An electrolyte additive combination and its application in aqueous zinc-iodine batteries
The halogen-free electrolyte formed by combining 3-piperidinecarboxylic acid and valine stabilizes the four-electron conversion of the iodine cathode and regulates the zinc anode interface, solving the problems of I+ hydrolysis and zinc corrosion in aqueous zinc-iodine batteries and achieving high energy density and long lifespan battery performance.
Patent Information
- Application Number
- CN202611254236.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-18
- Publication Date
- 2026-11-17
AI Technical Summary
In existing aqueous zinc-iodine batteries, the intermediate product I+ is easily hydrolyzed in the four-electron conversion reaction, and the discharge product I- has high solubility, leading to irreversible reaction and loss of active materials. Traditional halogen additives are corrosive and cannot simultaneously solve the zinc anode interface problem, affecting battery cycle life and safety.
A combination of 3-piperidinecarboxylic acid and valine was used as a halogen-free bifunctional additive to form a multidentate chelate supramolecular structure to stabilize I+. At the same time, the behavior of the zinc anode interface was regulated by hydroxyl and amino groups to prepare a halogen-free dilute aqueous electrolyte.
It significantly improves the reversibility and cycle life of the four-electron zinc-iodine battery, avoids halogen corrosion, enhances battery safety and long-term operational reliability, and meets the requirements for large-scale application.
Smart Images

Figure CN123120920A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of aqueous zinc-iodine battery technology, specifically to an electrolyte additive and its application in aqueous zinc-iodine batteries. Background Technology
[0002] Aqueous zinc-iodine batteries, with their inherent safety and low material cost, are considered strong candidates for next-generation large-scale energy storage systems. Traditional zinc-iodine batteries are based on elemental iodine (I₂) and iodine anions (I₂). - The two-electron conversion reaction between (I) 0 / I - Its theoretical capacity is only 211 mAh / g, and its discharge plateau is approximately 1.3 V (vs Zn / Zn). 2+ This limits the energy density and power density of batteries, restricting their practical application prospects.
[0003] In recent years, the four-electron conversion reaction (I4) activating the iodine cathode has been studied. - / I2 / I + This has become an important direction for overcoming the aforementioned performance bottlenecks. This reaction pathway can provide a theoretical capacity of up to 422 mAh / g and exhibits a dual voltage platform of approximately 1.8 V and 1.3 V, which can theoretically significantly improve the energy density and power density of aqueous zinc-iodine batteries, opening up new avenues for developing low-cost, high-specific-energy aqueous energy storage technologies.
[0004] However, achieving a reversible and stable four-electron iodine conversion reaction still faces significant challenges. The core issue lies in the intermediate product I4 of the four-electron reaction. + It is readily hydrolyzed in aqueous solution, leading to an irreversible reaction; simultaneously, the discharge product I... - High solubility in electrolytes can trigger severe shuttle effects, leading to loss of active materials and decreased coulombic efficiency. Since these problems all stem from the chemical environment of the electrolyte, optimized electrolyte design is considered a key step in overcoming the bottleneck of four-electron iodine cathode technology.
[0005] To address the aforementioned challenges, existing technologies primarily rely on introducing halide ions (such as Cl-) into the electrolyte. - ,Br - As a stabilizer, it complexes and stabilizes I by forming interhalogen compounds (such as ICl, IBr). + This inhibits hydrolysis and stimulates four-electron reactions. For example, patent specification CN119340508A discloses the use of chloride salts such as triethylamine hydrochloride, 1-butyl-1-methylpyrrolidine chloride, and pyridine hydrochloride, while patent specification CN122202568A uses organic bromide salts such as 1-vinyl-3-butylimidazolium bromide to achieve this goal.
[0006] Although the aforementioned halogen-containing strategies have achieved some success at the positive end, their inherent drawbacks cannot be ignored: on the one hand, halide ions (especially Cl-) can cause halogen ions to be released during the reaction process. - and Br - These additives are highly corrosive to zinc anodes, battery current collectors, connectors, and other metal components, accelerating battery performance degradation and introducing safety hazards. Furthermore, the function of these additives is often limited to the Io side of the positive electrode. + Stabilization cannot simultaneously address interfacial issues such as dendrite growth and hydrogen evolution side reactions on the zinc anode side, resulting in the cycle life and reliability of the entire battery failing to meet practical application requirements. Therefore, developing an aqueous electrolyte system that can effectively stabilize the four-electron conversion of the iodine cathode, simultaneously regulate the interfacial behavior of the zinc anode, and is free of halogen-corrosive components has become crucial for promoting the practical application of high-energy-density zinc-iodine batteries, but related technology reports are still scarce. Summary of the Invention
[0007] To address the aforementioned technical problems and shortcomings in the field, this invention provides an electrolyte combination additive for aqueous zinc-iodine batteries, particularly relating to the combined application of 3-piperidinecarboxylic acid and valine as halogen-free bifunctional additives, and their application in stabilizing the four-electron conversion reaction of the iodine cathode and the deposition / stripping behavior of the zinc anode.
[0008] The specific technical solution of this invention is as follows: In a first aspect, the present invention provides an electrolyte combination additive comprising 3-piperidinecarboxylic acid and valine in a molar ratio of (0.1-2) (e.g., 0.18, 0.19, 0.49, 0.5, 0.9, 1, 1.1, 1.9, etc.):(0.9-1).
[0009] Furthermore, the electrolyte additive combination is halogen-free.
[0010] When the above-mentioned electrolyte additive combination is applied to an aqueous solution of zinc trifluoromethanesulfonate, a dilute aqueous electrolyte without any additional halogens can be obtained, which can simultaneously achieve the effect of iodine on the positive electrode side. + Effective complexation stability, for I - / I3 - The shuttle adsorption suppression and the regulation of zinc anode interface deposition / stripping behavior synergistically improve the reversibility, cycle life and safety of four-electron zinc-iodine batteries at the full cell level.
[0011] In a second aspect, the present invention provides an electrolyte aqueous solution comprising 3-piperidinecarboxylic acid, valine, and zinc trifluoromethanesulfonate, wherein the molar ratio of 3-piperidinecarboxylic acid to valine is (0.1-2) (e.g., 0.18, 0.19, 0.49, 0.5, 0.9, 1, 1.1, 1.9, etc.):(0.9-1).
[0012] In some preferred embodiments, the molar ratio of zinc trifluoromethanesulfonate to valine is (0.9-3) (e.g., 1, 1.9, 2, etc.):(0.9-1).
[0013] In some preferred embodiments, the concentration of valine in the electrolyte aqueous solution is 0.9-1 mol / L.
[0014] Furthermore, no other halogen elements are added to the electrolyte aqueous solution except for zinc trifluoromethanesulfonate.
[0015] The present invention does not impose any particular limitation on the preparation method of the electrolyte aqueous solution.
[0016] The present invention provides an exemplary method for preparing an aqueous electrolyte solution, comprising: dissolving 3-piperidinecarboxylic acid, valine and zinc trifluoromethanesulfonate in deionized water to obtain the aqueous electrolyte solution.
[0017] Thirdly, the present invention provides the application of the electrolyte combination additive described in the first aspect or the electrolyte aqueous solution described in the second aspect in the preparation of aqueous zinc-iodine batteries.
[0018] Fourthly, the present invention provides an aqueous zinc-iodine battery, comprising a negative electrode zinc, a positive electrode iodine, a separator, and the electrolyte aqueous solution described in the second aspect.
[0019] In some preferred embodiments, the method for preparing the positive electrode iodine includes: After mixing iodine and activated carbon, the mixture is sealed in a glass tube and heated to 60-100℃ (e.g., 80℃) and kept at that temperature for 2-10 h (e.g., 5 h) (to allow the iodine to melt and fully impregnate the activated carbon pores). The mixture is then cooled to room temperature to obtain the activated carbon@iodine composite material. Activated carbon@iodine composite material, polyvinylidene fluoride and (conductive) carbon are mixed and N-methyl-2-pyrrolidone is used as solvent to form a slurry, which is then coated onto carbon paper and dried to obtain an iodine positive electrode sheet.
[0020] In some preferred embodiments, the mass ratio of iodine to activated carbon in the method for preparing the positive electrode iodine is 2:8 to 6:4, for example, 4:6.
[0021] In some preferred embodiments, in the method for preparing the positive electrode iodine, the mass ratio of activated carbon@iodine composite material, polyvinylidene fluoride, and carbon is 8:1:1.
[0022] In some preferred embodiments, the drying temperature in the method for preparing the positive electrode iodine is 35-45°C, for example, 40°C.
[0023] In some preferred embodiments, the drying time in the method for preparing the positive electrode iodine is 8-20 h, for example 12 h.
[0024] In some preferred embodiments, the diaphragm includes a glass fiber membrane or the like.
[0025] This invention can significantly stabilize I + , prevent I - and I3 - The shuttle effect enhances the reversibility and stability of the four-electron conversion reaction of the iodine cathode, while effectively improving the cycle stability of the zinc anode, inhibiting zinc anode corrosion, and obtaining a high-performance aqueous four-electron zinc-iodine battery.
[0026] Compared with the prior art, the beneficial effects of this invention are as follows: 1) The electrolyte additive of this invention is completely free of halide ions, thus avoiding the chemical corrosion of the zinc anode and battery metal components by traditional halogen additives, significantly improving battery safety and long-term operational reliability. Simultaneously, the electrolyte is a dilute aqueous solution of zinc trifluoromethanesulfonate, combining the advantages of low cost and high ionic conductivity, meeting the basic performance requirements of electrolytes for large-scale applications.
[0027] 2) 3-Piperidinic acid donates a lone pair of electrons to I through the nitrogen atom of the imine atom on the piperidine ring. + It forms chelate coordination bonds, effectively reducing I + Its electrophilic activity chemically inhibits its hydrolysis reaction. Simultaneously, 3-piperidinecarboxylic acid constructs a thermodynamically stable chair conformation in a three-dimensional space, with the hydrogen atoms and carboxyl groups on the ring exhibiting definite orientations in three-dimensional space. + After being embedded in the molecular framework, it is encapsulated within a specific molecular cavity. This cavity forms a kinetic barrier, effectively preventing water molecules from approaching the protected I through steric hindrance. + This further enhances I at the physical level. + Stability.
[0028] 3) Valine, as the second ligand, interacts with I through its carbonyl oxygen atom. + It forms a coordination bond with 3-piperidincaric acid to construct 3-piperidincaric acid-I + The multidentate chelate supramolecular structure of valine. Compared with single-molecule coordination, this dual-coordination structure has higher structural rigidity and can bind I... + It is more firmly locked inside the supramolecular cavity, significantly enhancing the resistance to I. + Its stabilizing and protective effect further inhibits I + Hydrolysis tendency.
[0029] 4) The hydroxyl group of 3-piperidinecarboxylic acid and the amino group of valine can synergistically chelate I. - and I3 - This effectively prevents its dissolution and shuttle behavior.
[0030] 5) 3-piperidinecarboxylic acid and valine can partially replace water molecules in the first solvent sheath of zinc ions, reducing the number of active water molecules that are directly coordinated with zinc ions, thus weakening the reduction and decomposition reaction of water molecules on the zinc anode surface from the source. At the same time, 3-piperidinecarboxylic acid and valine can spontaneously adsorb onto the zinc surface to form a physical isolation layer, effectively blocking the direct contact between water molecules in the bulk electrolyte and the zinc surface, further inhibiting zinc corrosion. Finally, 3-piperidinecarboxylic acid and valine also function as crystal plane guiding agents, which can guide zinc ions to preferentially deposit along the (101) crystal plane, promote the uniform and dense growth of zinc grains, inhibit the formation and development of zinc dendrites, thereby significantly improving the cycle stability of the zinc electrode. Attached Figure Description
[0031] Figure 1 The UV-Vis spectra of zinc-iodine batteries assembled from the 3-piperidinecarboxylic acid-valine-zinc trifluoromethanesulfonate mixed electrolyte (denoted as BPV-0.5) prepared in Example 1, the 3-piperidinecarboxylic acid-zinc trifluoromethanesulfonate (denoted as BP-0.5) prepared in Comparative Example 1, and the valine-zinc trifluoromethanesulfonate (BV) prepared in Comparative Example 2 after being charged to 1.9 V.
[0032] Figure 2 The cyclic voltammetry curves (scan rate of 1 mV / s) of zinc-iodine batteries assembled with the 3-piperidinecarboxylic acid-valine-zinc trifluoromethanesulfonate mixed electrolyte (denoted as BPV-0.5) prepared in Example 1, the 3-piperidinecarboxylic acid-zinc trifluoromethanesulfonate (denoted as BP-0.5) prepared in Comparative Example 1, and the valine-zinc trifluoromethanesulfonate (BV) prepared in Comparative Example 2 are shown.
[0033] Figure 3 The 3-piperidinecarboxylic acid-valine-zinc trifluoromethanesulfonate mixed electrolyte (denoted as BPV-0.5) prepared in Example 1 was used in an H-type electrolytic cell with I3. - Photos of the shuttle experiment.
[0034] Figure 4 The charge-discharge curves of the zinc-iodine battery assembled with the zinc mixed electrolyte (denoted as BPV-0.5) prepared in Example 1 at room temperature and a current density of 1 A / g are shown.
[0035] Figure 5 The graph shows a comparison of the cycling performance of zinc-iodine batteries assembled with the 3-piperidinecarboxylic acid-valine-zinc trifluoromethanesulfonate mixed electrolyte (denoted as BPV-0.5) prepared in Example 1, the 3-piperidinecarboxylic acid-zinc trifluoromethanesulfonate (denoted as BP-0.5) prepared in Comparative Example 1, and the valine-zinc trifluoromethanesulfonate (BV) prepared in Comparative Example 2 at room temperature and a current density of 1 A / g.
[0036] Figure 6Zinc||zinc symmetric cells assembled from the 3-piperidinic acid-valine-zinc trifluoromethanesulfonate mixed electrolyte (denoted as BPV-0.5) prepared in Example 1, the 3-piperidinic acid-zinc trifluoromethanesulfonate (denoted as BP-0.5) prepared in Comparative Example 1, and the valine-zinc trifluoromethanesulfonate (BV) prepared in Comparative Example 2, operated at 1 mA / cm². 2 and 1 mAh / cm 2 Cyclic performance under certain conditions.
[0037] Figure 7 The zinc||zinc symmetric cell assembled using the 3-piperidinecarboxylic acid-valine-zinc trifluoromethanesulfonate mixed electrolyte (denoted as BPV-0.5) prepared in Example 1 operates at 1 mA / cm². 2 and 1 mAh / cm 2 Scanning electron microscope image of the deposit morphology on the zinc electrode surface after 500 hours of cycling. Detailed Implementation
[0038] The present invention will be further described below with reference to the accompanying drawings and specific embodiments. It should be understood that these embodiments are for illustrative purposes only and are not intended to limit the scope of the invention. Operating methods not specifically specified in the following embodiments are generally performed under conventional conditions or as recommended by the manufacturer.
[0039] Example 1: 14.5 g of zinc trifluoromethanesulfonate (Zn(OTF)2, 99%), 1.29 g of 3-piperidinecarboxylic acid (99%), and 2.34 g of valine (90%) were added sequentially to deionized water and stirred thoroughly until completely dissolved. The mixture was then brought to a final volume of 20 mL to obtain a mixed solution with a zinc trifluoromethanesulfonate concentration of 2 M, a 3-piperidinecarboxylic acid concentration of 0.5 M, and a valine concentration of 1 M. This solution was designated as BPV-0.5.
[0040] Comparative Example 1: Add 14.5 g of zinc trifluoromethanesulfonate (Zn(OTF)2, 99%) and 1.29 g of 3-piperidinecarboxylic acid (99%) to deionized water, stir thoroughly until completely dissolved, and then bring the volume of the mixed solution to 20 mL to obtain a mixed solution with a zinc trifluoromethanesulfonate concentration of 2 M and a 3-piperidinecarboxylic acid concentration of 0.5 M. This solution is denoted as BP-0.5.
[0041] Comparative Example 2: Add 14.5 g of zinc trifluoromethanesulfonate (Zn(OTF)2, 99%) and 2.34 g of valine (90%) to deionized water, stir thoroughly until completely dissolved, and then bring the volume of the mixture to 20 mL to obtain a mixed solution with a zinc trifluoromethanesulfonate concentration of 2 M and a valine concentration of 1 M. This solution is denoted as BV.
[0042] The above mixed solution was used as the electrolyte to assemble a CR2025 button-type aqueous zinc-iodine battery. The negative electrode was a pure zinc sheet (99.9% purity), the positive electrode was an iodine composite electrode, and the separator was a glass fiber membrane. The preparation method of the iodine positive electrode was as follows: 40 mg of iodine and 60 mg of activated carbon were mixed, sealed in a glass tube, heated to 80°C, kept at that temperature for 5 h, and then naturally cooled to room temperature to obtain an activated carbon@iodine composite material. Then, 40 mg of this composite material, 5 mg of polyvinylidene fluoride (PVDF), and 5 mg of carbon (SuperP) were placed in an N-methyl-2-pyrrolidone solvent, mixed evenly to form a slurry, coated on carbon paper, dried at 40°C for 12 h, and cut to obtain the iodine positive electrode sheet.
[0043] The above-mentioned iodine positive electrode, zinc negative electrode and separator were assembled into a CR2025 button cell in air. After injecting the corresponding electrolyte, the electrochemical performance was tested using the Xinwei Battery Testing System.
[0044] The assembled zinc-iodine button cell was charged to 1.9 V, and then detected using ultraviolet-visible spectroscopy. Figure 1 As shown, in the BV electrolyte, only a broad absorption peak appears around 458 nm, corresponding to I₂; no I₂ was observed. + The signal indicates that valine alone cannot effectively stabilize I. + This cannot trigger the four-electron iodine conversion reaction. For BP-0.5, two clear peaks were detected at 343 nm and 458 nm, corresponding to I... + The presence of I2 indicates that 3-piperidinecarboxylic acid can stabilize a portion of I... + However, most of the I + It is converted to I2 through disproportionation and hydrolysis. In contrast, the BPV-0.5 electrolyte exhibits stronger I2 conversion. + The peak, while the I2 signal was almost indistinguishable, indicates that 3-piperidinecarboxylic acid and valine can provide a co-coordinating environment, effectively inhibiting I. + Hydrolysis significantly improves its stability. It is worth noting that I... + The peak shifted to 365 nm, indicating that I + The coordination structure has changed; it is no longer a monocoordinate 3-piperidinic acid-I + Instead, it is a dual-coordinated 3-piperidinic acid-I + -Valine.
[0045] Figure 2 The cyclic voltammetry (CV) curves of zinc-iodine batteries using BV, BP-0.5, and BPV-0.5 electrolytes are shown. BV exhibits a pair of redox peaks only at 1.24 / 1.10 V, corresponding to I... - / I 0The reaction did not show a second pair of redox peaks, indicating that only a two-electron conversion reaction occurred. BP-0.5 showed Ig at 1.28 / 1.15 V. - / I 0 In addition to the reaction peaks, a pair of peaks corresponding to I also appeared at 1.60 / 1.78 V. 0 / I + The redox peaks of the reaction indicate a four-electron conversion reaction, but the reduction peak at 1.60 V is smaller while the oxidation peak at 1.78 V is larger, revealing poor reversibility of the reaction. BPV-0.5 also exhibits two pairs of redox peaks, with the reduction peak being larger at higher voltages (1.67 V) and the oxidation peak (1.90 V) becoming smaller. 0 / I + The reversibility was significantly improved. Furthermore, the redox peaks in the low-voltage region were also significantly larger, indicating that the iodine dissolution shuttle behavior was further suppressed. - / I 0 The reversibility of the reaction is significantly improved.
[0046] Diffusion experiments were conducted using an H-type electrolytic cell. The right-hand container of the H-type electrolytic cell contained a colorless BPV-0.5 solution, while the left-hand container contained an equal volume of a brownish-yellow BPV-0.5 solution (containing 0.2 M I3). - The two sides are separated by a glass fiber membrane. After standing for 90 minutes, the solution on the right side remains colorless. Figure 3 I3 was not detected by ultraviolet-visible spectroscopy. - Characteristic signals indicate that 3-piperidinecarboxylic acid and valine effectively adsorb and limit I3. - The diffusion behavior was observed. In contrast, when using BP-0.5 solution, the solution on the right only turned slightly yellow after 90 minutes; when using BV solution, the solution on the right turned significantly yellow after 90 minutes. This indicates that 3-piperidinic acid alone can limit most iodine shuttle but still allows for a small amount of iodine shuttle, while valine alone has a weaker shuttle inhibition ability; the combination of the two provides the best inhibitory effect.
[0047] Figure 4 The charge-discharge curves of the zinc-iodine battery using BPV-0.5 electrolyte at 25℃ and a current density of 1 A / g show four voltage plateaus, indicating a four-electron conversion reaction. In contrast, the BV electrolyte only shows two plateaus, corresponding to a two-electron reaction. Although BP-0.5 shows four plateaus, its high-voltage plateau is shorter, reflecting I0.5... + Hydrolysis was not effectively inhibited, I 0 / I + The reversibility of the reaction is limited.
[0048] Figure 5The cycling performance of zinc-iodine batteries using BV, BP-0.5, and BPV-0.5 electrolytes at 25°C and a current density of 1 A / g was evaluated. After 200 cycles, BPV-0.5 still retained a capacity of 391 mAh / g. In contrast, BP-0.5's capacity decreased to 172 mAh / g after 200 cycles, and BV's capacity was only 135 mAh / g after 200 cycles.
[0049] The performance of BPV-0.5 is superior to that of the zinc-iodine battery with tribromopyridinium aqueous electrolyte disclosed in patent application CN121394608A, which has a capacity of 280 mAh / g at 0.2 A / g; superior to the specific capacity of the chlorobetaine choline additive disclosed in patent application CN120767440A, which has a specific capacity of 300 mAh / g at 1 A / g; superior to the discharge capacity of the amino acid additive disclosed in patent application CN120709535A, which has a discharge capacity of 136 mAh / g at 1 A / g; and superior to the specific capacity of the 1-ethyl-3-methylimidazolium chloride and sulfonylpyrrolidone copolymer eutectic electrolyte disclosed in patent application CN122118133A, which has a specific capacity of 382 mAh / g after 200 cycles at 0.5C.
[0050] Figure 6 Zinc||zinc symmetric cells using BV, BP-0.5, and BPV-0.5 electrolytes at 1 mA / cm 2 and 1 mAh / cm 2 Cyclic performance under certain conditions. The symmetric cell assembled with BV electrolyte failed due to short circuit after only 240 hours of cycling. BP-0.5 could cycle up to 1900 hours. BPV-0.5 could cycle stably for over 2000 hours. This indicates that 3-piperidinic acid can significantly stabilize the zinc electrode. Valine alone has limited effect, but its combination with 3-piperidinic acid can further improve the stability of the zinc electrode. X-ray diffraction (XRD) characterization of the zinc electrode using BPV-0.5 electrolyte after 500 hours of cycling showed no diffraction peaks of corrosion byproducts, while the zinc electrode using BP-0.5 showed weak byproduct diffraction peaks, and the zinc electrode using BV showed the strongest byproduct diffraction peaks. This indicates that the combined use of 3-piperidinic acid and valine can effectively suppress the corrosion side reactions of the zinc electrode. Further SEM observation of the cycled zinc electrode revealed that the zinc electrode using BPV-0.5 electrolyte had a vertically growing and tightly adhered zinc deposit on its surface. Figure 7 XRD analysis showed that the diffraction peak intensity of the (101) crystal plane was the most prominent, indicating that the zinc deposition had the preferred orientation of the (101) crystal plane.
[0051] Tafel curves of BV, BP-0.5, and BPV-0.5 electrolytes were tested using a three-electrode system. The corrosion potential of BPV-0.5 electrolyte was -1.06 V, while that of BP-0.5 was -1.09 V, and that of BV was -1.14 V. Meanwhile, the corrosion current of BPV-0.5 electrolyte was 4.51 mA / cm². 2 The corrosion currents for BP-0.5 and BV were 6.42 and 9.11 mA / cm, respectively. 2 The results showed that 3-piperidinecarboxylic acid could inhibit zinc corrosion, and the combination of 3-piperidinecarboxylic acid and valine had the strongest corrosion inhibition effect.
[0052] Example 2: 14.5 g of zinc trifluoromethanesulfonate (Zn(OTF)2, 99%), 0.5 g of 3-piperidinecarboxylic acid (99%), and 2.34 g of valine (90%) were added sequentially to deionized water and stirred thoroughly until completely dissolved. The mixture was then brought to a final volume of 20 mL to obtain a mixed solution with a zinc trifluoromethanesulfonate concentration of 2 M, a 3-piperidinecarboxylic acid concentration of 0.19 M, and a valine concentration of 1 M. This solution was designated as BPV-0.19.
[0053] The subsequent battery assembly and testing methods are the same as in Example 1.
[0054] The assembled zinc-iodine battery maintained a discharge capacity of 322 mAh / g after 200 cycles at 25°C and a current density of 1 A / g.
[0055] Example 3: 14.5 g of zinc trifluoromethanesulfonate (Zn(OTF)2, 99%), 2.58 g of 3-piperidinecarboxylic acid (99%), and 2.34 g of valine (90%) were added sequentially to deionized water and stirred thoroughly until completely dissolved. The mixture was then brought to a final volume of 20 mL to obtain a mixed solution with a zinc trifluoromethanesulfonate concentration of 2 M, a 3-piperidinecarboxylic acid concentration of 1.0 M, and a valine concentration of 1 M. This solution was designated as BPV-1.0.
[0056] The subsequent battery assembly and testing methods are the same as in Example 1.
[0057] The assembled zinc-iodine battery maintained a discharge capacity of 347 mAh / g after 200 cycles at 25°C and a current density of 1 A / g.
[0058] In summary, 3-piperidinic acid and valine can simultaneously couple I + Ions, preventing water molecules from reacting with I + Attacks, improve I + Stability; in addition, 3-piperidinecarboxylic acid and valine can also couple I- and I3 - This invention inhibits the dissolution and shuttle of iodine. The combined use of 3-piperidinecarboxylic acid and valine effectively stimulates the four-electron reaction of iodine. Furthermore, the two can synergistically regulate the solvation structure of zinc ions and adsorb them onto the zinc anode surface, suppressing side reactions and dendrite growth, and improving the cycle stability of the zinc electrode. This invention offers advantages such as low cost, ease of manufacture, and non-corrosiveness, making it suitable for large-scale applications of high-energy-density, long-life aqueous zinc-iodine batteries.
[0059] Furthermore, it should be understood that after reading the above description of the present invention, those skilled in the art can make various alterations or modifications to the present invention, and these equivalent forms also fall within the scope defined by the appended claims.
Claims
1. An electrolyte combination additive characterized in that, It includes 3-piperidinecarboxylic acid and valine in a molar ratio of (0.1-2):(0.9-1).
2. The electrolyte combination additive according to claim 1, characterized in that, The electrolyte additive combination is halogen-free.
3. An aqueous solution of an electrolyte, characterized in that, It includes 3-piperidinecarboxylic acid, valine and zinc trifluoromethanesulfonate, wherein the molar ratio of 3-piperidinecarboxylic acid to valine is (0.1-2):(0.9-1).
4. The electrolyte aqueous solution according to claim 3, characterized in that, The molar ratio of zinc trifluoromethanesulfonate to valine is (0.9-3):(0.9-1).
5. The electrolyte aqueous solution according to claim 3 or 4, characterized in that, The concentration of valine in the electrolyte aqueous solution is 0.9-1 mol / L.
6. The electrolyte aqueous solution according to claim 3, characterized in that, The electrolyte aqueous solution contains no other halogen elements besides zinc trifluoromethanesulfonate.
7. The use of the electrolyte combination additive according to claim 1 or 2 or the electrolyte aqueous solution according to any one of claims 3 to 6 in the preparation of aqueous zinc-iodine batteries.
8. An aqueous zinc-iodine battery, characterized in that, It includes a negative electrode zinc, a positive electrode iodine, a diaphragm, and an aqueous electrolyte solution as described in any one of claims 3 to 6.
9. The aqueous zinc-iodine battery according to claim 8, characterized in that, The method for preparing the positive electrode iodine includes: Iodine and activated carbon are mixed, sealed in a glass tube, heated to 60-100℃, kept at that temperature for 2-10 h, and cooled to room temperature to obtain activated carbon@iodine composite material; Activated carbon@iodine composite material, polyvinylidene fluoride and carbon are mixed and N-methyl-2-pyrrolidone is used as solvent to form a slurry, which is then coated onto carbon paper and dried to obtain an iodine positive electrode sheet.
10. The aqueous zinc-iodine battery according to claim 9, characterized in that, The mass ratio of iodine to activated carbon is 2:8 to 6:4; The mass ratio of activated carbon@iodine composite material, polyvinylidene fluoride, and carbon is 8:1:1; The drying temperature is 35-45℃; The drying time is 8-20 hours.
Citation Information
Patent Citations
Electrolyte for improving interface stability of four-electron aqueous zinc-iodine battery and aqueous zinc-iodine battery
CN119340508A
Aqueous zinc-iodine battery electrolyte containing amino acid additive and preparation method and application thereof
CN120709535A
Brine-containing electrolyte based on clobeticoline and application of brine-containing electrolyte in aqueous zinc-iodine battery with I- / I0 / I < + > four-electron positive valence conversion
CN120767440A
Electrolyte capable of being used for four-electron conversion reaction of aqueous zinc-iodine battery
CN121394608A
Eutectic electrolyte based on ionic liquid and application of eutectic electrolyte in aqueous zinc-iodine battery
CN122118133A