Power semiconductor devices with source and drain leads on both sides and their fabrication methods
By using a power semiconductor device structure with source and drain leads on both sides, the problems of parasitic parameters of metal interconnects and output capacitance limitations in existing technologies are solved, achieving improved low resistance and high frequency performance, making it suitable for medium and high frequency power switching applications.
Patent Information
- Application Number
- CN202611419656.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-14
- Publication Date
- 2026-11-17
AI Technical Summary
In existing gallium nitride-based p-GaN gate high electron mobility transistors, the parasitic parameters of the external metal interconnects and the output capacitance limit the switching efficiency and the maximum operating frequency in medium and high frequency power switching applications, and the traditional etching process affects the reliability of the device.
The power semiconductor device structure with source and drain leads on both sides is adopted. The source is located on the back side of the chip, while the drain and gate are located on the front side of the chip. By setting a silicon via array and multiple metal layers in the substrate, the source signal is directly led out from the back side, and the drain and gate signals are led out from the front side. Combined with a one-step back etching process, metal thickness loss and interface voids are avoided.
It significantly reduces drain-source capacitance and output capacitance, reduces high-frequency switching losses, lowers source-side parasitic resistance, improves device thermal management and interconnect reliability, is suitable for existing CMOS back-end processes, and meets the requirements of low on-resistance and high-frequency applications.
Smart Images

Figure CN123124389A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of power semiconductor devices, and more specifically, relates to a power semiconductor device with source and drain leads on both sides and a method for fabricating the same. Background Technology
[0002] Currently, gallium nitride-based p-GaN gate high electron mobility transistors (pGaN-HEMTs) have become the mainstream choice for mid-to-high frequency power switching applications. As the on-resistance of these devices enters the sub-milliohm range, parasitic parameters of the external metal interconnects and the output capacitance become key bottlenecks limiting switching efficiency, losses, and the maximum operating frequency.
[0003] Existing lateral structure devices typically place the source, drain, and gate on the front side of the chip, resulting in a large overlap of source and drain metal wirings in the vertical direction. This overlap area usually contributes 30% to 50% of the total source-drain capacitance, thereby increasing output capacitance, limiting switching losses under soft switching, and increasing voltage change rate under hard switching. Simultaneously, the source signal is led out through multiple layers of metal interconnects on the front side, resulting in a long path and high series resistance, making it difficult to meet the stringent requirements for interconnect parasitics in low on-resistance devices. Furthermore, when introducing through-silicon vias (TSVs) on the back side to optimize electrical or thermal performance, conventional two-step etching processes easily cause thickness loss and interface voids in the front metal layer, severely impacting the long-term reliability of the device. Therefore, there is an urgent need for a power semiconductor device and its fabrication method that can simultaneously reduce parasitic capacitance and interconnect resistance while improving the reliability of back-side interconnects. Summary of the Invention
[0004] The main objective of this invention is to provide a power semiconductor device with both source and drain leads and its fabrication method, so as to overcome the shortcomings of the prior art.
[0005] To achieve the above-mentioned objectives, the present invention adopts the following technical solution: The first aspect of this invention provides a power semiconductor device with both source and drain leads, comprising: a first metal layer, a substrate, a semiconductor epitaxial layer, an active region, and a first dielectric layer sequentially disposed in a predetermined direction, wherein the active region includes a source ohmic contact, a drain ohmic contact, and a gate metal; a groove is formed in the region of the first dielectric layer and the semiconductor epitaxial layer outside the active region, the bottom of the groove being located on the substrate surface or within the substrate; a second metal layer is disposed inside the groove and on the region of the first dielectric layer corresponding to the source ohmic contact, wherein a first conductive channel is disposed within the first dielectric layer connecting the second metal layer and the source ohmic contact; a second conductive channel is disposed within the substrate connecting the second metal layer at the bottom of the groove and the first metal layer. A conductive channel is provided to electrically connect the source ohmic contact to the first metal layer; the power semiconductor device further includes: a third metal layer and a fourth metal layer, respectively disposed in the regions of the first dielectric layer corresponding to the drain ohmic contact and the gate metal; a second dielectric layer covering the first dielectric layer, the second metal layer, the third metal layer and the fourth metal layer, wherein the regions of the second dielectric layer corresponding to the third metal layer and the fourth metal layer are respectively provided with corresponding first top layer metal and second top layer metal; conductive paths are also provided in the first dielectric layer and the second dielectric layer to electrically connect the drain ohmic contact, the third metal layer and the first top layer metal, and to electrically connect the gate metal, the fourth metal layer and the second top layer metal.
[0006] Preferably, the second metal layer and / or the third metal layer and / or the fourth metal layer adopt a first metal stack structure; the first metal stack structure includes a first barrier layer, a first adhesive layer, a first main conductive layer, a second barrier layer and a second adhesive layer arranged sequentially in the set direction.
[0007] Preferably, the material of the first barrier layer includes TiN, TaN, Ta, or W.
[0008] Preferably, the material of the first main conductive layer includes Al or an Al-based conductive alloy.
[0009] Preferably, the thickness of the first barrier layer is 0.2~0.5μm.
[0010] Preferably, the first barrier layer has an etching selectivity ratio greater than 100:1 relative to the etching chemicals used in the processing of the second conductive channel.
[0011] Preferably, the first top layer metal and / or the second top layer metal adopt a second metal stack structure; the second metal stack structure includes a barrier adhesion layer, a second main conductive layer, a third barrier layer and an anti-reflection passivation layer sequentially disposed in the set direction.
[0012] Preferably, the thickness of the substrate is 50~200μm.
[0013] Preferably, the thickness of the first metal layer is 10~50μm.
[0014] Preferably, the coverage of the first metal layer on the substrate surface is not less than 60%.
[0015] Preferably, the power semiconductor device further includes: a Kelvin source pad disposed on a region outside the active region of the first dielectric layer; a third top layer metal disposed in a region of the second dielectric layer corresponding to the Kelvin source pad, and the Kelvin source pad being electrically connected to the third top layer metal for being led out.
[0016] Preferably, the second conductive channel includes an array of through-silicon vias extending through the substrate along the predetermined direction.
[0017] Preferably, the diameter of a single through-silicon via in the through-silicon via array is 5~50μm.
[0018] Preferably, the distance between adjacent through-silicon vias in the through-silicon via array is 1.5 to 10 times the diameter of a single through-silicon via.
[0019] A second aspect of the present invention provides a method for fabricating a power semiconductor device with both source and drain leads, comprising: sequentially fabricating a substrate, a semiconductor epitaxial layer, an active region, and a first dielectric layer along a predetermined direction, wherein the active region includes a source ohmic contact, a drain ohmic contact, and a gate metal; forming a groove in the first dielectric layer and the semiconductor epitaxial layer in a region outside the active region, the bottom of the groove being located on the substrate surface or within the substrate; fabricating a first conductive channel, a first conductive path, and a second conductive path in the regions of the first dielectric layer corresponding to the source ohmic contact, the drain ohmic contact, and the gate metal, respectively, along the predetermined direction; fabricating a second metal layer inside the groove and on the region of the first dielectric layer corresponding to the source ohmic contact, wherein the first conductive channel connects the second metal layer and the source ohmic contact; and fabricating a second metal layer inside the groove and on the region of the first dielectric layer corresponding to the source ohmic contact, wherein the first conductive path connects the second metal layer and the source ohmic contact; and fabricating a first conductive channel in the first dielectric layer. A third metal layer and a fourth metal layer are respectively fabricated on the conductive path and the second conductive path; a second dielectric layer is fabricated on the first dielectric layer, the second metal layer, the third metal layer and the fourth metal layer, and a corresponding first top metal and a second top metal are respectively disposed in the regions of the second dielectric layer corresponding to the third metal layer and the fourth metal layer; a third conductive path connecting the third metal layer and the first top metal, and a fourth conductive path connecting the fourth metal layer and the second top metal are also fabricated in the second dielectric layer; a second conductive channel penetrating the substrate along the predetermined direction is fabricated in the substrate, and one end of the second conductive channel is connected to the second metal layer at the bottom of the groove; a first metal layer is fabricated on the side of the substrate away from the semiconductor epitaxial layer, and the first metal layer is connected to the other end of the second conductive channel.
[0020] Preferably, the second metal layer includes a first barrier layer, a first adhesive layer, a conductive layer, a second barrier layer, and a second adhesive layer sequentially disposed in the set direction; the second conductive channel includes an array of through-silicon vias penetrating the substrate along the set direction, and the first barrier layer is used as an etching stop layer when etching the through-silicon vias in the substrate.
[0021] Preferably, before processing the second conductive channel, the preparation method further includes: coating the surfaces of the first top layer metal and the second top layer metal with temporary bonding adhesive, and then performing wafer-level temporary bonding with the stripping carrier; thinning the side of the substrate away from the semiconductor epitaxial layer, wherein the thickness of the thinned substrate is 50~200μm.
[0022] Compared with the prior art, the beneficial effects of the present invention are as follows: The present invention provides a power semiconductor device with source and drain leads on both sides and a method for fabricating the same. By placing the source on the back side of the chip and the drain / gate on the front side, the contribution of the top metal overlap of the source and drain to the drain-source capacitance is eliminated at the device structure level. Combined with the increased vertical isolation distance due to the substrate thickness, the drain-source capacitance is reduced by 25%-40%, and the output capacitance is reduced by 15%-30%, significantly reducing high-frequency switching losses. The source is led out through the second conductive channel on the back side and the first metal layer, greatly shortening the interconnect path and making the parasitic resistance at the source end less than 0.05mΩ, meeting the low resistance requirement of sub-milliohm devices. The second conductive channel on the back side... A low thermal resistance metallization heat dissipation path is constructed beneath the through-channel, enhancing the device's thermal management capabilities. By pre-setting grooves outside the active region and forming substrate contacts, the substrate potential is clamped to the source via the second metal layer, improving dynamic on-resistance drift and common-mode noise suppression. A one-step back-side via etching process with the bottom barrier layer of the second metal layer as a natural stop layer is adopted, fundamentally avoiding the metal thickness loss and interface void failure modes caused by the traditional two-step process, thus improving the long-term reliability and mass production yield of the back-side interconnect. It is compatible with standard complementary metal-oxide-semiconductor (CMOS) back-end processes, requiring no additional dedicated equipment, and can be seamlessly introduced into existing 8-inch silicon-based gallium nitride production lines. Attached Figure Description
[0023] To more clearly illustrate the technical solutions in the embodiments of this application or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments recorded in this application. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.
[0024] Figure 1 This is a schematic diagram of the structure of a power semiconductor device with source and drain leads on both sides, provided in an embodiment of the present invention.
[0025] Figure 2 This diagram illustrates how the contribution of source-drain wiring overlap to the output capacitance varies with source-drain voltage.
[0026] Figure 3 This is a schematic diagram of the device structure after the substrate, semiconductor epitaxial layer, and active region fabrication process provided in the embodiments of the present invention.
[0027] Figure 4 This is a schematic diagram of the device structure after a conductive channel is fabricated in the first dielectric layer, as provided in an embodiment of the present invention.
[0028] Figure 5 This is a schematic diagram of the device structure after the groove has been processed, as provided in an embodiment of the present invention.
[0029] Figure 6 This is a schematic diagram of the device structure after processing the second metal layer, the third metal layer and the fourth metal layer, as provided in an embodiment of the present invention. Detailed Implementation
[0030] In view of the shortcomings of the prior art, the inventors of this invention, through long-term research and extensive practice, have proposed the technical solution of this invention. The following will further explain and illustrate this technical solution, its implementation process, and its principles.
[0031] Many specific details are set forth in the following description in order to provide a full understanding of the invention. However, the invention may also be practiced in other ways different from those described herein, and therefore the scope of protection of the invention is not limited to the specific embodiments disclosed below.
[0032] Furthermore, in the description of this invention, it should be understood that the terms "upper," "lower," "inner," "outer," "horizontal," "vertical," etc., indicate the orientation or positional relationship based on the orientation or positional relationship shown in the accompanying drawings. They are only for the convenience of describing this invention and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, or be constructed and operated in a specific orientation. Therefore, they should not be construed as limitations on this invention.
[0033] In the description of this specification, the references to terms such as "an embodiment," "a particular embodiment," or "the embodiment" indicate that a specific feature, structure, material, or characteristic described in connection with that embodiment or example is included in at least one embodiment or example of the invention. In this specification, the illustrative expressions of the above terms do not necessarily refer to the same embodiment or example. Furthermore, the specific features, structures, materials, or characteristics described may be combined in any suitable manner in one or more embodiments or examples.
[0034] Figure 1 This is a schematic diagram of a power semiconductor device with both source and drain leads provided in an embodiment of the present invention. (See attached diagram.) Figure 1A power semiconductor device with source and drain leads on both sides includes: a first metal layer, a substrate, a semiconductor epitaxial layer, an active region, and a first dielectric layer sequentially disposed in a predetermined direction. The active region includes a source ohmic contact, a drain ohmic contact, and a gate metal. A groove is formed in the region of the first dielectric layer and the semiconductor epitaxial layer outside the active region, with the bottom of the groove located on the substrate surface or within the substrate. A second metal layer is disposed inside the groove and on the region of the first dielectric layer corresponding to the source ohmic contact. A first conductive channel connecting the second metal layer and the source ohmic contact is disposed within the first dielectric layer. A second conductive channel connecting the second metal layer at the bottom of the groove and the first metal layer is disposed within the substrate, so as to electrically connect the source ohmic contact to the first metal layer. The power semiconductor device further includes: a third metal layer and a fourth metal layer, respectively disposed on the regions of the first dielectric layer corresponding to the drain ohmic contact and the gate metal; a second dielectric layer covering the first dielectric layer, the second metal layer, the third metal layer, and the fourth metal layer, with corresponding first top layer metal and second top layer metal disposed on the regions of the second dielectric layer corresponding to the third metal layer and the fourth metal layer, respectively. Conductive pathways (including) are also provided within the first dielectric layer and the second dielectric layer. Figure 1 The first conductive path, the second conductive path, the third conductive path, and the fourth conductive path are used to electrically connect the drain ohmic contact, the third metal layer, and the first top metal layer, and to electrically connect the gate metal, the fourth metal layer, and the second top metal layer.
[0035] The substrate is, for example, a silicon substrate. The semiconductor epitaxial layer includes, for example, a nucleation layer, a stress buffer layer, a channel layer, and a barrier layer sequentially disposed in a defined direction. The nucleation layer is, for example, an AlN nucleation layer, the channel layer is, for example, a GaN channel layer, and the barrier layer is, for example, an AlGaN barrier layer. The active region is used to control the injection and extraction of charge carriers. A first dielectric layer covers the active region and the surface of the semiconductor epitaxial layer, serving as insulation and planarization. Its material is, for example, silicon oxide, silicon nitride, or a combination thereof. Placing the groove outside the active region avoids damage to the core channel region of the device during the etching process, while providing a physical channel for clamping the subsequent substrate potential. The second metal layer fills the interior of the groove and directly contacts the substrate, while also covering the source pad region on the surface of the first dielectric layer. This integrated second metal layer structure not only simplifies the process flow but also ensures low-resistance convergence of the source signal path and the substrate ground path at the metal layer. In some examples, the second metal layer can also employ a multilayer metal stack structure to improve electromigration resistance and serve as a stop layer for subsequent back-side etching processes. The first conductive channel is, for example, a tungsten (W) via, which passes through the first dielectric layer to electrically connect the underlying source ohmic contact to the upper second metal layer.
[0036] With this vertical interconnect structure using the second conductive channel, the source signal no longer needs to be led out through multiple layers of metal wiring on the front side. Instead, it is directly transmitted from the active region through a short path of the first conductive channel, the second metal layer, and the second conductive channel to the first metal layer on the back side. This not only significantly shortens the source current path and reduces parasitic inductance and resistance, but also allows the source signal to be directly output from the back of the chip, laying the foundation for realizing physical source-drain separation. The first metal layer, for example, is a thick copper redistribution layer (RDL), which serves as both the source lead-out terminal and an efficient heat dissipation channel.
[0037] The third and fourth metal layers are co-located with the second metal layer but are insulated from each other, serving to receive drain and gate signals, respectively. The second dielectric layer acts as an interlayer insulation and passivation layer, protecting the underlying metal interconnects. The first and second top-layer metal layers serve as external interface pads on the front side of the chip, used to bring out drain and gate signals, respectively. There are no large-area source metal planes in the projected area beneath the first and second top-layer metal layers. The conductive paths within the first and second dielectric layers form the vertical lead-out paths for the drain and gate signals, allowing them to reach the front-side top-layer pads with the shortest path, reducing parasitic parameters caused by lateral wiring.
[0038] This invention achieves significant technical advantages through the aforementioned double-sided source-drain topology. First, because the source signal is completely moved to the first metal layer on the back side, while the drain and gate signals remain on the top metal layer on the front side, the vertical coupling distance between the source and drain increases from a few micrometers of interlayer dielectric thickness in conventional structures to the entire substrate thickness (50-200 μm) plus the semiconductor epitaxial layer thickness (approximately 2-5 μm). According to the parallel plate capacitance formula, when the plate spacing d increases by two orders of magnitude, the vertical coupling capacitance decreases significantly. Second, the maximum source plateau is completely eliminated below the top metal layer on the front side, directly reducing the parasitic capacitance component generated by the overlapping source and drain metal layers in conventional structures to zero. These two factors combined result in a significantly reduced drain-source capacitance C. ds It can reduce output capacitance C by 25%~40%. oss This can reduce losses by 15% to 30%, thereby significantly reducing high-frequency switching losses. At the same time, the shortening of the source interconnect path and the increase of the metallization cross-section result in a source-end parasitic resistance of less than 0.05mΩ, effectively supporting the performance of devices with sub-milliohm on-resistance.
[0039] The embodiments of the present invention provide Figure 1In this paper, auxiliary elements such as gate wiring, field plate, gate interconnect, and passivation layer details are omitted; the above omissions do not affect the presentation of the three core technical solutions of this invention: source and drain double-sided lead-out, one-step silicon via termination by the second metal layer, and substrate grounding. The via diameters of the first conductive channel, the first conductive path, and the second conductive path are, for example, 0.2~2μm.
[0040] Preferably, the second metal layer adopts the first metal stack structure. Preferably, the third metal layer adopts the first metal stack structure. Preferably, the fourth metal layer adopts the first metal stack structure. The first metal stack structure includes a first barrier layer, a first adhesive layer, a first main conductive layer, a second barrier layer, and a second adhesive layer sequentially disposed in a predetermined direction.
[0041] In a preferred embodiment, the first main conductive layer is made of aluminum (Al) or an aluminum-based conductive alloy (e.g., Al-Cu, Al-Si-Cu), and performs the main lateral current transport function. The thickness of the first main conductive layer is, for example, 1~2 μm. The first and second adhesive layers are used to enhance the adhesion between the main conductive layer and the upper and lower adhesive layers or barrier layers, preventing delamination during thermal cycling. The first barrier layer at the bottom has a dual function: it acts as a barrier to prevent impurities in the lower dielectric layer from diffusing upwards into the main conductive layer, and it also serves as a "natural etch stop layer" for subsequent back-side through-silicon via (TSV) etching processes. In a preferred embodiment, the first barrier layer is made of TiN, TaN, Ta, or W. The thickness of the first barrier layer is 0.2~0.5 μm, for example, 0.2 μm, 0.3 μm, 0.4 μm, or 0.5 μm. The first barrier layer has an etching selectivity greater than 100:1 relative to the etching chemicals used in the fabrication of the second conductive channel. Specifically, when fabricating the second conductive channel (i.e., through-silicon via) on the back side, a Bosch deep silicon etching process based on SF6 / C4F8 gas is typically used. When the etching penetrates the substrate and reaches the surface of the first barrier layer at the bottom of the second metal layer, the etching rate drops sharply or even stops automatically due to the extremely high chemical inertness and physical sputtering resistance of materials such as TiN and TaN to fluorine-containing plasma, thereby avoiding damage to the main conductive layer caused by over-etching. Compared to the traditional process that requires additional deposition of a dedicated etching termination layer and secondary etching, this invention utilizes the inherent first barrier layer in the first metal stack structure as a stop layer. This not only eliminates a mask and deposition process, but more importantly, it completely eliminates the metal thickness loss caused by secondary etching and the interface void defects caused by the lifting of the bottom of the sidewall insulating layer.
[0042] The first metal stack structure, along the opposite direction of the predetermined direction, includes, for example, Ti / TiN / Al / Ti / TiN. The bottom TiN can be replaced with TaN, Ta, W, or a Ti / TiN bilayer stack, as long as the thickness is sufficient and it has an etching selectivity greater than 100:1 for the etching chemicals used. The main Al can be replaced with Al-Cu or Al-Si-Cu.
[0043] Preferably, the first top layer metal adopts a second metal stack structure. Preferably, the second top layer metal adopts a second metal stack structure. The second metal stack structure includes a barrier adhesion layer, a second main conductive layer, a third barrier layer, and an anti-reflection passivation layer sequentially disposed in a predetermined direction. This four-layer structure is specifically designed for external interconnection and package adaptation on the front side of the chip. The second main conductive layer is, for example, an Al or Al-Cu layer with a thickness of 3~5μm, providing a low-resistance pad interface; the barrier adhesion layer (e.g., a Ti / TiN composite layer) ensures good adhesion between the thick aluminum layer and the underlying second main conductive layer; the third barrier layer (e.g., Ti) prevents the upper metal layer from diffusing into the main conductive layer; and the topmost anti-reflection passivation layer (e.g., TiN) not only reduces reflective interference during subsequent packaging photolithography alignment but also serves as an anti-oxidation and corrosion-resistant protective layer, allowing the top layer metal to directly support wire bonding or flip-chip bonding processes without additional surface treatment. The thickness of each top layer metal is, for example, 3~5μm.
[0044] The second metal stack structure is in the opposite direction of the set direction, for example, Ti / Al / Ti / TiN; it can also be replaced with Ti / AlSiCu / Ti / TiN, TaN / Al / Ta; when CMOS compatibility is not required, it can be replaced with electroplated thick Cu+Ni / Au.
[0045] To balance the device's electrical performance, heat dissipation capacity, and manufacturing process window, this embodiment also optimizes and limits key geometric dimensions. Preferably, the substrate thickness is 50~200μm. Examples of substrate thicknesses include 50μm, 70μm, 90μm, 110μm, 130μm, 150μm, 170μm, 190μm, and 200μm. This thickness range is the result of a trade-off between multiple factors: if the thickness is too thin, the substrate's mechanical strength is insufficient, making it prone to fragmentation or severe warping during thinning and via etching; if the thickness is too thick, on the one hand, it leads to an excessively large aspect ratio of the vias, increasing the difficulty of etching and filling; on the other hand, although the vertical isolation distance between the source and drain increases, the marginal benefit of reducing capacitance diminishes, and it is not conducive to the conduction of channel heat to the back side.
[0046] Preferably, the thickness of the first metal layer is 10~50μm, and the coverage of the first metal layer on the substrate surface is not less than 60%. The thickness of the first metal layer is, for example, 10μm, 20μm, 30μm, 40μm, or 50μm. As the source lead and heat dissipation substrate on the back side, the thickness and coverage of the first metal layer directly determine the parasitic resistance and thermal resistance of the device. A higher coverage ensures that the source current can be uniformly distributed on the back side, avoiding the generation of local hot spots, and also provides a low-resistance direct heat dissipation path for channel heat.
[0047] In a preferred embodiment, the power semiconductor device further includes: a Kelvin source pad disposed on a region outside the active region of the first dielectric layer; a third top layer metal disposed in a region of the second dielectric layer corresponding to the Kelvin source pad, the Kelvin source pad being electrically connected to the third top layer metal for being led out. Specifically, the Kelvin source pad is a dedicated signal terminal independent of the first metal layer carrying the main power current. It is directly connected to the source reference potential point inside the active region through an independent conductive path in the first dielectric layer, and led out to the third top layer metal on the front side through a via in the second dielectric layer. This independent four-terminal lead-out architecture completely decouples the return path of the drive circuit from the main power circuit physically. During high-frequency switching, when a transient current of tens of amperes flows through the first metal layer and the second conductive channel on the back side, an induced voltage spike will inevitably be generated on the parasitic inductance; if the drive ground line and the power ground line share the same terminal, this induced voltage will be directly superimposed on the gate-source drive signal, causing misleading turn-on or turn-off delay. By setting Kelvin source pads, the drive circuit only senses the pure source potential inside the chip, thereby effectively eliminating common-mode noise interference caused by high-current commutation and significantly improving the accuracy of gate drive and the electromagnetic compatibility of the system. This invention uses independent small arrays of through-silicon vias or fine M1→top-layer metal paths to bring out the Kelvin source outside the power source through-silicon via array, eliminating the interference of induced voltage on the high-current path to the gate drive.
[0048] In a preferred embodiment, the second conductive channel includes an array of through-silicon vias (TSVs) extending through the substrate along a predetermined direction. Compared to a single large-sized TSV, an array of small-sized TSVs can significantly reduce the risk of thermomechanical stress concentration in a single TSV while maintaining the total conductive cross-sectional area, and also provide a more uniform current distribution and heat dissipation path.
[0049] Further preferably, the diameter of a single through-silicon via (TSV) in the TSV array is 5–50 μm; the distance between adjacent TSVs in the TSV array is 1.5–10 times the diameter of a single TSV. The diameter of a single TSV is, for example, 5 μm, 10 μm, 20 μm, 30 μm, 40 μm, or 50 μm. The distance between adjacent TSVs in the TSV array is 1.5, 2, 3, 4, 5, 6, 7, 8, 9, or 10 times the diameter of a single TSV. The thickness of the insulating layer on the inner wall of the TSV is, for example, 100 nm–1 μm; the thickness of the barrier layer is, for example, 5–50 nm; the total number of parallel TSVs satisfies the requirement that the source-end interconnection ≤0.05 mΩ, to accommodate sub-milliohm devices.
[0050] The through-silicon via (TSV) filler metal is, for example, Cu, W, or a Cu-W composite. The insulating layer on the inner wall of the TSV is, for example, SiO2, Si3N4, or Al2O3. The diffusion barrier layer of the TSV is, for example, TaN, TiN, Ta, Ti, or Ru. The through-hole metal of the first conductive channel and each conductive path is, for example, W, Cu, Co, or Ru. The first metal layer is, for example, electroplated thick Cu, Cu / Ni / Ag, or Cu / Ni / Au. Types of power semiconductor devices with double-sided source-drain leads include, for example: p-GaN gate enhancement-mode high electron mobility transistors, hybrid metal-insulator-semiconductor / p-GaN gate transistors, depletion-mode gallium nitride devices, and generalized lateral gallium nitride metal-oxide-semiconductor field-effect transistors. The preferred operating voltage for these devices is 30~900V. Packaging options include disk-gate array packages, dual in-line flat no-lead packages, flip-chip, copper clips, copper clips with PCB embedding, and fan-out packages.
[0051] The power semiconductor device with dual-sided source and drain provided in this embodiment of the invention has drain and gate signals led to the top metal layer on the front side of the chip via tungsten front vias and multilayer metal stacking, and source signals led to the back side of the chip via a copper-silicon via array and a thick copper back redistribution layer. There is no source plane below the top metal layer on the front side. At the same time, a substrate electrode is pre-fabricated before the fabrication process of the second, third and fourth metal layers (collectively referred to as the M1 layer) to clamp the Si substrate to the source potential. The back silicon vias are fabricated using a one-step Bosch process with the thickened second metal layer as the natural etch stop layer. First, this invention significantly reduces drain-source capacitance and output capacitance by physically separating the source and drain at the device level. Second, this invention significantly reduces the parasitic interconnect resistance of sub-milliohm devices through a combination of short tungsten front-side vias, thick M1, thick top-layer metal drain, arrayed copper back-side vias, and thick back-side source pads. Third, this invention provides a low-resistance thermal path at the device level by directly connecting the copper-silicon via array beneath the channel, reducing junction-to-case thermal resistance. Fourth, this invention fundamentally eliminates the second metal layer thickness loss and via-second metal layer interface voids caused by conventional two-step via processes using a one-step back-side Bosch etching method terminated by the second metal layer, improving the integrity and long-term reliability of via interconnects. This invention is particularly suitable for high-frequency, high-current-density applications with on-resistance below 1mΩ and extreme sensitivity to output capacitance (especially drain-source capacitance).
[0052] Application areas of this invention include, for example: 48V→12V / 1V high-frequency, high-current-density DC-DC converters for data centers; onboard vertical power supply architectures for AI accelerator cards / graphics processors; server power supply units and telecommunications power supplies; onboard chargers and onboard DC-DC converters, 48V main mild hybrid systems; high-efficiency switching power supplies; wireless charging transmitters and high-frequency inverter modules; and high-density gallium nitride power modules in fast charging adapters for consumer electronics.
[0053] See Figure 2 The diagram illustrates the output capacitor C of the conventional wiring structure and the source-drain double-sided lead-out structure of this invention. oss The curve showing the change in drain voltage demonstrates the significant advantage of this invention in terms of parasitic capacitance. Figure 2 Data shows that in the low-voltage region, the parasitic capacitance generated by the overlap of source and drain metal wiring in the traditional structure accounts for a significant portion of the output capacitance C. oss The total proportion is approximately 30%; however, in the high-voltage region, due to the depletion layer expansion leading to a decrease in intrinsic capacitance, the proportion of wiring overlap capacitance further increases to approximately 70%. In contrast, the structure of this invention, by eliminating the maximum source-to-drain plane beneath the top metal layer and increasing the vertical coupling distance between the source and drain to the order of substrate thickness, has a significantly reduced output capacitance C. oss The curve is significantly lower than that of the conventional structure across the entire voltage range. Specifically, the drain-source capacitance C of this example device... dsCompared to traditional devices of the same specifications, the output capacitance C is reduced by approximately 34%. oss This represents a reduction of approximately 22%. This improvement directly leads to a significant decrease in switching losses, enabling the device to maintain higher conversion efficiency in high-frequency hard-switching topologies.
[0054] This invention provides two specific examples of power semiconductor devices with double-sided source-drain leads. Example 1 is a 100V / submilliohm pGaN-HEMT with the following parameters: substrate thickness = 80μm; through-silicon via (TSV) diameter = 15μm, TSV pitch = 30μm; the first metal layer is a 25μm thick Cu layer with 85% coverage; the Al-Cu body layer in the top metal layer is adjusted to 4.5μm. The chip is 2×2mm. 2 The number of source silicon vias is ~3000, and the source interconnect resistance is <0.03mΩ. Device performance: single-chip drain-source on-resistance is ~0.6mΩ, and interconnect parasitic contribution is <5%; drain-source capacitance is reduced from ~350pF to ~230pF; the common-mode noise peak caused by dV / dt is reduced by ~6dB after substrate grounding. It can be applied to 2MHz-level 48V→12V / 1V data center vertical power supply, and the switching loss is reduced by ≥25% compared with existing grid array packaged GaN HEMTs.
[0055] Example 2 illustrates examples of device package selection. (a) Grid array package / Dual in-line flat no-leads package: The back-side source heavy routing layer uses solder paste to attach leadframes to the chip pads as source leads, and the front-side drain / gate is led out using bonding wires or copper clips. (b) Flip chip package: The chip faces down, the top-side metal drain / gate is connected to the package substrate via bumps or copper pillars, and the back-side source heavy routing layer faces up and is connected to the heat sink. (c) Copper clip package: The back-side source heavy routing layer uses sintered silver to attach leadframes, the front-side copper clip connects to the drain, and bonding wires connect to the gate. (d) Copper clip embedded in printed circuit board package: The back-side source heavy routing layer is sintered to the inner copper foil of the printed circuit board, and the front-side top-side metal is directly interconnected through laser-drilled microvias on the printed circuit board, eliminating the need for bumps and enabling double-sided heat dissipation.
[0056] Based on the same inventive concept, this invention also provides a method for fabricating a power semiconductor device with both source and drain leads on both sides, used to fabricate the power semiconductor device with both source and drain leads on both sides as described in the above embodiments. The fabrication method includes the following steps S100-S700.
[0057] Step S100: The substrate, semiconductor epitaxial layer, active region and first dielectric layer are sequentially prepared along the set direction. The active region includes source ohmic contact, drain ohmic contact and gate metal.
[0058] The substrate is preferably a silicon-based gallium nitride substrate. The semiconductor epitaxial layer includes, for example, an AlN nucleation layer, a stress buffer layer (AlGaN graded or superlattice), a GaN channel layer, an AlGaN barrier layer, and a p-GaN gate cap layer. The device structure after fabrication of the substrate, semiconductor epitaxial layer, and active region is as follows: Figure 3 As shown.
[0059] In step S200, a groove is formed in the region outside the active region in the first dielectric layer and the semiconductor epitaxial layer, and the bottom of the groove is located on the substrate surface or inside the substrate.
[0060] In the reserved area outside the active region of the chip (usually the annular area inside the chip sealing ring, or the ground strip area at both ends of the source array), a photolithography + inductively coupled plasma dry etching process is used to etch through the first dielectric layer and the semiconductor epitaxial layer until the silicon substrate is exposed.
[0061] In step S300, along a set direction, a first conductive channel, a first conductive path, and a second conductive path are respectively processed in the regions of the first dielectric layer corresponding to the source ohmic contact, the drain ohmic contact, and the gate metal.
[0062] Specifically, the source, drain, and gate ohmic contacts are led out to the second, third, and fourth metal layers respectively by using a Ti / TiN barrier layer, chemical vapor deposition tungsten filling, and chemical mechanical polishing planarization.
[0063] The device structure after fabricating the first conductive channel, the first conductive path, and the second conductive path in the first dielectric layer is as follows: Figure 4 As shown, the device structure after creating grooves in the regions outside the active region in the first dielectric layer and the semiconductor epitaxial layer is as follows. Figure 5 As shown.
[0064] In step S400, a second metal layer is prepared inside the groove and in the region corresponding to the source ohmic contact in the first dielectric layer, and a first conductive channel connects the second metal layer and the source ohmic contact.
[0065] In step S500, a third metal layer and a fourth metal layer are respectively fabricated on the first conductive path and the second conductive path; a second dielectric layer is fabricated on the first dielectric layer, the second metal layer, the third metal layer, and the fourth metal layer. A corresponding first top metal and a second top metal are respectively disposed in the regions of the second dielectric layer corresponding to the third metal layer and the fourth metal layer. A third conductive path connecting the third metal layer and the first top metal, and a fourth conductive path connecting the fourth metal layer and the second top metal are also fabricated within the second dielectric layer. The device structure after fabricating the second metal layer, the third metal layer, and the fourth metal layer is as follows: Figure 6 As shown.
[0066] The drain and gate pads are led upwards through interlayer vias to the top layer metal on the front side of the chip. The top layer metal adopts a CMOS-compatible Ti / Al / Ti / TiN metal system (typical film layer combination: bottom Ti barrier / adhesion layer 30~80nm + main Al or Al-Cu layer 3~5μm + upper Ti barrier layer 30~80nm + top TiN anti-reflection passivation layer 30~100nm; total thickness of top layer metal 3~5μm), and is fabricated by sputtering deposition and dry etching patterning. This top layer metal consists only of drain and gate pads, and no source maximum plane is set below it. Independent Kelvin source pads can be selectively set (led out through independent small array silicon vias or fine lead paths from the second metal layer to the top layer metal) as low-noise reference terminals for the drive circuit.
[0067] In a preferred embodiment, before processing the second conductive channel (between steps S500 and S600), the preparation method further includes: coating the surfaces of the first and second top layer metals with temporary bonding adhesive, and then performing wafer-level temporary bonding with the release carrier; thinning the side of the substrate away from the semiconductor epitaxial layer, wherein the thickness of the thinned substrate is 50~200μm. The temporary bonding adhesive may be, for example, laser release adhesive, thermal release adhesive, or mechanical release adhesive, and its thickness may be, for example, 10~30μm; the temporary bonding temperature shall not exceed 200°C to ensure that the completed front-side metal stack is not damaged.
[0068] Specifically, a temporary bonding adhesive is applied to the top metal surface of the wafer after the front-side processing is completed. This adhesive is then vacuum-bonded to a glass substrate at a low temperature (≤ 200℃) to achieve wafer-level temporary bonding. The bonding adhesive layer is 30~80μm thick and serves as a stress buffer and surface protection during the back-side thinning and etching processes. After bonding, the back side of the silicon-based gallium nitride wafer substrate is sequentially mechanically ground (roughly ground to approximately 30μm remaining from the target thickness) → finely ground (to approximately 5μm remaining from the target thickness). The remaining substrate thickness after thinning is typically 50~200μm, selected within this range based on the through-silicon via (TSV) process capabilities and device voltage level. The thinning process must control the overall wafer thickness uniformity to ≤2μm to ensure that the subsequent one-step Bosch etching simultaneously reaches the second metal layer stop layer across the entire wafer.
[0069] Step S600: A second conductive channel is formed in the substrate, extending through the substrate in a set direction, and one end of the second conductive channel is connected to the second metal layer at the bottom of the groove.
[0070] Preferably, the second metal layer includes a first barrier layer, a first adhesive layer, a conductive layer, a second barrier layer, and a second adhesive layer sequentially disposed in the predetermined direction. The second conductive channel includes an array of through-silicon vias penetrating the substrate along the predetermined direction, wherein the first barrier layer serves as an etching stop layer when etching the through-silicon vias in the substrate.
[0071] The inner wall of the through-silicon via (TSV) is sequentially deposited with a SiO2 / SiN insulating layer (100 nm~1 μm), a TaN / TiN barrier layer (5~50 nm), and a Cu seed layer, followed by Cu electroplating for filling. Cu forms a void-free metal-metal contact with the thickened source pad in M1: Since the second metal layer acts as a natural stop layer in the first etching step, there is no need for secondary etching of the epitaxial structure. The surface of the second metal layer at the bottom of the TSV is a complete and flat metal surface before metallization, making it less likely to form bottom voids when Cu is electroplated from bottom to top for filling.
[0072] In step S700, a first metal layer is prepared on the side of the substrate away from the semiconductor epitaxial layer, and the first metal layer is connected to the other end of the second conductive channel.
[0073] Thick Cu (10~50μm) is electroplated and patterned on the back of the chip to cover the projection area of the source region and the substrate connection structure, with a coverage of ≥ 60%. It is connected in parallel with all source silicon vias to form the source bottom pad on the back of the chip. The surface is treated with Ni / Ag or Ni / Au to achieve a sinterable / solderable surface.
[0074] Through the above-described fabrication method, this invention achieves high-reliability manufacturing of power semiconductor devices with both source and drain leads on both sides. In particular, by reusing the bottom barrier layer of the second metal layer as a stop layer for through-silicon via (TSV) etching, and combining it with a high-precision temporary bonding thinning process, a one-step Bosch etching process was successfully implemented. This fundamentally solves the metal layer damage and interface void failure modes present in traditional two-step processes, significantly improving the long-term reliability and mass production yield of the device, while simplifying the process flow and reducing manufacturing costs. The overshoot depth of the Bosch etching is no greater than 0.3 μm, ensuring that the TiN surface is etched in but not pierced.
[0075] The power semiconductor device with source and drain leads on both sides and the fabrication method thereof provided in the embodiments of the present invention have the following beneficial effects.
[0076] (1) The drain-source capacitance is significantly reduced and the output capacitance is significantly reduced. The source and drain are physically separated at the device level. There is no passive maximum plane under the top metal layer on the front side. The only coupling between the two is through a small local area of the source pad in the second metal layer, and they are separated by a substrate thickness of 50~200μm. The drain-source capacitance is reduced by 25%~40%, and the output capacitance is reduced by 15%~30%, which greatly reduces the switching loss and the rise slope of the hard switching voltage.
[0077] (2) The parasitic interconnection of sub-milliohm devices is significantly reduced. The source path is changed to "second metal layer → second metal layer terminated short silicon via → thick back RDL → external substrate", and the source interconnection resistance is less than 0.05mΩ; the drain path is composed of a short conductive path + top metal, with low resistance throughout; the total parasitic interconnection is reduced by more than 60% compared with the traditional front three-terminal lead-out scheme.
[0078] (3) Optimization of device-level thermal resistance path. The back copper-silicon via array + thick RDL directly guides the channel heat to the back of the chip, which is equivalent to "metallizing" the thermal conduction path between the channel and the back. Downstream packaging can further reduce the system junction thermal resistance on the basis of the low thermal resistance at the device level.
[0079] (4) Dynamic potential clamping of the substrate improves device performance. The substrate is clamped to the source through the front substrate contact + second metal layer + back silicon via / RDL, which improves the dynamic drain-source on-resistance by 10%~30%, significantly reduces common-mode electromagnetic interference, and improves high-voltage breakdown consistency; at the same time, the electrical stress of the insulating layer on the sidewall of the silicon via is limited to the drain-source voltage range, which improves the long-term reliability of the silicon via.
[0080] (5) It fundamentally eliminates the second metal layer damage and bottom void failure modes of conventional two-step through-silicon via (TSV) processes. The thickened TiN at the bottom of the second metal layer serves as a natural etching stop layer, with a selectivity ratio of more than 100:1 for the three etching chemicals SF6 / C4F8, BCl3 / Cl2, and CHF3 / O2. When the one-step through-etch is completed, the bottom of the TSV directly exposes a complete, flat, and undamaged TiN metal surface. Subsequent sidewall insulation, bottom thin etchback, and electroplating filling all work on the already intact TiN surface. There is no consumption of the main Al layer of the second metal layer by secondary etching, nor are there bottom voids caused by secondary etching residues. The integrity and long-term reliability of the TSV interconnect are significantly improved, and the process cycle is shortened by 15% to 20%. This is the key process foundation for the large-scale application of high-current silicon-based gallium nitride power TSVs.
[0081] (6) Fully CMOS compatible and compatible with existing 8-inch silicon-based gallium nitride production lines; flexible packaging, with the device itself not bound to any specific packaging architecture.
[0082] It should be understood that the above embodiments are merely illustrative of the technical concept and features of the present invention, and are intended to enable those skilled in the art to understand the content of the present invention and implement it accordingly. They should not be construed as limiting the scope of protection of the present invention. All equivalent changes or modifications made in accordance with the spirit and essence of the present invention should be covered within the scope of protection of the present invention.
Claims
1. A power semiconductor device with both source and drain leads, characterized in that, include: A first metal layer, a substrate, a semiconductor epitaxial layer, an active region, and a first dielectric layer are sequentially disposed in a predetermined direction. The active region includes a source ohmic contact, a drain ohmic contact, and a gate metal. A groove is formed in the region outside the active region of the first dielectric layer and the semiconductor epitaxial layer, and the bottom of the groove is located on the substrate surface or inside the substrate; a second metal layer is provided inside the groove and in the region corresponding to the source ohmic contact in the first dielectric layer; a first conductive channel connecting the second metal layer and the source ohmic contact is provided in the first dielectric layer. A second conductive channel is provided in the substrate to connect the second metal layer at the bottom of the groove and the first metal layer, so as to connect the source ohmic contact to the first metal layer. The power semiconductor device further includes: a third metal layer and a fourth metal layer, respectively disposed in the regions of the first dielectric layer corresponding to the drain ohmic contact and the gate metal; The second dielectric layer covers the first dielectric layer, the second metal layer, the third metal layer and the fourth metal layer. The regions in the second dielectric layer corresponding to the third metal layer and the fourth metal layer are respectively provided with the first top metal and the second top metal. Conductive paths are also provided in the first dielectric layer and the second dielectric layer to electrically connect the drain ohmic contact, the third metal layer and the first top metal layer, and to electrically connect the gate metal, the fourth metal layer and the second top metal layer.
2. The power semiconductor device with source and drain leads on both sides according to claim 1, characterized in that, The second metal layer and / or the third metal layer and / or the fourth metal layer adopt a first metal stack structure; The first metal stack structure includes a first barrier layer, a first adhesive layer, a first main conductive layer, a second barrier layer, and a second adhesive layer arranged sequentially in the predetermined direction.
3. The power semiconductor device with source and drain leads on both sides according to claim 2, characterized in that, The material of the first barrier layer includes: TiN, TaN, Ta, or W; And / or, the material of the first main conductive layer includes: Al or Al-based conductive alloy; And / or, the thickness of the first barrier layer is 0.2~0.5μm; And / or, the first barrier layer has an etching selectivity ratio greater than 100:1 relative to the etching chemicals used in the processing of the second conductive channel.
4. The power semiconductor device with source and drain leads on both sides according to claim 1, characterized in that, The first top layer metal and / or the second top layer metal adopt a second metal stack structure; The second metal stack structure includes a barrier adhesion layer, a second main conductive layer, a third barrier layer, and an anti-reflection passivation layer, which are sequentially disposed in the set direction.
5. The power semiconductor device with source and drain leads on both sides according to claim 1, characterized in that, The thickness of the substrate is 50~200μm; And / or, the thickness of the first metal layer is 10~50μm; And / or, the coverage of the first metal layer on the substrate surface is not less than 60%.
6. The power semiconductor device with source and drain leads on both sides according to claim 1, characterized in that, The power semiconductor device further includes: a Kelvin source pad disposed on a region outside the active region of the first dielectric layer; a third top layer metal disposed in a region of the second dielectric layer corresponding to the Kelvin source pad, and the Kelvin source pad being electrically connected to the third top layer metal to be led out; And / or, the second conductive channel includes an array of through-silicon vias extending through the substrate along the predetermined direction.
7. The power semiconductor device with source and drain leads on both sides according to claim 6, characterized in that, The diameter of a single through-silicon via in the silicon via array is 5~50μm; And / or, the distance between adjacent through-silicon vias in the through-silicon via array is 1.5 to 10 times the diameter of a single through-silicon via.
8. A method for fabricating a power semiconductor device with both source and drain leads, characterized in that, include: A substrate, a semiconductor epitaxial layer, an active region, and a first dielectric layer are sequentially prepared along a predetermined direction. The active region includes a source ohmic contact, a drain ohmic contact, and a gate metal. A groove is formed in the region outside the active region in the first dielectric layer and the semiconductor epitaxial layer, and the bottom of the groove is located on the substrate surface or inside the substrate. Along the predetermined direction, a first conductive channel, a first conductive path, and a second conductive path are respectively processed in the regions of the first dielectric layer corresponding to the source ohmic contact, the drain ohmic contact, and the gate metal. A second metal layer is fabricated inside the groove and in the region corresponding to the source ohmic contact in the first dielectric layer, and a first conductive channel connects the second metal layer and the source ohmic contact. A third metal layer and a fourth metal layer are respectively fabricated on the first conductive path and the second conductive path; a second dielectric layer is fabricated on the first dielectric layer, the second metal layer, the third metal layer and the fourth metal layer, and a corresponding first top metal and a second top metal are respectively provided in the regions of the second dielectric layer corresponding to the third metal layer and the fourth metal layer; a third conductive path connecting the third metal layer and the first top metal, and a fourth conductive path connecting the fourth metal layer and the second top metal are also fabricated in the second dielectric layer. A second conductive channel is formed in the substrate along the predetermined direction, and one end of the second conductive channel is connected to the second metal layer at the bottom of the groove. A first metal layer is prepared on the side of the substrate away from the semiconductor epitaxial layer, and the first metal layer is connected to the other end of the second conductive channel.
9. The method for fabricating a power semiconductor device with source and drain leads on both sides according to claim 8, characterized in that, The second metal layer includes a first barrier layer, a first adhesive layer, a conductive layer, a second barrier layer, and a second adhesive layer disposed sequentially in the predetermined direction; The second conductive channel includes an array of through-silicon vias extending through the substrate along the set direction, wherein the first barrier layer is used as an etching stop layer when etching the through-silicon vias in the substrate.
10. The method for fabricating a power semiconductor device with source and drain leads on both sides according to claim 8, characterized in that, Before fabricating the second conductive channel, the preparation method further includes: After applying temporary bonding adhesive to the surfaces of the first and second top metal layers, wafer-level temporary bonding is performed with the release substrate; The side of the substrate away from the semiconductor epitaxial layer is thinned, and the thickness of the thinned substrate is 50~200μm.