A method for preparing a battery
By employing pulsed pressure wetting and pulsed high and low current formation processes, the bottlenecks in wetting and formation in sodium-ion battery manufacturing have been solved, resulting in a significant reduction in battery manufacturing cycle and performance improvement. This technology is applicable to various batteries such as sodium-ion, lithium-ion, potassium-ion, and zinc-ion batteries.
Patent Information
- Application Number
- CN202611086551.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-07-21
- Publication Date
- 2026-11-17
AI Technical Summary
Sodium-ion batteries have low manufacturing efficiency and high cost, especially in the electrolyte wetting and battery formation processes, where there are significant bottlenecks. Existing methods cannot effectively shorten the manufacturing cycle and affect battery performance and safety.
The process combines pulsed pressure wetting with pulsed high and low current formation, using intermittent mechanical pressure to drive electrolyte penetration and promote uniform growth of the solid electrolyte interface (SEI), thus shortening the wetting and formation time.
It significantly shortens the manufacturing cycle of sodium-ion batteries, reduces manufacturing costs, and maintains or improves the electrochemical performance of the batteries, making it suitable for various ion battery systems.
Smart Images

Figure CN123120893A_ABST
Abstract
Description
Technical Field
[0001] This disclosure relates to the field of battery technology, and in particular to a method for preparing a battery. Background Technology
[0002] With the continued advancement of the "dual carbon" goals, renewable energy sources such as wind and solar power are entering a stage of large-scale development, urgently requiring large-scale electrochemical energy storage technologies that are low-cost, highly stable, and adaptable to a wide temperature range as a key component. Sodium-ion batteries, with their advantages of abundant and widely distributed sodium resources, low cost, excellent safety, and good compatibility with lithium-ion battery processes, have become a core technology solution for large-scale energy storage, power supply in high-altitude and cold regions, and low-speed electric vehicles, and are also an important strategic supplement to lithium-ion batteries.
[0003] However, the industrialization of sodium-ion batteries still faces bottlenecks such as low manufacturing efficiency and high cost. Among these, electrolyte wetting and battery formation are two key processes that restrict production capacity and cost. Regarding electrolyte wetting, sodium-ion battery electrodes (especially hard carbon anodes) have high porosity and tortuosity, and the sodium ion radius (0.95 Å) is much larger than that of lithium ions. This results in significantly slower electrolyte permeation kinetics in porous electrodes and separators compared to lithium-ion batteries. Traditional processes typically require 24–72 hours of room temperature settling to achieve complete wetting, which not only severely restricts production cycle time but also increases the cost of factory and equipment space.
[0004] Existing accelerated wetting methods have significant limitations: heating wetting, while reducing electrolyte viscosity, accelerates electrolyte decomposition and electrode side reactions, affecting battery cycle life; vacuum wetting can only accelerate the initial filling of electrolyte and cannot effectively penetrate into the closed pores inside the electrode, ultimately requiring a long period of settling; material modification, such as laser drilling and hydrophilic treatment, to improve electrode wettability increases process complexity and material costs, and may also damage the integrity of the electrode structure.
[0005] In battery formation, a stable solid electrolyte interface (SEI) is formed on the negative electrode surface during the initial charge. The quality of this interface directly determines the battery's performance, lifespan, and safety. Traditional processes typically employ low-current constant-current charging at C / 10 to C / 20, taking 10 to 20 hours and accounting for nearly one-third of the battery manufacturing cost. Existing high-current formation schemes have inherent drawbacks: constant-current high-current formation leads to severe concentration polarization and interface polarization, resulting in uneven SEI thickness, a predominance of organic phase in the composition, increased interface impedance, and even localized sodium deposition, thus deteriorating battery cycle performance and safety. While single-pulse formation can alleviate polarization, it lacks synergistic optimization with the wetting process, failing to fully realize the potential for improved manufacturing efficiency.
[0006] More importantly, existing technologies optimize either the wetting or formation process alone, without considering the inherent relationship between the two: insufficient electrolyte wetting leads to uneven SEI formation during formation, while an unreasonable formation process further exacerbates interface defects. Therefore, there is an urgent need for a technology that can simultaneously address the two major efficiency bottlenecks of sodium-ion batteries—wetting and formation—to achieve a significant reduction in manufacturing cycle time and a synergistic improvement in performance. Summary of the Invention
[0007] To address the aforementioned technical problems, this disclosure provides a method for preparing sodium ions. This method combines pulsed pressure wetting with pulsed high- and low-current formation. By applying intermittent mechanical pressure, the electrolyte is actively driven to penetrate rapidly into the internal pores of the porous electrode and separator, reducing the wetting time from 24-72 hours to less than 1 hour. The formation process, combining pulsed high and low currents, alleviates polarization while promoting simultaneous SEI growth, reducing the formation time from 10-20 hours to 0.5-2 hours. These two methods synergistically form an integrated manufacturing process of rapid penetration and uniform film formation. While maintaining battery electrochemical performance comparable to traditional processes, the overall manufacturing cycle is significantly shortened, resulting in a substantial reduction in manufacturing costs.
[0008] In a first aspect, this disclosure provides a method for preparing a battery, comprising the following steps: 1) Inject electrolyte into the assembled dry battery to obtain an electrolyte-filled battery; after vacuum pre-wetting and vacuum sealing, a vacuum-sealed battery is obtained. 2) The vacuum-sealed battery is subjected to pulsed pressure immersion, and after standing, an electrolyte-immersed battery is obtained; 3) The battery is formed by immersing it in the electrolyte, degassing it, and then resealing it to obtain the target battery; The method of formation includes any one of the following: 31) Charge at a constant current of 1C~2C for 1~3s, charge at a constant current of 0.1~0.2C for 2~6s, then let stand for 1~2s, repeat this cycle until the upper limit voltage is reached; 32) Charge at a constant current of 1C~2C for 1~3s, charge at a constant current of 0.1~0.2C for 2~6s, then discharge at a constant current of 0.4~0.6C for 1~2s, repeating this cycle until the upper limit voltage is reached.
[0009] It should be understood that pulse pressurization is a sub-type of intermittent mechanical pressurization, referring to a periodic dynamic pressurization process that achieves rapid pressure increase, extremely short pressure holding, and rapid pressure release through electrically controlled pressure actuators (solenoid valves, high-pressure pumps, pneumatic valves). The single-cycle pressure waveform is in the form of spike pulses, without a long-term pressure stabilization platform, and continuously cycles with high-frequency, instantaneous alternating high and low pressure differences, thereby periodically disrupting the pressure balance inside and outside the system.
[0010] In this disclosure, the electrolyte is actively driven to penetrate by applying intermittent mechanical pressure, allowing it to quickly penetrate into the internal pores of the porous electrode and separator, reducing the immersion time from 24-72 hours to less than 1 hour. The pulsed high and low current formation process includes the first formation using pulse charging after immersion, which alleviates concentration polarization through periodic charging-resting / discharging and promotes the synchronous and uniform growth of the solid electrolyte interface (SEI). Moreover, the pulsed pressure immersion and pulsed high and low current formation process work together to achieve a total battery immersion and formation time of ≤4 hours, and the battery's initial coulombic efficiency, cycle stability, and rate performance are comparable to those of conventional processes.
[0011] The following are preferred technical solutions of this disclosure, but are not intended to limit the technical solutions provided by this disclosure. The technical objectives and beneficial effects of this disclosure can be better achieved through the following technical solutions.
[0012] As a preferred technical solution of this disclosure, the vacuum pre-wetting is to place the liquid-filled battery under a pressure of -80~-90kPa for 3~10 minutes to obtain a vacuum pre-wetting battery.
[0013] As an example, the pressure during vacuum pre-impregnation can be selected as a range of values consisting of -80 kPa, -82 kPa, -83 kPa, -85 kPa, -86 kPa, -90 kPa, or any point value, preferably -83 kPa to -86 kPa; more preferably -85 kPa.
[0014] As an example, the vacuum pre-impregnation time can be specifically selected as a range of values consisting of 3 min, 5 min, 6 min, 7 min, 8 min, 10 min, or any point value, preferably 5 min to 8 min; more preferably 6 min.
[0015] In this disclosure, vacuum pre-impregnation under the above conditions can complete the initial filling of electrolyte into the macroscopic pores of the battery cell in a short time, taking into account both pre-impregnation efficiency and vacuum equipment energy consumption, and avoiding insufficient pore filling due to insufficient vacuum time or excessive vacuum time increasing process time.
[0016] As a preferred technical solution of this disclosure, the vacuum sealing is to seal the vacuum pre-wetted battery under a pressure of -80~-90kPa.
[0017] In this disclosure, the vacuum sealing uses a negative pressure environment of -80~-90 kPa, which can maintain the pore-filling state of the electrolyte during the pre-wetting stage, prevent air from re-entering the cell pores during the sealing process and offsetting the previous vacuum wetting effect, thus ensuring the basis for subsequent pulse pressurization.
[0018] As a preferred technical solution of this disclosure, the pulsed pressure impregnation is to apply a mechanical pressure of 5~20kPa to the vacuum-sealed battery.
[0019] As an example, the mechanical pressure during pulsed pressurization can be selected as a range of values consisting of 5 kPa, 8 kPa, 10 kPa, 13 kPa, 15 kPa, 18 kPa, 20 kPa, or any point value, with 10 kPa being the preferred pressure.
[0020] In this disclosure, the mechanical pressure applied during pulsed pressure wetting ranges from 5 to 20 kPa. If the pressure is too low, it cannot effectively enhance electrolyte penetration; if the pressure is too high, it may cause battery deformation or damage to internal components. Preferably, the pressure is 10 kPa, which ensures mechanical safety while achieving effective wetting. It can both rely on periodic squeezing to push the electrolyte into the electrode-sealed micropores to increase the wetting rate and avoid damaging internal components such as electrode sheets and separators due to excessive pressure, thus balancing the wetting effect and the integrity of the battery structure.
[0021] As a preferred technical solution of this disclosure, the immersion time is 30~60min.
[0022] As an example, the wetting time can be selected as a range of values, such as 30 min, 40 min, 45 min, 50 min, 60 min, or any combination of these values, with 50 min being preferred. If the pulse time is too short, effective wetting cannot be achieved; if the pulse time is too long, the battery will already be fully wetted, and increasing the time will result in wasted costs. The aforementioned wetting time allows the electrolyte to fully penetrate into the deep pores of the electrode to achieve complete wetting, avoiding uneven wetting of pores and defects in the later formation of the SEI film caused by insufficient wetting time. At the same time, it avoids occupying the production line and increasing manufacturing costs due to excessively long pressurization time.
[0023] As a preferred technical solution of this disclosure, the immersion temperature is 20℃~45℃. This immersion temperature eliminates the need for additional heating equipment, thus preventing electrolyte decomposition and exacerbating electrode side reactions that could damage battery cycle life due to high temperatures. It also ensures stable electrolyte viscosity and maintains good permeability, reducing equipment investment and energy consumption.
[0024] As an example, the immersion temperature can be specifically selected as a range of values consisting of 20℃, 25℃, 28℃, 30℃, 35℃, 40℃, 45℃ or any other point value; preferably 20℃~25℃.
[0025] As a preferred technical solution of this disclosure, during the pulse pressure impregnation process of the vacuum-sealed battery, the thickness change of the battery is controlled within 0.5%~1.5%; the pulse mode is a high-frequency pulse, with pressure applied for 0.2s~1s and rested for 0.2s~1s.
[0026] As an example, the battery thickness change rate can be selected as a range of values consisting of 0.5%, 0.8%, 1.1%, 1.3%, 1.5%, or any point value, preferably 0.5% to 0.8%.
[0027] As an example, the pulse pattern can be 0.2s pressurization followed by 0.2s rest; 0.5s pressurization followed by 0.5s rest; 0.8s pressurization followed by 0.8s rest; or 1s pressurization followed by 1s rest.
[0028] In this disclosure, excessively high high-frequency pulse rates not only place higher demands on the equipment and increase costs, but also fail to significantly improve the wetting effect and efficiency. Conversely, excessively low high-frequency pulse rates have limited effect on improving electrolyte wetting efficiency. Therefore, selecting a pulse mode of 0.2s~1s pressurization / 0.2s~1s resting can significantly improve the wetting effect and efficiency.
[0029] As a preferred technical solution of this disclosure, the standing time is 5-10 minutes at room temperature.
[0030] As an example, the room temperature is 20℃~25℃, specifically 20℃, 22℃, 24℃, and 25℃.
[0031] As an example, the settling time can be selected as 5 min, 7 min, 8 min, or 10 min.
[0032] As a preferred technical solution of this disclosure, the degassing and secondary sealing are carried out under a vacuum of -80~-90 kPa.
[0033] As an example, the degassing and secondary sealing pressure can be selected as a range of values consisting of -80 kPa, -82 kPa, -83 kPa, -85 kPa, -86 kPa, -90 kPa, or any point value, preferably -83 kPa to -86 kPa; more preferably -85 kPa.
[0034] The above-mentioned pressure is selected for degassing and sealing in this disclosure, which can efficiently remove trace amounts of gas generated during the formation stage, avoid gas retention inside the cell, increase interface impedance, reduce battery capacity and cycle stability, and simultaneously complete the final sealing of the battery and ensure storage stability.
[0035] As a preferred technical solution of this disclosure, the assembly process of the dry battery is as follows: (11) Prepare a positive electrode active slurry by mixing and stirring the positive electrode active material, conductive agent and binder; in the positive electrode active slurry, the mass ratio of each component is active material: conductive agent: binder = 90%~97%: 1.5%~5%: 1.5%~5%; (12) The positive electrode slurry is uniformly coated on the positive electrode current collector, and the surface density of the positive electrode slurry coating on both sides is 70 g / m².2 ~500g / m 2 ; Obtain the positive electrode sheet; (13) The positive electrode sheet is rolled to achieve a compaction density of 1.3 g / cm³. 3 ~3.3g / cm 3 ; (14) Mix and stir the negative electrode active material, conductive agent and binder to prepare negative electrode active slurry; the mass ratio of each substance in the negative electrode active slurry is active material: conductive agent: binder = 87%~96%: 1%~5%: 3%~8%; (15) The negative electrode slurry is uniformly coated on the negative electrode current collector, and the surface density of the negative electrode slurry coating on both sides is 30 g / m². 2 ~190g / m 2 To obtain the negative electrode sheet; (16) The negative electrode sheet is rolled to achieve a compaction density of 0.8 g / cm³. 3 ~1.6g / cm 3 ; (17) Separate the positive electrode and the negative electrode with a separator, arrange them in a regular pattern and stack or wind them multiple times; connect the positive electrode tab to the positive current collector and the negative electrode tab to the negative current collector; assemble the positive electrode, the negative electrode, and the separator to obtain a dry battery.
[0036] Secondly, this disclosure provides a battery, which is prepared by the method described above; The batteries include sodium-ion batteries, lithium-ion batteries, potassium-ion batteries, zinc-ion batteries, and magnesium-ion batteries.
[0037] As a preferred technical solution of this disclosure, the battery assembly method includes, but is not limited to, stacking and winding.
[0038] This disclosure relies on a pre-pulse pressurization rapid wetting and pulse-coordinated formation process, which ensures uniform and sufficient electrolyte wetting inside the cell and the formation of a uniform low-resistance SEI film on the negative electrode. The battery has excellent first coulombic efficiency, high-rate charge and discharge performance, and long-cycle capacity retention. This preparation process can be adapted to various assembly methods such as stacking and winding of cells. There is no mechanical extrusion damage inside the cell, resulting in high product consistency. It is suitable for various application scenarios such as energy storage, low-speed vehicles, and small electrical equipment.
[0039] Thirdly, this disclosure provides an electrical device, which includes the aforementioned battery. The electrical device equipped with an ion battery prepared using the aforementioned optimized process has fewer battery wetting and formation defects, lower interface impedance, stable discharge output, strong fast charging capability, and slow battery capacity decay over long-term use, significantly extending the overall lifespan of the device. Simultaneously, the total time spent on battery preparation is significantly reduced, lowering battery procurement costs and effectively reducing the overall production and maintenance costs of the electrical device, making it suitable for large-scale mass production.
[0040] The technical solution provided in this disclosure has the following advantages compared with the prior art: 1. This disclosure employs a pulsed pressure wetting method, which actively drives the electrolyte penetration into the porous structure through periodic squeezing and releasing of the battery cell. This reduces the wetting time of sodium-ion batteries from the traditional 24-72 hours to less than 1 hour, significantly improving wetting efficiency. This process requires no modification to the battery materials or structure; it can be achieved simply by applying mechanical pressure after assembly. It is fully compatible with existing production lines, exhibits excellent process compatibility, has low equipment modification costs, and can be applied on a large scale. Furthermore, the mild pressure conditions do not damage the electrodes, separator, or encapsulation structure, avoiding battery performance degradation caused by mechanical damage.
[0041] 2. This disclosure employs a pulsed high-low current formation process, which effectively alleviates concentration polarization and interface polarization under high current through periodic charge-rest / discharge cycles, promoting the synchronous nucleation and growth of SEI across the entire electrode surface. Compared with traditional low-current formation, the formation time is significantly shortened from 10-20 hours to 1-2 hours, and the formed SEI is thinner, more uniform, rich in inorganic components such as NaF, and has lower interface impedance. This effectively suppresses electrolyte side reactions and sodium dendrite growth, resulting in battery cycle stability and rate performance comparable to or even better than traditional processes.
[0042] 3. This disclosure achieves, for the first time, the synergistic optimization of the two bottleneck processes of impregnation and formation, with significant results. The total time consumed by both processes is reduced from the traditional 34-92 hours to ≤4 hours, increasing production efficiency by more than 8 times. The shortened manufacturing cycle directly reduces the costs associated with factory space, equipment, and labor, while also minimizing electrolyte decomposition losses during prolonged high-temperature static conditions. Overall manufacturing costs are significantly reduced; the method disclosed in this disclosure can lower the manufacturing cost of sodium-ion batteries by 15%-30%, significantly enhancing the product's market competitiveness.
[0043] 4. This disclosure significantly improves manufacturing efficiency without compromising the electrochemical performance of the battery: the initial coulombic efficiency, cycle stability, and rate performance are comparable to those of traditional processes; the method has a wide range of applications, applicable not only to all mainstream battery systems and battery forms (whether pouch or prismatic, stacked or wound, with or without a negative electrode, etc.), but also to lithium-ion batteries, potassium-ion batteries, zinc-ion batteries, magnesium-ion batteries, etc., all of which can be manufactured rapidly. Attached Figure Description
[0044] The accompanying drawings, which are incorporated in and form a part of this specification, illustrate embodiments consistent with this disclosure and, together with the description, serve to explain the principles of this disclosure.
[0045] To more clearly illustrate the technical solutions in the embodiments of this disclosure or the prior art, the accompanying drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, for those skilled in the art, other drawings can be obtained based on these drawings without creative effort.
[0046] Appendix Figure 1 This is a schematic diagram of the pulse immersion pressure variation in this disclosure.
[0047] Appendix Figure 2 Ultrasonic transmission images of the battery under different immersion conditions disclosed herein.
[0048] Appendix Figure 3 This is a schematic diagram of the pulsed formation process current variation part of this disclosure.
[0049] Appendix Figure 4 This is a comparison chart of the rate charging performance of sodium-ion batteries disclosed in this publication and those of comparative examples.
[0050] Appendix Figure 5 This is a comparison chart of the rate discharge performance of sodium-ion batteries disclosed in this publication and those of comparative examples.
[0051] Appendix Figure 6 This is a comparison chart of the 2C cycle performance of sodium-ion batteries disclosed in this publication and those of comparative examples. Detailed Implementation
[0052] To better understand the above-mentioned objectives, features, and advantages of this disclosure, the solutions disclosed herein will be further described below. It should be noted that, unless otherwise specified, the embodiments and features described herein can be combined with each other.
[0053] Numerous specific details are set forth in the following description in order to provide a full understanding of this disclosure, but this disclosure may also be implemented in other ways different from those described herein; obviously, the embodiments in the specification are only some, and not all, of the embodiments of this disclosure.
[0054] This disclosure provides a method for preparing a battery, comprising the following steps: 1) Prepare a positive electrode active slurry by mixing and stirring the positive electrode material, conductive agent SP, and binder PVDF; the raw material ratio of the positive electrode active slurry is active material: conductive agent: binder = 90%~97%: 1.5%~5%: 1.5%~5%; 2) The positive electrode slurry is uniformly coated onto the positive electrode current collector, with a double-sided surface density of 70 g / m². 2 ~500g / m 2 The positive electrode sheet is rolled to achieve a compaction density of 1.3 g / cm³. 3 ~3.3g / cm 3 ; 3) Prepare a negative electrode active slurry by mixing and stirring the negative electrode material, conductive agent, and binder PVDF. The raw material ratio of the negative electrode active slurry is active material: conductive agent: binder = 87%~96%: 1%~5%: 3%~8%; 4) The negative electrode slurry is uniformly coated on the negative electrode current collector, and the surface density of the negative electrode slurry coating on both sides is 30 g / m². 2 ~190g / m 2 The negative electrode sheet is rolled to achieve a compaction density of 0.8 g / cm³. 3 ~1.6g / cm 3 ; 5) Separate the positive and negative electrode plates with a diaphragm, arrange them in a regular pattern, and stack or wind them multiple times. 6) Connect the positive tab to the positive current collector and the negative tab to the negative current collector; 7) Place the semi-finished battery in a 55℃ vacuum oven and bake for 24 hours; 8) The battery is sealed to obtain a dry-state battery; 9) Inject electrolyte into the assembled dry cell; let it stand for 3 to 10 minutes under a pressure of -80 to -90 kPa, and then seal it; 10) Place the sealed battery in the flat plate pressurization device. The pressurization temperature environment is room temperature, the mechanical pressure is set to 5~20kPa, the pressurization frequency is 0.2s~1s pressurization / 0.2s~1s rest, the pulse time is 30~60min, and intermittent mechanical pressure is applied. After pressurization, let it stand at room temperature for 5~10min.
[0055] 11) After immersion, charge the battery at a constant current of 1C~2C for 1~3s, charge at a constant current of 0.1~0.2C for 2~6s, then let it rest for 1~2s, repeat this cycle until the upper limit voltage is reached, and then charge at a constant voltage until the current drops to C / 20; or, charge the battery at a constant current of 1C~2C for 1~3s, charge at a constant current of 0.1~0.2C for 2~6s, then discharge at a constant current of 0.4~0.6C for 1~2s, repeat this cycle until the upper limit voltage is reached, and then charge at a constant voltage until the current drops to C / 20; 12) Discharge the gas generated during the formation process under a vacuum of -80~-90 kPa and perform secondary sealing.
[0056] The following explanation is provided through specific examples.
[0057] Unless otherwise specified, the raw materials, reagents or chemical substances used in the embodiments and comparative examples disclosed herein are all conventional products obtained through commercial channels and can be selected and obtained by those skilled in the art based on known technical knowledge.
[0058] Example 1 A method for preparing a sodium-ion battery includes the following steps: S1. Preparation of dry-state batteries (11) Prepare a positive electrode active slurry by mixing and stirring the positive electrode active material NFPP, conductive agent SP and binder PVDF; in the positive electrode active slurry, the mass percentage of each component is 94% active material, 3% conductive agent SP and 3% binder PVDF; (12) The positive electrode slurry is uniformly coated on the aluminum foil, and the surface density of the positive electrode slurry coating on both sides is 300 g / m². 2 ; Obtain the positive electrode sheet; (13) Roll the positive electrode sheet to achieve a compaction density of 2 g / cm³. 3 ; (14) The negative electrode active material hard carbon, conductive agent SP and binder PVDF are mixed and stirred to prepare a negative electrode active slurry; the mass ratio of each substance in the negative electrode active slurry is 93% active material, 2% conductive agent and 5% binder; (15) The negative electrode paste is uniformly coated on the aluminum foil, and the surface density of the negative electrode paste coating on both sides is 103 g / m². 2 To obtain the negative electrode sheet; (16) The negative electrode sheet is rolled to achieve a compaction density of 0.97 g / cm³. 3 ; (17) Separate the positive electrode and the negative electrode with a separator, arrange them in a regular pattern and stack them multiple times; connect the positive electrode tab to the positive current collector and the negative electrode tab to the negative current collector; assemble the positive electrode, the negative electrode and the separator, and place the semi-finished battery in a vacuum oven at 55°C for 24 hours to obtain a dry sodium-ion battery.
[0059] S2. Inject electrolyte into the assembled dry sodium-ion battery. The electrolyte is 1M NaPF6-G2 to obtain the liquid-filled battery. After pre-wetting under -85kPa vacuum for 5min and sealing, a vacuum-sealed battery is obtained.
[0060] S3. The vacuum-sealed battery was pulse-pressurized and immersed for 50 min at a mechanical pressure of 10 kPa and 25°C, and then allowed to stand for 7 min to obtain an electrolyte-immersed battery. During the pulse pressurization process, the battery thickness change was controlled within 0.8%. The pulse mode was high-frequency pulse, with 0.5 s pressurization and 0.5 s rest.
[0061] S4. The electrolyte is used to wet the battery for formation, degassing at -85kPa and sealing it a second time to obtain the target sodium-ion battery; wherein the formation method is as follows: 1.5C constant current charging for 2s, 0.2C constant current charging for 4s, followed by resting for 1s, and repeating the cycle until the upper limit voltage is reached. After reaching the upper limit voltage, constant voltage charging is performed until the current drops to C / 20.
[0062] Example 2 A method for preparing a lithium-ion battery includes the following steps: S1. Preparation of dry-state batteries (11) Prepare a positive electrode active slurry by mixing and stirring the positive electrode active material LFP, conductive agent SP and binder PVDF; in the positive electrode active slurry, the mass percentage of each component is 96% active material, 1.5% conductive agent SP and 2.5% binder PVDF; (12) The positive electrode slurry is uniformly coated on the aluminum foil, and the surface density of the positive electrode slurry coating on both sides is 70 g / m². 2 ; Obtain the positive electrode sheet; (13) The positive electrode sheet is rolled to achieve a compaction density of 2.4 g / cm³. 3 ; (14) Prepare a negative electrode active slurry by mixing and stirring the negative electrode active material artificial graphite, conductive agent SP and binder PVDF; the mass ratio of each substance in the negative electrode active slurry is 96.5% active material, 1% conductive agent and 2.5% binder; (15) The negative electrode paste is uniformly coated on the copper foil, and the double-sided surface density of the negative electrode paste is 36 g / m². 2 To obtain the negative electrode sheet; (16) Roll the negative electrode sheet to achieve a compaction density of 1.5 g / cm³. 3 ; (17) Separate the positive electrode and the negative electrode with a separator, arrange them in a regular pattern and stack them multiple times; connect the positive electrode tab to the positive current collector and the negative electrode tab to the negative current collector; assemble the positive electrode, the negative electrode and the separator, and place the semi-finished battery in a vacuum oven at 55°C for 24 hours to obtain a dry lithium-ion battery.
[0063] S2. Inject electrolyte into the assembled dry lithium-ion battery. The electrolyte is 1M LiPF6-EC / DEC=1 / 1 (volume ratio) and contains 10 wt% fluoroethylene carbonate (FEC) to obtain the liquid-filled battery. After pre-wetting under -80kPa vacuum for 10min and sealing, a vacuum-sealed battery is obtained.
[0064] S3. The vacuum-sealed battery is pulse-pressurized and immersed for 60 min at a mechanical pressure of 5 kPa and 20°C, and then left to stand for 5 min to obtain an electrolyte-immersed battery. During the pulse pressurization process, the battery thickness change is controlled within 0.5%. The pulse mode is high-frequency pulse, with 0.2 s pressurization and 0.2 s rest.
[0065] S4. The electrolyte is used to wet the battery for formation, degassing at -80kPa and sealing it a second time to obtain the target lithium-ion battery; wherein, the formation method is: 1C constant current charging for 1s, 0.1C constant current charging for 2s, followed by resting for 2s, and repeating the cycle until the upper limit voltage is reached. After reaching the upper limit voltage, constant voltage charging is performed until the current drops to C / 20.
[0066] Example 3 A method for preparing a potassium-ion battery includes the following steps: S1. Preparation of dry-state batteries (11) Prepare a positive electrode active slurry by mixing and stirring the positive electrode active material PBA, conductive agent SP and binder PVDF; in the positive electrode active slurry, the mass percentage of each component is 90% active material, 4% conductive agent SP and 6% binder PVDF; (12) The positive electrode slurry is uniformly coated on the aluminum foil, and the surface density of the positive electrode slurry coating on both sides is 500 g / m². 2 ; Obtain the positive electrode sheet; (13) The positive electrode sheet is rolled to achieve a compaction density of 1.9 g / cm³. 3 ; (14) A negative electrode active material hard carbon, conductive agent SP and binder PVDF are mixed and stirred to prepare a negative electrode active slurry; the mass ratio of each substance in the negative electrode active slurry is 92% active material, 3% conductive agent SP and 5% binder PVDF; (15) The negative electrode paste is uniformly coated on the copper foil, and the double-sided surface density of the negative electrode paste is 300 g / m². 2 To obtain the negative electrode sheet; (16) The negative electrode sheet is rolled to achieve a compaction density of 1.05 g / cm³. 3 ; (17) Separate the positive electrode and the negative electrode with a separator, arrange them in a regular pattern and stack them multiple times; connect the positive electrode tab to the positive current collector and the negative electrode tab to the negative current collector; assemble the positive electrode, the negative electrode and the separator, and place the semi-finished battery in a vacuum oven at 55°C for 24 hours to obtain a dry magnesium ion battery.
[0067] S2. Inject electrolyte into the assembled dry magnesium-ion battery. The electrolyte is 2.5M KFSI-TEP to obtain the liquid-filled battery. After pre-wetting under -90kPa vacuum for 3 minutes and sealing, a vacuum-sealed battery is obtained.
[0068] S3. The vacuum-sealed battery is pulse-pressurized and immersed for 30 minutes at a mechanical pressure of 20 kPa and 45°C, and then left to stand for 10 minutes to obtain an electrolyte-immersed battery. During the pulse pressurization process, the battery thickness change is controlled within 1.5%. The pulse mode is high-frequency pulse, with 1 second of pressurization and 1 second of rest.
[0069] S4. The electrolyte is used to wet the battery for formation, degassing at -90kPa and sealing it a second time to obtain the target magnesium-ion battery; wherein, the formation method is: 1.5C constant current charging for 2s, 0.2C constant current charging for 4s, followed by resting for 1s, and repeating the cycle until the upper limit voltage is reached. After reaching the upper limit voltage, constant voltage charging is performed until the current drops to C / 20.
[0070] Example 4 This embodiment provides a method for preparing a sodium-ion battery. Compared with Embodiment 1, the only difference is that: in the positive electrode active slurry, the mass ratio of each component is active material: conductive agent SP: binder PVDF = 95%: 2.5%: 2.5%; and the double-sided surface density of the positive electrode slurry coating is 200 g / m². 2 The compaction density of the positive electrode is 2.1 g / cm³. 3 The active material composition of the negative electrode active slurry is: conductive agent SP: binder PVDF = 92%: 4%: 4%; the double-sided surface density of the negative electrode slurry coating is 70 g / m². 2 The compaction density of the negative electrode is 0.99 g / cm³. 3 .
[0071] Example 5 This embodiment provides a method for preparing a sodium-ion battery. Compared with Embodiment 1, the only differences are: the vacuum pre-wetting pressure is -82 kPa and the time is 5 min; the mechanical pressure of pulse pressurization is 8 kPa and the wetting time is 40 min; the wetting temperature is 28℃; the thickness change rate is 1.1%; the pulse mode is 0.6 s pressurization / 0.6 s resting; the resting time is 8 min; and the degassing and secondary sealing pressure is -82 kPa.
[0072] Example 6 This embodiment provides a method for preparing a sodium-ion battery. Compared with Embodiment 1, the only differences are: the vacuum pre-wetting pressure is -83 kPa and the time is 7 min; the mechanical pressure of pulse pressurization is 13 kPa and the wetting time is 45 min; the wetting temperature is 30℃; the thickness change rate is 1.3%; the pulse mode is 0.8 s pressurization / 0.8 s resting; and the degassing and secondary sealing pressure is -83 kPa.
[0073] Example 7 This embodiment provides a method for preparing a sodium-ion battery. Compared with Embodiment 1, the only differences are: the vacuum pre-wetting pressure is -90 kPa and the time is 8 min; the mechanical pressure of pulse pressurization is 15 kPa; the wetting temperature is 35 °C; and the degassing and secondary sealing pressure is -90 kPa.
[0074] Example 8 This embodiment provides a method for preparing a sodium-ion battery. The only difference from Embodiment 1 is that the mechanical pressure of the pulse pressurization is 18 kPa and the immersion temperature is 40°C.
[0075] In Examples 1 to 8, the schematic diagrams of the pulse immersion pressure changes are shown below. Figure 1 A schematic diagram of the pulsed formation process current variation is shown below. Figure 3 The ultrasonic transmission images of the battery under different wetting conditions in the embodiments are shown in the figure. Figure 2 .
[0076] Comparative Example 1 This comparative example provides a method for preparing a sodium-ion battery. Compared with Example 1, Comparative Example 1 only involves pulsed pressure wetting. During formation, it is charged at constant current to 3.6 V at C / 10 and then at constant voltage to C / 20 (approximately 12 hours).
[0077] Comparative Example 2 This comparative example provides a method for preparing a sodium-ion battery. Compared with Example 1, Comparative Example 2 only involves pulse formation. The vacuum-sealed battery is left to stand at 25°C for 40 hours and then pulsed (approximately 1.6 hours) using the method of Example 1.
[0078] Comparative Example 3 This comparative example provides a method for preparing a sodium-ion battery. Compared with Example 1, Comparative Example 3 allows the vacuum-sealed battery to stand at room temperature for 40 hours, then charges it to 3.6 V at a constant current of C / 10 and then at a constant voltage of C / 20 (approximately 12 hours).
[0079] The evolution time of the preparation methods of Example 1 and Comparative Examples 1 to 3 was compared, and the results are shown in Table 1.
[0080] Table 1
[0081] As shown in Table 1, the total preparation time of Comparative Example 1, which only uses pulsed pressure wetting and traditional long-term constant current formation, reached 13 hours. The total preparation time of Comparative Example 2, which only uses pulsed high and low current formation and traditional long-term static wetting, reached as high as 42 hours. Comparative Example 3, which uses traditional processes for both wetting and formation, had the longest total manufacturing cycle, reaching 52 hours. In contrast, Example 1, which uses the synergistic process of pulsed pressure wetting and pulsed high and low current formation of the present invention, only took 2.5 hours. Compared with the three comparative examples, the manufacturing cycle was significantly reduced. This fully demonstrates that the present invention combines the two processes of pulsed pressure rapid wetting and pulsed high and low current formation, which can simultaneously solve the two major manufacturing bottlenecks of electrolyte wetting and negative electrode SEI formation. It completely breaks through the industry pain point of excessively long step-by-step wetting and formation processes in traditional processes. The total time of the two core processes can be reduced to less than 4 hours, and the production efficiency is increased by more than 8 times compared with traditional processes. It can significantly shorten the overall battery manufacturing cycle and reduce the comprehensive production costs caused by long-term occupation of factory buildings, equipment, and labor.
[0082] The sodium-ion batteries prepared in Example 1 and Comparative Examples 1 to 3 were subjected to performance tests. The test indicators included initial coulombic efficiency (%), initial discharge capacity (Ah), capacity retention rate after 920 cycles at 2C at 25°C (%), capacity retention rate after 15C charging at 25°C (%), capacity retention rate after 20C discharging at 25°C (%), and SEI interface impedance (mΩ).
[0083] The testing process is as follows: The initial coulombic efficiency and first discharge capacity of sodium-ion batteries were determined under the following conditions: the battery was charged to 3.65V at a constant current of 1C (1.3A) in an environment of 25℃, the cutoff current was 0.1C, and the battery was discharged to 2.0V at a constant current of 1C. The voltage range was 2.0-3.65V. The initial coulombic efficiency = initial discharge capacity / initial charge capacity × 100%.
[0084] The capacity retention of a sodium-ion battery was determined after 920 cycles at 2C and 25℃. The test conditions were: constant current charge-discharge cycling at 2C in a 25℃ environment, with a voltage range of 2.0-3.65V. The discharge capacity of the first cycle was recorded as C0, and the discharge capacity after 920 cycles was recorded as C... x Capacity retention rate = C x / C0×100%.
[0085] The capacity retention rate of a sodium-ion battery at 25℃ and a 15C charging rate was determined. The test conditions were as follows: in a 25℃ environment, the battery was discharged at a constant current of 1C (1.3A) to 2.0V, and then charged at a constant current of 1C to 3.65V. The charging capacity was recorded as C0, and the voltage range was 2.0-3.65V. Then, the battery was discharged at a constant current of 1C (1.3A) to 2.0V, and then charged at a constant current of 15C to 3.65V. The charging capacity was recorded as C0. x Rate-of-charge capacity retention rate = C x / C0×100%.
[0086] The capacity retention rate of a sodium-ion battery at 25℃ and a 20C discharge rate was determined. The test conditions were as follows: At 25℃, the battery was charged at a constant current and constant voltage of 1C (1.3A) to 3.65V, with a cutoff current of 0.1C, and then discharged at a constant current of 1C to 2.0V. The discharge capacity was recorded as C0, and the voltage range was 2.0-3.65V. Then, the battery was charged at a constant current and constant voltage of 1C (1.3A) to 3.65V, with a cutoff current of 0.1C, and then discharged at a constant current of 15C to 2.0V. The discharge capacity was recorded as C0. x Rate discharge capacity retention rate = C x / C0×100%.
[0087] The SEI interface impedance was determined using the following method: Refer to T / DCB 024-2024 "Method for Testing Electrochemical Impedance of Lithium-ion Batteries". The test results are shown in Table 2. Figures 4-6 .
[0088] Table 2
[0089] As shown in Table 2, the initial coulombic efficiency, initial discharge capacity, long-cycle capacity retention, and high and low rate charge-discharge performance of each group of samples are at similar levels. The electrochemical indicators of Example 1 are even slightly better than those of the three comparative examples. Specifically, the SEI interface impedance of Example 1 is only 1.28 mΩ, far lower than that of Comparative Examples 1 and 3 which use traditional constant current formation, and only slightly higher than that of Comparative Example 2 which only optimizes the wetting process. (Combined with the attached...) Figure 2 Ultrasonic transmission images under different infiltration conditions, with attachment Figure 4 To be continued Figure 6Rate and cycle performance curves further corroborate that the pulsed pressure wetting of this invention relies on periodic extrusion to drive the electrolyte to fully penetrate the deep micropores of the electrode, resulting in uniform electrolyte wetting without blank areas inside the cell. Combined with the alternating pulsed high and low current formation mode, it can effectively alleviate the concentration polarization and interface polarization generated during high-current charging and discharging through intermittent high and low current and static / micro-discharge cycles. This promotes the synchronous formation of a thin, uniform, and stable SEI film rich in inorganic components on the negative electrode surface, significantly reducing interface impedance and suppressing continuous side reactions and sodium dendrite formation in the electrolyte. Solutions that only optimize the wetting or formation process have obvious shortcomings. Comparative Example 1, which only uses pulsed pressure wetting and adopts traditional constant current formation, and the entire traditional process are superior. Comparative Example 3 suffered from severe polarization during formation, resulting in uneven SEI film thickness and significantly increased interfacial impedance. Consequently, its rate discharge performance and cycle stability were slightly reduced. Comparative Example 2, which employed pulsed formation but relied on prolonged natural immersion for wetting, had a lower SEI impedance, but prolonged immersion easily caused trace electrolyte decomposition and loss, leading to a slight decline in rate charging performance. In contrast, the synergistic optimization of the two processes in this invention significantly reduces manufacturing time while fully preserving or even slightly improving the battery's initial capacity, coulombic efficiency, rate charge / discharge performance, and long-cycle stability. It balances efficient manufacturing with excellent electrochemical performance, making it suitable for the large-scale mass production of various ion batteries such as sodium-ion, lithium-ion, and potassium-ion batteries, and possessing outstanding industrial application value.
[0090] It should be noted that, in this document, relational terms such as "first" and "second" are used merely to distinguish one entity or operation from another, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Furthermore, the terms "comprising," "including," or any other variations thereof are intended to cover non-exclusive inclusion, such that a process, method, article, or apparatus that comprises a list of elements includes not only those elements but also other elements not expressly listed, or elements inherent to such a process, method, article, or apparatus. Without further limitations, an element defined by the phrase "comprising one..." does not exclude the presence of other identical elements in the process, method, article, or apparatus that includes said element.
[0091] The above description is merely a specific embodiment of this disclosure, enabling those skilled in the art to understand or implement it. Various modifications to these embodiments will be readily apparent to those skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of this disclosure. Therefore, this disclosure is not to be limited to the embodiments described herein, but is to be accorded the widest scope consistent with the principles and novel features disclosed herein.
Claims
1. A method for preparing a battery, characterized in that, The process includes the following: 1) Inject electrolyte into the assembled dry battery to obtain an electrolyte-filled battery; after vacuum pre-wetting and vacuum sealing, a vacuum-sealed battery is obtained. 2) The vacuum-sealed battery is subjected to pulsed pressure immersion, and after standing, an electrolyte-immersed battery is obtained; 3) The battery is formed by immersing it in the electrolyte, degassing it, and then resealing it to obtain the target battery; The method of formation includes any one of the following: 31) Charge at a constant current of 1C~2C for 1~3s, charge at a constant current of 0.1~0.2C for 2~6s, then let stand for 1~2s, repeat this cycle until the upper limit voltage is reached; 32) Charge at a constant current of 1C~2C for 1~3s, charge at a constant current of 0.1~0.2C for 2~6s, then discharge at a constant current of 0.4~0.6C for 1~2s, repeating this cycle until the upper limit voltage is reached.
2. The preparation method according to claim 1, characterized in that, The vacuum pre-wetting process involves placing the liquid-filled battery under a pressure of -80 to -90 kPa for 3 to 10 minutes to obtain a vacuum pre-wetted battery.
3. The preparation method according to claim 1, characterized in that, The vacuum sealing involves sealing the vacuum-pre-wetted battery under a pressure of -80 to -90 kPa.
4. The preparation method according to claim 1, characterized in that, The pulsed pressure immersion refers to applying a mechanical pressure of 5~20 kPa to the vacuum-sealed battery; preferably 10 kPa; the immersion time is 30~60 min; and the immersion temperature is 20~45℃, preferably room temperature.
5. The preparation method according to claim 1, characterized in that, During the pulsed pressure impregnation process of the vacuum-sealed battery, the thickness change of the battery is controlled within 0.5%~1.5%; the pulse mode is a high-frequency pulse, with pressure applied for 0.2s~1s and rested for 0.2s~1s.
6. The preparation method according to claim 1, characterized in that, The settling period is 5-10 minutes at room temperature.
7. The preparation method according to claim 1, characterized in that, The degassing and secondary sealing are carried out under a vacuum of -80 to -90 kPa.
8. A battery, characterized in that, The battery is prepared by the method according to any one of claims 1 to 7; The batteries include sodium-ion batteries, lithium-ion batteries, potassium-ion batteries, zinc-ion batteries, and magnesium-ion batteries.
9. The battery according to claim 8, characterized in that, The battery assembly methods include, but are not limited to, stacking and winding.
10. An electrical appliance, characterized in that, The electrical equipment includes the battery as described in claim 8.