A method, apparatus and lithium-ion battery for preventing multiple electrode layers from being processed
By using an electrostatic sheet and an ion fan to eliminate static electricity during the manufacturing process of lithium-ion battery electrodes, the problem of electrode adhesion was solved, improving stacking efficiency and battery quality.
Patent Information
- Application Number
- CN202611238021.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-14
- Publication Date
- 2026-11-17
AI Technical Summary
In the manufacturing process of lithium-ion batteries, the electrodes are prone to adhesion during stacking, resulting in multiple electrodes, which affects production efficiency and wastes materials. Existing methods have limited effectiveness.
By placing the electrode on a table covered with an electrostatic sheet and using an ion blower to neutralize static electricity, combined with a grounding wire to eliminate static voltage, the static voltage is controlled within a preset range.
It effectively prevents electrode adhesion, improves stacking efficiency, reduces material waste, enhances the utilization rate of internal battery space, simplifies operation, and is compatible with existing production lines.
Smart Images

Figure CN123124186A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of electrode processing, and more particularly to a method, apparatus and lithium-ion battery for preventing multiple electrodes from being processed. Background Technology
[0002] In the manufacturing process of lithium-ion batteries, current technologies for polymer lithium batteries rely on stacking machines. Most stacking machines face significant challenges when picking up and stacking electrode sheets. This is due to the thinness and difficulty in separating the electrode sheets, a problem stemming from the process and material characteristics. The surface of the positive electrode sheet is essentially a smooth, mirror-like structure, with layers tightly bonded together. The addition of static electricity further strengthens the adhesion between the electrode layers, making separation even more difficult. Although an electrode sheet can be picked up each time, there are often excess sheets. The process requires 1 piece per batch, ultimately leading to material waste and wasted battery internal space. Furthermore, the multi-layer calculation and separation process significantly reduces efficiency.
[0003] To address the issue of multiple electrode plates, traditional methods involve interventions such as brushing, ionization, plate shaking, and ultrasonic waves. While each batch of material has a different morphology, these methods have limitations; the multiple-plate phenomenon persists, or the exploratory plate separation process reduces equipment efficiency. Furthermore, material handling during transport can lead to creases and material loss, increasing battery safety risks. These methods only provide temporary relief; finding a simple and effective solution to the multiple-plate problem remains a pressing issue.
[0004] like Figure 3 The diagram illustrates the static electricity elimination principle of an ion fan. The ion fan contains an AC high-voltage generator that produces over 7KV of high voltage. This generator ionizes the air to generate a large number of positive and negative charges, which are then blown out by the fan. This creates an airflow of positive and negative charges that neutralizes the charge on the surface of objects. When an object's surface carries a negative charge, it attracts positive charges from the airflow; conversely, when an object's surface carries a positive charge, it attracts negative charges from the current. This process neutralizes the static electricity on the object's surface, achieving the purpose of eliminating static electricity. Summary of the Invention
[0005] The purpose of this invention is to provide a method, device and lithium-ion battery for preventing multiple electrode plates from being processed. The electrode plates are placed on a table and blown by an ion fan to neutralize the static ions on the electrode plates. A grounded electrostatic pad is placed on the table to reduce the static voltage on the electrode plates.
[0006] To solve the above technical problems, the following technical solution is adopted:
[0007] In a first aspect, the present invention provides a method for preventing multiple electrodes from being processed, comprising the following steps:
[0008] Several electrode sheets are stacked and collected into a material box, and the material box is placed on a table with an electrostatic coating.
[0009] The work surface is grounded via a grounding wire, and the electrostatic insulation is grounded via a grounding wire.
[0010] Turn on the ion fan on the table to blow air into the material box, and let the electrode plates in the material box stand for the preset time.
[0011] Optionally, the preset duration is 15-25 minutes.
[0012] Optionally, the air outlet of the ion fan is aligned with the height of the material box.
[0013] Optionally, after the electrode plates in the material box have been left to stand for a preset time, the electrostatic voltage on the surface of the electrode plates is measured by an electrostatic tester. If the electrostatic voltage value is greater than the preset value, the plates are left to stand for an extended period.
[0014] Optionally, the preset value of the electrostatic voltage is 50V.
[0015] Optionally, before stacking and collecting several electrode sheets into a material box, the electrode roll is vacuum baked to obtain a dry electrode roll, and then the dry electrode roll is cut into several electrode sheets by a punching machine.
[0016] In a second aspect, the present invention provides an electrode processing apparatus, which is used in the electrode anti-multiple-sheet method described in the first aspect, and the processing apparatus includes a workbench, an electrostatic sheet, and an ion fan.
[0017] The electrostatic sheet is laid on the surface of the workbench, and the electrostatic sheet is grounded through a grounding wire one, while the surface of the workbench is grounded through a grounding wire two.
[0018] The ion fan is installed on the table.
[0019] Thirdly, the present invention provides a lithium-ion battery, wherein the electrode sheets in the lithium-ion battery are obtained by the electrode sheet anti-multiple-sheet treatment method described in the first aspect.
[0020] Compared with the prior art, the beneficial effects achieved by the present invention are as follows:
[0021] The electrode stacking prevention method provided by this invention involves placing the electrode tray on a surface covered with an anti-static sheet and blowing ion air into the tray to remove static electricity from the electrode sheets inside, thus preventing two or more electrode sheets from sticking together during stacking. This method is simple to operate and compatible with existing electrode stacking production lines. Attached Figure Description
[0022] Figure 1This is a schematic diagram of the electrode sheet in a static state in an embodiment of the present invention;
[0023] Figure 2 This is a structural diagram of the processing device in an embodiment of the present invention;
[0024] Figure 3 This is a schematic diagram of the static electricity removal principle of the ion fan of the present invention.
[0025] Explanation of reference numerals in the attached figures:
[0026] 1. Workbench; 2. Electrostatic strip; 3. Grounding wire one; 4. Grounding wire two; 5. Ionizing fan; 6. Material box. Detailed Implementation
[0027] The technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. The following description of at least one exemplary embodiment is merely illustrative and is in no way intended to limit the present invention or its application or use.
[0028] Furthermore, the terms "first," "second," etc., are used for descriptive purposes only and should not be construed as indicating or implying relative importance or implicitly specifying the number of technical features indicated. Therefore, a feature defined with "first," "second," etc., may explicitly or implicitly include one or more of that feature.
[0029] Example 1
[0030] This invention provides a method for preventing multiple electrodes from being processed, comprising the following steps:
[0031] Step 1: After vacuum baking the positive and negative electrode rolls, dry positive and negative electrode rolls are obtained. The positive and negative electrode rolls are then cut into single electrode sheets using a punching machine.
[0032] Step 2: Stack several electrode sheets and collect them into the material box 6, and place the material boxes 6 on the table covered with electrostatic sheet 2;
[0033] Step 3: The tabletop is grounded through a wire, the electrostatic shield 2 is grounded through a wire, and the ion fan 5 is installed on the tabletop;
[0034] Step 4: Turn on the ion fan 5 to blow air into the material box 6, and let the electrode plates in the material box 6 remain still for the preset time.
[0035] The electrode sheet includes a positive electrode sheet and a negative electrode sheet. The positive electrode sheet is formed by positive electrode roll cutting, and the negative electrode sheet is formed by negative electrode roll cutting.
[0036] In step one above, the preparation of the positive electrode sheet is specifically as follows:
[0037] Place the positive electrode roll into a vacuum oven to remove excess moisture. The vacuum oven is set to a temperature of 100℃. The specific baking process and parameters are shown in the table below.
[0038] After baking, the positive electrode rolls undergo a moisture content test. If the moisture content is ≤300ppm, the positive electrode rolls are considered qualified and can proceed to the slicing process.
[0039] Table 1: Vacuum Baking Process Parameters for Positive Electrode Sheets
[0040]
[0041] As shown in Table 1, the heating and baking temperature of the positive electrode roll is 100℃. The baking process consists of 7 steps, from step 1 to step 7, which are performed continuously. Each step corresponds to different times and upper and lower vacuum limits. In the first four steps, the positive electrode roll is heated to 100℃, and a blower is turned on to remove the evaporated water vapor. The last three steps are cooling processes. Slow cooling prevents water vapor from condensing and adhering to the positive electrode roll, ensuring its dryness. After repeated baking, a positive electrode roll with a qualified moisture content is obtained.
[0042] The specific preparation of the negative electrode roll is as follows:
[0043] Place the negative electrode roll into a vacuum oven to remove excess moisture. The vacuum oven is set to a temperature of 80℃, and the specific baking process is shown in the table below.
[0044] After baking, the negative electrode rolls undergo a moisture content test. If the moisture content is ≤100ppm, the negative electrode rolls are considered qualified and can proceed to the slicing process.
[0045] Table 2: Vacuum Baking Process Parameters for Negative Electrode Sheets
[0046]
[0047] As shown in Table 2, the vacuum baking process of the negative electrode roll is similar to that of the positive electrode roll, except that the heating and baking temperature of the negative electrode roll is 80℃.
[0048] After obtaining positive and negative electrode rolls with qualified moisture content, the electrode rolls are formed into several single-piece electrode sheets through stamping. The positive and negative electrode sheets are separately placed into the material box 6, and the material box 6 is placed in an array on the table.
[0049] like Figure 1 As shown, in step three above, the electrostatic skin 2 is grounded through grounding wire 3, and the table surface is grounded through grounding wire 4.
[0050] The dual independent grounding of the work surface and the electrostatic discharge pad 2 eliminates the potential difference between them, achieving redundancy in the electrostatic discharge path and improving the reliability of electrostatic discharge. This prevents residual static electricity from remaining on the work surface after the electrostatic discharge pad 2 has discharged, thus avoiding potential differences between it and the electrode plates on the work surface.
[0051] In step four, the ion fan 5 is installed on one side edge of the table, with the air outlet facing the material box 6. The height of the air outlet of the ion fan 5 is the same as the height of the material box 6. The ion fan 5 is turned on to blow air into the material box 6.
[0052] Steps three and four are used to discharge static electricity from the electrode sheets in the material box 6, preventing multiple electrode sheets from sticking together when they are picked up during the stacking process.
[0053] In this embodiment, the material box 6 is placed on the table for 20 minutes. After 20 minutes of settling, the electrostatic voltage of the electrode plates in each material box 6 is sampled and measured. Specifically, an electrostatic tester is used to measure one electrode plate. When the electrostatic voltage value measured by the electrostatic tester is greater than 50V, it is recorded, and the material box 6 is allowed to continue to be settling while ionizing air is continuously blown onto the material box 6 to control the electrostatic voltage of the electrode plate to not exceed -50V or +50V.
[0054] A lithium-ion battery is formed by stacking an equal number of electrodes that have undergone the above process with electrodes that have not undergone the above process, specifically:
[0055] Example:
[0056] The positive and negative electrode sheets from the 180 PCS electrode sheets are respectively placed into the material box 6. The material box 6 is placed on the table with the electrostatic skin 2 grounded, the electrostatic skin 2 is grounded, the table is grounded, and the ion fan 5 is turned on.
[0057] After the material box 6 was left to stand for 20 minutes, the electrostatic voltage of the electrode plates in the material box 6 was measured to be 42V by the electrostatic detector.
[0058] The material box 6 is loaded into the stacking machine and stacked to form a battery cell.
[0059] The produced battery cell contains 180 electrode pieces, with a sheet coverage rate of 0%.
[0060] Comparative Example 1:
[0061] The positive and negative electrode sheets from the 180 PCS electrode sheets are respectively placed into the material box 6.
[0062] After the material box 6 was left to stand for 20 minutes, the electrostatic voltage of the electrode plates in the material box 6 was measured to be 120V by the electrostatic detector.
[0063] The material box 6 is loaded into the stacking machine and stacked to form a battery cell.
[0064] The produced battery cell contains 157 electrode pieces, with a piece ratio of 15%.
[0065] Comparative Example 2:
[0066] The positive and negative electrode sheets from the 180 PCS electrode sheets are respectively placed into the material box 6.
[0067] After the material box 6 was left to stand for 20 minutes, the electrostatic voltage of the electrode plates in the material box 6 was measured to be 152V by the electrostatic detector.
[0068] The material box 6 is loaded into the stacking machine and stacked to form a battery cell.
[0069] The produced battery cell contains 154 electrode pieces, with a piece ratio of 17%.
[0070] Table 3: Comparison of Conditions and Results for Examples and Comparative Examples
[0071]
[0072] As shown in Table 3, the results of the first condition embodiment indicate that when the worktable is connected to the electrostatic wire and the electrostatic sheath 2 is grounded, and the ionizing air is continuously blown, after standing for 20 minutes, the electrostatic voltage of the electrode sheet in the material box 6 continuously decreases, dropping to 42V. Verification using the stacking machine shows that the wafer loading rate drops to below 0%, demonstrating a very significant effect. The results of the first condition comparison 1 show that when the worktable is not connected to the electrostatic wire and grounded, and there is no ion blowing, although it is left to stand for 20 minutes, the electrostatic voltage is 120V, and verification using the stacking machine shows a wafer loading rate of 15%, with many wafers still present. The results of the first condition comparison 2 show that when the worktable is not connected to the electrostatic wire and grounded, and there is no ion blowing, although it is left to stand for 20 minutes, the electrostatic voltage is 152V, and verification using the stacking machine shows a wafer loading rate of 7%, with many wafers still present. Combining the above data, this method is very effective, controlling the electrostatic voltage to ≤+50V / -50V.
[0073] In the embodiment, when the electrode sheets obtained through static settling, electrostatic grounding, and ionization treatment were stacked, the stripping rate was 0. Comparative Examples 1 and 2 only underwent static settling, resulting in stripping rates of 15% and 17%, respectively. The electrostatic voltage measured after static settling in Comparative Example 1 was 120, and in Comparative Example 2 it was 152. This means that a higher electrostatic value results in a higher stripping rate, and electrostatic discharge affects the stripping bias during electrode stacking. Therefore, the electrostatic voltage of the electrode sheets obtained after static settling, electrostatic grounding, and ionization treatment in this embodiment was 42, which is much lower than the electrostatic values in Comparative Examples 1 and 2, indicating a low stripping rate of 0.
[0074] In this embodiment, after the electrode sheet is left to stand for the above steps, the electrostatic voltage of the electrode sheet is measured to ensure that the electrostatic voltage value is less than 50V, thereby ensuring a low strip ratio during stacking.
[0075] The electrode anti-multiple-sheet treatment method provided in this embodiment effectively reduces the static electricity of the electrode sheets and significantly improves the multiple-sheet effect of stacked electrodes. Compared with existing static elimination methods, there is no risk of electrode sheets being broken, thus improving the quality of the battery. This method is fully compatible with existing stacking production lines, and is low in cost and easy to operate.
[0076] Example 2
[0077] This embodiment provides a processing device for processing electrode sheets, as described in Embodiment 1. It includes a workbench 1, an electrostatic sheet 2, and an ion fan 5. The electrostatic sheet 2 is laid on the surface of the workbench 1, and the surface of the workbench 1 is connected to a grounding busbar via a second grounding wire 4. The electrostatic sheet 2 is also connected to the grounding busbar via a first grounding wire 3.
[0078] like Figure 1 , Figure 2 As shown, a grounding clip is installed at one corner of the electrostatic shield 2. One end of the grounding wire 3 is connected to the grounding clip, and the other end is connected to the grounding busbar. One end of the grounding wire 4 is connected to the table surface, and the other end is connected to the same grounding busbar.
[0079] The ion fan 5 is located at the edge of the tabletop, with its air outlet facing the material box 6 on the tabletop.
[0080] It also includes an electrostatic detector for measuring electrostatic voltage, which detects the electrostatic voltage value on the electrode plates.
[0081] Example 3
[0082] This embodiment provides a lithium-ion battery. The electrode sheets in the lithium-ion battery are obtained using the electrode sheet anti-multiple-sheet treatment method described in Embodiment 1. The resulting electrode sheets can prevent multiple sheets from sticking together during stacking in a stacking machine, ensuring the utilization rate of the internal space of the lithium-ion battery.
[0083] The above description is only a preferred embodiment of the present invention. It should be noted that for those skilled in the art, several improvements and modifications can be made without departing from the technical principles of the present invention, and these improvements and modifications should also be considered within the scope of protection of the present invention.
Claims
1. A method for preventing multiple electrodes from being processed, characterized in that, Includes the following steps: Several electrode sheets are stacked and collected into a material box, and the material box is placed on a table with an electrostatic coating. The work surface is grounded via a grounding wire, and the electrostatic insulation is grounded via a grounding wire. Turn on the ion fan on the table to blow air into the material box, and let the electrode plates in the material box stand for the preset time.
2. The electrode anti-multiple-electrode processing method according to claim 1, characterized in that, The preset duration is 15-25 minutes.
3. The electrode anti-multiple-electrode processing method according to claim 1, characterized in that, The air outlet of the ion fan is aligned with the height of the material box.
4. The electrode anti-multiple-electrode processing method according to claim 1, characterized in that, After the electrode plates in the material box have been left to stand for a preset time, the electrostatic voltage on the surface of the electrode plates is measured by an electrostatic tester. If the electrostatic voltage value is greater than the preset value, the standing time continues.
5. The electrode anti-multiple-electrode processing method according to claim 4, characterized in that, The preset value for the electrostatic voltage is 50V.
6. The electrode anti-multiple-electrode processing method according to claim 1, characterized in that, Before stacking and collecting several electrode sheets into the material box, the electrode rolls are vacuum baked to obtain dry electrode rolls, and then the dry electrode rolls are cut into several electrode sheets by a punching machine.
7. An electrode processing apparatus, characterized in that, The processing device is used in the electrode anti-multiple electrode method according to any one of claims 1-6, and the processing device includes a workbench, an electrostatic sheet and an ion fan; The electrostatic sheet is laid on the surface of the workbench, and the electrostatic sheet is grounded through a grounding wire one, while the surface of the workbench is grounded through a grounding wire two. The ion fan is installed on the table.
8. A lithium-ion battery, characterized in that, The electrode sheets in the lithium-ion battery are obtained by the electrode sheet anti-multiple sheet treatment method according to any one of claims 1-6.