Solid electrolytes and their preparation methods, solid batteries
By introducing amide additives into the solid electrolyte and mutually adsorbing them with the π-electron conjugated structure of the amide solvent, the residual amount of amide solvent is increased, the crystallinity is reduced, and combined with the ion transport effect of metal salt, a stable SEI film is formed, which solves the problem of low ionic conductivity caused by the high crystallinity of fluoropolymers and improves the performance of the battery.
Patent Information
- Application Number
- CN202611585235.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-10-14
- Publication Date
- 2026-11-17
AI Technical Summary
The high crystallinity of fluorinated polymers results in low ionic conductivity of solid electrolytes, which limits the rate performance of batteries.
The introduction of amide additives with NC=Oπ electron conjugation structure allows them to mutually adsorb with amide solvents, increasing the residual amount of amide solvents in the solid electrolyte, reducing the crystallinity of fluoropolymers, and synergistically forming a stable composite SEI film through the participation of metal ions provided by metal salts in ion transport.
It improves the ionic conductivity of the solid electrolyte and the cycle stability of the battery, reduces the interfacial impedance, and enhances the overall performance of the battery.
Smart Images

Figure SMS_6 
Figure QLYQS_1
Abstract
Description
Technical Field
[0001] This invention relates to the field of solid electrolyte technology, specifically to a solid electrolyte and its preparation method, and a solid battery. Background Technology
[0002] Solid-state batteries use solid electrolytes instead of traditional liquid electrolytes, showing broad application prospects in energy storage and power batteries. Among various solid electrolyte materials, fluorinated polymers are commonly used due to their excellent electrochemical performance. However, because fluorine atoms have small radii and high electronegativity, fluorinated polymers have high crystallinity, which severely inhibits the mobility of molecular chains, resulting in low ionic conductivity of the solid electrolyte and thus limiting the rate performance of the battery. Summary of the Invention
[0003] To address the shortcomings of existing technologies, this application provides a solid electrolyte, its preparation method, and a solid battery.
[0004] The solid electrolyte disclosed in this application includes: a fluoropolymer, a metal salt and an amide additive dispersed in the fluoropolymer, and an amide solvent remaining in the fluoropolymer. Both the amide additive and the amide solvent have an NC=Oπ electron conjugated structure. The amide additive adsorbs the amide solvent through the NC=Oπ electron conjugated structure to increase the residual amount of the amide solvent in the fluoropolymer.
[0005] Preferably, the amide additive is an amide metal salt.
[0006] Preferably, the amide additive is a diformylamino metal salt.
[0007] Preferably, the chemical formula of the amide solvent is: In the formula, R is an alkyl group.
[0008] Preferably, the fluoropolymer is selected from one or more of polyvinylidene fluoride, polyvinylidene fluoride-hexafluoropropylene copolymer, polyfluoroethylene carbonate, and polytetrafluoroethylene.
[0009] Preferably, the mass ratio of metal salt to amide additive is ≥5:1.
[0010] Preferably, the mass ratio of the metal salt to the fluoropolymer is (0.6~1.2):1.
[0011] This application also discloses a method for preparing a solid electrolyte, comprising the following steps: adding a metal salt, a fluoropolymer and an amide additive to an amide solvent, mixing them evenly to obtain a precursor solution; heating the precursor solution to remove free amide solvent to obtain a solid electrolyte.
[0012] Preferably, the mass ratio of amide solvent to metal salt is (12~20):1.
[0013] This application also discloses a solid-state battery, including the solid-state electrolyte described above.
[0014] The beneficial effects of this application are as follows: By introducing amide additives with an NC=Oπ electron conjugated structure, based on the principle of "like dissolves like," the amide additives and amide solvents with the same NC=Oπ electron conjugated structure mutually adsorb through the π electron conjugated structure, resulting in more amide solvent remaining in the solid electrolyte, effectively increasing the residual amount of amide solvent in the solid electrolyte. The residual amide solvent acts as a plasticizer, which can reduce the crystallinity of fluoropolymers, improve the mobility of polymer chains, and thus improve the ionic conductivity of the solid electrolyte. At the same time, the metal ions provided by the metal salt participate in ion transport as charge carriers, and the synergistic effect of the amide additives and amide solvents helps to form a stable composite SEI film at the negative electrode interface, reducing interfacial impedance and improving the cycle stability of the battery. Detailed Implementation
[0015] Several embodiments of this application will be disclosed below. For clarity, many practical details will be described in the following description. However, it should be understood that these practical details should not be used to limit this application. That is, in some embodiments of this application, these practical details are not essential.
[0016] Furthermore, the use of terms such as "first" and "second" in this application is for descriptive purposes only and does not specifically refer to any order or sequence, nor is it intended to limit this application. They are merely used to distinguish components or operations described using the same technical terms and should not be construed as indicating or implying relative importance or implicitly specifying the number of indicated technical features. Therefore, a feature defined with "first" or "second" may explicitly or implicitly include at least one of those features. Additionally, the technical solutions of various embodiments can be combined with each other, but only if they are feasible for those skilled in the art. If a combination of technical solutions is contradictory or impossible to implement, it should be considered that such a combination of technical solutions does not exist and is not within the scope of protection claimed in this application.
[0017] To further understand the content, features, and effects of this application, the following embodiments are provided and detailed below.
[0018] Example 1: The solid electrolyte in this embodiment includes a fluoropolymer, a metal salt and an amide additive dispersed in the fluoropolymer, and an amide solvent remaining in the fluoropolymer. Both the amide additive and the amide solvent have an NC=Oπ electron conjugated structure. The amide additive adsorbs the amide solvent through the NC=Oπ electron conjugated structure to increase the residual amount of the amide solvent in the fluoropolymer.
[0019] In the preparation of solid electrolytes, amide solvents are usually used to dissolve fluorinated polymers. Although the small amount of solvent molecules remaining after drying can play a plasticizing role, reduce the crystallinity of fluorinated polymers, and improve the ionic conductivity of solid electrolytes, most of the amide solvents are removed during the drying process, leaving a small amount of residual solvent. Therefore, the improvement effect on the ionic conductivity of solid electrolytes is limited and cannot meet the needs of practical applications.
[0020] This embodiment introduces amide additives with an NC=Oπ electron conjugated structure. Based on the principle of "like dissolves like," the amide additives and amide solvents, which also have an NC=Oπ electron conjugated structure, adsorb each other through the π electron conjugation structure, resulting in more amide solvent remaining in the solid electrolyte and effectively increasing the residual amount of amide solvent in the solid electrolyte. The residual amide solvent acts as a plasticizer, reducing the crystallinity of the fluoropolymer and improving the mobility of polymer chains, thereby increasing the ionic conductivity of the solid electrolyte. Simultaneously, the metal ions provided by the metal salt participate in ion transport as charge carriers, and the synergistic effect of the amide additives and amide solvents helps to form a stable composite SEI film at the negative electrode interface, reducing interfacial impedance and improving the cycle stability of the battery.
[0021] Preferably, the amide additive is an amide metal salt. In specific applications, the amide metal salt is added to the solid electrolyte. The metal ions in the amide metal salt can increase the number of metal ions in the solid electrolyte, which helps to improve the ionic conductivity of the solid electrolyte. At the same time, since the metal ions in the amide metal salt are positively charged, they interact with the amide oxygen groups in the amide solvent, which can further adsorb more amide solvent, thereby increasing the content of residual amide solvent in the fluoropolymer, thus reducing the crystallinity of the fluoropolymer, improving the mobility of polymer chain segments, and thus improving the ionic conductivity of the solid electrolyte. In addition, due to the high electronegativity of nitrogen and oxygen atoms, the carbon atoms in the amide solvent and amide metal salt are positively charged and easily reduced at the negative electrode interface. The amide solvent can generate an organic SEI component containing nitrogen and oxygen, while the fluoropolymer and amide metal salt generate an inorganic SEI component rich in sodium fluoride, nitrate, and carbonate. In this way, an organic / inorganic composite SEI film can be formed, which helps to improve interface stability and reduce interface impedance.
[0022] It is important to note that the anions of amide metal salts can adsorb amide solvents, forming a solvated structure in the solid electrolyte. This eliminates the need for fluorinated polymers to share the dissolving capacity of the amide metal salt anions, thus maintaining the ionic conductivity of the solid electrolyte. Compared to methods that significantly increase the metal salt content in the solid electrolyte to increase the amount of amide solvent adsorbed, this embodiment increases the amount of solvent residue without introducing a large number of bulky metal salt anions that require polymer chains to dissolve. This avoids a decrease in the ionic conductivity and mechanical properties of the solid electrolyte due to reduced polymer chain mobility.
[0023] Preferably, the amide additive is a diformamide metal salt. In this specific application, the diformamide metal salt is selected from sodium diformamide. The diformamide anion of sodium diformamide has two amide structures (NC=Oπ electron conjugated structure) similar to those of amide solvents. Based on the principle of like dissolves like, it can adsorb more amide solvent residues in the solid electrolyte.
[0024] Preferably, the chemical formula of the amide solvent is: In the formula, R represents an alkyl group. The amide solvent in this embodiment is selected from one or both of N,N-dimethylformamide (DMF) and N,N-dimethylacetamide (DMA). In practical applications, amide solvent molecules can act as plasticizers in solid electrolytes, reducing the crystallinity of fluoropolymers and enhancing the mobility of polymer chains, thereby improving the ionic conductivity of the solid electrolyte. Simultaneously, amide solvents can participate in the formation of nitrogen- and oxygen-containing organic SEI components at the negative electrode interface, jointly constructing a stable composite SEI film with the inorganic SEI components generated from fluoropolymers and amide metal salts.
[0025] Preferably, the metal salt is selected from one or more of sodium hexafluorophosphate, sodium perchlorate, sodium difluorooxalate borate, sodium bis(oxalate borate), sodium bis(fluorosulfonyl)imide, sodium bis(trifluoromethanesulfonyl)imide, and sodium trifluorosulfonate. In specific applications, the metal salt in this embodiment is a sodium salt. Sodium salts can dissociate into sodium ions in a solid electrolyte. These sodium ions act as charge carriers and can migrate directionally within the solid electrolyte, thereby achieving ion conduction. Simultaneously, sodium ions also participate in the formation of the SEI film at the negative electrode interface, jointly constructing a stable inorganic SEI component with the inorganic components generated by the fluoropolymer and amide-based metal salts. Of course, in other embodiments, the metal salt is not limited to sodium salts; other metal salts, such as lithium salts and potassium salts, can be selected according to actual needs.
[0026] Preferably, the mass ratio of metal salt to amide additive is ≥5:1. In specific applications, a mass ratio of metal salt to amide additive of ≥5:1 not only ensures that the amide additive effectively adsorbs amide solvents to increase the residual amount of amide solvents, but also avoids excessive amide solvent residue due to excessive amide additives. This prevents excessive amide solvents from occupying coordination sites of fluoropolymers and reducing the transport efficiency of metal ions, and also avoids the formation of loose organic components at the negative electrode interface, which would lead to increased interfacial impedance and decreased cycle stability of the battery.
[0027] Preferably, the fluoropolymer is selected from one or more of polyvinylidene fluoride (PVDF), polyvinylidene fluoride-hexafluoropropylene copolymer (PVDF-HFP), polyfluoroethylene carbonate (PFEC), and polytetrafluoroethylene (PTFE).
[0028] Preferably, the mass ratio of metal salt to fluoropolymer is (0.6~1.2):1. In specific applications, this ratio range ensures that the solid electrolyte has a sufficient number of metal ions to meet the ionic conductivity requirements, while avoiding excessive metal salt leading to saturation of the fluoropolymer's solubility and a decrease in the mechanical properties of the solid electrolyte.
[0029] Example 2: The preparation method of the solid electrolyte in this embodiment includes the following steps: S1: Add the metal salt, fluoropolymer, and amide additive to an amide solvent and mix thoroughly to obtain a precursor solution. In specific applications, add the metal salt, fluoropolymer, and amide additive to an amide solvent and mechanically stir at 400 rpm to 900 rpm for 1 to 8 hours at 20°C to 40°C to ensure complete dissolution and homogeneous mixing of all components, thus obtaining the precursor solution.
[0030] S2: The precursor solution is heated to remove free amide solvents, yielding a solid electrolyte. In practical applications, the precursor solution is poured onto a glass plate and dried in an oven at 50℃~80℃ for 1h~10h to remove free amide solvents, resulting in a solid electrolyte. This drying temperature and time range ensures that free amide solvents are largely removed during the drying process. Due to the mutual adsorption of π-electron conjugated structures, a small amount of amide solvent is retained in the solid electrolyte, resulting in an easily peelable film-like solid electrolyte.
[0031] Preferably, the mass ratio of the amide solvent to the metal salt is (12~20):1. In practical applications, this ratio range allows each component to fully dissolve and form a stable precursor solution, and retains an appropriate amount of amide solvent in the solid electrolyte after preparation, thereby effectively reducing the crystallinity of the fluoropolymer and improving the ionic conductivity of the solid electrolyte.
[0032] Preferably, the amide additive is an amide metal salt. Specifically, in this embodiment, the amide additive is preferably a diformylamino metal salt.
[0033] Preferably, the chemical formula of the amide solvent is: In the formula, R is an alkyl group.
[0034] Preferably, the metal salt is selected from one or more of sodium hexafluorophosphate, sodium perchlorate, sodium difluorooxalate borate, sodium bis(oxalate borate), sodium difluorosulfonyl imide, sodium bis(trifluoromethylsulfonyl)imide, and sodium trifluorosulfonate.
[0035] Preferably, the fluoropolymer is selected from one or more of polyvinylidene fluoride (PVDF), polyvinylidene fluoride-hexafluoropropylene copolymer (PVDF-HFP), polyfluoroethylene carbonate (PFEC), and polytetrafluoroethylene (PTFE).
[0036] Preferably, the mass ratio of metal salt to amide additive is ≥5:1. In practical applications, this ratio range ensures that the amide additive effectively adsorbs amide solvent during the drying process, increasing the residual amount of amide solvent, while avoiding excessive amide solvent residue due to excessive amide additive. This prevents excessive residual amide solvent from occupying coordination sites of fluoropolymers and reducing metal ion transport efficiency, and also prevents excessive residual amide solvent from causing the formation of loose organic components at the negative electrode interface during battery cycling.
[0037] Preferably, the mass ratio of metal salt to fluoropolymer is (0.6~1.2):1. In specific applications, this ratio range ensures that the solid electrolyte has a sufficient number of metal ions to meet the ionic conductivity requirements, while avoiding excessive metal salt that could lead to saturation of the fluoropolymer's solubility and a decrease in the mechanical properties of the solid electrolyte.
[0038] Example 3: The solid-state battery in this embodiment includes a positive electrode, a negative electrode, and a film-like solid electrolyte located between the positive and negative electrode. The solid electrolyte is the solid electrolyte of Embodiment 1.
[0039] Because it uses the solid electrolyte of Example 1, the solid-state battery assembled in this example has a high cycle capacity retention rate.
[0040] This embodiment does not have special requirements for the composition of the positive and negative electrode sheets; existing positive and negative electrode sheets can be used. In specific applications, the positive electrode sheet includes a positive active material (NaNi). 1 / 3 Fe 1 / 3 Mn 1 / 3The positive electrode active material consists of O2, conductive agents (CNTs), binders (polytetrafluoroethylene), and current collectors (aluminum foil). The mass ratio of the positive electrode active material, conductive agent, and binder is 8:1:1. The negative electrode is a sodium metal sheet.
[0041] The following are examples and comparative examples of preparing film-like solid electrolytes: Sample Example 1: The preparation method of the solid electrolyte in this sample example includes the following steps: S1: Add 9g of sodium bis(trifluoromethanesulfonyl)imide, 12g of polyvinylidene fluoride and 0.1g of sodium diformamide to 144g of N,N-dimethylformamide, and mechanically stir at 700rpm for 3h at 25℃ to obtain a precursor solution.
[0042] S2: The precursor solution was poured onto a glass plate and dried in an oven at 60°C for 5 hours to obtain a film-like solid electrolyte.
[0043] Sample Example 2: The preparation method of the solid electrolyte in this sample example includes the following steps: S1: Add 9g of sodium bis(trifluoromethanesulfonyl)imide, 12g of polyvinylidene fluoride and 0.3g of sodium diformamide to 144g of N,N-dimethylformamide, and mechanically stir at 700rpm for 3h at 25℃ to obtain a precursor solution.
[0044] S2: The precursor solution was poured onto a glass plate and dried in an oven at 60°C for 5 hours to obtain a film-like solid electrolyte.
[0045] Sample Example 3: The preparation method of the solid electrolyte in this sample example includes the following steps: S1: Add 9g of sodium bis(trifluoromethanesulfonyl)imide, 12g of polyvinylidene fluoride and 0.8g of sodium diformamide to 144g of N,N-dimethylformamide, and mechanically stir at 700rpm for 3h at 25℃ to obtain a precursor solution.
[0046] S2: The precursor solution was poured onto a glass plate and dried in an oven at 60°C for 5 hours to obtain a film-like solid electrolyte.
[0047] Sample Example 4: The preparation method of the solid electrolyte in this sample example includes the following steps: S1: Add 9g of sodium bis(trifluoromethanesulfonyl)imide, 12g of polyvinylidene fluoride and 1.0g of sodium diformamide to 144g of N,N-dimethylformamide, and mechanically stir at 700rpm for 3h at 25℃ to obtain a precursor solution.
[0048] S2: The precursor solution was poured onto a glass plate and dried in an oven at 60°C for 5 hours to obtain a film-like solid electrolyte.
[0049] Sample Example 5: The preparation method of the solid electrolyte in this sample example includes the following steps: S1: Add 9g of sodium bis(trifluoromethanesulfonyl)imide, 12g of polyvinylidene fluoride and 1.5g of sodium diformamide to 144g of N,N-dimethylformamide, and mechanically stir at 700rpm for 3h at 25℃ to obtain a precursor solution.
[0050] S2: The precursor solution was poured onto a glass plate and dried in an oven at 60°C for 5 hours to obtain a film-like solid electrolyte.
[0051] Sample Example 6: The preparation method of the solid electrolyte in this sample example includes the following steps: S1: 9g of sodium bis(trifluoromethanesulfonyl)imide, 12g of polyvinylidene fluoride-hexafluoropropylene copolymer and 0.8g of sodium diformamide were added to 144g of N,N-dimethylformamide and mechanically stirred at 700rpm for 3h at 25℃ to obtain a precursor solution.
[0052] S2: The precursor solution was poured onto a glass plate and dried in an oven at 60°C for 5 hours to obtain a film-like solid electrolyte.
[0053] Sample Example 7: The preparation method of the solid electrolyte in this sample example includes the following steps: S1: Add 9g of sodium bis(trifluoromethanesulfonyl)imide, 12g of polyvinylidene fluoride and 0.8g of sodium diformamide to 144g of N,N-dimethylacetamide, and mechanically stir at 700rpm for 3h at 25℃ to obtain a precursor solution.
[0054] S2: The precursor solution was poured onto a glass plate and dried in an oven at 60°C for 5 hours to obtain a film-like solid electrolyte.
[0055] Comparative Example 1: The preparation method of the solid electrolyte in this comparative example includes the following steps: S1: Add 9g of sodium bis(trifluoromethanesulfonyl)imide, 12g of polyvinylidene fluoride and 2.0g of sodium diformamide to 144g of N,N-dimethylformamide, and mechanically stir at 700rpm for 3h at 25℃ to obtain a precursor solution.
[0056] S2: The precursor solution was poured onto a glass plate and dried in an oven at 60°C for 5 hours to obtain a film-like solid electrolyte.
[0057] Comparative Example 2: The preparation method of the solid electrolyte in this comparative example includes the following steps: S1: Add 9g of sodium bis(trifluoromethanesulfonyl)imide and 12g of polyvinylidene fluoride to 144g of N,N-dimethylformamide, and mechanically stir at 700rpm for 3h at 25℃ to obtain a precursor solution.
[0058] S2: The precursor solution was poured onto a glass plate and dried in an oven at 60°C for 5 hours to obtain a film-like solid electrolyte.
[0059] The residual solvent content and sodium ion transport number (t) of the solid electrolyte membranes prepared by Samples 1 to 7, Comparative Examples 1 and 2 were tested. Na+ The tests include ionic conductivity (σ) testing and capacity retention testing after 300 cycles at 25°C. Specific test methods are as follows: Residual solvent content test: Weigh the total mass of the solid electrolyte membrane obtained after drying in step S2, and subtract the mass of the metal salt, fluoropolymer, and amide additives added in step S1 to calculate the residual solvent mass. The calculation formula is as follows: Residual solvent mass = Total mass of solid electrolyte membrane - Mass of metal salt - Mass of fluoropolymer - Mass of amide additives.
[0060] Sodium ion transport number (t) Na+ Testing: The Bruce-Vincent method was used for testing. The solid electrolyte membrane and sodium sheet obtained in step S2 were assembled into a sodium sheet|solid electrolyte membrane|sodium sheet symmetrical coin cell. The coin cell was placed on an electrochemical workstation for AC impedance testing, with a frequency range of 10 Hz. 5 Hz to 10 -1 The interfacial impedance R0 was determined by electrochemical impedance spectroscopy at Hz. A constant voltage of 10 mV was then applied for polarization, and the current-time curves were recorded over 3600 seconds to obtain the initial current I0 and the average steady-state current I0 over the last 600 seconds. ss After polarization, the interfacial impedance R was measured again. ss According to the formula The sodium ion transport number (t) of the solid electrolyte membrane was calculated. Na+ ), where ΔV is the applied constant voltage (10mV).
[0061] Ion conductivity (σ) test: The solid electrolyte membrane obtained in step S2 and the stainless steel sheet were assembled into a stainless steel sheet|solid electrolyte membrane|stainless steel sheet coin cell, wherein the stainless steel sheet has a radius of 0.8 cm and an area of 2.01 cm².2 The solid electrolyte membrane thickness is 20 μm. The coin cell was placed on an electrochemical workstation for AC impedance testing, with a frequency range of 10 Hz. 5 Hz to 10 -1 Hz, according to the formula The ionic conductivity of the solid electrolyte membrane was calculated, where L is the thickness of the solid electrolyte membrane (20 μm) and S is the area of the solid electrolyte membrane equal to that of the stainless steel sheet (2.01 cm²). 2 ), R b The solid electrolyte phase resistance is obtained by fitting the Nyquist plot.
[0062] Capacity retention test after 300 cycles at 25℃: The positive electrode active material (NaNi) 1 / 3 Fe 1 / 3 Mn 1 / 3 O2, conductive agents (CNTs), and binders (polytetrafluoroethylene) are mixed uniformly in an organic solvent at a mass ratio of 8:1:1 to obtain a positive electrode slurry. The positive electrode slurry is coated onto aluminum foil and dried to obtain a positive electrode sheet. Using a sodium metal sheet as the negative electrode sheet, the solid electrolyte membrane obtained in step S2 is assembled with the positive and negative electrode sheets to obtain a positive electrode sheet|solid electrolyte membrane|negative electrode sheet coin cell. The coin cell is placed at 25°C and charged at a constant current of 0.2C to 3.9V, then discharged at a constant current of 0.5C to 1.5V, and cycled for 300 cycles. The discharge capacity of the first and third cycles is recorded, and the capacity retention rate (%) after 300 cycles at 25°C is calculated as: discharge capacity of the third cycle ÷ discharge capacity of the first cycle × 100%.
[0063] The test results are shown in Table 1: Table 1
[0064] As shown in Table 1, a comparison between Samples 1-5 and Comparative Example 1 reveals that when the mass ratio of sodium salt to sodium diformamide is ≥5:1, the sodium ion transport number and ionic conductivity of the prepared solid electrolyte membrane are both higher than those of Comparative Example 1. This is because after adding sodium diformamide, the diformamide anion and the amide solvent have a similar NC=O π-electron conjugated structure, which allows them to adsorb each other through this similar π-electron conjugated structure, thus retaining more amide solvent in the fluoropolymer. Simultaneously, the sodium ions introduced by sodium diformamide act as charge carriers, enhancing the ionic conductivity of the solid electrolyte membrane. Their positive charge also gives them a strong interaction with the amide oxygen groups in the amide solvent, further adsorbing more amide solvent and leaving it in the fluoropolymer. This reduces the crystallinity of the fluoropolymer, increases the mobility of polymer chains, and improves the ionic conductivity of the solid electrolyte membrane. Furthermore, at the negative electrode interface, the nitrogen- and oxygen-rich, low-resistance organic SEI component generated by amide solvents combines with the sodium fluoride, nitrogen, and oxygen-rich, high-strength inorganic SEI component generated by fluoropolymers and sodium diformamide to form an organic / inorganic composite SEI film, thus improving interfacial stability. A comparison of Samples 6 and 7 with Comparative Example 1 shows that using other types of fluoropolymers or amide solvents also improves the performance of solid electrolyte membranes.
[0065] A comparison of Sample Example 3, Comparative Example 1, and Comparative Example 2 reveals that the addition of excessive amide additives leads to a certain degree of degradation in the ionic conductivity, sodium ion transport number, and cycle stability of the assembled coin cell of the solid electrolyte membrane. This is because the excessive addition of amide additives results in more amide solvent remaining in the solid electrolyte membrane. This excess residual solvent occupies the coordination sites of the fluoropolymer, reducing the sodium ion transport efficiency and thus decreasing the ionic conductivity and sodium ion transport number of the solid electrolyte membrane. Simultaneously, the excessive amide solvent decomposes at the negative electrode interface, generating a large amount of loose organic components. These components continuously break down and regenerate during battery cycle charging and discharging, leading to increased interfacial impedance and decreased battery cycle performance.
[0066] In summary, this embodiment introduces amide additives with an NC=Oπ electron conjugated structure. Based on the principle of "like dissolves like," the amide additives and amide solvents, which also have an NC=Oπ electron conjugated structure, mutually adsorb through the π electron conjugated structure, resulting in more amide solvent remaining in the solid electrolyte and effectively increasing the residual amount of amide solvent in the solid electrolyte. The residual amide solvent acts as a plasticizer, reducing the crystallinity of the fluoropolymer and improving the mobility of polymer chains, thereby increasing the ionic conductivity of the solid electrolyte. Simultaneously, the metal ions provided by the metal salt participate in ion transport as charge carriers, and the synergistic effect of the amide additives and amide solvents helps to form a stable composite SEI film at the negative electrode interface, reducing interfacial impedance and improving the cycle stability of the battery.
[0067] The above description is merely an embodiment of this application and is not intended to limit the scope of this application. Various modifications and variations can be made to this application by those skilled in the art. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of this application should be included within the scope of the claims of this application.
Claims
1. A solid state electrolyte, characterized by, include: The fluoropolymer, the metal salt and amide additive dispersed in the fluoropolymer, and the amide solvent remaining in the fluoropolymer, wherein the amide additive and the amide solvent both have an NC=Oπ electron conjugated structure, and the amide additive adsorbs the amide solvent through the NC=Oπ electron conjugated structure to increase the residual amount of the amide solvent in the fluoropolymer.
2. The solid electrolyte according to claim 1, characterized in that, The amide additives are amide metal salts.
3. The solid-state electrolyte of claim 2, wherein, The amide additive is a diformylamino metal salt.
4. The solid electrolyte according to claim 1, characterized in that, The chemical formula of the amide solvent is wherein R is an alkyl group.
5. The solid-state electrolyte of claim 1, wherein, The fluoropolymer is selected from one or more of polyvinylidene fluoride, polyvinylidene fluoride-hexafluoropropylene copolymer, polyfluoroethylene carbonate, and polytetrafluoroethylene.
6. The solid-state electrolyte of claim 1, wherein, The mass ratio of the metal salt to the amide additive is ≥5:
1.
7. The solid-state electrolyte of claim 1, wherein, The mass ratio of the metal salt to the fluoropolymer is (0.6~1.2):
1.
8. A method of producing a solid-state electrolyte as claimed in any one of claims 1 to 7, characterized in that, Includes the following steps: Metal salts, fluoropolymers, and amide additives are added to an amide solvent and mixed thoroughly to obtain a precursor solution. The precursor solution is heated to remove free amide solvents, yielding a solid electrolyte.
9. The method of claim 8, wherein the solid-state electrolyte is prepared by a method comprising: The mass ratio of the amide solvent to the metal salt is (12~20):
1.
10. A solid state battery, characterized by, Includes the solid electrolyte as described in any one of claims 1-7.