A method for reducing the background oxygen impurity concentration in nitride semiconductor materials
By introducing compressive stress regulating materials and organic source treatment before the growth of nitride semiconductor materials, the problem of high oxygen impurity concentration was solved, improving crystal quality and device performance, especially the electron mobility of GaN-based HEMT materials.
Patent Information
- Application Number
- CN202510614679.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2025-05-13
- Publication Date
- 2026-11-17
AI Technical Summary
Existing technologies struggle to effectively reduce oxygen impurity concentration in nitride semiconductor materials, leading to device performance degradation and reliability issues, especially in GaN-based HEMT materials, where conventional methods negatively impact crystal quality and electron mobility.
Before growing nitride semiconductor materials, an impurity blocking structure is adopted, and stress-modifying materials such as nitrides containing Al and/or B are used to increase the difficulty of oxygen impurity incorporation by introducing compressive stress, and oxygen impurities in the reaction chamber are consumed by combining with oxygen through an organic source.
Without affecting crystal quality, the oxygen impurity concentration is significantly reduced, thereby improving crystal quality and electron mobility, and enhancing device performance and reliability.
Smart Images

Figure CN123124376A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of semiconductor technology, and specifically relates to a method for reducing the background impurity concentration of oxygen in nitride semiconductor materials. Background Technology
[0002] Third-generation semiconductor materials, such as gallium nitride (GaN), possess excellent properties such as direct wide bandgap, good chemical stability, and strong radiation resistance, and are widely used in the fabrication of semiconductor lasers, light-emitting diodes, power switches, and other devices. Due to its spontaneous polarization and piezoelectric polarization effects, a high-density, high-electron-mobility two-dimensional electron gas can be formed between wurtzite GaN and AlGaN, which can be used to fabricate high-electron-mobility transistors (HEMTs), showing broad application prospects in fields such as fast charging for mobile phones, new energy vehicles, big data centers, and radar communications.
[0003] However, the epitaxial substrates used for the epitaxial growth of nitride semiconductor materials, such as GaN-based materials, often have a native oxide layer. Furthermore, during the epitaxial fabrication process, the reaction chamber environment, the carrier gas used for epitaxial growth, and the precursors such as the metal-organic source (~1 ppm) inevitably contain oxygen. This leads to the unintentional incorporation of oxygen impurities during the epitaxial growth of nitride semiconductor materials. Taking nitrogen-polar GaN semiconductor materials with highly reactive surface chemistry as an example, due to the higher dangling bond density of Ga atoms on the surface (three times that of gallium-polar GaN materials), its ability to adsorb oxygen impurities is stronger, resulting in an internal oxygen impurity concentration that is 1-2 orders of magnitude higher than that of gallium-polar GaN materials. Since oxygen impurities in GaN materials often occupy nitrogen atom lattice sites (O... N Therefore, Mg-doped p-type GaN exhibits donor-type impurities, resulting in a high background carrier concentration in GaN materials. This leads to problems such as large leakage current, severe RF loss, and inability to turn off HEMT devices, seriously affecting device performance. Furthermore, for Mg-doped p-type GaN, donor-type oxygen impurities compensate for Mg acceptor doping, significantly reducing the hole concentration in pGaN, leading to increased resistivity and even inversion.
[0004] To mitigate the adverse effects of unintentional oxygen impurities, GaN-based HEMT materials typically require high-concentration acceptor doping of GaN before the growth of the heterojunction electron channel to compensate for oxygen donor impurities, such as acceptor doping with Fe and C. However, the deep-level traps generated by Fe and C doping can capture charge carriers in the heterojunction channel, causing severe current collapse during device operation and affecting device performance and reliability.
[0005] Taking GaN materials as an example, to reduce the concentration of unintentional oxygen impurities in GaN materials, existing technologies generally employ methods such as altering the growth conditions of the GaN / AlGaN layer, including lowering the growth temperature, reducing the growth rate, and increasing the V / III ratio during growth. However, methods that achieve low unintentional oxygen impurity concentrations by changing growth conditions have significant limitations. For instance, D. Koleske et al. reported in their paper (Journal of Crystal Growth, 242, 55-69, 2002) that lowering the GaN growth temperature can reduce oxygen impurity incorporation, but it leads to an increase in C impurity concentration, thereby reducing crystal growth quality. Similarly, M. Mesrine et al. reported in their paper (Appl. Phys. Lett. 72, 350-352, 1998) that lowering the growth temperature reduces ammonia cracking efficiency and the effective V / III ratio, making it difficult to further reduce unintentional oxygen impurity incorporation. Furthermore, lowering the growth temperature weakens the migration ability of surface-adsorbed atoms, making it difficult for atoms to migrate to the step edges for growth. This affects the step flow growth mode, which in turn affects the steepness of the heterojunction interface and enhances electron scattering, leading to a decrease in electron mobility. Existing technology CN114758948A removes oxygen impurities from the substrate surface by introducing Ga / high-temperature volatilization. However, because silicon substrates react with Ga, and NH3 is easily generated in MOCVD and other equipment, introducing a Ga source easily leads to the direct formation of GaN, making it difficult to achieve the purpose of removing oxygen impurities. Therefore, the application of this method in silicon substrates and MOCVD equipment is limited.
[0006] It is evident that reducing the incorporation of unintentional oxygen impurities in nitride semiconductor materials to achieve high-quality, high-resistivity nitride semiconductor materials has become an urgent need for the development of semiconductor devices, especially GaN-based HEMT materials and devices. Summary of the Invention
[0007] To solve all or part of the above-mentioned technical problems, the present invention provides the following technical solutions:
[0008] A first aspect of the present invention is to provide a method for reducing the background impurity concentration of oxygen in a nitride semiconductor material, comprising:
[0009] An impurity barrier structure is grown on a substrate within a reaction chamber, the impurity barrier structure being made of a stress-regulating material.
[0010] Nitride semiconductor material is grown on the impurity barrier structure;
[0011] The lattice constant of the stress-regulating material contained in the impurity barrier structure is smaller than that of the nitride semiconductor material, so that the subsequently grown nitride semiconductor material is under compressive stress.
[0012] The stress-modulating material with a smaller lattice constant in the impurity barrier structure can introduce compressive stress during the subsequent growth of nitride semiconductor materials with a larger lattice constant, thereby utilizing compressive stress to increase the number of oxygen incorporation sites into the nitrogen lattice (O). N The formation energy of oxygen impurities makes it more difficult for oxygen impurities to be incorporated into nitride semiconductor materials, thereby reducing the concentration of unintentional oxygen impurities and the background carrier concentration.
[0013] Existing methods for reducing unintentional oxygen impurity concentration by altering growth conditions often lead to decreased epitaxial layer crystal quality and surface roughness. The method provided by this invention reduces the background oxygen concentration without affecting the surface and crystal quality of the nitride semiconductor material layer. The impurity blocking structure establishes compressive stress during subsequent growth of nitride semiconductor materials with high lattice constants, promoting dislocation bending and effectively improving crystal quality while reducing dislocation density.
[0014] In some embodiments, the stress-modulating material includes Al-containing nitrides and / or B-containing nitrides. On one hand, these materials can reduce the concentration of unintentional oxygen impurities by introducing compressive stress. On the other hand, Al and B are strong oxygen-binding elements, and the Al- and / or B-containing precursors introduced during growth have a strong binding capacity with oxygen impurities, thereby consuming oxygen impurities in the environment during growth and further reducing the concentration of unintentional oxygen impurities. Based on the synergistic effect of these two aspects, the background oxygen concentration in the nitride semiconductor material grown by this method is significantly reduced.
[0015] Furthermore, the Al-containing nitride includes one or more combinations of AlN, AlGaN, AlInN, AlInGaN, and BAlN.
[0016] Furthermore, the B-containing nitride includes one or a combination of BN, BGaN, BInN, and BInGaN.
[0017] In some embodiments, the impurity blocking structure includes a first Al-containing nitride layer.
[0018] Furthermore, the thickness of the first Al-containing nitride layer is 1-200 nm.
[0019] In some embodiments, the method specifically includes:
[0020] S1. Place the substrate in the reaction chamber and grow the first Al-nitride-containing layer on the substrate;
[0021] S2. A nitride semiconductor material layer is grown on the first Al-containing nitride layer. The first Al-containing nitride layer causes the grown nitride semiconductor material layer to be under compressive stress.
[0022] Furthermore, step S1 specifically includes: growing the first Al-containing nitride layer at 900-1350℃ and 50-400mbar.
[0023] Furthermore, step S2 may include, for example, growing a nitride semiconductor material layer at 800-1350°C and 50-600 mbar.
[0024] In some embodiments, the method further includes:
[0025] S3. Repeat steps S1-S2 at least once in a loop;
[0026] S4. At least one more nitride semiconductor material layer is grown on the nitride semiconductor material layer grown in the last step S2. The nitride semiconductor material layer obtained in step S4 is also under compressive stress.
[0027] Multiple cycles can provide stronger compressive stress and achieve a better reduction in oxygen impurity concentration.
[0028] Furthermore, step S4 may include, for example, growing at least one more nitride semiconductor material layer on the nitride semiconductor material layer grown in the last step S2 under conditions of 800-1350°C and 50-600 mbar.
[0029] In some embodiments, the impurity blocking structure further includes a second Al-nitride layer, the second Al-nitride layer being made of a different material than the first Al-nitride layer. The first and second Al-nitride layers are sequentially arranged in a direction away from the substrate. By setting the first and second Al-nitride layers with different materials, the compressive stress can be further enhanced, resulting in a better reduction effect on oxygen impurity concentration.
[0030] In some preferred embodiments, the first Al-nitride layer is an AlN layer and the second Al-nitride layer is an AlGaN layer, wherein the nitride semiconductor material includes GaN. In this case, the second Al-nitride layer not only enhances compressive stress but also acts as a buffer layer to reduce lattice mismatch between the AlN layer and GaN, thereby preventing the subsequent GaN from transforming into a three-dimensional island growth mode.
[0031] Furthermore, the thickness of the second Al-containing nitride layer is 1-200 nm.
[0032] In some embodiments, the method specifically includes:
[0033] S1. Place the substrate in the reaction chamber and grow an impurity barrier structure on the substrate. Step S1 includes S11 and S12:
[0034] S11. The first Al-nitride-containing layer is grown on the substrate;
[0035] S12. Grow a second Al-containing nitride layer on the first Al-containing nitride layer;
[0036] S2. A nitride semiconductor material layer is grown on the second Al-containing nitride layer.
[0037] Furthermore, step S11 specifically includes: growing the first Al-containing nitride layer under pressure conditions of 900-1350℃ and 50-400mbar.
[0038] Furthermore, step S12 specifically includes: growing the second Al-containing nitride layer under pressure conditions of 800-1350℃ and 50-600mbar.
[0039] Furthermore, step S2 may include, for example, growing a nitride semiconductor material layer at 800-1350°C and 50-600 mbar.
[0040] In some embodiments, the method further includes:
[0041] S3. Repeat steps S1 to S2 at least once;
[0042] S4. Grow at least one more nitride semiconductor material layer on the nitride semiconductor material layer grown in the last execution step S2.
[0043] Furthermore, step S4 may include, for example, growing at least one more nitride semiconductor material layer on the nitride semiconductor material layer grown in the last execution of step S2 under conditions of 800-1350°C and 50-600 mbar.
[0044] In the aforementioned step of growing the nitride semiconductor material layer, any epitaxial growth process of semiconductor materials known in the art can be employed, and the present invention does not impose any particular limitation thereon. One advantage of the method provided by the present invention is that it does not require reducing the unintentional doping concentration by changing the growth process of the nitride semiconductor material layer. Therefore, the process parameters for growing the nitride semiconductor material layer mentioned above are exemplary and are not intended to limit the present invention.
[0045] When growing the impurity barrier structure, any aluminum source or boron source known in the art can be used, preferably an organoaluminum source or organoboron source, such as TMAl or TEAl, but not limited thereto. The nitrogen source and other metal sources are selected based on the material containing the Al nitride to be formed. Both the nitrogen source and other metal sources can be sourced from materials known in the art, and this invention does not impose any particular limitations.
[0046] The organic aluminum source and organic boron source can be introduced in a continuous, pulsed, or intermittent manner, but are not limited to these methods.
[0047] In some embodiments, the nitride semiconductor material includes GaN, InN, AlInN, InGaN, AlGaN, AlInGaN, BAlGaN, AlScN, BAlN, or PAlN.
[0048] In some embodiments, the substrate is a substrate, and the method grows the impurity barrier structure on the substrate.
[0049] In some embodiments, the method further includes removing the oxide layer from the substrate, the oxide layer removal process comprising:
[0050] The substrate is placed in a reaction chamber, and an organic source containing an element that can combine with oxygen is introduced into the reaction chamber, so that the element reacts with oxygen atoms on the surface of the substrate to remove the oxide layer on the surface of the substrate.
[0051] Furthermore, the organic source contains at least one of the elements that can combine with oxygen, namely Al and B.
[0052] Furthermore, the organic source includes one or a combination of organoaluminum sources and organoboron sources.
[0053] In some embodiments, the organic source is pulsed into the reaction chamber.
[0054] Furthermore, the pulsed introduction specifically includes: under conditions of 800-1100℃ and 50-400mbar, introducing the organic source into the reaction chamber for 1-500s every 1-100s, thereby allowing it to fully react with oxygen atoms on the substrate surface.
[0055] Furthermore, the oxide layer removal process also includes: treating the substrate at a temperature of 600-1300℃ for 10s-20min, and then introducing the organic source to further remove the oxide layer, which results in a better treatment effect.
[0056] In some embodiments, the method further includes nitriding the substrate, specifically comprising: nitriding the substrate by introducing NH3 at a temperature of 900-1350°C. The nitriding time can be 10s-20min.
[0057] The substrate can be made of sapphire, silicon, self-supporting AlN single crystal, self-supporting GaN single crystal, silicon carbide, diamond, etc., and the present invention does not make any particular limitation on it.
[0058] In some embodiments, the substrate includes a substrate and a nitrogen polar nucleation layer formed on the substrate, and the method grows the impurity barrier structure on the nitrogen polar nucleation layer.
[0059] Furthermore, the nitrogen polar nucleation layer can be a nitrogen polar GaN nucleation layer.
[0060] Furthermore, the thickness of the nitrogen polar nucleation layer is 5-200 nm.
[0061] In embodiments where the substrate has a nitrogen polar nucleation layer, the substrate may first undergo oxide removal and / or nitriding treatment before the nitrogen polar nucleation layer is grown on the substrate.
[0062] Furthermore, growing a nitrogen polar nucleation layer on the substrate specifically includes growing the nitrogen polar nucleation layer at a temperature of 550–650°C.
[0063] Furthermore, after growing the nitrogen polar nucleation layer, the obtained structure is further subjected to annealing treatment. The annealing treatment temperature can be 900-1350℃, and the annealing treatment time can be 10-1200s.
[0064] The method described in this invention can be implemented using known epitaxial growth materials in the art, such as metal-organic chemical vapor deposition (MOCVD), molecular beam epitaxy (MBE), hydride vapor phase epitaxy (HVPE), and pulsed laser deposition (PLD), with MOCVD being preferred.
[0065] A second aspect of the present invention is to provide a method for reducing the background impurity concentration of oxygen in a nitride semiconductor material, comprising:
[0066] A nitride layer is grown on a substrate within a reaction chamber. During the growth of the nitride layer, an organic source containing an element capable of binding with oxygen is pulsed in, so that the organic source consumes the concentration of oxygen impurities in the reaction chamber.
[0067] Nitride semiconductor material is grown on the nitride layer.
[0068] The method provided in the second aspect of this invention utilizes an organic source with strong oxygen-binding capabilities for pulsed growth, significantly reducing the oxygen concentration in the environment. Therefore, the concentration of oxygen impurities incorporated during subsequent growth of nitride semiconductor materials is reduced. Furthermore, the pulsed induction method can reduce the impact of compressive stress accumulation on wafer warpage, while simultaneously consuming residual oxygen impurities in the reaction chamber and providing compressive stress to suppress subsequent oxygen impurities.
[0069] In some embodiments, the substrate is a base plate, and the method grows the nitride layer on the base plate.
[0070] In some embodiments, the substrate includes a substrate and a nitrogen polar nucleation layer formed on the substrate, and the method grows the nitride layer on the nitrogen polar nucleation layer.
[0071] In some embodiments, the organic source contains at least one of Al and B, which are elements capable of binding with oxygen. The strong binding energy of Al and B with oxygen can rapidly deplete the concentration of oxygen impurities in the reaction chamber environment.
[0072] In some embodiments, the organic source includes one or a combination of organoaluminum sources and organoboron sources.
[0073] Furthermore, the organoaluminum source includes, but is not limited to, one or more of TMAl and TEAl.
[0074] Furthermore, organic boron sources include, but are not limited to, TEB.
[0075] In some embodiments, the thickness of the nitride layer is 10-300 nm.
[0076] In some embodiments, the material of the nitride layer may include GaN, InN, InGaN, etc.
[0077] In some embodiments, the pulsed introduction of the organic source specifically includes: during the growth of the nitride layer, introducing the organic source for 1-500 seconds every 1-100 seconds.
[0078] In some embodiments, the method specifically includes: growing a GaN layer by introducing a gallium source and a nitrogen source into the reaction chamber at 800-1350℃ and 50-600mbar; simultaneously, introducing at least one of an organoaluminum source and an organoboron source for 1-500s every 1-100s, utilizing the strong binding energy of Al and / or B with oxygen to consume the oxygen concentration in the reaction chamber.
[0079] The method for growing nitride semiconductor materials can be any method known in the art, and the present invention does not impose any particular limitation on it.
[0080] Further embodiments of the method described in the second aspect of the present invention, such as substrate selection, oxide layer removal and / or nitriding treatment of the substrate, material and growth method of the nitrogen polar nucleation layer, etc., have been specifically described in the first aspect of the present invention and will not be repeated here.
[0081] A third aspect of the present invention provides a method for reducing the background impurity concentration of oxygen in an epitaxial structure, comprising:
[0082] The substrate is pretreated, the pretreatment comprising: placing the substrate in a reaction chamber, introducing an organic source into the reaction chamber, the organic source containing an element capable of combining with oxygen, and causing the element to react with oxygen atoms on the surface of the substrate to remove the oxide layer on the surface of the substrate;
[0083] An epitaxial structure is grown on the pretreated substrate.
[0084] By utilizing strong oxygen-binding elements in the organic source to effectively bind oxygen impurities at the substrate interface, the diffusion of oxygen impurities into the subsequently grown epitaxial structure is reduced, thereby effectively reducing the concentration of unintentionally doped oxygen impurities in the subsequently grown epitaxial structure.
[0085] In some embodiments, the organic source contains at least one of the elements that can bind with oxygen, namely Al and B.
[0086] In some embodiments, the organic source includes one or a combination of organoaluminum sources and organoboron sources.
[0087] In some embodiments, the organic source is pulsed into the reaction chamber.
[0088] In some embodiments, the pulsed introduction specifically includes: introducing the organic source into the reaction chamber for 1-500 seconds at 800-1100℃ and 50-400mbar every 1-100 seconds, thereby reacting with oxygen atoms on the substrate surface.
[0089] In some embodiments, the pretreatment further includes: placing the substrate in a reaction chamber and treating the substrate at a temperature of 600-1300°C for 10s-20min, and then introducing the organic source, which at this time has a better effect on suppressing the concentration of unintentionally doped oxygen in subsequent growth.
[0090] In some embodiments, prior to growing the epitaxial structure, the process further includes: introducing a nitrogen source to nitrid the pretreated substrate.
[0091] The substrate can be made of sapphire, silicon, self-supporting AlN single crystal, self-supporting GaN single crystal, silicon carbide, diamond, etc., and the present invention does not make any particular limitation on it.
[0092] Compared with the prior art, the present invention has at least the following beneficial effects:
[0093] (1) This invention introduces compressive stress into the subsequent epitaxial growth of nitride semiconductor materials with larger lattice constants by forming an impurity barrier structure with a smaller lattice constant. This compressive stress enhances the oxygen impurity incorporation barrier and reduces the concentration of unintentional oxygen impurities in the nitride semiconductor material. Compared to existing methods that reduce the concentration of unintentional oxygen impurities by changing the semiconductor material growth conditions, the method provided by this invention effectively avoids problems such as decreased crystal quality and surface roughness of the epitaxial layer caused by changes in reaction chamber conditions.
[0094] (2) During the growth of impurity barrier structures based on nitrides containing Al and / or B, precursor sources containing Al and / or B need to be introduced. These precursor sources containing Al and / or B have a strong binding energy with oxygen impurities, so they can consume oxygen impurities in the reaction chamber and further reduce the concentration of unintentional oxygen impurities in the semiconductor material. Attached Figure Description
[0095] To more clearly illustrate the technical solutions in the embodiments of this application or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments recorded in this application. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.
[0096] Figure 1 This is a schematic diagram of the epitaxial structure obtained in Example 1.
[0097] Figure 2 This is a schematic cross-sectional view of the Hall test structure of the ohmic contact electrode prepared in Example 1 for testing the concentration of unintentional oxygen impurities.
[0098] Figure 3 The image shows a comparison of the Hall effect test results for the structures in Example 1 and Comparative Example 1.
[0099] Figure 4 This is a schematic diagram of the epitaxial structure obtained in Example 2.
[0100] Figure 5 This is a schematic diagram of the epitaxial structure obtained in Example 3.
[0101] Figure 6 This is a detailed cross-sectional view of layer 302 in Example 3.
[0102] Figure 7 This is a secondary ion mass spectrum (SIMS) of the structure in Example 3 showing the change in oxygen ion intensity.
[0103] Figure 8 This is a schematic diagram of the epitaxial structure obtained in Example 7.
[0104] Figure 9 This is a detailed cross-sectional view of layer 402 in Example 7.
[0105] Figure 1 In the diagram: 100 is the substrate, 101 is the GaN nucleation layer, 102 is the AlN layer, 103 is the GaN layer, and 104 is the GaN ohmic contact electrode.
[0106] Figure 4 In the diagram: 200 is the substrate, 201 is the AlN layer, and 202 is the GaN layer.
[0107] Figure 5 In the middle: 300 is the substrate, 301 is the GaN nucleation layer, 302 is the composite structure layer, and 303 is the GaN layer; Figure 6 In the diagram, 310 is the AlN layer, 320 is the AlGaN layer, and 330 is the GaN layer.
[0108] Figure 8 In the middle: 400 is the substrate, 401 is the GaN nucleation layer, 402 is the composite structure layer, and 403 is the GaN layer; Figure 9 In the diagram, 410 is an AlN layer and 420 is a GaN layer. Detailed Implementation
[0109] The technical solutions of the present invention will be described in detail below with reference to specific embodiments, so that those skilled in the art can better understand and implement the technical solutions of the present invention. The specific functional details disclosed herein should not be construed as limiting, but are merely intended to form the basis of the claims and to teach those skilled in the art to employ the representative basis of the invention in different ways in any suitable detailed embodiment.
[0110] In addition, unless otherwise specified, all raw materials used in the following embodiments can be purchased from the market or other sources, and all production and testing equipment used are known in the art, as are the testing methods used.
[0111] Example 1
[0112] Example 1 provides a method for reducing the background impurity concentration in GaN thin films using a single-layer impurity barrier layer, specifically including the following steps:
[0113] S1: Place the sapphire substrate 100 in the reaction chamber of the MOCVD device and adjust the temperature to 1240℃ for 10 minutes to remove surface damage and oxide layer of the substrate 100.
[0114] S2: Adjust the temperature to 1130℃, introduce 5slm NH3, and nitrid the substrate 100 for 4min.
[0115] S3: Turn off NH3, adjust the temperature to 700℃, and under a pressure of 100mbar, introduce TMGa and NH3 to grow a GaN nucleation layer 101 with a thickness of 20nm on the substrate 100.
[0116] S4: Turn off TMGa and heat the temperature to 1210℃ for annealing for 10 minutes.
[0117] S5: The temperature is increased to 1300℃, and under a pressure of 100mbar, TMAl and 2L NH3 are introduced to grow an AlN layer 102 with a thickness of 50nm on the GaN nucleation layer.
[0118] S6: Turn off TMAl, adjust the pressure to 100mbar and the temperature to 1210℃, introduce 33L of NH3 and TMGa, and grow GaN layer 103 on AlN layer 102.
[0119] Figure 1 This is a schematic diagram of the epitaxial structure obtained in Example 1. The epitaxial structure includes a sapphire substrate 100, and a GaN nucleation layer 101, an AlN layer 102, and a GaN layer 103 sequentially grown on the substrate 100. The AlN layer 102 ensures that the subsequently grown GaN is under compressive stress. Because the GaN is under compressive stress, O... N The increased formation energy makes it more difficult for oxygen impurities to be incorporated into GaN, thereby reducing the concentration of unintentional oxygen impurities in GaN and lowering the background carrier concentration.
[0120] Comparative Example 1
[0121] The only difference between Comparative Example 1 and Example 1 is that step S5 in Example 1 is omitted; that is, Comparative Example 1 does not form an AlN layer and directly grows GaN on the GaN nucleation layer. The rest is the same as in Example 1 and will not be described again here.
[0122] Based on the GaN layer prepared in Example 1 and Comparative Example 1, a metal electrode Ti / Al / Ni / Au was deposited to form an ohmic contact for van der Berg Hall testing. Figure 2 This is a schematic cross-sectional view of a Hall test structure with an ohmic contact electrode formed on the epitaxial structure of Example 1, where 104 is a metal electrode Ti / Al / Ni / Au. Figure 3 The experimental structure based on Example 1 (corresponding to) Figure 3 The wAl(Ga)N buffer in the example and the reference structure based on Comparative Example 1 (corresponding to Figure 3 The room temperature Hall effect test results of the w / oAl(Ga)N buffer showed that the background carrier concentration of the epitaxial structure without the AlN layer was 5 × 10⁻⁶. 17 cm-3 The background carrier concentration of the structure in Example 1 is 3 × 10⁻⁶. 17 cm -3 .
[0123] Example 2
[0124] Example 2 provides a method for reducing the background impurity concentration in GaN thin films using a single-layer impurity barrier layer, specifically including the following steps:
[0125] S1: The SiC substrate 200 is introduced into the reaction chamber of the molecular beam epitaxy (MBE) device, heated to 650°C and held for 60 min to remove water vapor from the surface of the substrate 200.
[0126] S2: Open the Al source furnace baffle to pulse-introduce TMAl, and open the nitrogen source furnace baffle to introduce NH3. Adjust the temperature to 650℃ and the pressure to 10^-5mbar, and grow an AlN layer 201 with a thickness of 10nm on the SiC substrate 200.
[0127] S3: Close the Al source furnace baffle and the nitrogen source furnace baffle, reduce the temperature to 600℃, control the pressure at 10^-5mbar, open the Ga source baffle and the nitrogen source baffle, introduce TMGa and NH3, and grow the GaN layer 202 on the AlN layer 201.
[0128] Figure 4 This is a schematic diagram of the epitaxial structure obtained in Example 2. The structure includes a substrate 200 and an AlN layer 201 and a GaN layer 202 sequentially disposed on the substrate 200.
[0129] Al and oxygen have a strong binding interaction. Therefore, the process of growing the AlN layer 201 using TMAl can consume oxygen impurities in the reaction chamber. Furthermore, the reaction between TMAl and the oxide layer on the SiC substrate surface can remove oxygen from the SiC surface. In addition, the AlN layer 201 can also put the subsequently grown GaN layer 202 under compressive stress, further reducing the background oxygen impurity concentration in the GaN layer 202.
[0130] Example 3
[0131] Example 3 provides a method for reducing the background impurity concentration of a GaN layer using a multilayer impurity blocking structure, specifically including the following steps:
[0132] S1: Place the sapphire substrate 300 in the reaction chamber of the MOCVD device and process the substrate at 1240℃ for 10 minutes to remove surface damage and oxide layer.
[0133] S2: Adjust the temperature to 1130℃ and introduce 5L of NH3 to nitrid the substrate for 4 minutes.
[0134] S3: Turn off NH3, and introduce TMGa and NH3 at a temperature of 700℃ and a pressure of 100mbar to grow a GaN nucleation layer 301 with a thickness of 20nm on the substrate.
[0135] S4: Turn off TMGa and anneal at 1210℃ for 10 min.
[0136] S5: Increase the temperature to 1300℃, and under a pressure of 100mbar, introduce TMAl to provide Al atoms, and introduce 2LNH3 to grow an AlN layer 310 with a thickness of 50nm on the GaN nucleation layer 301, so as to ensure that the subsequently grown GaN is under compressive stress.
[0137] S6: Reduce the temperature to 1210℃, and under a pressure of 100mbar, introduce TMAl to provide Al atoms, introduce TMGa to provide Ga atoms, and introduce 10L NH3 to grow an AlGaN layer 320 with a thickness of 10nm on the AlN layer 310, thereby increasing the compressive stress on the subsequently grown GaN.
[0138] S7: Turn off the TMAl source flow. Under a pressure of 100 mbar and a temperature of 1210℃, introduce 33 L of NH3 and TMGa to grow a 100 nm thick GaN layer 330 on the AlGaN layer 320. Because the GaN in the GaN layer 330 is under compressive stress, O... N The increased formation energy makes it more difficult for oxygen impurities to be incorporated into GaN, thereby reducing the concentration of unintentional oxygen impurities in GaN and lowering the background carrier concentration. AlN layer 310, AlGaN layer 320, and GaN layer 330 constitute a repeating unit.
[0139] S8: Repeat S5-S7 a total of 3 times to form a composite structure layer 302 with 3 repeating units.
[0140] S9: Turn off TMA1, and grow a 1 μm thick GaN layer 303 on the GaN layer 330 grown in the last execution step S7. Since the GaN in GaN layer 303 is under compressive stress, O... N The increased formation energy makes it more difficult for oxygen impurities to be incorporated into GaN, thereby reducing the concentration of unintentional oxygen impurities in GaN and lowering the background carrier concentration.
[0141] Figure 5 This is a schematic diagram of the epitaxial structure obtained in this embodiment. Figure 6 yes Figure 5Detailed cross-sectional view of floor 302. Combined with... Figure 5 , Figure 6 As can be seen, the epitaxial structure obtained in this embodiment includes a sapphire substrate 300, and a GaN nucleation layer 301, a composite structure layer 302 and a GaN layer 303 sequentially disposed on the sapphire substrate 300; wherein the composite structure layer has multiple repeating units, and each repeating unit includes an AlN layer 310, an AlGaN layer 320 and a GaN layer 330 sequentially disposed.
[0142] The impurity barrier structure in Example 3 has an AlN layer 310 and an AlGaN layer 320. On the one hand, the AlN layer 310 utilizes the strong bonding ability between Al and O to consume oxygen impurities in the reaction chamber, thereby reducing the concentration of oxygen impurities incorporated into the subsequent grown structure. On the other hand, the AlN layer can put the subsequently grown AlGaN and GaN layers under compressive stress, further reducing the oxygen impurity concentration. The AlGaN layer 320 serves as a buffer layer, reducing the lattice mismatch between the AlN layer and GaN to prevent the subsequent GaN from transforming into a three-dimensional island growth mode. On the other hand, it further provides compressive stress to further reduce the oxygen impurity concentration of the subsequently grown GaN layer.
[0143] Example 4
[0144] Example 4 is basically the same as Example 3, except that step S6 is not performed in Example 4. That is, the impurity blocking structure in Example 4 only has an AlN layer and no AlGaN layer. The rest is the same as in Example 3, and will not be described again here.
[0145] Example 5
[0146] Example 5 is basically the same as Example 3, except that step S5 is not performed in Example 5. That is, the impurity blocking structure in Example 5 only has an AlGaN layer and no AlN layer. The rest is the same as in Example 3, and will not be described again here.
[0147] Comparing Examples 3-5, it was found that, compared with the schemes having only an AlN layer (Example 4) or only an AlGaN layer (Example 5), the scheme of Example 3 can provide compressive stress for both the AlN layer and the AlGaN layer, resulting in stronger accumulated compressive stress and a better effect on reducing the incorporation of oxygen impurities in the GaN layer.
[0148] Example 6
[0149] Example 6 is basically the same as Example 3, except that Example 6 does not repeat steps S5-S7, and the rest is the same as Example 3, which will not be described again here.
[0150] Compared with Examples 3 and 6, by repeating steps S5-S7, the compressive stress can be further increased, thereby achieving a stronger effect in reducing the concentration of oxygen impurities.
[0151] Comparative Example 2
[0152] The only difference between Comparative Example 2 and Example 3 is that Comparative Example 2 does not perform steps S5-S8, that is, Comparative Example 2 does not grow a composite structure layer, but directly forms a GaN layer on the GaN nucleation layer.
[0153] Secondary ion mass spectrometry (SIMS) was used to measure the changes in oxygen ion intensity of GaN in the epitaxial structures prepared in Example 3 and Comparative Example 2. The SIMS data for the changes in oxygen ion intensity of GaN in the epitaxial structure prepared in Example 3 are shown below. Figure 7 As shown. In Comparative Example 2, the oxygen concentration in the GaN under tensile stress is 5.8 × 10⁻⁶. 17 cm -3 In Example 3, the GaN oxygen concentration in GaN layer 330 was reduced to 4.4 × 10⁻⁶. 17 cm -3 .
[0154] Example 7
[0155] S1: Place the sapphire substrate 400 in the reaction chamber of the MOCVD device and treat the sapphire substrate 400 at a temperature of 1240℃ for 10 minutes to remove surface damage and oxide layer.
[0156] S2: At a temperature of 1130℃, 5L NH3 is introduced into the reaction chamber to nitrid the sapphire substrate 400 for 4 minutes.
[0157] S3: Turn off NH3, introduce TMGa and NH3 at a temperature of 700℃ and a pressure of 100mbar, and grow a GaN nucleation layer 401 with a thickness of 20nm on the substrate 400.
[0158] S4: Turn off TMGa and anneal for 10 minutes under the conditions of ammonia gas introduction and temperature of 1210℃.
[0159] S5: Increase the temperature to 1300℃ and introduce TMAl under a pressure of 100mbar to provide Al atoms, and grow an AlN layer 410 with a thickness of 20nm on the GaN nucleation layer 401.
[0160] S6: Turn off the TMAl source, reduce the temperature to 1210℃, and under a pressure of 100mbar, introduce TMGa to grow a GaN layer 420 with a thickness of 20nm on the AlN layer 410. The AlN layer 410 and the GaN layer 420 constitute a repeating unit.
[0161] S7: Repeat steps S5-S6 a total of 3 times to form a composite structure layer 402 with 3 repeating units.
[0162] S8: Maintain the temperature at 1210℃ and the pressure at 100mbar, turn off TMAl, introduce TMGa and NH3, and grow a GaN layer 403 on the GaN layer 420 grown in the last step S6.
[0163] Figure 8 This is a schematic diagram of the epitaxial structure obtained in Example 7. Figure 9 The image shown is a detailed cross-sectional view of the composite structure layer 402 in Example 7. (Combined with...) Figure 8 , Figure 9 It is known that the epitaxial structure obtained in Example 7 includes a sapphire substrate 400, a GaN nucleation layer 401, a composite structure layer 402 and a GaN layer 403 arranged sequentially; wherein the composite structure layer 402 includes three repeating units, each repeating unit having an AlN layer 410 and a GaN layer 420 arranged sequentially.
[0164] Example 8
[0165] S1: Place the sapphire substrate in the reaction chamber of the MOCVD device and adjust the temperature to 1240℃ for 10 minutes to remove surface damage and oxide layer from the substrate.
[0166] S2: Adjust the temperature to 1130℃, introduce 5slm NH3, and nitrid the substrate for 4min.
[0167] S3: Turn off NH3, adjust the temperature to 700℃, and under a pressure of 100mbar, introduce TMGa and NH3 to grow a GaN nucleation layer with a thickness of 20nm on the substrate.
[0168] S4: Turn off TMGa and raise the temperature to 1210℃ for annealing for 10 minutes.
[0169] S5: Maintain the temperature at 1210℃ and the reaction chamber pressure at 100mbar. Introduce TMGa and 33L NH3 to grow a 200nm GaN layer. Simultaneously, introduce triethylboron (TEB) for 10s every 10s to rapidly consume the oxygen impurity concentration in the reaction chamber environment by utilizing the strong bonding between B and O.
[0170] S6: Turn off TEB, and under conditions of 100 mbar pressure and 1210℃, introduce 33 L of NH3 and TMGa to grow a GaN layer.
[0171] This embodiment uses the intermittent introduction of a TEB source, mainly utilizing the strong binding effect of B and O to consume oxygen impurities in the cavity, thereby reducing the incorporation of oxygen impurities into the GaN layer.
[0172] Example 9
[0173] S1: Place the sapphire substrate in the reaction chamber of the MOCVD device and adjust the temperature to 1240℃ for 10 minutes to remove surface damage and oxide layer from the substrate.
[0174] S2: At a temperature of 1000℃ and a pressure of 100mbar, TEB is introduced for 10s every 20s to further remove the oxide layer on the substrate surface by utilizing the strong bonding between B and O.
[0175] S3: Turn off the triethylboron (TEB) source, adjust the temperature to 1130℃, introduce 5slm NH3, and nitrid the substrate for 4min.
[0176] S4: Turn off NH3, adjust the temperature to 700℃, and under a pressure of 100mbar, introduce TMGa and NH3 to grow a GaN nucleation layer with a thickness of 20nm on the substrate.
[0177] S5: Turn off TMGa, raise the temperature to 1210℃, and anneal for 10 minutes at 100mbar pressure.
[0178] S6: Increase the temperature to 1300℃, and under a pressure of 100mbar, introduce TMAl and 2slmNH3 to grow an AlN layer with a thickness of 20nm on the GaN nucleation layer.
[0179] S7: Turn off TMAl, lower the temperature to 1210℃, maintain the pressure at 100mbar, introduce 33L of NH3, and introduce TMGa to grow a GaN layer on the AlN layer.
[0180] In Example 9, prior to nitriding, the substrate was further treated using the strong bonding ability of B and O to further remove the oxide layer on the substrate surface, thereby reducing the concentration of oxygen impurities incorporated into subsequent layers.
[0181] Example 10
[0182] Example 10 provides a method for reducing the background impurity concentration of a GaN layer using a multilayer impurity blocking structure, specifically including the following steps:
[0183] S1: Place the sapphire substrate 300 in the reaction chamber of the MOCVD device and process the substrate at 1240℃ for 10 minutes to remove surface damage and oxide layer.
[0184] S2: Adjust the temperature to 1130℃ and introduce 5L of NH3 to nitrid the substrate for 4 minutes.
[0185] S3: Turn off NH3, and introduce TMGa and NH3 at a temperature of 700℃ and a pressure of 100mbar to grow a GaN nucleation layer 301 with a thickness of 20nm on the substrate.
[0186] S4: Turn off TMGa and anneal at 1210℃ for 10 min.
[0187] S5: At a temperature of 900℃ and a pressure of 50mbar, TMAl is introduced to provide Al atoms, and 2LNH3 is introduced to grow an AlN layer 310 with a thickness of 1nm on the GaN nucleation layer 301, so as to ensure that the subsequently grown GaN is under compressive stress.
[0188] S6: Reduce the temperature to 800℃, and under a pressure of 50mbar, introduce TMAl to provide Al atoms, introduce TMGa to provide Ga atoms, and introduce 10L NH3 to grow an AlGaN layer 320 with a thickness of 1nm on the AlN layer 310, thereby increasing the compressive stress on the subsequently grown GaN.
[0189] S7: Turn off the TMAl source flow. Under conditions of 1210℃ and 100mbar, introduce 33L of NH3 and TMGa to grow a 10nm thick GaN layer 330 on the AlGaN layer 320. Since the GaN in the GaN layer 330 is under compressive stress, O... N The increased formation energy makes it more difficult for oxygen impurities to be incorporated into GaN, thereby reducing the concentration of unintentional oxygen impurities in GaN and lowering the background carrier concentration. AlN layer 310, AlGaN layer 320, and GaN layer 330 constitute a repeating unit.
[0190] S8: Repeat S5-S7 a total of 5 times to form a composite structure layer 302 with 5 repeating units.
[0191] S9: Turn off TMA1, and grow a 1 μm thick GaN layer 303 on the GaN layer 330 grown in the last execution step S7. Since the GaN in GaN layer 303 is under compressive stress, O... N The increased formation energy makes it more difficult for oxygen impurities to be incorporated into GaN, thereby reducing the concentration of unintentional oxygen impurities in GaN and lowering the background carrier concentration.
[0192] The effect of Example 10 is comparable to that of Example 3.
[0193] Example 11
[0194] Example 11 provides a method for reducing the background impurity concentration of a GaN layer using a multilayer impurity blocking structure, specifically including the following steps:
[0195] S1: Place the sapphire substrate 300 in the reaction chamber of the MOCVD device and process the substrate at 1240℃ for 10 minutes to remove surface damage and oxide layer.
[0196] S2: Adjust the temperature to 1130℃ and introduce 5L of NH3 to nitrid the substrate for 4 minutes.
[0197] S3: Turn off NH3, and introduce TMGa and NH3 at a temperature of 700℃ and a pressure of 100mbar to grow a GaN nucleation layer 301 with a thickness of 20nm on the substrate.
[0198] S4: Turn off TMGa and anneal at 1210℃ for 10 min.
[0199] S5: At a temperature of 1350℃ and a pressure of 400mbar, TMAl is introduced to provide Al atoms, and 2LNH3 is introduced to grow an AlN layer 3l0 with a thickness of 200nm on the GaN nucleation layer 301, so as to ensure that the subsequently grown GaN is under compressive stress.
[0200] S6: At a temperature of 1350℃ and a pressure of 600mbar, TMAl is introduced to provide Al atoms, TMGa is introduced to provide Ga atoms, and 10LNH3 is introduced to grow an AlGaN layer 320 with a thickness of 200nm on the AlN layer 310, thereby increasing the compressive stress on the subsequently grown GaN.
[0201] S7: Turn off the TMAl source flow. Under conditions of 1210℃ and 100mbar, introduce 33L of NH3 and TMGa to grow a 100nm thick GaN layer 330 on the AlGaN layer 320. Since the GaN in the GaN layer 330 is under compressive stress, O... N The increased formation energy makes it more difficult for oxygen impurities to be incorporated into GaN, thereby reducing the concentration of unintentional oxygen impurities in GaN and lowering the background carrier concentration. AlN layer 310, AlGaN layer 320, and GaN layer 330 constitute a repeating unit.
[0202] S8: Repeat S5-S7 twice to form a composite structure layer 302 with two repeating units.
[0203] S9: Turn off TMA1, and grow a 1 μm thick GaN layer 303 on the GaN layer 330 grown in the last execution step S7. Since the GaN in GaN layer 303 is under compressive stress, O... N The increased formation energy makes it more difficult for oxygen impurities to be incorporated into GaN, thereby reducing the concentration of unintentional oxygen impurities in GaN and lowering the background carrier concentration.
[0204] The effect of Example 11 is comparable to that of Example 3.
[0205] Example 12
[0206] Example 12 is basically the same as Example 9, except that step S2 in Example 12 is:
[0207] Under conditions of 800°C and 50 mbar, TEB was introduced for 500 seconds every 100 seconds to further remove the oxide layer on the substrate surface by utilizing the strong bonding between boron and oxygen. The rest of the procedure was the same as in Example 9 and will not be described again here.
[0208] The effect of Example 12 is comparable to that of Example 9.
[0209] Example 13
[0210] Example 13 is basically the same as Example 9, except that step S2 in Example 12 is:
[0211] Under conditions of 1100℃ and 400mbar, TEB was introduced for 1 second every 1 second to further remove the oxide layer on the substrate surface by utilizing the strong bonding between B and O. The rest of the implementation was the same as in Example 9, and will not be described again here.
[0212] The effect of Example 13 is comparable to that of Example 9.
[0213] In summary, this invention overcomes the limitations of existing methods that reduce unintentional oxygen impurity concentration by altering the growth conditions of nitride semiconductor materials, thus avoiding a decline in the crystal quality of the nitride semiconductor material layer (e.g., increased dislocation density, increased point defects). The method provided by this invention utilizes impurity blocking structures (e.g., Al(Ga,In)N insertion layers) to establish compressive stress during the subsequent growth of nitride semiconductor materials with high lattice constants, promoting dislocation bending and effectively improving crystal quality while reducing dislocation density. This allows for a reduction in unintentional oxygen impurity concentration without affecting the surface and growth quality of the nitride semiconductor material layer.
[0214] All aspects, embodiments, features, and examples of this invention are to be regarded as illustrative in all respects and are not intended to limit the invention, the scope of which is defined only by the claims. Other embodiments, modifications, and uses will become apparent to those skilled in the art without departing from the spirit and scope of the invention as claimed.
[0215] In addition, the inventors of this case also conducted experiments with other raw materials, process operations, and process conditions described in this specification, referring to the aforementioned embodiments, and obtained relatively ideal results in all cases.
[0216] Although the invention has been described with reference to illustrative embodiments, those skilled in the art will understand that various other changes, omissions, and / or additions can be made without departing from the spirit and scope of the invention, and that elements of the embodiments can be substituted with substantially equivalents. Furthermore, many modifications can be made without departing from the scope of the invention to adapt particular situations or materials to the teachings of the invention. Therefore, this invention is not intended to be limited to the specific embodiments disclosed for carrying out the invention, but rather is intended to encompass all embodiments falling within the scope of the appended claims. Moreover, unless specifically stated otherwise, any use of the terms first, second, etc., does not indicate any order or importance, but is used to distinguish one element from another.
Claims
1. A method of reducing the background impurity concentration of oxygen in a nitride semiconductor material, characterized by, include: An impurity barrier structure is grown on a substrate within a reaction chamber, the impurity barrier structure comprising a stress-modulating material; Nitride semiconductor material is grown on the impurity barrier structure; The lattice constant of the stress-regulating material contained in the impurity barrier structure is smaller than that of the nitride semiconductor material, so that the subsequently grown nitride semiconductor material is under compressive stress.
2. The method of claim 1, wherein: The stress-regulating material includes Al-containing nitrides and / or B-containing nitrides; preferably, the Al-containing nitrides include one or more combinations of AlN, AlGaN, AlInN, AlInGaN, and BAlN, and the B-containing nitrides include one or more combinations of BN, BGaN, BInN, and BInGaN. And / or, the nitride semiconductor material comprises one or more of GaN, InN, AlInN, InGaN, AlGaN, AlInGaN, BAlGaN, AlScN, BAlN, and PAlN; And / or, the substrate is a substrate, and the method grows the impurity barrier structure on the substrate; or, the substrate includes a substrate and a nitrogen polar nucleation layer formed on the substrate, and the method grows the impurity barrier structure on the nitrogen polar nucleation layer.
3. The method according to claim 2, characterized in that: The impurity blocking structure includes a first Al-nitride-containing layer; Preferably, the thickness of the first Al-containing nitride layer is 1-200 nm.
4. The method according to claim 3, characterized in that, The method specifically includes: S 1. Place the substrate in the reaction chamber and grow the first Al-containing nitride layer on the substrate; S2. Grow a nitride semiconductor material layer on the first Al-containing nitride layer; Preferably, the method further includes: S3. Repeat steps S1-S2 at least once. S4. Grow at least one more nitride semiconductor material layer on the nitride semiconductor material layer grown in the last execution step S2.
5. The method according to claim 3, characterized in that: The impurity blocking structure further includes a second Al-containing nitride layer, the material of which is different from that of the first Al-containing nitride layer, and the first Al-containing nitride layer and the second Al-containing nitride layer are arranged sequentially in a direction away from the substrate; Preferably, the thickness of the second Al-containing nitride layer is 1-200 nm.
6. The method according to claim 5, characterized in that, Specifically, it includes: S1. Place the substrate in the reaction chamber and grow an impurity barrier structure on the substrate. Step S1 includes S11 and S12: S11. The first Al-nitride-containing layer is grown on the substrate; S12. Grow a second Al-containing nitride layer on the first Al-containing nitride layer; S2. A nitride semiconductor material layer is grown on the second Al-containing nitride layer; Preferably, the method further includes: S3. Repeat steps S1 to S2 at least once; S4. Grow at least one more nitride semiconductor material layer on the nitride semiconductor material layer grown in the last execution step S2.
7. The method according to claim 2, characterized in that, The process also includes removing the oxide layer from the substrate, the oxide layer removal process comprising: The substrate is placed in a reaction chamber, and an organic source containing an element that can combine with oxygen is introduced into the reaction chamber, so that the element reacts with oxygen atoms on the surface of the substrate to remove the oxide layer on the surface of the substrate. Preferably, the organic source contains at least one of the elements that can combine with oxygen, namely Al and B. Preferably, the organic source is pulsed into the reaction chamber. More preferably, the pulsed introduction specifically includes: introducing the organic source into the reaction chamber for 1-500 seconds at 1-100 seconds every 1-500 seconds under conditions of 800-1100℃ and 50-400mbar. Preferably, the oxide layer removal process further includes: treating the substrate at a temperature of 600-1300°C for 10s-20min, and then introducing the organic source.
8. A method for reducing the background oxygen impurity concentration in a nitride semiconductor material, characterized in that, include: A nitride layer is grown on a substrate within a reaction chamber. During the growth of the nitride layer, an organic source containing an element capable of binding with oxygen is pulsed in, so that the organic source consumes the concentration of oxygen impurities in the reaction chamber. Nitride semiconductor material is grown on the nitride layer.
9. The method according to claim 8, characterized in that: The substrate is a substrate, and the method grows the nitride layer on the substrate; or, the substrate includes a substrate and a nitrogen polar nucleation layer formed on the substrate, and the method grows the nitride layer on the nitrogen polar nucleation layer; And / or, the organic source contains at least one of the elements that can bind with oxygen, including Al and B; And / or, the organic source includes one or more of organoaluminum sources and organoboron sources; And / or, the thickness of the nitride layer is 10-300 nm; And / or, the pulsed introduction of the organic source specifically includes: during the growth of the nitride layer, introducing the organic source for 1-500 seconds at intervals of 1-100 seconds.
10. A method for reducing the background impurity concentration of oxygen in an epitaxial structure, characterized in that, include: The substrate is pretreated, the pretreatment comprising: placing the substrate in a reaction chamber, introducing an organic source into the reaction chamber, the organic source containing an element capable of combining with oxygen, and causing the element to react with oxygen atoms on the surface of the substrate to remove the oxide layer on the surface of the substrate; An epitaxial structure is grown on the pretreated substrate; Preferably, the organic source contains at least one of the elements that can combine with oxygen, namely Al and B. Preferably, the organic source is pulsed into the reaction chamber. More preferably, the pulsed introduction specifically includes: at 800-1100℃ and 50-400mbar, the organic source is introduced into the reaction chamber for 1-500s every 1-100s. And / or, the pretreatment further includes: placing the substrate in the reaction chamber and treating the substrate at a temperature of 600-1300°C for 10s-20min, and then introducing the organic source.