Separator and secondary battery
By introducing a hydrogen absorption layer into the secondary battery separator and utilizing a combination of modified hydrogen absorption materials and shell materials, the safety hazards and capacity decay caused by hydrogen accumulation are solved, thereby improving the safety and lifespan of the secondary battery.
Patent Information
- Application Number
- CN202611462455.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-20
- Publication Date
- 2026-11-17
AI Technical Summary
Existing secondary battery separators lack hydrogen absorption capacity, causing gas to accumulate inside the battery, leading to safety hazards, rapid capacity decay, and short cycle life.
A polyolefin-based base membrane with a hydrogen absorption functional layer is used. The hydrogen absorption functional layer includes a modified hydrogen absorption material and a shell material. The shell material covers the surface of the hydrogen absorption material. The hydrogen absorption functional layer is located on one or both sides of the base membrane, absorbing hydrogen and avoiding electrical contact with the base membrane, thus reducing short circuits and self-discharge.
It effectively absorbs hydrogen, prevents gas accumulation, improves safety performance, slows down capacity decay, and extends cycle life.
Smart Images

Figure CN123121075A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of secondary battery technology, and more particularly to a separator and a secondary battery. Background Technology
[0002] Currently, the separator in secondary batteries mainly serves as a physical barrier and facilitates ion conduction. However, it lacks the ability to absorb hydrogen gas generated during the charge-discharge cycle of the secondary battery. As a result, the gas accumulates inside the secondary battery, leading to increased internal pressure, swelling, leakage, or even rupture. This poses a safety hazard and consumes the electrolyte and active materials (such as active sodium in sodium-ion batteries), resulting in accelerated capacity decay and shortened cycle life.
[0003] Therefore, there is an urgent need for a separator and a secondary battery to solve the above-mentioned technical problems. Summary of the Invention
[0004] In view of this, the present invention proposes a separator and a secondary battery to solve the technical problems that existing separators lack hydrogen absorption capacity, which leads to safety hazards in secondary batteries, while capacity decay is difficult to delay and cycle life is difficult to improve.
[0005] The technical solution of this invention is implemented as follows: In a first aspect, the present invention provides a diaphragm comprising: Polyolefin-based films; A hydrogen-absorbing functional layer, wherein the hydrogen-absorbing functional layer is located on at least one side of the polyolefin-based film; The hydrogen absorption functional layer includes a modified hydrogen absorption material, which includes a hydrogen absorption material and a shell material covering the surface of the hydrogen absorption material. The shell material is selected from at least one of aluminum oxides, aluminates, aluminum hydroxides, and ionic conductor materials.
[0006] In some embodiments, the mass ratio of the shell material to the hydrogen-absorbing material in the modified hydrogen-absorbing material is (0.05 to 0.4):1; The shell material has a D50 particle size of 0.5 μm to 5 μm, and the hydrogen-absorbing material has a D50 particle size of 0.5 μm to 7 μm.
[0007] In some embodiments, the modified hydrogen-absorbing material has a mass fraction of 50% to 99% in the hydrogen-absorbing functional layer.
[0008] In some embodiments, the modified hydrogen-absorbing material has a mass fraction of 80% to 95% in the hydrogen-absorbing functional layer.
[0009] In some embodiments, the hydrogen-absorbing functional layer further includes an adhesive selected from at least one of polyvinylidene fluoride, styrene-butadiene rubber, sodium carboxymethyl cellulose, polyacrylic acid, and waterborne polyurethane.
[0010] In some embodiments, the ratio of the total thickness of the hydrogen-absorbing functional layer to the thickness of the polyolefin-based film is (0.1 to 1):1.
[0011] In some embodiments, the total thickness of the polyolefin-based membrane is 5 μm to 25 μm, and the porosity of the polyolefin-based membrane is 30% to 50%.
[0012] In some embodiments, the polyolefin-based membrane is selected from at least one of polyethylene and polypropylene, and the hydrogen-absorbing material is selected from AB. (5-x) M x Type alloy materials, AB (2-x) M x Type alloy materials, AB (1-x) M x Alloy materials and A2B (1-x) M x At least one of the following alloy materials, wherein the shell material is selected from Al2O3, β-Al2O3, γ-AlOOH, Na3Zr2Si2PO4. 12 At least one of NaTi2(PO4)3, Na3V2(PO4)3 and Na3V2(PO4)2F3; Wherein, A is selected from at least one of Ti, Zr, Ca, Mg, V, Nb, lanthanide rare earth elements and actinide rare earth elements, B is selected from at least one of Fe, Co, Ni, Cr, Cu, Mn and Al, M is selected from at least one metallic element that is different from A and different from B, and 0≤x<0.4.
[0013] In some embodiments, the hydrogen-absorbing material is selected from LaNi5, TiMn, TiFe, and LaNi. 4.7 Al 0.3 TiMn 1.82 Ni 0.18 TiFe 0.9 Ni 0.1 and Mg2Ni 0.86 Cr 0.14 At least one of them.
[0014] Secondly, the present invention also provides a secondary battery, the secondary battery comprising the separator as described above.
[0015] The separator and secondary battery of the present invention have the following advantages over the prior art: By setting a hydrogen absorption functional layer and using a modified hydrogen absorption material with a shell material coated on the surface of the hydrogen absorption material in the hydrogen absorption functional layer, when the separator is applied to the secondary battery, it effectively absorbs hydrogen during the charge-discharge cycle, preventing gas from accumulating inside the secondary battery. At the same time, the shell material avoids electrical contact between the hydrogen absorption material and the polyolefin base film, reducing the risk of short circuit and self-discharge of the secondary battery, effectively improving the safety performance of the secondary battery, delaying the capacity decay of the secondary battery, and improving the cycle life of the secondary battery. Attached Figure Description
[0016] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.
[0017] Figure 1 This is a schematic diagram of the first structure of the diaphragm of the present invention; Figure 2 This is a schematic diagram of a second structure of the diaphragm of the present invention. Detailed Implementation
[0018] The technical solutions of the present invention will be clearly and completely described below with reference to the embodiments of the present invention. Obviously, the described embodiments are only a part of the embodiments of the present invention, and not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those of ordinary skill in the art without creative effort are within the scope of protection of the present invention.
[0019] Currently, existing membranes lack hydrogen absorption capacity. When applied to secondary batteries, the gas accumulates inside the battery, leading to technical problems such as difficulty in improving safety performance, slowing down capacity decay, and extending cycle life.
[0020] Please see Figure 1 and Figure 2 In a first aspect, the present invention provides a diaphragm 100, comprising: Polyolefin base film 110; Hydrogen-absorbing functional layer 120, wherein the hydrogen-absorbing functional layer 120 is located on at least one side of the polyolefin base film 110; The hydrogen absorption functional layer 120 includes a modified hydrogen absorption material, which includes a hydrogen absorption material and a shell material covering the surface of the hydrogen absorption material. The shell material is selected from at least one of aluminum oxides, aluminates, aluminum hydroxides, and ionic conductor materials.
[0021] The separator 100 provided in this application, through the setting of a hydrogen absorption functional layer 120, and the use of a modified hydrogen absorption material with a shell material coated on the surface of the hydrogen absorption material in the hydrogen absorption functional layer 120, effectively absorbs hydrogen during the charge-discharge cycle when the separator 100 is applied to a secondary battery. This prevents the gas from accumulating inside the secondary battery, while the shell material avoids electrical contact between the hydrogen absorption material and the polyolefin base membrane 110, reducing the risk of short circuits and self-discharge in the secondary battery, effectively improving the safety performance of the secondary battery, delaying the capacity decay of the secondary battery, and improving the cycle life of the secondary battery.
[0022] In some embodiments, the hydrogen-absorbing functional layer 120 is located on at least one side surface of the polyolefin-based film 110.
[0023] Please see Figure 1 and Figure 2 In some embodiments, the hydrogen-absorbing functional layer 120 is located on one side surface of the polyolefin-based film 110. Alternatively, the hydrogen-absorbing functional layer 120 is located on opposite side surfaces of the polyolefin-based film 110. When the hydrogen-absorbing functional layer 120 is located on opposite side surfaces of the polyolefin-based film 110, the hydrogen-absorbing functional layer 120 includes a first hydrogen-absorbing functional sublayer 120a and a second hydrogen-absorbing functional sublayer 120b, wherein the first hydrogen-absorbing functional sublayer 120a is located on one side surface of the polyolefin-based film 110, and the second hydrogen-absorbing functional sublayer 120b is located on the side surface of the polyolefin-based film 110 away from the first hydrogen-absorbing functional sublayer 120a.
[0024] In some embodiments, the ratio of the total thickness of the hydrogen-absorbing functional layer 120 to the thickness of the polyolefin base film 110 is (0.1 to 1):1, for example, it can be 0.1:1, 0.16:1, 0.2:1, 0.5:1, 0.6:1, 0.8:1, 1:1, etc. Preferably, the ratio of the total thickness of the hydrogen-absorbing functional layer 120 to the thickness of the polyolefin base film 110 is (0.2 to 0.6):1, which is beneficial for maintaining the ion conduction function of the separator 100. When the hydrogen-absorbing functional layer 120 includes a first hydrogen-absorbing functional sublayer 120a and a second hydrogen-absorbing functional sublayer 120b, the thickness of the hydrogen-absorbing functional layer 120 is the sum of the thicknesses of the first hydrogen-absorbing functional sublayer 120a and the second hydrogen-absorbing functional sublayer 120b.
[0025] In some embodiments, the total thickness of the polyolefin-based membrane 110 is 5 μm to 25 μm, for example, it can be 5 μm, 10 μm, 15 μm, 20 μm, 25 μm, etc.; the porosity of the polyolefin-based membrane 110 is 30% to 50%, for example, it can be 30%, 35%, 40%, 45%, 50%, etc. By controlling the polyolefin-based membrane 110, the separator 100 can effectively act as a physical barrier when applied to a secondary battery, while ensuring that the length of the ion migration path and the number of ion migration channels are appropriate. In conjunction with the use of the hydrogen absorption functional layer 120, it can effectively and timely absorb the hydrogen generated during the charging and discharging process of the secondary battery, reduce the gas production rate, delay the capacity decay of the secondary battery, and improve the cycle life of the secondary battery.
[0026] In some embodiments, the material of the polyolefin-based film 110 is selected from at least one of polyethylene and polypropylene. That is, the polyolefin-based film 110 can be a polyethylene film, a polypropylene film, or a composite film of a polyethylene film and a polypropylene film. When the polyolefin-based film 110 is a composite film of a polyethylene film and a polypropylene film, the number of polyethylene film layers in the polyolefin-based film 110 can be one or more layers, and the number of polypropylene film layers in the polyolefin-based film 110 can be one or more layers. For example, the polyolefin-based film 110 can be formed by combining one layer of polyethylene film and one layer of polypropylene film, or the polyolefin-based film 110 can be a three-layer composite film formed by combining one layer of polyethylene film and one layer of polypropylene film located on both sides of the polyethylene film.
[0027] In some embodiments, the polyolefin-based membrane 110 is selected from commercially available polyethylene-based membranes and / or polypropylene-based membranes used in secondary batteries.
[0028] In some embodiments, the hydrogen-absorbing functional layer 120 further includes an adhesive for fixing the hydrogen-absorbing functional layer 120 to at least one surface of the polyolefin base film 110. The adhesive is selected from at least one of polyvinylidene fluoride, styrene-butadiene rubber, sodium carboxymethyl cellulose, polyacrylic acid, and waterborne polyurethane.
[0029] In some embodiments, the hydrogen-absorbing functional layer 120 is composed of the adhesive and the modified hydrogen-absorbing material.
[0030] In some embodiments, the modified hydrogen-absorbing material has a mass fraction of 50% to 99% in the hydrogen-absorbing functional layer 120, for example, 50%, 60%, 80%, 75%, 95%, 99%, etc.; preferably, the modified hydrogen-absorbing material has a mass fraction of 80% to 95% in the hydrogen-absorbing functional layer 120. When the hydrogen-absorbing functional layer 120 includes a first hydrogen-absorbing functional sublayer 120a and a second hydrogen-absorbing functional sublayer 120b, the modified hydrogen-absorbing material has a mass fraction of 50% to 99% in the first hydrogen-absorbing functional sublayer 120a, preferably 80% to 95%; the modified hydrogen-absorbing material has a mass fraction of 50% to 99% in the second hydrogen-absorbing functional sublayer 120b, preferably 80% to 95%. The mass fraction of the modified hydrogen-absorbing material in the first hydrogen-absorbing functional sublayer 120a and the mass fraction of the modified hydrogen-absorbing material in the second hydrogen-absorbing functional sublayer 120b may be the same or different. The modified hydrogen-absorbing material is used in the separator 100 to absorb hydrogen generated during charging and discharging when applied to a secondary battery. By controlling the mass fraction of the modified hydrogen-absorbing material in the hydrogen-absorbing functional layer 120, it is beneficial for the hydrogen-absorbing functional layer 120 to fully absorb hydrogen while reducing the shedding of the modified hydrogen-absorbing material, thereby reducing the risk of self-discharge and short circuit inside the secondary battery caused by the modified hydrogen-absorbing material.
[0031] In some embodiments, the modified hydrogen-absorbing material includes a hydrogen-absorbing material and a shell material covering the surface of the hydrogen-absorbing material. The shell material is used to isolate the hydrogen-absorbing material from the polyolefin-based membrane, avoiding electrical contact between the hydrogen-absorbing material and the polyolefin-based membrane, thereby reducing the short-circuit risk when the separator 100 is used in a secondary battery and reducing self-discharge inside the secondary battery.
[0032] In some embodiments, the hydrogen-absorbing material is selected from AB. (5-x) M x Type alloy materials, AB (2-x) M x Type alloy materials, AB (1-x) M x Alloy materials and A2B (1-x) M xAt least one of the following alloy materials. Wherein, A is selected from at least one of Ti, Zr, Ca, Mg, V, Nb, lanthanide rare earth elements, and actinide rare earth elements; B is selected from at least one of Fe, Co, Ni, Cr, Cu, Mn, and Al; M is selected from at least one metallic element different from A and different from B; 0 ≤ x < 0.4. For example, x can be 0, 0.1, 0.2, 0.25, 0.3, 0.35, 0.38, etc. By controlling the stoichiometric ratio of the doping element M in the chemical formula of the hydrogen-absorbing material, it is beneficial to improve the oxidation resistance and stability of the hydrogen-absorbing material, thereby extending the service life of the hydrogen-absorbing functional layer 120, and further improving the service life of the secondary battery using the separator 100.
[0033] In some embodiments, A is selected from at least one of La, Ti and Mg, B is selected from at least one of Ni, Mn and Fe, and M is selected from at least one of Al, Ni and Cr.
[0034] In some embodiments, the hydrogen-absorbing material is selected from LaNi5, TiMn, TiFe, and LaNi. 4.7 Al 0.3 TiMn 1.82 Ni 0.18 TiFe 0.9 Ni 0.1 and Mg2Ni 0.86 Cr 0.14 At least one of them.
[0035] In some embodiments, the shell material is at least one of a non-conductive aluminum metal compound and an ion-conducting material.
[0036] In some embodiments, the shell material is selected from Al2O3, β-Al2O3, γ-AlOOH, and Na3Zr2Si2PO4. 12 At least one of NaTi2(PO4)3, Na3V2(PO4)3 and Na3V2(PO4)2F3.
[0037] In some embodiments, the mass ratio of the shell material to the hydrogen-absorbing material in the modified hydrogen-absorbing material is (0.05 to 0.4):1, for example, it can be 0.05:1, 0.1:1, 0.2:1, 0.25:1, 0.3:1, 0.4:1, etc. By controlling the mass ratio of the shell material to the hydrogen-absorbing material, it is beneficial for the shell material to fully coat the hydrogen-absorbing material, isolate the hydrogen-absorbing material from the polyolefin-based membrane, thereby reducing the short-circuit risk of the secondary battery using the separator 100 and reducing the self-discharge inside the secondary battery. At the same time, it ensures that the hydrogen-absorbing material fully and promptly absorbs the hydrogen generated during the charging and discharging process of the secondary battery.
[0038] In some embodiments, the D50 particle size of the hydrogen-absorbing material is 0.5 μm to 7 μm, for example, it can be 0.5 μm, 1 μm, 2 μm, 3 μm, 5 μm, 7 μm, etc. By controlling the D50 particle size of the hydrogen-absorbing material within the above range, the particle size distribution of the hydrogen-absorbing material is controlled to be smaller than the thickness of the polyolefin-based membrane, preventing short circuits in the diaphragm 100. At the same time, the hydrogen-absorbing material has a larger specific surface area, thereby increasing the contact area between the hydrogen-absorbing material and hydrogen and improving the hydrogen adsorption effect of the hydrogen-absorbing functional layer 120.
[0039] In some embodiments, the D50 particle size of the shell material is 0.5 μm to 5 μm, for example, it can be 0.5 μm, 1 μm, 2 μm, 2.5 μm, 3 μm, 4 μm, 5 μm, etc. By controlling the D50 particle size of the shell material to match the D50 particle size of the hydrogen-absorbing material, it is beneficial to improve the uniformity of the coating of the shell material on the hydrogen-absorbing material, improve the density of the coating layer formed by the shell material, and facilitate the full contact between the shell material and the hydrogen-absorbing material, thereby improving the bonding strength between the shell material and the hydrogen-absorbing material and thus improving the coating effect of the shell material on the hydrogen-absorbing material.
[0040] In some embodiments, the modified hydrogen-absorbing material may be selected from LaNi5@NZSP, TiMn2@NZSP, TiFe@NZSP, LaNi 4.7 Al 0.3 @NZSP、TiMn 1.82 Ni 0.18 @NZSP、TiFe 0.9 Ni 0.1 @NZSP、Mg2Ni 0.86 Cr 0.14 At least one of @NZSP.
[0041] In some embodiments, the modified hydrogen-absorbing material as described above can be prepared by the following method: The shell material and the hydrogen-absorbing material are mixed at a mass ratio to obtain a mixture; the mixture is then mixed with an aqueous solution of polyvinylpyrrolidone (PVP) to obtain a slurry, wherein the mass fraction of PVP in the aqueous solution of PVP is 2%; the slurry is spray-dried to obtain a precursor powder; the precursor powder is calcined at 800°C for 1 hour in a nitrogen atmosphere to obtain a finished product; the finished product is then ground to obtain the modified hydrogen-absorbing material.
[0042] In secondary batteries, such as sodium-ion batteries, during the first charge-discharge and cycle processes, the decomposition of the electrolyte on the surface of the negative electrode, structural changes in the positive electrode active material, and impurity reactions can all lead to gas generation. Hydrogen is one of the main components of this gas. This is especially true in secondary batteries with little or no negative electrode active material, where active metals (such as sodium) are directly deposited on the current collector of the negative electrode. This results in poor interfacial stability and makes it easier for the SEI (Solid Electrolyte Interphase) film to continuously break and repair itself, as well as for electrolyte decomposition. Consequently, it is easier to generate reducing hydrogen gas during charge-discharge cycles. The separator 100 provided by this invention, through the setting of a hydrogen absorption functional layer 120, and the use of a modified hydrogen absorption material with a shell material coated on the surface of the hydrogen absorption material in the hydrogen absorption functional layer 120, effectively absorbs hydrogen during the charge-discharge cycle when the separator 100 is applied to a secondary battery. This prevents the gas from accumulating inside the secondary battery, while the shell material avoids electrical contact between the hydrogen absorption material and the polyolefin base film 110, reducing the risk of short circuits and self-discharge in the secondary battery, effectively improving the safety performance of the secondary battery, delaying the capacity decay of the secondary battery, and improving the cycle life of the secondary battery. It also has high application potential in secondary batteries with few or no negative electrode active materials.
[0043] In a second aspect, the present invention provides a secondary battery, comprising: a separator 100 as described above.
[0044] The secondary battery provided by this invention utilizes the separator 100 as described above, and takes advantage of the hydrogen absorption functional layer 120 within the separator 100. The hydrogen absorption functional layer 120 uses a modified hydrogen absorption material with a shell material coated on its surface. When the separator 100 is applied to the secondary battery, it effectively absorbs hydrogen during charge-discharge cycles, preventing gas accumulation inside the secondary battery. Simultaneously, the shell material prevents electrical contact between the hydrogen absorption material and the polyolefin base film 110, reducing the risk of short circuits and self-discharge in the secondary battery. This effectively improves the safety performance of the secondary battery, slows down capacity decay, and extends its cycle life.
[0045] In some embodiments, the secondary battery further includes a positive electrode and a negative electrode, and the separator 100 is disposed between the positive electrode and the negative electrode.
[0046] In some embodiments, the secondary battery is a sodium-ion battery.
[0047] The technical solution of the present invention will be further described in detail below with reference to specific embodiments.
[0048] Example 1 The diaphragm provided in this embodiment is prepared by the following method: S1. Preparation of modified hydrogen-absorbing material: The shell material NZSP (Na3Zr2Si2PO4) is prepared. 12 The hydrogen-absorbing material LaNi5 was mixed with the hydrogen-absorbing material LaNi5 at a mass ratio of 1:10 and mixed evenly to obtain a mixture. The mixture was then mixed with an aqueous solution of polyvinylpyrrolidone (PVP) and stirred evenly to obtain a slurry (solid content 32.5%). The mass fraction of PVP in the aqueous solution of polyvinylpyrrolidone (PVP) was 2%. The slurry was spray-dried (inlet temperature controlled at 180℃, outlet temperature 90℃) to obtain precursor powder. The precursor powder was calcined at 800℃ for 1 hour in a nitrogen atmosphere to obtain the finished product. The finished product was ground to obtain the modified hydrogen-absorbing material LaNi5@NZSP.
[0049] S2. Preparation of the diaphragm: The modified hydrogen-absorbing material and PVDF (polyvinylidene fluoride) powder were uniformly mixed at a mass ratio of 9:1, and NMP (N-methyl-2-pyrrolidone) was added and stirred evenly to form a hydrogen-absorbing functional layer slurry. The hydrogen-absorbing functional layer slurry was coated onto one side of a PE (polyethylene) base film by gravure coating. The thickness of the polyethylene base film was 12 micrometers. After drying in an oven at 95℃ and 6m / min, the diaphragm was obtained. The thickness of the hydrogen-absorbing functional layer in the diaphragm was 2.4μm.
[0050] Examples 2 to 5 Examples 2 to 5 are similar to Example 1, except that in step S1, the D50 particle size of the hydrogen-absorbing material is adjusted so that the D50 particle sizes of the hydrogen-absorbing material in the obtained modified hydrogen-absorbing material are 0.5 μm, 1 μm, 5 μm, and 7 μm, respectively.
[0051] Examples 6 to 8 Examples 6 to 8 are similar to Example 1, except that in step S1, the D50 particle size of the shell material is adjusted so that the D50 particle size of the shell material in the obtained modified hydrogen absorption material is 0.5 μm, 3 μm, and 5 μm, respectively.
[0052] Examples 9 to 11 Examples 9 to 11 are similar to Example 1, except that in step S1, the mass ratio of the shell material to the hydrogen-absorbing material in the modified hydrogen-absorbing material is 0.05:1, 0.2:1, and 0.4:1, respectively.
[0053] Examples 12 to 17 Examples 12 to 17 are similar to Example 1, except that in step S1, the hydrogen-absorbing material is replaced with NaTi2(PO4)3(NTP), Na3V2(PO4)3(NVP), Na3V2(PO4)2F3(NVPF), β-Al2O3, Al2O3, and γ-AlOOH, respectively.
[0054] Examples 18 to 22 Examples 18 to 22 are similar to Example 1, except that in step S2, the mass ratio of the modified hydrogen-absorbing material to PVDF is adjusted to 1:1, 3:1, 4:1, 95:5, and 99:1, respectively, and the parameters of the gravure coating are adjusted to keep the thickness ratio of the hydrogen-absorbing functional layer to the PE base film unchanged.
[0055] Examples 23 to 25 Examples 23 to 25 are similar to Example 1, except that in step S2, the parameters of the gravure coating are adjusted to maintain the thickness ratio of the hydrogen absorption functional layer to the PE base film at 0.1:1, 0.6:1, and 1:1, respectively.
[0056] Examples 26 to 31 Examples 26 to 31 are similar to Example 1, except that in step S1, the modified hydrogen-absorbing material is replaced with TiMn2@NZSP, TiFe@NZSP, and LaNi, respectively. 4.7 Al 0.3 @NZSP、TiMn 1.82 Ni 0.18 @NZSP、TiFe 0.9 Ni 0.1 @NZSP、Mg2Ni 0.86 Cr 0.14 @NZSP.
[0057] Examples 32 to 33 Examples 32 and 33 are similar to Example 1, except that in step S2, Example 32 uses a polypropylene (PP) base film with a thickness of 14 μm, and Example 33 uses a PE / PP composite base film formed by sequentially stacking PP base film, PE base film and PP base film, with the PP base film having a thickness of 2 μm and the PE base film having a thickness of 10 μm.
[0058] Examples 34 to 37 Examples 34 to 37 are similar to Example 1, except that in step S2, the PE base films used are 5μm, 10μm, 20μm, and 25μm, respectively.
[0059] Example 38 Example 38 is similar to Example 1, except that in step S2, the hydrogen absorption functional layer slurry is coated on both sides of the PE base film by gravure coating, and the thickness of the hydrogen absorption functional layer on one side of the resulting diaphragm is 1.2 μm.
[0060] Comparative Example 1 This comparative example uses the same PE base film as the separator as in Example 1.
[0061] Comparative Example 2 This comparative example is similar to Example 1, except that step S1 is omitted. In step S2, hydrogen-absorbing material LaNi5 and PVDF (polyvinylidene fluoride) powder are mixed uniformly at a mass ratio of 9:1, and then NMP (N-methyl-2-pyrrolidone) is added and stirred evenly to form a hydrogen-absorbing functional layer slurry.
[0062] Comparative Example 3 This comparative example is similar to Example 1, except that in step S1, the D50 particle size of the hydrogen-absorbing material is 0.3 μm.
[0063] Comparative Example 4 This comparative example is similar to Example 1, except that in step S1, the D50 particle size of the hydrogen-absorbing material is 8 μm.
[0064] Comparative Example 5 This comparative example is similar to Example 1, except that in step S1, the shell material is NZSP (Na3Zr2Si2PO4). 12 It is mixed with hydrogen-absorbing material LaNi5 at a mass ratio of 0.03:1.
[0065] Comparative Example 6 This comparative example is similar to Example 1, except that in step S1, the shell material is NZSP (Na3Zr2Si2PO4). 12 It is mixed with hydrogen-absorbing material LaNi5 at a mass ratio of 0.5:1.
[0066] Comparative Example 7 This comparative example is similar to Example 1, except that in step S2, the mass ratio of the modified hydrogen-absorbing material to PVDF is 4:6.
[0067] Comparative Example 8 This comparative example is similar to Example 1, except that in step S2, the ratio of the thickness of the hydrogen absorption functional layer of the obtained separator to the thickness of the PE base film is 0.05:1.
[0068] Comparative Example 9 This comparative example is similar to Example 1, except that in step S2, the ratio of the thickness of the hydrogen absorption functional layer of the obtained separator to the thickness of the PE base film is 1.1:1.
[0069] The parameters of the diaphragms obtained in the above embodiments and comparative examples are shown in Table 1.
[0070] Table 1. Diaphragm parameters of the examples and comparative examples Modified hydrogen absorption materials Hydrogen-absorbing material particle size D50 (μm) Mass fraction of modified hydrogen-absorbing material in hydrogen-absorbing functional layer The ratio of the total thickness of the hydrogen absorption functional layer to the thickness of the base film Shell material particle size D50 (μm) Mass ratio of shell material to hydrogen-absorbing material Example 1 <![CDATA[LaNi5@NZSP]]> 3 90% 0.2 1 0.1 Example 2 <![CDATA[LaNi5@NZSP]]> 0.5 90% 0.2 1 0.1 Example 3 <![CDATA[LaNi5@NZSP]]> 1 90% 0.2 1 0.1 Example 4 <![CDATA[LaNi5@NZSP]]> 5 90% 0.2 1 0.1 Example 5 <![CDATA[LaNi5@NZSP]]> 7 90% 0.2 1 0.1 Example 6 <![CDATA[LaNi5@NZSP]]> 3 90% 0.2 0.5 0.1 Example 7 <![CDATA[LaNi5@NZSP]]> 3 90% 0.2 3 0.1 Example 8 <![CDATA[LaNi5@NZSP]]> 3 90% 0.2 5 0.1 Example 9 <![CDATA[LaNi5@NZSP]]> 3 90% 0.2 1 0.05 Example 10 <![CDATA[LaNi5@NZSP]]> 3 90% 0.2 1 0.2 Example 11 <![CDATA[LaNi5@NZSP]]> 3 90% 0.2 1 0.4 Example 12 <![CDATA[LaNi5@NTP]]> 3 90% 0.2 1 0.1 Example 13 <![CDATA[LaNi5@NVP]]> 3 90% 0.2 1 0.1 Example 14 <![CDATA[LaNi5@NVPF]]> 3 90% 0.2 1 0.1 Example 15 <![CDATA[LaNi5@β-Al2O3]]> 3 90% 0.2 1 0.1 Example 16 <![CDATA[LaNi5@Al2O3]]> 3 90% 0.2 1 0.1 Example 17 <![CDATA[LaNi5@γ-AlOOH]]> 3 90% 0.2 1 0.1 Example 18 <![CDATA[LaNi5@NZSP]]> 3 50% 0.2 1 0.1 Example 19 <![CDATA[LaNi5@NZSP]]> 3 75% 0.2 1 0.1 Example 20 <![CDATA[LaNi5@NZSP]]> 3 80% 0.2 1 0.1 Example 21 <![CDATA[LaNi5@NZSP]]> 3 95% 0.2 1 0.1 Example 22 <![CDATA[LaNi5@NZSP]]> 3 99% 0.2 1 0.1 Example 23 <![CDATA[LaNi5@NZSP]]> 3 90% 0.1 1 0.1 Example 24 <![CDATA[LaNi5@NZSP]]> 3 90% 0.6 1 0.1 Example 25 <![CDATA[LaNi5@NZSP]]> 3 90% 1 1 0.1 Example 26 <![CDATA[TiMn2@NZSP]]> 3 90% 0.2 1 0.1 Example 27 TiFe@NZSP 3 90% 0.2 1 0.1 Example 28 <![CDATA[LaNi 4.7 To the 0.3 @NZSP]]> 3 90% 0.2 1 0.1 Example 29 <![CDATA[TiMn 1.82 Ni 0.18 @NZSP]]> 3 90% 0.2 1 0.1 Example 30 <![CDATA[TiFe 0.9 Ni 0.1 @NZSP]]> 3 90% 0.2 1 0.1 Example 31 <![CDATA[Mg2Ni 0.86 Cr 0.14 @NZSP]]> 3 90% 0.2 1 0.1 Example 32 <![CDATA[LaNi5@NZSP]]> 3 90% 0.2 1 0.1 Example 33 <![CDATA[LaNi5@NZSP]]> 3 90% 0.2 1 0.1 Example 34 <![CDATA[LaNi5@NZSP]]> 3 90% 0.2 1 0.1 Example 35 <![CDATA[LaNi5@NZSP]]> 3 90% 0.2 1 0.1 Example 36 <![CDATA[LaNi5@NZSP]]> 3 90% 0.2 1 0.1 Example 37 <![CDATA[LaNi5@NZSP]]> 3 90% 0.2 1 0.1 Example 38 <![CDATA[LaNi5@NZSP]]> 3 90% 0.1 on one side 1 0.1 Comparative Example 1 / / / / / 0.1 Comparative Example 2 <![CDATA[LaNi5]]> 3 90% 0.2 / 0.1 Comparative Example 3 <![CDATA[LaNi5@NZSP]]> 0.3 90% 0.2 1 0.1 Comparative Example 4 <![CDATA[LaNi5@NZSP]]> 8 90% 0.2 1 0.1 Comparative Example 5 <![CDATA[LaNi5@NZSP]]> 3 90% 0.2 1 0.03 Comparative Example 6 <![CDATA[LaNi5@NZSP]]> 3 90% 0.2 1 0.5 Comparative Example 7 <![CDATA[LaNi5@NZSP]]> 3 40% 0.2 1 0.1 Comparative Example 8 <![CDATA[LaNi5@NZSP]]> 3 90% 0.05 1 0.1 Comparative Example 9 <![CDATA[LaNi5@NZSP]]> 3 90% 1.1 1 0.1 The separators provided in the above embodiments and comparative examples were assembled to obtain pouch batteries, and the self-discharge rate (k-value) after 7 days at room temperature, capacity retention rate after 200 cycles at room temperature, and gas generation rate after 200 cycles at room temperature were tested. The results are shown in Table 2. The assembly method of the pouch battery is as follows:
[0071] Preparation of the positive electrode sheet: Polyanionic positive electrode active material Na4Fe3(PO4)P2O7 (NFPP), conductive carbon black SP, and binder PVDF were mixed evenly at a mass ratio of 94:2.7:3. NMP was then added and stirred to form a positive electrode slurry. This slurry was coated onto one side of a 15μm aluminum foil. After drying and rolling, a single-sided positive electrode sheet was obtained with a compacted density of 2.1 g / cm³ and a coated surface density of 192 g / m³. 2 The prepared single-sided electrode sheet is cut into positive electrode sheets of 5.6cm×6.8cm for later use.
[0072] Preparation of the negative electrode sheet: Hard carbon, conductive carbon black, and dispersant sodium carboxymethyl cellulose (CMC) were mixed evenly at a mass ratio of 93.5:2.5:1.3. Deionized water was added and stirred to form a slurry. SBR (styrene-butadiene rubber) binder was then added (SBR to hard carbon mass ratio of 2.7:93.5), and the mixture was stirred to form a negative electrode slurry. After coating one side of aluminum foil, the slurry was dried and rolled to obtain a single-sided negative electrode sheet with a compaction density of 0.95 g / cm³. 3 The density of the coating surface is 31 g / m² 2 The prepared single-sided electrode sheet is cut into negative electrode sheets of 6cm×7.2cm for later use.
[0073] Soft-pack battery assembly: The positive electrode, negative electrode, and separator of the examples and comparative examples are used to make a single-layer stacked soft-pack battery. After baking to remove water and adding electrolyte (electrolyte: 1 mol / L NaPF6; solvent: propylene carbonate PC, diethyl carbonate DEC, ethylene carbonate EC, the volume ratio of the three solvents is PC:DEC:EC=2:6:2), the resulting electrolyte-filled cell is left to stand at 45°C for 24 hours for later use.
[0074] Battery formation and capacity testing: After the liquid filling is completed, the soft-pack cell is placed at 45°C for negative pressure formation. After the formation is completed, the cell is subjected to double sealing treatment. Then, the cell is subjected to capacity testing at room temperature within the voltage range of 1.5V-3.4V to adjust the state of charge (SOC) of the cell to 50% to obtain the soft-pack battery to be tested.
[0075] The self-discharge rate k value at room temperature (25℃±2℃) for 7 days was tested as follows: The open circuit voltage of the above soft pack battery on day 0 was measured as V0. After being left to stand at room temperature for 7 days, the open circuit voltage of the above soft pack battery was measured as V7. Then the k value is (V0-V7) / 7, and the unit is mV / day.
[0076] The capacity retention rate after 200 cycles at room temperature (25℃±2℃) was measured as follows: The voltage window was from 2V to 3.3V. Three charge-discharge cycles were performed at a charge rate of 0.33C and a discharge rate of 0.33C. The discharge capacity of the third cycle was taken as C0. 200 charge-discharge cycles were then performed using C0 as the charge and discharge rate, and the discharge capacity of the 200th cycle was obtained as C0. 200 The capacity retention rate after 200 cycles at room temperature is (C). 200 -C0) / C0×100%.
[0077] The gas generation rate after 200 cycles at room temperature (25℃±2℃) was measured as follows: Before the capacity retention test after 200 cycles, the initial volume V1 of the pouch battery was obtained at room temperature using the water displacement method, and the volume V2 of the pouch battery was obtained at room temperature using the water displacement method after the 200th cycle. The gas generation rate after 200 cycles at room temperature was (V2-V1) / V1×100%.
[0078] Table 2 shows the performance test results of the pouch cells using the separators from the examples and comparative examples. Self-discharge rate k-value of battery cell after 7 days of static storage at room temperature (mV / day) Capacity retention rate after 200 cycles % Gas production rate % after 200 cycles Example 1 1.47 93.1 5.3 Example 2 1.22 91.6 6.2 Example 3 1.57 91.9 6.9 Example 4 1.52 90.8 7.6 Example 5 1.39 90.7 9.4 Example 6 1.16 91.1 5.1 Example 7 1.73 90.9 6.4 Example 8 1.77 92.1 7.3 Example 9 1.62 92.6 5.8 Example 10 1.51 90.8 6.6 Example 11 1.68 91.3 7.7 Example 12 1.45 90.4 9.2 Example 13 1.33 91.7 8.6 Example 14 1.19 92.5 5.4 Example 15 1.36 90.9 8.0 Example 16 1.85 91.3 9.7 Example 17 1.91 87.8 11.3 Example 18 1.58 90.5 8.9 Example 19 1.62 91.7 5.1 Example 20 1.50 91.9 4.9 Example 21 1.45 92.0 4.7 Example 22 1.66 92.3 4.6 Example 23 1.29 93.4 7.1 Example 24 1.41 89.5 5.0 Example 25 1.80 88.3 4.3 Example 26 1.75 90.4 9.2 Example 27 1.34 91.7 8.6 Example 28 1.66 92.5 5.4 Example 29 1.85 90.9 8.0 Example 30 1.37 91.3 8.7 Example 31 1.24 87.8 9.3 Example 32 1.55 91.5 6.1 Example 33 1.63 91.8 6.6 Example 34 1.48 90.2 7.4 Example 35 1.29 90.8 8.3 Example 36 1.26 92.3 9.6 Example 37 1.13 90.6 10.2 Example 38 1.36 92.4 4.2 Comparative Example 1 1.42 58.7 42.6 Comparative Example 2 10.73 92.2 5.5 Comparative Example 3 6.22 90.1 5.0 Comparative Example 4 5.49 89.2 23.7 Comparative Example 5 8.51 83.6 6.3 Comparative Example 6 1.44 91.1 31.8 Comparative Example 7 2.07 87.2 13.7 Comparative Example 8 8.73 76.3 6.4 Comparative Example 9 1.85 72.9 9.8 As can be seen from the comparison of the above embodiments with Comparative Example 1 in Table 2, the separator provided by the present invention, through the setting of the hydrogen absorption functional layer, effectively absorbs hydrogen during the charge-discharge cycle when the separator is applied to the secondary battery, preventing the gas from accumulating inside the secondary battery, delaying the capacity decay of the secondary battery, and improving the cycle life of the secondary battery.
[0079] A comparison of the results of the above embodiments and Comparative Example 2 in Table 2 shows that the modified hydrogen-absorbing material obtained by coating the hydrogen-absorbing material with a shell material in the hydrogen-absorbing functional layer of the separator provided by the present invention avoids electrical contact between the hydrogen-absorbing material and the polyolefin base film through the shell material, effectively reducing the self-discharge of the secondary battery, reducing the short-circuit risk of the secondary battery, further delaying the capacity decay of the secondary battery, and improving the cycle life of the secondary battery.
[0080] A comparison of the results of Examples 1 to 5 with those of Comparative Examples 3 and 4 in Table 2 shows that controlling the D50 particle size of the hydrogen absorption material to be between 0.5 μm and 7 μm helps to prevent short circuits in the membrane and enhances the hydrogen adsorption effect of the hydrogen absorption functional layer.
[0081] A comparison of the results in Table 2 of Examples 1, 9 to 11 with Comparative Examples 5 and 6 shows that by controlling the mass ratio of shell material to hydrogen-absorbing material to (0.05 to 0.4):1, it is more beneficial to obtain a separator that can both reduce the internal self-discharge of the secondary battery and fully absorb the hydrogen generated by the secondary battery using the hydrogen-absorbing material.
[0082] A comparison of the results of Examples 1, 18 to 22 and Comparative Example 7 in Table 2 shows that by controlling the mass percentage of the modified hydrogen-absorbing material in the hydrogen-absorbing functional layer to be 50% to 99%, preferably 80% to 95%, it is more beneficial to obtain a separator that reduces the internal self-discharge of the secondary battery, effectively absorbs hydrogen when applied to the secondary battery, delays the capacity decay of the secondary battery, and improves the cycle life of the secondary battery.
[0083] A comparison of the results in Table 2 of Examples 1, 23 to 25 with Comparative Examples 8 and 9 shows that by controlling the ratio of the total thickness of the hydrogen absorption functional layer in the separator to the thickness of the polyolefin base film to be (0.1 to 1):1, preferably (0.2 to 0.6):1, it is more beneficial to obtain a separator that can effectively absorb hydrogen generated during the charging and discharging process of the secondary battery, reduce the self-discharge inside the secondary battery, and maintain the ion conduction function.
[0084] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the protection scope of the present invention.
Claims
1. A diaphragm, characterized in that, include: Polyolefin-based films; A hydrogen-absorbing functional layer, wherein the hydrogen-absorbing functional layer is located on at least one side of the polyolefin-based film; The hydrogen absorption functional layer includes a modified hydrogen absorption material, which includes a hydrogen absorption material and a shell material covering the surface of the hydrogen absorption material. The shell material is selected from at least one of aluminum oxides, aluminates, aluminum hydroxides, and ionic conductor materials.
2. The diaphragm as described in claim 1, characterized in that, In the modified hydrogen-absorbing material, the mass ratio of the shell material to the hydrogen-absorbing material is (0.05 to 0.4):1; The shell material has a D50 particle size of 0.5 μm to 5 μm, and the hydrogen-absorbing material has a D50 particle size of 0.5 μm to 7 μm.
3. The diaphragm as described in claim 1, characterized in that, The modified hydrogen-absorbing material has a mass fraction of 50% to 99% in the hydrogen-absorbing functional layer.
4. The diaphragm as described in claim 3, characterized in that, The modified hydrogen-absorbing material has a mass fraction of 80% to 95% in the hydrogen-absorbing functional layer.
5. The diaphragm as described in claim 3, characterized in that, The hydrogen absorption functional layer further includes an adhesive, which is selected from at least one of polyvinylidene fluoride, styrene-butadiene rubber, sodium carboxymethyl cellulose, polyacrylic acid, and waterborne polyurethane.
6. The diaphragm as described in claim 1, characterized in that, The ratio of the total thickness of the hydrogen absorption functional layer to the thickness of the polyolefin base film is (0.1 to 1):
1.
7. The diaphragm as described in claim 1, characterized in that, The total thickness of the polyolefin-based membrane is 5 μm to 25 μm, and the porosity of the polyolefin-based membrane is 30% to 50%.
8. The diaphragm as described in any one of claims 1 to 7, characterized in that, The polyolefin-based membrane is selected from at least one of polyethylene and polypropylene, and the hydrogen-absorbing material is selected from AB. (5-x) M x Type alloy materials, AB (2-x) M x Type alloy materials, AB (1-x) M x Alloy materials and A2B (1-x) M x At least one of the following alloy materials, wherein the shell material is selected from Al2O3, β-Al2O3, γ-AlOOH, Na3Zr2Si2PO4. 12 At least one of NaTi2(PO4)3, Na3V2(PO4)3 and Na3V2(PO4)2F3; Wherein, A is selected from at least one of Ti, Zr, Ca, Mg, V, Nb, lanthanide rare earth elements and actinide rare earth elements, B is selected from at least one of Fe, Co, Ni, Cr, Cu, Mn and Al, M is selected from at least one metallic element that is different from A and different from B, and 0≤x<0.
4.
9. The diaphragm as described in claim 8, characterized in that, The hydrogen-absorbing material is selected from LaNi5, TiMn, TiFe, and LaNi. 4.7 Al 0.3 TiMn 1.82 Ni 0.18 TiFe 0.9 Ni 0.1 and Mg2Ni 0.86 Cr 0.14 At least one of them.
10. A secondary battery, characterized in that, The secondary battery includes a separator as described in any one of claims 1 to 9.