embodiment uses a specific combination of auxiliary lithium salts to optimize the interface. Except for the type of auxiliary lithium salt in step S3, the rest is the same as in Example 1. The auxiliary lithium salts are LiFSI, LiDFOB and LiNO3, and the resulting product is denoted as HEPF-1(FDN).
[0047] Comparative Example 1 This comparative example prepared a conventional electrolyte using only 1.4 mol / L LiTFSI as the lithium salt, without adding any auxiliary lithium salt. All other steps were identical to those in Example 1. The resulting membrane was denoted as LEPF.
[0048] Comparative Example 2 This comparative example prepared a single auxiliary lithium salt electrolyte. The main lithium salt was the same as in Example 1, namely 1.4 mol / L LiTFSI. Only one auxiliary lithium salt was added, namely 0.1 mol / L LiFSI. The other steps were the same as in Example 1. The resulting membrane was denoted as SPE-LiFSI.
[0049] Comparative Example 3 This comparative example prepared a high-entropy electrolyte containing unmodified filler. It used inorganic filler without any surface modification and barium titanate (BaTiO3) submicron particles without any surface modification. The rest was exactly the same as in Example 4. The resulting membrane was denoted as HEPF-1 / uBT.
[0050] Compared to Example 4, this is used to anticipate the degree to which the uniformity, mechanical properties, and interfacial ion transport performance of the electrolyte membrane decrease due to poor compatibility and easy agglomeration of the filler with the polymer matrix.
[0051] Comparative Example 4 This comparative example prepared a composite electrolyte of a conventional lithium salt and a polymerizable fluorinated solvent. 1.4 mol / L LiTFSI was used as the lithium salt, without adding any auxiliary lithium salt. However, the organic solvent in step S2 was replaced with the polymerizable fluorinated solvent hexafluorobutyl methacrylate (HFBMA), and azobisisobutyronitrile (AIBN), a thermal initiator accounting for 0.5% of the HFBMA monomer mass, was added to the precursor solution. After subsequent film formation, in-situ thermal polymerization was initiated at 70°C for 24 hours. The remaining steps were the same as in Example 1. The resulting film was denoted as LEPF / pHFBMA.
[0052] Compared with Example 1, this comparative example is used to verify that in the absence of a high-entropy lithium salt system, the polymer network formed is too rigid and lacks the synergistic plasticizing effect of multiple anions, resulting in blocked ion transport channels and a significant decrease in ion conductivity, thus proving the irreplaceability of the high-entropy lithium salt system.
[0053] Comparative Example 5 This comparative example prepared an electrolyte lacking the LiDFOB component. Except for the type of auxiliary lithium salt in step S3, all other steps were the same as in Example 1. The main lithium salt remained 1.4 mol / L LiTFSI, and the auxiliary lithium salts consisted only of LiFSI and LiNO3, both at a concentration of 0.1 mol / L. LiDFOB was not added. The remaining steps were identical to those in Example 1. The resulting membrane was designated HEPF-FN.
[0054] This comparative example is used to verify the role of LiDFOB in high-entropy lithium salt systems. It aims to demonstrate that without LiDFOB, a dense, high-ionic-conductivity SEI film cannot be formed on the surface of the lithium metal anode, resulting in a significant reduction in interface stability and a substantial decrease in lithium-ion transference number and cycle life.
[0055] Comparative Example 6 The specific procedures for preparing a porous composite electrolyte impregnated with lithium salt electrolyte in this comparative example are as follows: First, a porous PVDF framework was prepared by electrospinning: 8 wt% PVDF (Mw=400,000) was dissolved in DMF and stirred at 50℃ for 4 h to obtain a spinning solution. Electrospinning was performed using an electrospinning machine under the conditions of 15 kV voltage, feed speed 0.5 mL / h, receiving distance 15 cm, and ambient humidity <30%. The PVDF nanofiber nonwoven fabric was collected and vacuum dried at 60℃ for 24 h to obtain a porous PVDF framework with a thickness of about 80 μm and three-dimensional interconnected pores.
[0056] A concentrated electrolyte was prepared by dissolving 1.4 mol / L LiTFSI in dimethyl ethylene glycol (DME). The porous PVDF framework was then immersed in the electrolyte and soaked in a vacuum atmosphere at 40°C for 2 hours. After removal, excess electrolyte on the surface was gently wiped off with filter paper to obtain LEPF / Porous.
[0057] This comparative example is used to verify the transport advantages of high-entropy salt systems over single lithium salts within a confined space.
[0058] Performance Tests and Results The electrolyte membranes obtained in the above embodiments and comparative examples were subjected to the following performance tests.
[0059] Ion conductivity test: Electrochemical impedance spectroscopy (EIS) was used to determine the result according to the formula σ = d / (R). b Calculate the ionic conductivity using the formula σ = d × A, where σ is the ionic conductivity, d is the film thickness, A is the electrode area, and R is the electrode area. b This is the bulk resistance.
[0060] Lithium-ion transference number test: By combining DC polarization and EIS testing, the electrolyte membrane was assembled into a symmetrical cell using the Bruce-Vincent method.
[0061] Battery cycle performance test: The electrolyte membrane was assembled into a full cell, and constant current charge-discharge tests were performed on the Blue Electric test system using the Newway Battery Test System to record the cycle life.
[0062] The HEPF-1 obtained in Example 1 was characterized by SEM, and the results are as follows: Figure 1 As shown; the LEPF prepared in Example 1 was characterized by SEM, and the results are as follows. Figure 2 As shown in the figure, the electrolyte membrane surface of Example 1 is more uniform and dense, with no obvious defects, indicating that the high-entropy lithium salt system helps to improve the film uniformity of PVDF-based electrolytes.
[0063] The HEPF-1 prepared in Example 1 was characterized by XRD, and the results are as follows: Figure 3 As shown: Compared with the LEPF of Comparative Example 1, the HEPF-1 of Example 1 showed a significant increase in the intensity of the diffraction peak corresponding to the piezoelectric β-phase of PVDF at 2θ≈20.2°, which confirms that the high-entropy lithium salt system of the present invention has the ability to induce the formation of a high content of β-phase in PVDF. The high content of β-phase endows the PVDF matrix with strong polarity and piezoelectric properties, thereby helping to guide the uniform deposition of lithium ions and suppress the growth of lithium dendrites.
[0064] Temperature-dependent impedance tests were performed on the electrolyte membranes of Example 1 and Comparative Example 1, and Arrhenius curves were plotted. The results are as follows: Figure 4 As shown, the ion transport activation energy of Example 1 is 0.13 eV, which is significantly lower than that of Comparative Example 1 (0.21 eV), indicating that the high-entropy lithium salt system effectively reduces the lithium-ion migration energy barrier.
[0065] The electrolyte membranes from Example 1 and Comparative Example 1 were assembled into a Li|Li symmetric cell, and the temperature was measured at 0.2 mA·cm⁻¹. -2 Constant current cycling tests were performed at current density, and the results are as follows: Figure 5 As shown, the symmetric battery of Example 1 cycled stably for more than 1000 hours, while Comparative Example 1 showed a significant increase in voltage polarization after 200 hours, indicating that the high-entropy lithium salt system significantly improved the interfacial stability with the lithium metal anode.
[0066] The electrolyte membranes of Example 1 and Comparative Example 1 were assembled into Li|LiFePO4 full cells, and constant current charge-discharge tests were performed at a 1C rate. The results are as follows. Figure 6 As shown, the full cell of Example 1 maintained a high capacity retention rate after 1000 cycles, while the capacity of Comparative Example 1 decreased significantly after 50 cycles.
[0067] The lithium-ion transference number of the electrolyte membranes of Example 1 and Comparative Example 1 was tested, and the results are as follows: Figure 7 and Figure 8 As shown. Calculated using the Bruce-Vincent method, the lithium-ion transference number of Example 1 was 0.69, significantly higher than that of Comparative Example 1 (0.24), indicating that the high-entropy lithium salt system effectively promoted selective lithium-ion transport and reduced concentration polarization.
[0068] The electrolyte membranes obtained in Examples 1-3 and Comparative Examples 1-2 were subjected to performance tests, and the results are summarized in Table 1.
[0069] Table 1. Comparison of the composition and performance of different electrolytes As shown in Table 1, Example 1 (main lithium salt 1.4 mol / L, each auxiliary lithium salt 0.1 mol / L) significantly outperformed Comparative Example 1 (traditional single LiTFSI salt, cycle life only 200 hours) and Comparative Example 2 (single auxiliary lithium salt LiFSI, cycle life 400 hours) in terms of lithium dendrite suppression, symmetric battery cycle life (1000 hours), and full-cell cycle performance (1000 cycles at 1C rate). Although the performance of Examples 2 and 3 was slightly lower than that of Example 1, it was still far superior to the comparative examples, indicating that the high-entropy synergistic effect can be achieved in the range of main lithium salt concentration of 1.2~1.6 mol / L and each auxiliary lithium salt concentration of 0.08~0.12 mol / L, with the ratio in Example 1 being the optimal.
[0070] To further evaluate the performance of the high-entropy system of the present invention under different enhancement strategies, supplementary tests were conducted on the electrolyte membranes obtained in Examples 1, 4, 5 and Comparative Examples 1-6, and the results are summarized in Table 2.
[0071] Table 2. Comparison of the composition and performance of different electrolytes Table 2 further reveals the performance of the high-entropy system of the present invention under different enhancement strategies: (1) The basic high-entropy formulation (HEPF-1) has a room temperature ionic conductivity of 6.5 × 10⁻⁶. -4 S·cm -1 The lithium-ion transference number is 0.48, and the symmetric battery cycle life is 1000 hours, which is superior to the traditional single-salt system (LEPF) and single auxiliary lithium salt system (SPE-LiFSI), confirming the necessity of multi-anion synergy.
[0072] (2) After introducing modified BaTiO3 filler (HEPF-1 / BT), the lithium-ion transference number was significantly increased to 0.72, the cycle life exceeded 1500 hours, and the mechanical strength was increased to 15.2 MPa. In contrast, the performance of the unmodified filler (HEPF-1 / uBT) was reduced due to agglomeration and interface defects, which proved the necessity of filler surface modification.
[0073] (3) When a specific combination of auxiliary lithium salts (HEPF-1(FDN), which is forced to contain LiFSI, LiDFOB and LiNO3) is used, the cycle life exceeds 1800 hours, which is the best among all samples. The cycle life of the comparative example 5 (HEPF-FN) without LiDFOB drops to 600 hours, which confirms the key role of LiDFOB in constructing a stable SEI film.
[0074] (4) The polymerizable solvent system (HEPF-1 / pHFBMA) achieves a wide electrochemical window of >5.0V and has no free solvent, resulting in excellent safety. In contrast, the traditional salt system (LEPF / pHFBMA) suffers from a sharp drop in conductivity to 8.0×10⁻⁶ due to the lack of plasticizing effect from the high-entropy salt. -5 S·cm -1 .
[0075] The porous confined structure (HEPF-1 / Porous) achieves a density of 1.6 × 10⁻⁶. -3 S·cm -1 Its ultra-high ionic conductivity, approaching that of liquid electrolytes, is significantly superior to that of traditional salt systems (LEPF / Porous, 8.5×10⁻⁶). -5 S·cm -1 ).
[0076] As shown in Tables 1 and 2, the high-entropy lithium salt system of this invention, through the synergistic coordination of multiple anions, comprehensively outperforms existing technologies in terms of ionic conductivity, lithium-ion transference number, interfacial stability, and cycle life. Furthermore, by introducing modified fillers, optimizing the auxiliary lithium salt combination, and employing polymerizable solvents or porous confined structures, one or more key properties of the electrolyte can be further enhanced to meet the needs of different application scenarios.
[0077] The scope of protection claimed by this invention is not limited to the specific embodiments described above. Moreover, for those skilled in the art, this invention can have various modifications and alterations. Any modifications, improvements, and equivalent substitutions made within the concept and principles of this invention should be included within the scope of protection of this invention.
Claims
1. A PVDF-based high-entropy lithium salt solid electrolyte, characterized in that, include: PVDF polymer matrix, A high-entropy lithium salt system, dispersed in a PVDF polymer matrix, consists of a main lithium salt and four auxiliary lithium salts; The main lithium salt is lithium bis(trifluoromethanesulfonyl)imide, and the auxiliary lithium salts are lithium bis(fluoromethanesulfonyl)imide, lithium hexafluorophosphate, lithium difluorooxalate borate, and lithium nitrate, respectively; the molar ratio of the main lithium salt to each auxiliary lithium salt is (3~4):(0.2~0.3). In the high-entropy lithium salt system, the anions of the four auxiliary lithium salts form a multi-anion cooperative coordination structure in the PVDF matrix. The cooperative coordination structure makes the intensity of the PVDF β phase diffraction peak at 2θ≈20.2° in the XRD pattern of the PVDF-based high-entropy lithium salt solid electrolyte higher than that of the PVDF solid electrolyte containing only lithium bis(trifluoromethanesulfonyl)imide, and the lithium ion transference number of the PVDF-based high-entropy lithium salt solid electrolyte is ≥0.
45.
2. The PVDF-based high-entropy lithium salt solid electrolyte according to claim 1, characterized in that, The thickness of the PVDF-based high-entropy lithium salt solid electrolyte is 50–150 μm.
3. The PVDF-based high-entropy lithium salt solid electrolyte according to claim 1, characterized in that, The ion transport activation energy of the PVDF-based high-entropy lithium salt solid electrolyte is ≤0.15eV.
4. A method for preparing a PVDF-based high-entropy lithium salt solid electrolyte according to any one of claims 1 to 3, characterized in that, Includes the following steps: S1, take PVDF powder and vacuum dry it at 60~80℃ for 12~24 hours; S2. Add the dried PVDF powder to an organic solvent and stir at 40~60℃ for 2~4 hours to obtain a PVDF polymer solution with a mass fraction of 8%~12%. S3. Add the main lithium salt lithium bis(trifluoromethanesulfonyl)imide and four auxiliary lithium salts lithium bis(fluoromethanesulfonyl)imide, lithium hexafluorophosphate, lithium difluorooxalate borate, and lithium nitrate sequentially to the PVDF polymer solution, so that the concentration of the main lithium salt in the electrolyte precursor solution is 1.2~1.6 mol / L and the concentration of each auxiliary lithium salt is 0.08~0.12 mol / L. After making up the volume, stir at 25~40℃ in the dark for 24~48 hours to obtain a homogeneous electrolyte precursor solution. S4. The electrolyte precursor solution is poured onto the substrate, coated or cast into a film, and dried to obtain a PVDF-based high-entropy lithium salt solid electrolyte.
5. The method for preparing a PVDF-based high-entropy lithium salt solid electrolyte according to claim 4, characterized in that, In step S3, the four auxiliary lithium salts are added in the following order: lithium difluorosulfonylimide, lithium hexafluorophosphate, lithium difluorooxalate borate, and lithium nitrate, with a stirring interval of 10-30 minutes between each addition.
6. The method for preparing a PVDF-based high-entropy lithium salt solid electrolyte according to claim 4, characterized in that, In step S2, the organic solvent is DMF; in step S4, the drying includes initial drying at 40~60℃ for 6~12 hours, followed by continued drying in a vacuum drying oven at 50~70℃ for 24~48 hours.
7. The method for preparing a PVDF-based high-entropy lithium salt solid electrolyte according to claim 4, characterized in that, In step S3, before adding the main lithium salt and the auxiliary lithium salt, surface-modified inorganic filler is added to the PVDF polymer solution. The inorganic filler is selected from one or more of BaTiO3, LLZTO, LLZO, Al2O3, SiO2 and TiO2, and the amount of inorganic filler added is 1% to 30% of the PVDF powder.
8. The application of a PVDF-based high-entropy lithium salt solid electrolyte as described in any one of claims 1 to 3 in lithium metal batteries, characterized in that, The lithium metal battery includes a positive electrode, a negative electrode, and a PVDF-based high-entropy lithium salt solid electrolyte disposed between the positive and negative electrodes; the active material of the positive electrode is one of lithium transition metal oxide and lithium transition metal phosphate, and the negative electrode is a lithium metal foil or a lithium-plated copper foil.