Crystalline silicon solar cells and their fabrication methods

By using copper sulfide as a hole-selective transport layer in crystalline silicon solar cells, and combining it with doping and interface layer optimization, the parasitic absorption and interface passivation problems of traditional materials are solved, achieving efficient photoelectric conversion and improved stability.

CN123124455APending Publication Date: 2026-11-17ZHEJIANG SCI-TECH UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611408929.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-11
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

In traditional crystalline silicon solar cells, hole-selective contact materials suffer from problems such as strong parasitic absorption, poor thermal stability, low conductivity, and unsatisfactory interface passivation, which limit the improvement of cell efficiency.

Method used

Copper sulfide material is used as a hole-selective transport layer. The stoichiometric ratio of copper to sulfur is controlled to be less than or equal to 1.2. Metal cations such as Ga3+, Al3+, and Pb2+ are doped. Combined with an alumina interface layer and a molybdenum oxide layer, band matching and interface passivation are optimized.

Benefits of technology

This achieves highly efficient hole selectivity and transport, improving the photoelectric conversion efficiency of crystalline silicon solar cells and significantly enhancing the cell's conversion efficiency and stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123124455A_ABST
    Figure CN123124455A_ABST
Patent Text Reader

Abstract

This invention belongs to the field of batteries, specifically relating to crystalline silicon solar cells and their fabrication methods. It sequentially includes a first electrode, a silicon nitride passivation layer, and a phosphorus-doped n-type electrode. + The solar cell comprises a crystalline silicon layer, a p-type monocrystalline silicon substrate, a hole-selective transport layer, and a second electrode. The hole-selective transport layer includes copper sulfide material, wherein the stoichiometric ratio of copper to sulfur in the copper sulfide material is less than or equal to 1.2. This hole-selective transport layer exhibits excellent hole transport performance, high stability, and low-temperature fabrication advantages, making it suitable for crystalline silicon heterojunction solar cells and other novel crystalline silicon solar cells. It can significantly improve cell conversion efficiency and thermal stability, demonstrating promising application prospects.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of batteries, specifically relating to crystalline silicon solar cells and their preparation methods. Background Technology

[0002] Currently, the contradiction between the depletion crisis of fossil fuels and the ever-increasing global energy demand is becoming increasingly acute, and the resulting air pollution and climate change are major challenges facing all of humanity. Against this backdrop, solar photovoltaic power generation, as an inexhaustible and renewable energy source, is undoubtedly one of the core solutions for the future energy system.

[0003] Photovoltaic technology is the cornerstone of the global energy transition, with crystalline silicon (c-Si) solar cells holding over 95% of the commercial market share due to their mature industry chain and stable performance. In crystalline silicon solar cells, achieving efficient and stable hole-selective contact is crucial for improving cell conversion efficiency and reliability. Traditional high-efficiency silicon heterojunction (SHJ) technology uses hydrogenated amorphous silicon (a-Si:H) as the contact layer, which suffers from strong parasitic absorption and poor thermal stability. Transition metal oxides (such as MoO₂)... X V2O X While p-type oxides (such as NiO and Cu2O) have made progress in improving the efficiency of hole-selective materials, their performance is sensitive to the work function and their stability is poor. P-type oxides generally have better stability, but they also suffer from low conductivity and poor passivation at the silicon interface, which limits further improvements in battery efficiency. Summary of the Invention

[0004] This invention relates to crystalline silicon solar cells and their fabrication methods. The hole-selective transport layer can effectively achieve high-efficiency selectivity and transport of holes, thereby improving the photoelectric conversion efficiency of crystalline silicon solar cells.

[0005] To address the aforementioned technical problems, the first aspect of this invention provides a crystalline silicon solar cell, comprising, in sequence, a first electrode, a silicon nitride passivation layer, a phosphorus-doped n+ crystalline silicon layer, a p-type monocrystalline silicon substrate, a hole-selective transport layer, and a second electrode. The hole-selective transport layer comprises a copper sulfide material, wherein the stoichiometric ratio of copper to sulfur in the copper sulfide material is less than or equal to 1.2. That is, the copper sulfide material has a large number of copper vacancies and a very small number of sulfur vacancies.

[0006] In some embodiments, the stoichiometric ratio of copper to sulfur in the copper sulfide material is less than or equal to 0.99.

[0007] In some embodiments, the copper sulfide material is further doped with a first metal cation, the first doped metal cation including Ga. 3+ Al 3+ Pb2+ One or more of them.

[0008] In some embodiments, the copper vacancy concentration in copper sulfide doped with the first metal cation is a first concentration, and the sulfur vacancy concentration is a second concentration; the copper vacancy concentration in copper sulfide not doped with the first metal cation is a third concentration, and the sulfur vacancy concentration is a fourth concentration, wherein the first concentration is greater than the third concentration, and the second concentration is less than the fourth concentration.

[0009] In some implementations, the work function of the hole-selective transport layer is ≥5.0 eV.

[0010] In some embodiments, the thickness of the hole-selective transport layer is 5 to 40 nm.

[0011] In some embodiments, an alumina interface layer is included between the p-type single-crystal silicon substrate and the hole-selective transport layer.

[0012] In some embodiments, the thickness of the alumina interface layer is 0.5~1.5 nm.

[0013] In some embodiments, the copper sulfide material includes monovalent copper ions, divalent copper ions, monovalent sulfide ions, and divalent sulfide ions, wherein Cu 2+ :Cu + Greater than or equal to 50%, S 2- :S - Greater than or equal to 50%.

[0014] In some embodiments, the side of the hole-selective transport layer facing away from the p-type single-crystal silicon substrate further includes a molybdenum oxide layer or a vanadium-doped molybdenum oxide layer.

[0015] A second aspect of the present invention provides a method for preparing a crystalline silicon solar cell, comprising:

[0016] A substrate is provided, the substrate comprising a first electrode, a silicon nitride passivation layer, and a phosphorus-doped n-type electrode sequentially disposed therefrom. + crystalline silicon layer and p-type single-crystal silicon substrate;

[0017] A first precursor solution is spin-coated onto a p-type single-crystal silicon substrate, followed by a first annealing treatment to obtain a first film layer; wherein, the first precursor solution includes Cu... 2+ A methanol solution, wherein Cu in the first precursor solution 2+ The molar concentration is 0.01-0.05 mol / L, the first annealing time is 1-5 minutes, and the atmosphere for the first annealing is air, reducing atmosphere, inert atmosphere or vacuum.

[0018] A second precursor solution is spin-coated onto the first film layer. After reacting for 10-60 seconds, a second film layer is formed. The second precursor includes S. 2- The S 2- The molar concentration is 0.01-0.05 mol / L;

[0019] The second film layer is washed and subjected to a second annealing treatment to obtain a hole selective transport layer; the temperature of the second annealing treatment is 100-200℃, the time of the second annealing treatment is 10-25 minutes, and the atmosphere of the second annealing treatment is air atmosphere, reducing atmosphere, inert atmosphere or vacuum conditions.

[0020] A second electrode is fabricated on the hole-selective transport layer.

[0021] In some embodiments, the first precursor solution further includes a first metal cation, the first metal cation including Ga. 3+ Al 3+ Pb 2+ One or more of the following, wherein the first metal cation reacts with the Cu 2+ The molar ratio is (0.5~3):100.

[0022] In some embodiments, fabricating the second electrode on the hole-selective transport layer includes:

[0023] An alumina interface layer is prepared on the hole selective transport layer by atomic layer deposition. Preferably, the thickness of the alumina interface layer is 0.5~1.5 nm.

[0024] A third aspect of the present invention provides a crystalline silicon solar cell, comprising, in sequence, a first electrode, an electron transport layer, a light absorption layer, a hole selective transport layer, and a second electrode, wherein the light absorption layer comprises N-type silicon; wherein the hole selective transport layer comprises copper sulfide material, and the stoichiometric ratio of copper to sulfur in the copper sulfide material is less than or equal to 1.2.

[0025] Beneficial effects:

[0026] (1) In the crystalline silicon solar cell of the present invention, the hole-selective transport layer includes copper sulfide. By controlling the stoichiometric ratio of copper to sulfur to be less than or equal to 1.2, the copper sulfide has a high hole concentration and conductivity, and matches the valence band of the monocrystalline silicon substrate. The crystalline silicon solar cell of the present invention is applicable to PN junction silicon crystalline silicon solar cells and silicon heterocrystalline silicon solar cells. Copper sulfide, as a hole-selective transport layer, avoids the negative effects such as Auger recombination and parasitic absorption caused by traditional doped silicon structures.

[0027] (2) The crystalline silicon solar cell of the present invention, wherein the copper sulfide high-performance hole-selective transport layer comprises a layer formed by doping Ga 3+ Al 3+ or Pb 2+ The inherent acceptor defect concentration of copper vacancies in the high-performance hole-selective transport layer of copper sulfide can be increased. Doping with the first metal cation enhances the copper vacancy concentration, thereby increasing the work function and optimizing band matching with p-Si, promoting hole transport via the valence band. Simultaneously, reducing the sulfur vacancy concentration achieves passivation of the silicon interface through interfacial sulfur enrichment, suppressing minority carrier recombination. These two processes work synergistically to achieve highly efficient selective collection and separation of holes. The primary hole transport mechanism in the high-performance hole-selective transport layer of copper sulfide / c-Si heterojunction is valence band matching transport. Valence band matching transport requires the high-performance hole-selective transport layer of copper sulfide to contain a large number of copper vacancy defect levels and a reduction in sulfur vacancy defect levels to achieve high hole selectivity. Furthermore, stacking a molybdenum oxide layer with a higher work function or a vanadium-doped molybdenum oxide layer on the copper sulfide surface further induces band bending, enhancing hole selectivity.

[0028] (3) Crystalline silicon solar cells based on a high-performance hole-selective transport layer of copper sulfide exhibit significantly improved photoelectric performance. Example 1 (doped and containing an Al2O3 interface layer) achieved a high conversion efficiency (PCE) of 21.89%, compared to the undoped Example 2 (20.53%) and the Cu-only example. 1.1 Example 6 (18.63%) of S showed significant advantages. Even without the Al2O3 layer (Example 3, 20.26%), it was far superior to the base cell without any transport layer (Comparative Example 1, 15.32%), demonstrating its core value.

[0029] (4) Experiments have shown that Ga 3+ The doped copper sulfide transport layer at different thicknesses (e.g., 7 nm, 21 nm, 34 nm) all exhibited better performance than undoped copper sulfide (see Table 1, Examples 3, 7, 8 and 6), indicating that the doping strategy has good applicability.

[0030] (5) Crystalline silicon solar cells based on a hole-selective transport layer of copper sulfide / molybdenum oxide stack exhibit superior photoelectric performance. Example 9 (doped and containing an Al2O3 interface layer) achieved a maximum conversion efficiency of 23.09% for p-type silicon, and Example 10 (doped and containing an amorphous silicon interface layer) achieved a maximum conversion efficiency of 23.37% for n-type silicon heterojunction, both higher than devices containing a single-layer hole transport layer, demonstrating the importance of bandgap modulation.

[0031] (6) The preparation method of the present invention is simple, operates at low temperature (≤200°C) throughout, has strong compatibility and high efficiency, and has good application prospects. Attached Figure Description

[0032] Figure 1 This is a schematic diagram of the fabrication of a high-performance hole-selective transport layer of copper sulfide according to an embodiment of the present invention;

[0033] Figure 2 This is a schematic diagram of the structure of a crystalline silicon solar cell according to an embodiment of the present invention;

[0034] Figure 3a The τ of p-Si with copper sulfide hole selective transport layer passivation in Embodiment 1 and Comparative Example 1 of this invention is... eff picture;

[0035] Figure 3b These are the JV curves of the crystalline silicon solar cells of Embodiment 1 and Comparative Example 1 of the present invention;

[0036] Figure 4a This is a band structure simulation diagram of the crystalline silicon solar cell of Embodiment 2 of the present invention;

[0037] Figure 4b This is a band structure simulation diagram of the crystalline silicon solar cell of Embodiment 1 of the present invention;

[0038] Figure 5a These are the effective lifetime-minority carrier density curves of the crystalline silicon solar cells in Examples 3-6 of this invention;

[0039] Figure 5b These are the JV curves of the crystalline silicon solar cells of Examples 3-6 of this invention;

[0040] Figure 6a These are the effective lifetime-minority carrier density curves of the crystalline silicon solar cells in Examples 7-8 of this invention;

[0041] Figure 6b These are the JV curves of the crystalline silicon solar cells of Examples 7-8 of this invention;

[0042] Figure 7 This is a band structure simulation diagram of the crystalline silicon solar cell of Embodiment 9 of the present invention.

[0043] Figure 8a This is a schematic diagram of the structure of the crystalline silicon solar cell of Embodiment 10 of the present invention;

[0044] Figure 8b This is the JV curve of the crystalline silicon solar cell of Embodiment 10 of the present invention. Detailed Implementation

[0045] The first aspect of this application provides a crystalline silicon solar cell, comprising, in sequence, a first electrode, a silicon nitride passivation layer, a phosphorus-doped n+ crystalline silicon layer, a p-type monocrystalline silicon substrate, a hole-selective transport layer, and a second electrode. The hole-selective transport layer comprises a copper sulfide material, wherein the stoichiometric ratio of copper to sulfur in the copper sulfide material is less than or equal to 1.2. That is, the copper sulfide material has a large number of copper vacancies and a very small number of sulfur vacancies.

[0046] In this embodiment, the CuS high-performance hole-selective transport layer relies on the direct valence band hole transport mechanism. This requires the CuS high-performance hole-selective transport layer to have a high work function, valence band level positions matching the silicon crystals, and a passivation effect of sulfur on the silicon crystals. The high work function and matching valence band level positions require the CuS high-performance hole-selective transport layer to have a high copper vacancy concentration. The passivation effect of interfacial sulfur on the silicon crystals requires the CuS high-performance hole-selective transport layer to have a low sulfur vacancy concentration, i.e., a copper to sulfur stoichiometric ratio Cu:S ≤ 1.2. Cu:S can be 1.2, 1.1, 1, 0.9, 0.8, 0.5, etc.

[0047] In some embodiments, the stoichiometric ratio of copper to sulfur in the copper sulfide material is less than or equal to 0.99.

[0048] In some embodiments, the copper sulfide material is further doped with a first metal cation, the first doped metal cation including Ga. 3+ Al 3+ Pb 2+ One or more of the following. The CuS high-performance hole-selective transport layer is doped with a first metal cation, which is different from the monovalent and divalent copper ions in the CuS high-performance hole-selective transport layer. The first metal cation includes Ga. 3+ Al 3+ or Pb 2+ One or more of them. Ga-doped 3+ Al 3+ or Pb 2+ It can replace Cu in CuS + Ions increase the concentration of copper vacancy intrinsic acceptor defects and suppress the concentration of sulfur vacancy intrinsic donor defects in the CuS high-performance hole-selective transport layer, thereby improving hole selectivity.

[0049] In some embodiments, the copper vacancy concentration in copper sulfide doped with the first metal cation is a first concentration, and the sulfur vacancy concentration is a second concentration; the copper vacancy concentration in copper sulfide not doped with the first metal cation is a third concentration, and the sulfur vacancy concentration is a fourth concentration, wherein the first concentration is greater than the third concentration, and the second concentration is less than the fourth concentration.

[0050] In some implementations, the work function of the hole-selective transport layer is ≥5.0 eV.

[0051] In some embodiments, the thickness of the hole-selective transport layer is 5 to 40 nm.

[0052] In some embodiments, an alumina interface layer is included between the p-type single-crystal silicon substrate and the hole-selective transport layer.

[0053] In some embodiments, the thickness of the alumina interface layer is 0.5~1.5 nm.

[0054] In some embodiments, the copper sulfide material includes monovalent copper ions, divalent copper ions, monovalent sulfide ions, and divalent sulfide ions, wherein Cu 2+ :Cu + Greater than or equal to 50%, S 2- :S - Greater than or equal to 50%.

[0055] In some embodiments, the side of the hole-selective transport layer facing away from the p-type single-crystal silicon substrate further includes a molybdenum oxide layer or a vanadium-doped molybdenum oxide layer.

[0056] The present invention also includes a second aspect providing a method for fabricating a crystalline silicon solar cell, which in some embodiments includes:

[0057] A substrate is provided, the substrate comprising a first electrode, a silicon nitride passivation layer, and a phosphorus-doped n-type electrode sequentially disposed therefrom. + crystalline silicon layer and p-type single-crystal silicon substrate;

[0058] A first precursor solution is spin-coated onto a p-type single-crystal silicon substrate, followed by a first annealing treatment to obtain a first film layer; wherein, the first precursor solution includes Cu... 2+ A methanol solution, wherein Cu in the first precursor solution 2+ The molar concentration is 0.01-0.05 mol / L, the first annealing time is 1-5 minutes, and the atmosphere for the first annealing is air, reducing atmosphere, inert atmosphere or vacuum.

[0059] A second precursor solution is spin-coated onto the first film layer. After reacting for 10-60 seconds, a second film layer is formed. The second precursor includes S. 2- The S 2- The molar concentration is 0.01-0.05 mol / L;

[0060] The second film layer is washed and subjected to a second annealing treatment to obtain a hole selective transport layer; the temperature of the second annealing treatment is 100-200℃, the time of the second annealing treatment is 10-25 minutes, and the atmosphere of the second annealing treatment is air atmosphere, reducing atmosphere, inert atmosphere or vacuum conditions.

[0061] A second electrode is fabricated on the hole-selective transport layer.

[0062] In some embodiments, the first precursor solution further includes a first metal cation, the first metal cation including Ga. 3+ Al 3+ Pb 2+ One or more of the following, wherein the first metal cation reacts with the Cu 2+ The molar ratio is (0.5~3):100.

[0063] In some embodiments, fabricating the second electrode on the hole-selective transport layer includes:

[0064] An alumina interface layer is prepared on the hole selective transport layer by atomic layer deposition. Preferably, the thickness of the alumina interface layer is 0.5~1.5 nm.

[0065] Specifically, in the embodiments of this application, the crystalline silicon solar cell includes a hole-selective transport layer 6.

[0066] In some embodiments, from top to bottom, it also includes a silver electrode gate line 1, a silicon nitride passivation layer 2, and a phosphorus-doped n-type electrode. + The structure comprises a crystalline silicon layer 3, a p-type single-crystal silicon substrate 4, an alumina interface layer 5, and a silver electrode 7, with the CuS high-performance hole-selective transport layer 6 located between the alumina interface layer 5 and the silver electrode 7.

[0067] A third aspect of the present invention provides a crystalline silicon solar cell, comprising, in sequence, a first electrode, an electron transport layer, a light absorption layer, a hole selective transport layer, and a second electrode, wherein the light absorption layer comprises N-type silicon; wherein the hole selective transport layer comprises copper sulfide material, and the stoichiometric ratio of copper to sulfur in the copper sulfide material is less than or equal to 1.2.

[0068] For ease of understanding, the following specific implementation methods are provided. It should be noted that the silicon wafers used in the following embodiments and comparative examples are p-type or n-type with a resistivity of 1~5 Ω·cm. <100> The silicon wafers are oriented with a thickness of 130-160 μm.

[0069] Example 1

[0070] The fabrication of crystalline silicon solar cells includes the following steps:

[0071] 1) The silicon wafer surface is treated with a 1% NaOH aqueous solution to form an inverted pyramid-shaped textured structure. The treated silicon wafer is then immersed in a hydrofluoric acid aqueous solution to remove the oxide layer and residual NaOH on the surface, and then rinsed repeatedly with deionized water to obtain the treated p-type single crystal silicon substrate (p-Si).

[0072] 2) The silicon wafers cleaned in step 1 are immediately fed into a high-temperature diffusion furnace. Under an inert gas atmosphere, POCl3 vapor is introduced into a quartz tube, where phosphorus atoms diffuse into the p-Si to form phosphorus-doped n-Si. + Crystalline silicon layer.

[0073] 3) In the p-Si processed in step 2, n + A 70nm thick SiN layer is deposited on the crystalline silicon layer using a PECVD process. X A :H thin film was used as a passivation layer and antireflection layer to obtain a pretreated silicon wafer. Subsequently, a silver gate was fabricated using screen printing and then... (The sentence is incomplete and requires more context to translate accurately). o Silver gate electrodes were obtained by rapid sintering at temperature C.

[0074] 4) The p-Si processed in step 3 is fed into an ALD device. The silicon wafer is placed in a vacuum chamber and heated to approximately 200°C. Trimethylaluminum (TMA) vapor and deionized water vapor are circulated through the wafer, with intermittent purging using an inert gas. The two precursors are present in the n-phase of the silicon wafer. + A self-limiting reaction occurs on the back surface of the crystalline silicon layer, depositing an aluminum oxide film layer by layer. This cycle is repeated until a thickness of 1 nm is achieved.

[0075] 5) The fabrication process of the gallium-doped CuS high-performance hole-selective transport layer is as follows: Figure 1 As shown, a copper precursor solution with a concentration of 7.25 mg / mL was prepared using Cu(NO3)2·3H2O as the solute and methanol as the solvent. A 1.0% Ga(NO3)3·xH2O solution was added to the copper precursor, and the mixture was stirred at 25°C for 1 minute, followed by ultrasonic treatment at 25°C for 1 hour to achieve thorough mixing, ultimately yielding Ga… 3+ The copper precursor solution was then used. Finally, 70 μL of the precursor solution was spin-coated onto the alumina surface treated in step 4 at 2500 rpm for 5 seconds, followed by annealing in air at 80°C for 1 minute to remove residual solvent, thus obtaining a gallium-doped copper layer.

[0076] 6) A sulfur precursor solution with a concentration of 2.34 mg / mL was prepared using Na₂S as the solute and methanol as the solvent. After sealing, the solution was stirred at 25°C for 1 minute, followed by ultrasonic treatment at 25°C for 1 hour to achieve thorough mixing, ultimately obtaining the sulfur precursor solution. 70 μL of this precursor solution was spin-coated onto the gallium-doped copper layer treated in step 5 at 2500 rpm for 5 seconds. After reacting for 10 seconds, the layer was rinsed with methanol. Subsequently, it was annealed in air at 140°C for 15 minutes to remove residual solvent, obtaining a gallium-doped CuS high-performance hole-selective transport layer.

[0077] 7) Place the p-Si from step 6 into a thermal evaporation deposition apparatus, and start the vacuum pump to evacuate the reaction chamber pressure to 10. -3 Under a vacuum state of Pa, an evaporation boat containing Ag particles was heated to deposit a 200 nm thick Ag electrode on the surface of a gallium-doped CuS high-performance hole-selective transport layer at a rate of 0.7 Å / s, thus completing the fabrication of a crystalline silicon solar cell. This yielded a p-Si / Al₂O₃ / CuS:Ga 3+ Crystalline silicon solar cells.

[0078] Obtain as Figure 2 The crystalline silicon solar cell shown also includes, from top to bottom, silver electrode grid lines 1, silicon nitride passivation layer 2, and phosphorus-doped n... + The structure comprises a crystalline silicon layer 3, a p-type single-crystal silicon substrate 4, an alumina interface layer 5, and a silver electrode 7, with the CuS high-performance hole-selective transport layer 6 located between the alumina interface layer 5 and the silver electrode 7.

[0079] Example 2

[0080] The difference from Example 1 lies in step 5), where a copper precursor solution with a concentration of 7.25 mg / mL is prepared using Cu(NO3)2·3H2O as the solute and methanol as the solvent. This solution is then ultrasonically treated at 25°C for 1 hour to ensure thorough mixing, ultimately yielding the copper precursor solution. Finally, 70 μL of this precursor solution is spin-coated onto the alumina surface treated in step 4 at 2500 rpm for 5 seconds, followed by annealing in air at 80°C for 1 minute to remove residual solvent, resulting in a copper element layer.

[0081] Finally, p-Si / Al2O3 / Cu was obtained. 1.1 S-structure crystalline silicon solar cells.

[0082] The JV parameters of the battery are obtained through testing, such as... Figure 3a As shown, in Example 2, p-Si / Al2O3 / Cu 1.1 The output parameters of the S-structure crystalline silicon solar cell are: J SC =39.72 mA / cm2 V OC =625.7 mV, FF=82.6%, PCE=20.53%. p-Si / Al2O3 / Cu of Example 1 0.93 S:Ga 3+ The output parameters of a crystalline silicon solar cell are: J SC =40.32mA / cm 2 V OC =650.3 mV, FF=83.5%, PCE=21.89%. It can be seen that the introduction of the gallium-doped CuS high-performance hole-selective transport layer significantly improves the Vt of the crystalline silicon solar cell. OC The high work function (FF) and PCE of gallium-doped CuS (GaS) hole-selective transport layer are due to the higher work function and optimized bandgap matching with p-Si, which promotes hole transport via the valence band. The GaS high-performance hole-selective transport layer achieves passivation of the silicon interface through interfacial sulfur enrichment, suppressing minority carrier recombination. These two processes work synergistically to achieve efficient selective collection and separation of holes. Simultaneously, the introduction of an ultrathin Al2O3 interfacial layer further promotes hole transport through tunneling and enhances field-effect passivation.

[0083] The gallium-doped CuS high-performance hole-selective transport layer from step 5 of Example 1 and the CuS high-performance hole-selective transport layer from step 5 of Example 2 were deposited on a p-Si surface, and the minority carrier lifetime τ was detected. eff Value and saturation current density J0, such as Figure 3b As shown, Cu in Example 2 1.1 τ corresponding to S thin film eff It is 278.9 μs, and J0 is 47.0 fA / cm. 2 Example 1: Introducing Ga into a CuS thin film 3+ After that, its τ eff Increased to 530.5 μs, J0 decreased to 10.3 fA / cm 2 This demonstrates that the passivation performance of the CuS high-performance hole-selective transport layer in Example 1 of this application is improved. The band structures of gallium-doped CuS in contact with p-Si and CuS in contact with p-Si in Examples 1 and 2 are... Figure 4a and Figure 4bAs can be seen, in the CuS / p-Si heterojunction of Example 2, the energy band of the p-Si surface bends downward, and there is a 0.15 eV barrier between the valence band top of CuS and the valence band top of p-Si, which is not conducive to hole transport. In contrast, in the gallium-doped CuS / p-Si heterojunction with a high-performance hole selective transport layer in Example 1, the gallium-doped CuS has a high work function, which can induce the energy band of the p-Si surface to bend upward. At the same time, the valence band top of the gallium-doped CuS is closer to the valence band top of p-Si, promoting hole transport and thus significantly improving the hole selectivity of the battery.

[0084] Example 3

[0085] The preparation steps are similar to those in Example 1, except that step 4) is not performed.

[0086] 4) A copper precursor solution with a concentration of 7.25 mg / mL was prepared using Cu(NO3)2·3H2O as the solute and methanol as the solvent. A 1.0% Ga(NO3)3·xH2O solution was added to the copper precursor, and the mixture was stirred at 25°C for 1 minute, followed by ultrasonic treatment at 25°C for 1 hour to ensure thorough mixing, ultimately yielding Ga… 3+ A copper-doped precursor solution was prepared. Finally, 70 μL of this precursor solution was taken and applied to the silicon wafer treated in step 3). + The back surface of the crystalline silicon layer was spin-coated at 2500 rpm for 5 seconds, and then annealed in air at 80°C for 1 minute to remove residual solvent, thus obtaining a gallium-doped copper element layer.

[0087] Finally, p-Si / Cu was obtained 0.93 S:Ga 3+ Crystalline silicon solar cells.

[0088] Example 4

[0089] The preparation steps are similar to those in Example 1, except that step 4) is not performed.

[0090] 4) A copper precursor solution with a concentration of 7.25 mg / mL was prepared using Cu(NO3)2·3H2O as the solute and methanol as the solvent. A 0.5% Ga(NO3)3·xH2O solution was added to the copper precursor, and the mixture was stirred at 25°C for 1 minute, followed by ultrasonic treatment at 25°C for 1 hour to ensure thorough mixing, ultimately obtaining a low-concentration Ga... 3+ A copper-doped precursor solution was prepared. Finally, 70 μL of this precursor solution was taken and applied to the silicon wafer treated in step 3). + The back surface of the crystalline silicon layer was spin-coated at 2500 rpm for 5 seconds, and then annealed in air at 80°C for 1 minute to remove residual solvent, thus obtaining a gallium-doped copper element layer.

[0091] Finally, p-Si / Cu was obtained 1.0 S:Ga 3+ (Low-doped) crystalline silicon solar cells.

[0092] Example 5

[0093] The preparation steps are similar to those in Example 1, except that step 4) is not performed.

[0094] 4) A copper precursor solution with a concentration of 7.25 mg / mL was prepared using Cu(NO3)2·3H2O as the solute and methanol as the solvent. A 3.0% Ga(NO3)3·xH2O solution was added to the copper precursor, and the mixture was stirred at 25°C for 1 minute, followed by ultrasonic treatment at 25°C for 1 hour to ensure thorough mixing, ultimately obtaining a high concentration of Ga. 3+ A copper-doped precursor solution was prepared. Finally, 70 μL of this precursor solution was taken and applied to the silicon wafer treated in step 3). + The back surface of the crystalline silicon layer was spin-coated at 2500 rpm for 5 seconds, and then annealed in air at 80°C for 1 minute to remove residual solvent, thus obtaining a gallium-doped copper element layer.

[0095] Finally, p-Si / Cu was obtained 0.75 S:Ga 3+ (Highly doped) crystalline silicon solar cells.

[0096] Example 6

[0097] The preparation steps are similar to those in Example 1, except that step 4) is not performed.

[0098] 4) A copper precursor solution with a concentration of 7.25 mg / mL was prepared using Cu(NO3)2·3H2O as the solute and methanol as the solvent. The solution was then sonicated at 25°C for 1 hour to ensure thorough mixing, ultimately yielding the copper precursor solution. Finally, 70 μL of this precursor solution was used to prepare the silicon wafer treated in step 3. + The silicon layer was spin-coated on the back surface at 2500 rpm for 5 seconds, and then annealed in air at 80°C for 1 minute to remove residual solvent, thus obtaining a copper element layer.

[0099] Finally, p-Si / Cu was obtained 1.1 S-structure crystalline silicon solar cells.

[0100] The JV parameters of the battery are obtained through testing, such as... Figure 5a and Figure 5b As shown, p-Si / Cu in Example 6 1.1 The PCE of the S-structure crystalline silicon solar cell is 18.63%, and the p-Si / Cu of Example 3 is also mentioned. 0.93 S:Ga 3+The PCE of the structured crystalline silicon solar cell is 20.26%, and the p-Si / Cu solar cell in Example 4... 1.0 S:Ga 3+ The PCE of the structured crystalline silicon solar cell is 19.61%, and the p-Si / Cu of Example 5... 0.75 S:Ga 3+ The PCE of the crystalline silicon solar cell is 19.36%, and specific parameters are shown in Table 1. It can be seen that the introduction of the gallium-doped CuS high-performance hole-selective transport layer significantly improves the VE of the crystalline silicon solar cell. OC FF and PCE. The reason is that the gallium-doped CuS high-performance hole-selective transport layer provides a higher work function and optimizes the bandgap matching with p-Si, promoting hole transport in the valence band. The gallium-doped CuS high-performance hole-selective transport layer achieves silicon interface passivation through interfacial sulfur enrichment, suppressing minority carrier recombination. The two work together to achieve efficient selective collection and separation of holes. Too low a concentration of Ga... 3+ Insufficient doping to achieve a high work function makes band alignment with p-Si difficult, resulting in insufficient hole selectivity in CuS. Excessively high Ga concentrations... 3+ Doping CuS introduces excessive gallium ions, leading to Ga... 3+ Entering the interstitial sites of CuS lattice, electrons recombine with majority carrier holes, reducing the hole selectivity of CuS. Based on the data in Table 1, it can be seen that at an optimal thickness of approximately 21 nm, 1.0% Ga... 3+ Doping can most effectively improve the V of the battery OC with PCE.

[0101] Example 7

[0102] The preparation steps are similar to those in Example 1, except that step 4) is not performed.

[0103] 4) A copper precursor solution with a concentration of 2.42 mg / mL was prepared using Cu(NO3)2·3H2O as the solute and methanol as the solvent. A 1% Ga(NO3)3·xH2O solution was added to the copper precursor, and the mixture was stirred at 25°C for 1 minute, followed by ultrasonic treatment at 25°C for 1 hour to ensure thorough mixing, ultimately yielding Ga… 3+ A copper-doped precursor solution was prepared. Finally, 70 μL of this precursor solution was taken and applied to the silicon wafer treated in step 3). + The back surface of the crystalline silicon layer was spin-coated at 3000 rpm for 5 seconds, and then annealed in air at 80°C for 1 minute to remove residual solvent, thus obtaining a gallium-doped copper element layer.

[0104] 5) A sulfur precursor solution with a concentration of 0.78 mg / mL was prepared using Na₂S as the solute and methanol as the solvent. After sealing, the solution was stirred at 25°C for 1 minute, followed by ultrasonic treatment at 25°C for 1 hour to achieve thorough mixing, ultimately obtaining the sulfur precursor solution. 70 μL of this precursor solution was spin-coated onto the gallium-doped copper layer treated in step 4 at 3000 rpm for 5 seconds. After reacting for 10 seconds, the layer was rinsed with methanol. Subsequently, it was annealed in air at 140°C for 15 minutes to remove residual solvent, obtaining a thin gallium-doped CuS high-performance hole-selective transport layer.

[0105] Finally, p-Si / Cu was obtained 0.93 S:Ga 3+ (Thin) structure crystalline silicon solar cells.

[0106] Example 8

[0107] The preparation steps are similar to those in Example 1, except that step 4) is not performed.

[0108] 4) A copper precursor solution with a concentration of 12.08 mg / mL was prepared using Cu(NO3)2·3H2O as the solute and methanol as the solvent. A 1% Ga(NO3)3·xH2O solution was added to the copper precursor, and the mixture was stirred at 25°C for 1 minute, followed by ultrasonic treatment at 25°C for 1 hour to ensure thorough mixing, ultimately yielding Ga… 3+ A copper-doped precursor solution was prepared. Finally, 70 μL of this precursor solution was taken and applied to the silicon wafer treated in step 3). + The back surface of the crystalline silicon layer was spin-coated at 1500 rpm for 5 seconds, and then annealed in air at 80°C for 1 minute to remove residual solvent, thus obtaining a gallium-doped copper element layer.

[0109] 5) A sulfur precursor solution with a concentration of 3.90 mg / mL was prepared using Na₂S as the solute and methanol as the solvent. After sealing, the solution was stirred at 25°C for 1 minute, followed by ultrasonic treatment at 25°C for 1 hour to achieve thorough mixing, ultimately obtaining the sulfur precursor solution. 70 μL of this precursor solution was spin-coated onto the gallium-doped copper layer treated in step 4 at 1500 rpm for 5 seconds. After reacting for 10 seconds, the layer was rinsed with methanol. Subsequently, it was annealed in air at 140°C for 15 minutes to remove residual solvent, obtaining a thick gallium-doped CuS high-performance hole-selective transport layer.

[0110] Finally, p-Si / Cu was obtained 0.93 S:Ga 3+ (Thick) structure crystalline silicon solar cell.

[0111] Comparative Example 1

[0112] The preparation steps are similar to those in Example 1, except that steps 4 to 6 are not performed.

[0113] Obtain a crystalline silicon solar cell without a CuS layer.

[0114] The JV parameters of the battery are obtained through testing, such as... Figure 6a and Figure 6b As shown, the PCE of the p-Si crystalline silicon solar cell in Comparative Example 1 is 15.32%, and that of the p-Si / Cu solar cell in Example 7 is... 0.93 S:Ga 3+ The PCE of the structural crystalline silicon solar cell is 19.45%, and the p-Si / Cu solar cell in Example 8... 0.93 S:Ga 3+ The PCE of the crystalline silicon solar cell is 19.42%, and specific parameters are shown in Table 1. It can be seen that, compared with Comparative Example 1 without a transport layer, the introduction of the gallium-doped CuS high-performance hole-selective transport layer significantly improves the VE of the crystalline silicon solar cell. OC FF and PCE. It is worth noting that even at different thicknesses (7 nm and 34 nm), the doped CuS:Ga 3+ The batteries fabricated with the transport layer (Examples 7 and 8) also showed higher efficiencies than those with the undoped CuS transport layer (Example 6, PCE = 18.63%), further demonstrating the effectiveness of GaS. 3+ Doping is universal and effective in improving the hole selectivity of CuS. A thinner transport layer (7nm) may cause slight fluctuations in passivation effect due to incomplete coverage, while a thicker transport layer (34nm) affects the fill factor due to its increased resistance. However, both can achieve better overall performance than the undoped system through doping optimization.

[0115] Example 9

[0116] The preparation steps are similar to those in Example 1, except that after step 6), molybdenum oxide or vanadium-doped molybdenum oxide is deposited.

[0117] 7) Place the p-Si from step 6 into a thermal evaporation deposition apparatus, and start the vacuum pump to evacuate the reaction chamber pressure to 10. -3 Under a vacuum state of Pa, an evaporation boat containing a mixture of vanadium oxide and molybdenum oxide particles was heated to deposit a 5 nm thick vanadium-doped molybdenum oxide film at a rate of 0.5 Å / s, forming Cu. 0.93 S:Ga 3+ / MoO3:V 5+ Stacked hole selective transport layer.

[0118] Finally, p-Si / Al2O3 / Cu was obtained. 0.93 S:Ga 3+ / MoO3:V 5+The structured crystalline silicon solar cell achieved the highest conversion efficiency of 23.09% (Table 1).

[0119] Example 10

[0120] Using an n-Si wafer, a similar cleaning and texturing process as in step 1 of Example 1 was performed. Subsequently, a 5 nm thick intrinsic amorphous silicon (a-Si:H(i)) layer was deposited on both sides of the n-Si wafer using plasma-enhanced chemical vapor deposition (PECVD) as a surface passivation layer. An n-type doped amorphous silicon layer was then deposited on the front surface of the n-Si wafer containing intrinsic amorphous silicon, followed by sputtering to deposit a transparent conductive layer. Silver paste was then screen-printed and subjected to 190°C... o The front surface electrode was prepared by low-temperature heat treatment at C for 30 minutes.

[0121] Following steps 5-7 of Example 1, the preparation of the copper sulfide or copper sulfide / molybdenum oxide stacked hole-selective transport layer and electrode on the n-Si back surface was completed. The final product obtained was n-Si / a-Si:H(i) / Cu. 0.93 S:Ga 3+ / MoO3:V 5+ Heterogeneous crystalline silicon solar cells, specifically structured as follows: Figure 8a As shown, the highest conversion efficiency of 23.37% was achieved. Figure 8b (Table 1).

[0122] Table 1. Performance parameters of crystalline silicon solar cells prepared using the copper sulfide high-performance hole-selective transport layer of Examples 1-10 and Comparative Example 1 of the present invention.

[0123] sample transport layer Cu:S Thickness (nm) Doping concentration (%) Alumina thickness (nm) <![CDATA[V OC (mV)]]> <![CDATA[J SC (mA / cm 2 )]]> FF(%) PCE (%) Example 1 <![CDATA[Cu 0.93 S:Ga 3+ ]]> 0.93:1 21 1.0 1.0 650.3 40.32 83.5 21.89 Example 2 <![CDATA[Cu 1.1 S]]> 1.1:1 21 / 1.0 625.7 39.72 82.6 20.53 Example 3 <![CDATA[Cu 0.93 S:Ga 3+ ]]> 0.93:1 21 1.0 / 623.9 39.75 81.7 20.26 Example 4 <![CDATA[Cu 1.0 S:Ga 3+ ]]> 0.1:1 21 0.5 / 616.5 39.67 80.2 19.61 Example 5 <![CDATA[Cu 0.75 S:Ga 3+ ]]> 0.75:1 21 3.0 / 614.1 39.63 79.6 19.36 Example 6 <![CDATA[Cu 1.1 S]]> 1.1:1 21 / / 598.2 39.36 79.1 18.63 Example 7 <![CDATA[Cu 0.93 S:Ga 3+ ]]> 0.93:1 7 1.0 / 604.4 39.79 80.9 19.45 Example 8 <![CDATA[Cu 0.93 S:Ga 3+ ]]> 0.93:1 34 1.0 / 631.5 39.45 77.9 19.42 Example 9 <![CDATA[Cu 0.93 S:Ga 3+ / MoO3:V 5+ ]]> 0.93:1 21 / 5 1.0 1.0 678.5 41.0 83.0 23.09 Example 10 <![CDATA[Cu 0.93 S:Ga 3+ / MoO3:V 5+ ]]> 0.93:1 21 / 5 1.0 / 732.2 39.9 80.0 23.37 Comparative Example 1 / / / / / 554.2 38.66 71.5 15.32

[0124] Obviously, the above embodiments are merely illustrative examples for clear explanation and are not intended to limit the implementation. For those skilled in the art, any modifications, equivalent substitutions, or improvements made based on the above description and within the methods and principles of this invention should be included within the scope of protection of this invention. It is neither necessary nor possible to exhaustively describe all embodiments here. However, obvious variations or modifications derived therefrom are still within the scope of protection of this invention.

Claims

1. A crystalline silicon solar cell, characterized in that, It consists of, in sequence, a first electrode, a silicon nitride passivation layer, and a phosphorus-doped n-type electrode. + The device comprises a crystalline silicon layer, a p-type single-crystal silicon substrate, a hole-selective transport layer, and a second electrode. The hole-selective transport layer includes a copper sulfide material, wherein the stoichiometric ratio of copper to sulfur in the copper sulfide material is less than or equal to 1.

2.

2. The crystalline silicon solar cell according to claim 1, characterized in that, The stoichiometric ratio of copper to sulfur in the copper sulfide material is less than or equal to 0.

99.

3. The crystalline silicon solar cell according to claim 1 or 2, characterized in that, The copper sulfide material is further doped with a first metal cation, the first doped metal cation including Ga. 3+ Al 3+ Pb 2+ One or more of them.

4. The crystalline silicon solar cell according to claim 3, characterized in that, In copper sulfide doped with the first metal cation, the copper vacancy concentration is a first concentration and the sulfur vacancy concentration is a second concentration; in copper sulfide not doped with the first metal cation, the copper vacancy concentration is a third concentration and the sulfur vacancy concentration is a fourth concentration, wherein the first concentration is greater than the third concentration and the second concentration is less than the fourth concentration.

5. The crystalline silicon solar cell according to claim 1, 2, or 4, characterized in that, The work function of the hole-selective transport layer is ≥5.0 eV; and / or, The thickness of the hole-selective transport layer is 5~40 nm; and / or, An alumina interface layer is included between the p-type single-crystal silicon substrate and the hole selective transport layer. Preferably, the thickness of the alumina interface layer is 0.5~1.5 nm.

6. The crystalline silicon solar cell according to claim 1, 2, or 4, characterized in that, The copper sulfide material comprises monovalent copper ions, divalent copper ions, monovalent sulfide ions, and divalent sulfide ions, wherein Cu 2+ :Cu + Greater than or equal to 50%, S 2- :S - Greater than or equal to 50%.

7. The crystalline silicon solar cell according to claim 1, 2, or 4, characterized in that, The side of the hole selective transport layer facing away from the p-type single-crystal silicon substrate also includes a molybdenum oxide layer or a vanadium-doped molybdenum oxide layer.

8. A method for fabricating a crystalline silicon solar cell, characterized in that, include: A substrate is provided, the substrate comprising a first electrode, a silicon nitride passivation layer, and a phosphorus-doped n-type electrode sequentially disposed therefrom. + crystalline silicon layer and p-type single-crystal silicon substrate; A first precursor solution is spin-coated onto a p-type single-crystal silicon substrate, followed by a first annealing treatment to obtain a first film layer; wherein, the first precursor solution includes Cu... 2+ A methanol solution, wherein Cu in the first precursor solution 2+ The molar concentration is 0.01-0.05 mol / L, the first annealing time is 1-5 minutes, and the atmosphere for the first annealing is air, reducing atmosphere, inert atmosphere or vacuum. A second precursor solution is spin-coated onto the first film layer. After reacting for 10-60 seconds, a second film layer is formed. The second precursor includes S. 2- The S 2- The molar concentration is 0.01-0.05 mol / L; The second film layer is washed and subjected to a second annealing treatment to obtain a hole selective transport layer; the temperature of the second annealing treatment is 100-200℃, the time of the second annealing treatment is 10-25 minutes, and the atmosphere of the second annealing treatment is air atmosphere, reducing atmosphere, inert atmosphere or vacuum conditions. A second electrode is fabricated on the hole-selective transport layer.

9. The method for preparing a crystalline silicon solar cell according to claim 8, characterized in that, The first precursor solution also includes a first metal cation, which includes Ga. 3+ Al 3+ Pb 2+ One or more of the following, wherein the first metal cation reacts with the Cu 2+ The molar ratio is (0.5~3):

100.

10. A crystalline silicon solar cell, characterized in that, It comprises, in sequence, a first electrode, an electron transport layer, a light absorption layer, a hole selective transport layer, and a second electrode, wherein the light absorption layer comprises N-type silicon; The hole-selective transport layer comprises copper sulfide material, wherein the stoichiometric ratio of copper to sulfur in the copper sulfide material is less than or equal to 1.2.