A low deep level doped silicon-based micro-ring photoelectric detector and a preparation method thereof

By introducing a low-concentration deep-level impurity doping absorption region and a lateral built-in electric field to separate charge carriers within the silicon microring resonant cavity, the problems of lattice damage and dark current caused by high-concentration doping in the prior art are solved, and the high efficiency photoelectric response and stability of the low-deep-level doped silicon-based microring photodetector are realized.

CN123124466APending Publication Date: 2026-11-17UNIV OF JINAN +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611467452.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-21
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing deep-level doped silicon-based photodetectors for communication bands rely on high impurity concentrations, which lead to lattice damage, dark current, and optical losses, making it difficult to reduce impurity doping concentrations while ensuring effective photoelectric response.

Method used

A low-deep-level doped silicon-based microring photodetector is employed. By introducing a low-concentration deep-level impurity doping absorption region into the silicon microring resonant cavity and forming P-type and N-type doped regions on the inner and outer sides of the resonant cavity, the photogenerated carriers are separated by the lateral built-in electric field. Combined with the silicon microring resonance enhancement mechanism, the effective action path of photons in the impurity doped region is extended.

Benefits of technology

While reducing the doping concentration of deep-level impurities, it achieves effective subbandgap absorption of photons in the communication band and room-temperature photodetection, reduces lattice damage and dark current, and improves photoelectric responsivity and device stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123124466A_ABST
    Figure CN123124466A_ABST
Patent Text Reader

Abstract

This invention provides a low-deep-level doped silicon-based microring photodetector and its fabrication method, relating to the field of optoelectronic device technology. The photodetector includes an SOI substrate, an input waveguide, a silicon microring resonant cavity, a deep-level impurity-doped absorption region, a P-type doped region, an N-type doped region, and a metal electrode. The deep-level impurity-doped absorption region is located within the optical mode operating region of the silicon microring resonant cavity, with a doping concentration lower than the solid solubility of the impurity in silicon. The P-type and N-type doped regions are respectively located on the inner and outer sides of the microring, forming a lateral electric field to collect photogenerated carriers. This invention achieves all-silicon-based photodetector in the room-temperature communication band by extending the effective path of light in the low-concentration deep-level impurity-doped absorption region, reducing lattice damage, dark current, and additional optical losses, and improving device responsivity, stability, and compatibility with CMOS processes.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of optoelectronic device technology, specifically to a low-deep-level doped silicon-based microring photodetector and its fabrication method. Background Technology

[0002] Silicon photonics, relying on mature CMOS-compatible processes, offers advantages such as high integration, low cost, and stable processes, making it an important technological platform for fabricating on-chip photodetectors. However, silicon, with its bandgap of approximately 1.1 eV and intrinsic absorption cutoff wavelength of about 1100 nm, exhibits high transparency in communication bands such as 1310 nm and 1550 nm, making it difficult to directly generate effective light absorption and photoelectric response. This limits the application of all-silicon-based photodetectors in communication bands.

[0003] To achieve silicon-based photodetectors in the communication band, existing methods mainly include germanium / silicon heterointegration, photon-assisted tunneling, two-photon absorption, defect engineering, and deep-level doping. Among these, germanium / silicon heterointegration increases the complexity of epitaxial growth and process integration; photon-assisted tunneling easily introduces significant dark current and noise; two-photon absorption depends on high light intensity; and defect engineering makes it difficult to precisely control the type, density, and distribution of defects. In contrast, deep-level doping, by introducing impurity levels into the silicon bandgap, achieves subbandgap absorption in the communication band, making it an effective approach to constructing all-silicon-based photodetectors.

[0004] Existing deep-level doped silicon-based photodetectors for communication bands typically rely on high impurity concentrations, such as introducing impurities like Se, Te, and Au into the silicon lattice at concentrations close to or exceeding their solid solubility in silicon, to increase deep-level or impurity state density and enhance subbandgap absorption. However, high-concentration doping and its accompanying lattice damage increase nonradiative recombination centers, shorten carrier lifetime, reduce carrier mobility and collection efficiency, and introduce significant dark current and additional optical losses. How to reduce deep-level impurity doping concentration while ensuring effective photoelectric response is a key technical problem that urgently needs to be solved for all-silicon-based photodetectors for communication bands. Summary of the Invention

[0005] To address the technical problems existing in the background art, the present invention provides a low-deep-level doped silicon-based microring photodetector and its fabrication method.

[0006] The first aspect of the present invention provides a low-deep-level doped silicon-based microring photodetector, comprising an SOI substrate, an input waveguide, a silicon microring resonant cavity, a deep-level impurity doped absorption region, a P-type doped region, an N-type doped region, and a metal electrode; The silicon microring resonant cavity is disposed in the top silicon layer of the SOI substrate and coupled to the input waveguide light to enable the communication band light to propagate multiple times in the top silicon layer, thereby extending the effective path of the communication band light in the deep energy level impurity doped absorption region. The deep-level impurity doped absorption region is disposed within the optical mode operating region of the silicon microring resonator, and is used to introduce deep levels in the silicon bandgap and realize subbandgap absorption of photons in the communication band. The doping concentration of the deep-level impurity in the deep-level impurity doped absorption region is lower than the solid solubility of the deep-level impurity in silicon. The P-type doped region is disposed on the inner side of the silicon microring resonator, and the N-type doped region is disposed on the outer side of the silicon microring resonator. The P-type doped region and the N-type doped region are used to form a transverse built-in electric field in the silicon microring resonator region to separate and collect photogenerated carriers generated by subbandgap absorption. The metal electrode is electrically connected to the P-type doped region and the N-type doped region, respectively.

[0007] Furthermore, the deep-level impurities include one or more of Te, Se, S, Au, and Ti.

[0008] Furthermore, the deep-level impurity is Te.

[0009] Furthermore, the doping concentration of the deep-level impurity is at least an order of magnitude lower than its solid solubility in silicon.

[0010] Furthermore, the doping concentration of the deep-level impurity is 10. 14 -10 17 cm -3 .

[0011] Furthermore, the P-type doped region and the N-type doped region are respectively spaced apart from the silicon microring resonator to reduce the additional loss of the optical mode of the silicon microring resonator due to free carrier absorption; the P-type doped region is formed by boron ion implantation, and the N-type doped region is formed by phosphorus ion implantation or arsenic ion implantation; the resonant wavelength of the silicon microring resonator is located in the communication band, and the resonant wavelength is in the range of 1250-1600nm.

[0012] A second aspect of the present invention provides a method for fabricating the above-mentioned low-deep-level doped silicon-based microring photodetector, comprising: Step 1: Obtain an SOI substrate, wherein the SOI substrate comprises a silicon substrate, a silicon dioxide buried oxide layer, and a top silicon layer; Step 2: An input waveguide and a silicon microring resonator are fabricated in the top silicon layer, and the input waveguide is optically coupled to the silicon microring resonator. Step 3: A P-type doped region is formed inside the silicon microring resonator, and an N-type doped region is formed outside the silicon microring resonator, so as to form a transverse built-in electric field in the silicon microring resonator region. Step 4: Introduce deep-level impurities into the optical mode operating region of the silicon microring resonator to form a deep-level impurity doped absorption region. The doping concentration of the deep-level impurities is lower than their solid solubility in silicon. Step 5: Prepare metal electrodes on the P-type doped region and the N-type doped region to obtain the photodetector.

[0013] Furthermore, in step two, the input waveguide and the silicon microring resonator are fabricated using electron beam lithography and reactive ion etching processes; a coupling gap exists between the input waveguide and the silicon microring resonator to couple the incident light of the communication band into the silicon microring resonator.

[0014] Furthermore, in step three, the P-type doped region is formed by boron ion implantation, and the N-type doped region is formed by phosphorus ion implantation or arsenic ion implantation. The P-type and N-type dopants are then activated by annealing. The P-type and N-type doped regions are kept at a preset distance from the silicon microring resonator to reduce the additional absorption loss of the optical mode of the silicon microring resonator by the heavily doped region.

[0015] Furthermore, in step four, the deep-level impurity is Te, which is introduced into the silicon microring resonator region through multi-energy staged ion implantation, so that the Te doping distribution at least partially overlaps with the optical mode action region of the silicon microring resonator. Step four is followed by annealing to repair some lattice damage caused by deep-level impurity implantation and activate deep-level doping centers.

[0016] Compared with existing technologies, the present invention provides a low-deep-level doped silicon-based microring photodetector and its fabrication method. Based on the resonance enhancement mechanism of the silicon microring resonator, the effective interaction path of communication band light in the low-concentration deep-level impurity doped absorption region is extended by the microring structure, so that photons can circulate multiple times in the microring to increase the number of interactions with deep-level impurities. Thus, effective sub-bandgap absorption of photons in the communication band and room-temperature photodetection are achieved without relying on high-concentration deep-level impurity doping. Attached Figure Description

[0017] The accompanying drawings, which form part of this disclosure, are used to provide a further understanding of this disclosure. The illustrative embodiments of this disclosure and their descriptions are used to explain this disclosure and do not constitute an undue limitation of this disclosure.

[0018] Figure 1This is a schematic cross-sectional view of the waveguide-coupled photodetector with boron ions, phosphorus ions, and tellurium ions implanted and deposited as a gold film, provided in Embodiment 1 of the present invention.

[0019] Figure 2 This is a schematic diagram of the main structure of the waveguide-coupled photodetector provided in Embodiment 1 of the present invention for realizing photoelectric conversion in the C-band of optical communication.

[0020] Figure 3 This is the reverse bias provided in Embodiment 1 of the present invention. The responsivity curves of photodetectors with incident light power under 10V conditions are shown for low-deep-level doped silicon-based microrings, low-concentration Te-doped straight waveguides without microring resonators, and high-concentration Te-doped straight waveguides.

[0021] Figure 4 The responsivity curves of photodetectors with reverse bias voltage under an incident light power of 100nW, including those with low-deep-level doped silicon microrings, low-concentration Te-doped straight waveguides without microring resonators, and high-concentration Te-doped straight waveguide structures, are provided in Embodiment 1 of the present invention.

[0022] Figure 5 This is a process flow diagram of the fabrication and application of a low-deep-level doped silicon-based microring photodetector in photoelectric conversion, provided in Embodiment 2 of the present invention.

[0023] In the figure, 1 is a gold film; 2 is a silicon-based tellurium-doped region; 3 is a silicon-based boron-doped region; 4 is a silicon-based phosphorus-doped region; 5 is a waveguide; 6 is a cone; 7 is an i-Si layer; 8 is a silicon dioxide layer; 9 is a silicon layer; 10 is an incident beam; and 11 is a grating coupler. Detailed Implementation

[0024] It should be noted that the following detailed descriptions are exemplary and intended to provide further illustration of the invention. Unless otherwise specified, all technical and scientific terms used in this invention have the same meaning as commonly understood by one of ordinary skill in the art to which this invention pertains.

[0025] It should be noted that the terminology used herein is for the purpose of describing particular embodiments only and is not intended to limit the exemplary embodiments of the present invention. As used herein, unless the context clearly indicates otherwise, the singular form is also intended to include the plural form. Furthermore, it should be understood that the terms “comprising” and “having”, and any variations thereof, are intended to cover non-exclusive inclusion, for example, a process, method, system, product, or apparatus that comprises a series of steps or units is not necessarily limited to those steps or units explicitly listed, but may include other steps or units not explicitly listed or inherent to such processes, methods, products, or apparatus.

[0026] Where there is no conflict, the embodiments and features in the embodiments of the present invention can be combined with each other.

[0027] All data acquisition in this embodiment is carried out in accordance with laws and regulations and with user consent, and the data is used legally.

[0028] Example 1 This embodiment provides a low-deep-level doped silicon-based microring photodetector, including: an SOI substrate, an input waveguide, a silicon microring resonant cavity, a deep-level impurity doped absorption region, a P-type doped region, an N-type doped region, and a metal electrode.

[0029] The silicon microring resonant cavity is disposed in the top silicon layer of the SOI substrate and coupled to the input waveguide light to allow the communication band light to propagate multiple times in the top silicon layer, thereby extending the effective path of the communication band light in the deep energy level impurity doped absorption region.

[0030] The deep-level impurity doped absorption region is located within the optical mode operating region of the silicon microring resonator, and is used to introduce deep levels in the silicon bandgap and realize sub-bandgap absorption of photons in the communication band. The doping concentration of the deep-level impurity in the deep-level impurity doped absorption region is lower than the solid solubility of the deep-level impurity in silicon.

[0031] The P-type doped region is disposed on the inner side of the silicon microring resonator, and the N-type doped region is disposed on the outer side of the silicon microring resonator. The P-type doped region and the N-type doped region are used to form a transverse built-in electric field in the silicon microring resonator region to separate and collect photogenerated carriers generated by subbandgap absorption.

[0032] The metal electrode is electrically connected to the P-type doped region and the N-type doped region, respectively.

[0033] The deep-level impurity includes one or more of Te, Se, S, Au, and Ti; preferably, the deep-level impurity is Te. The doping concentration of the deep-level impurity is lower than its solid solubility in silicon, preferably at least one order of magnitude lower, and more preferably at least two orders of magnitude lower.

[0034] The resonant wavelength of the silicon microring resonator is located in the communication band, preferably in the range of 1250-1600nm, and more preferably in the range of 1550nm.

[0035] The photodetector described in this embodiment is used for detecting photoelectric signals in the communication band of an SOI chip. Preferably, the photodetector is used for room temperature detection of C-band optical signals near 1550nm.

[0036] As an alternative to this embodiment, the deep-level impurity ions can also be one or more of Se, S, Au, and Ti, introduced into the silicon microring resonator region via single-energy injection or multi-energy staged injection to form a low-concentration deep-level impurity doped absorption region. The deep-level impurity doped absorption region overlaps with the optical mode interaction region of the silicon microring resonator, enabling effective interaction between communication band light and the absorption region when the microring resonance condition is met. The doping concentration of the deep-level impurity is lower than its solid solubility in silicon, preferably at least one order of magnitude lower, and more preferably at least two orders of magnitude lower. By extending the effective interaction path of communication band light in the low-concentration deep-level impurity doped absorption region through the silicon microring resonator, it is also possible to achieve sub-bandgap light absorption and photoelectric response at room temperature in the 1550nm communication band while reducing the deep-level impurity doping concentration. This alternative embodiment indicates that the present invention is not limited to the Te-doped silicon system, but can also be applied to other deep-level impurity doped systems capable of forming deep levels in silicon and generating sub-bandgap absorption in the communication band.

[0037] In one specific embodiment, combined with Figure 1 The cross-sectional structure shown indicates that the SOI substrate specifically comprises a silicon-based morphological structure consisting of a silicon layer 9, a silicon dioxide layer 8, and an i-Si layer 7. From bottom to top, it includes the silicon layer 9 (corresponding to the silicon substrate of the SOI substrate) serving as the bottom supporting substrate, the silicon dioxide layer 8 disposed on the silicon layer 9 (corresponding to the buried oxide layer of the SOI substrate), and the i-Si layer 7 disposed on the silicon dioxide layer 8 (corresponding to the top silicon layer of the SOI substrate). The silicon dioxide layer 8 is located between the silicon layer 9 and the i-Si layer 7, forming an insulating isolation layer (i.e., the buried oxide layer of the SOI substrate). The i-Si layer 7 serves as the main functional layer of the device, supporting the photoelectric conversion regions such as the silicon microring resonator, doped region, and waveguide structure described later.

[0038] Silicon-based boron-doped region 3 and silicon-based phosphorus-doped region 4 are formed in the i-Si layer 7 (i.e., the top silicon layer of the SOI substrate), corresponding to the P-type doped region and the N-type doped region, respectively. The silicon-based boron-doped region 3 and silicon-based phosphorus-doped region 4 are located at different positions within the device's functional regions, forming corresponding P-type and N-type doped regions, thereby establishing a lateral built-in electric field in the device for separating and collecting photogenerated carriers. A gold film 1 is disposed above the corresponding doped regions and forms an electrical connection with the silicon-based boron-doped region 3 and silicon-based phosphorus-doped region 4, serving as an electrode or ohmic contact structure to extract the electrical signal generated by the photogenerated carriers, corresponding to the metal electrode.

[0039] The silicon-based doped tellurium region 2 is disposed on the upper part of the i-Si layer 7 and located within the optical mode operating region of the silicon microring resonator, corresponding to the deep-level impurity doped absorption region. It is used to introduce deep-level impurities into the silicon-based material, forming a functional region capable of sub-bandgap absorption of light in the communication band. Through tellurium ion doping, the silicon-based doped tellurium region 2 enhances the light absorption capability of the silicon material in the communication band, thereby achieving photoelectric conversion.

[0040] The two sides of waveguide 5 are connected to the narrow end of cone 6, forming together on top of i-Si layer 7, and together they constitute the input waveguide. Cone 6 is a mode conversion structure located at the end of waveguide 5, used to achieve optical mode matching between the on-chip waveguide and grating coupler 11. Waveguide 5 is used to transmit communication band optical signals and guide them to the silicon microring resonant cavity region. Waveguide 5, cone 6, silicon-based tellurium doped region 2, silicon-based boron doped region 3, and silicon-based phosphorus doped region 4 spatially cooperate with each other, enabling incident light to undergo sub-bandgap absorption with silicon-based tellurium doped region 2 when propagating in the waveguide structure, and to separate and collect photogenerated carriers under the action of the transverse built-in electric field formed by silicon-based boron doped region 3 and silicon-based phosphorus doped region 4.

[0041] The detector provided in this embodiment provides a device platform through an SOI layered structure composed of a silicon layer 9, a silicon dioxide layer 8, and an i-Si layer 7. The silicon layer 9 serves as the bottom supporting substrate, the silicon dioxide layer 8 serves as the insulating buried oxide layer, and the i-Si layer 7 serves as the top silicon functional layer. The silicon-based doped tellurium region 2 disposed in the i-Si layer 7 achieves light absorption in the communication band. The silicon-based doped boron region 3 and the silicon-based doped phosphorus region 4 form carrier separation and collection regions. The gold film 1 enables the extraction of electrical signals. The waveguide 5 and the cone 6 enable the input, transmission, and coupling of optical signals, thereby constituting an SOI-based waveguide-coupled silicon-based photodetector structure.

[0042] like Figure 2 The schematic diagram of the model structure shown illustrates the overall three-dimensional layout of the device on the SOI substrate, demonstrating the relationship between the input of optical signals in the communication band, waveguide transmission, micro-ring resonance enhancement, and the extraction of electrical signals after photoelectric conversion.

[0043] As shown in the figure, the device is mounted on a rectangular sheet substrate, which can be understood as an SOI substrate structure. Below the substrate is a silicon layer, and above it are a silicon dioxide layer and a top silicon functional layer. A linear waveguide structure is formed on the substrate surface, extending along the length of the device. Periodic strip structures, grating couplers 11, are located at both ends to achieve optical coupling between the external optical fiber and the on-chip waveguide. An incident beam 10 is schematically shown above the grating coupler 11 on the left side of the figure, indicating that external communication band light is coupled into the on-chip waveguide at this location.

[0044] A ring structure, a silicon microring resonator, is positioned on one side of the straight waveguide. The straight waveguide and the silicon microring resonator are arranged adjacent to each other, forming a coupling gap. This allows communication-band light from the input waveguide to enter the silicon microring resonator via evanescent field coupling. When the incident light wavelength meets the microring resonance condition, the light circulates multiple times within the microring resonator, thereby extending the effective interaction path between the light and the deep-level doped absorption region and improving the subbandgap absorption efficiency of C-band light in the low-concentration deep-level doped region.

[0045] The diagram also shows symbols for power supply / bias connections near the microring structure, indicating the relationship between the applied bias voltages to the P-type and N-type doped regions inside and outside the microring and their corresponding metal electrodes. This region corresponds to the P-type doped region formed by boron ion implantation, the N-type doped region formed by phosphorus ion implantation, the low-concentration Te deep-level doped absorption region, and the metal electrodes. After light is absorbed in the microring to generate photogenerated carriers, they are separated and collected by the transverse built-in electric field formed by the P-type and N-type doped regions, and finally output as a photocurrent signal through the metal electrodes.

[0046] Depend on Figure 2 It can be seen that the working principle of the waveguide-coupled photodetector is as follows: external C-band light enters the input waveguide through the grating coupler, and is coupled to the silicon microring resonator through the waveguide. In the microring resonator, it undergoes enhanced interaction with the low-concentration Te deep-level doped absorption region and generates photogenerated carriers. Subsequently, the electrical signal is collected and output through the P / N doped region and metal electrodes.

[0047] To further verify the technical effectiveness of this invention, a comparative experiment was conducted to quantitatively compare the detection performance of three photodetector structures. The results are as follows: Figure 3 and Figure 4 As shown. Figure 3 reverse bias Under 10V conditions, the responsivity curves of low-deep-level doped silicon-based microrings (photodetectors provided in Embodiment 1 of this invention), low-concentration Te-doped straight waveguides without microring resonators (Comparative Example 1), and high-concentration Te-doped straight waveguide structure photodetectors (Comparative Example 2) are shown as a function of incident light power. Figure 4 The figures show the responsivity curves of the three photodetectors with reverse bias under an incident light power of 100 nW. In Comparative Example 1, the Te ion implantation energy, implantation dose, and annealing conditions are the same as those in the preparation method provided in Example 2 of this invention, and the Te doping concentration is consistent with that of this example. In Comparative Example 2, the Te ion implantation dose is higher than that of this example, and the Te doping concentration is close to or exceeds the solid solubility of Te in silicon.

[0048] Specifically, the low-concentration Te-doped straight waveguide structure without a microring resonator provided in Comparative Example 1 includes: fabricating a grating coupler and a straight waveguide structure in the top silicon layer of an SOI substrate, without fabricating a silicon microring resonator; implanting boron ions and phosphorus ions on both sides of the straight waveguide to form a lateral PN junction; subsequently, low-dose Te ion implantation is performed in the straight waveguide region, with the Te ion implantation energy, implantation dose, and annealing conditions being the same as steps eight and nine of this embodiment, ensuring that the Te doping concentration remains consistent with this embodiment, and annealing treatment is performed to form a low-concentration Te deep-level doped absorption region. The results show that in this comparative scheme, communication band light only passes through the low-concentration Te deep-level doped absorption region once along the straight waveguide direction, lacking the multiple cyclic propagation and effective path extension provided by the microring resonator. Therefore, under the same Te doping concentration conditions, the effective interaction between light and the Te deep-level doped absorption region is weak, limiting the subbandgap absorption probability and photoelectric response. This indicates that under conditions of low Te doping concentration far below the solid solubility, ordinary straight waveguide structures cannot fully utilize the deep energy level absorption of low-concentration Te; while the silicon microring resonator in this embodiment can reduce the Te doping concentration required to achieve effective photoelectric detection by extending the effective action path.

[0049] Specifically, the high-concentration Te-doped straight waveguide photodetector provided in Comparative Example 2 includes: fabricating a grating coupler and a straight waveguide structure in the top silicon layer of an SOI substrate, without fabricating a silicon microring resonator; forming P-type and N-type doped regions on both sides of the straight waveguide, respectively; subsequently, high-dose Te ion implantation is performed in the straight waveguide region to make the Te doping concentration close to or exceed the solid solubility of Te in silicon, and annealing is performed to form a high-concentration Te deep-level doped absorption region. By increasing the Te doping concentration, the Te-related deep level or impurity state density can be increased, thereby enhancing the subbandgap absorption in the communication band. The results show that this control scheme relies on a high Te doping concentration to obtain sufficient absorption in the communication band. High concentrations of Te impurities and their accompanying ion implantation damage tend to increase nonradiative recombination centers, shorten carrier lifetime, reduce carrier mobility and collection efficiency, and may introduce larger dark currents and additional optical losses. In addition, high-concentration Te doping may also have an adverse effect on the transmission loss of the silicon waveguide and the stability of the device. This indicates that although increasing the Te doping concentration can enhance subbandgap absorption, it can lead to problems such as lattice damage, carrier recombination, dark current, and optical loss. However, this embodiment extends the effective path of light in the low-concentration Te deep-level doped absorption region by using a silicon microring resonant structure, which can achieve room-temperature photoelectric detection in the communication band while reducing the Te doping concentration.

[0050] like Figure 3 Under reverse bias of -10 V, when the incident light power is 100 nW (1×10⁻⁶), -7At a power of approximately 0.75 A / W, the photodetector provided in this embodiment exhibits a responsivity of approximately 0.50 A / W, compared to approximately 0.40 A / W in Comparative Example 2 and approximately 0.50 A / W in Comparative Example 1. As the incident light power monotonically increases, the responsivity of all three structures decreases due to the saturation of subbandgap absorption, but remains high across the entire incident light power range (1×10⁻⁶ W). -7 W~2×10 -3 Within W), the responsivity of the photodetector provided in this embodiment is consistently significantly higher than that of Comparative Example 1 and Comparative Example 2.

[0051] like Figure 4 Under an incident light power of 100 nW, the responsivity of all three structures monotonically increases with increasing reverse bias voltage, which is consistent with the mechanism by which the transverse built-in electric field enhances the separation and collection efficiency of photogenerated carriers. When the reverse bias voltage increases to 10 V, the responsivity of the photodetector provided in this embodiment reaches approximately 0.75 A / W, which is an improvement of approximately 87.5% (nearly 1.9 times) compared to Comparative Example 1 (approximately 0.40 A / W) and approximately 50% (1.5 times) compared to Comparative Example 2 (approximately 0.50 A / W). Within the full reverse bias voltage range of 1 V to 10 V, the responsivity curve of the photodetector provided in this embodiment remains at the top.

[0052] Based on the results of the comparative experiments above, this embodiment employs a low-concentration Te deep-level doped silicon microring resonator structure. The Te deep-level doped absorption region is positioned within the optical mode action region of the silicon microring resonator, with P-type and N-type doped regions formed on the inner and outer sides of the microring, respectively. When the 1550nm communication band light meets the microring resonance condition, the light circulates multiple times within the silicon microring resonator, thereby extending its effective interaction path in the low-concentration Te deep-level doped absorption region and increasing the sub-bandgap absorption probability. Photogenerated carriers generated by Te deep-level absorption are separated and collected under the influence of the transverse built-in electric field, thus achieving room-temperature photoelectric detection in the communication band. Compared to a low-concentration doping scheme without a microring, this embodiment introduces a silicon microring resonator structure under the same low Te doping concentration, resulting in a longer effective interaction path between the communication band light and the Te deep-level doped absorption region. This enhances the effective sub-bandgap absorption of low-concentration Te deep-level doped silicon without increasing the Te doping concentration, effectively addressing the problem of insufficient optical response in low-concentration deep-level doped straight waveguide structures. Compared with high-concentration doped straight waveguide schemes, this embodiment does not rely on high-concentration Te doping close to or exceeding solid solubility, which is beneficial to reducing lattice damage, nonradiative recombination, dark current and additional optical losses caused by high-concentration deep-level impurity doping, and is also beneficial to maintaining the quality factor and device stability of silicon microring resonators.

[0053] Example 2 like Figure 5This embodiment provides a method for fabricating a low-deep-level doped silicon-based microring photodetector as provided in Embodiment 1, comprising: S1. Obtain an SOI substrate, wherein the SOI substrate comprises a silicon substrate, a silicon dioxide buried oxide layer, and a top silicon layer.

[0054] Specifically, an SOI silicon wafer is used as the substrate, the SOI silicon wafer comprising a 2000nm thick buried oxide layer of silicon dioxide and a 220nm thick top silicon layer. The surface of the SOI silicon wafer is cleaned sequentially with acetone and isopropanol, dried with N2, and then baked on a hot plate at 120°C for 2 minutes to obtain a clean SOI substrate.

[0055] S2. An input waveguide and a silicon microring resonator are fabricated in the top silicon layer, and the input waveguide is optically coupled to the silicon microring resonator.

[0056] Specifically, electron beam lithography and inductively coupled plasma reactive ion etching (ICP-RI) processes are used to fabricate a grating coupler, a tapered transition structure, an input / output waveguide, and a silicon microring resonator in the top silicon layer. A coupling gap exists between the input waveguide and the silicon microring resonator to couple communication band incident light into the silicon microring resonator.

[0057] S3. A P-type doped region is formed inside the silicon microring resonator, and an N-type doped region is formed outside the silicon microring resonator, so as to form a transverse built-in electric field in the silicon microring resonator region.

[0058] Specifically, boron ions are implanted into the inner region of the silicon microring resonator using an ion implantation device to form a P-type doped region. The distance between the P-type doped region and the silicon microring resonator is 550 nm; the boron ion implantation energy is 7 keV, and the implantation dose is 2 × 10⁻⁶. 13 ions / cm 2 .

[0059] Furthermore, phosphorus ions were implanted into the outer region of the silicon microring resonator using an ion implantation device to form an N-type doped region. The distance between the N-type doped region and the silicon microring resonator was 550 nm; the phosphorus ion implantation energy was 18 keV, and the implantation dose was 1.7 × 10⁻⁶. 13 ions / cm 2 .

[0060] Furthermore, secondary ion implantation is performed in the electrode contact region between the P-type and N-type doped regions to form an ohmic contact region. The implantation energy in the P-type contact region is 2 keV, and the implantation dose is 3.5 × 10⁻⁶. 13 ions / cm 2 The injection energy in the N-type contact region was 5 keV, and the injection dose was 2.7 × 10⁻⁶. 13 ions / cm2 .

[0061] Furthermore, the sample was placed in an inert atmosphere and subjected to rapid thermal annealing at 1100°C for 7 seconds to repair some of the lattice damage caused by ion implantation and to activate the boron and phosphorus dopants.

[0062] S4. Introduce deep-level impurities into the optical mode operating region of the silicon microring resonator to form a deep-level impurity doped absorption region. The doping concentration of the deep-level impurities is lower than their solid solubility in silicon.

[0063] Specifically, a positive electron beam resist polymethyl methacrylate is spin-coated onto the sample surface, and a Te ion implantation window is formed in the silicon microring resonant cavity region through electron beam lithography, development, rinsing and drying.

[0064] Furthermore, using an ion implantation device, Te ions were implanted in the silicon microring resonant cavity region in two steps to form a low-concentration Te deep-level doped absorption region. The first Te ion implantation energy was 150 keV, and the implantation dose was 3 × 10⁻⁶. 10 ions / cm 2 The second Te ion implantation energy was 50 keV, and the implantation dose was 1.25 × 10⁻⁶. 10 ions / cm 2 By multi-energy staged implantation, Te is used to form a deep-level doped region in the top silicon layer that overlaps with the micro-ring optical mode. The Te doping concentration is lower than the solid solubility of Te in silicon, preferably much lower.

[0065] Furthermore, the sample was placed in an inert atmosphere and subjected to rapid thermal annealing at 900°C for 7 seconds to repair some of the lattice damage caused by Te ion implantation and to activate the Te deep-level doping centers.

[0066] S5. Prepare metal electrodes on the P-type doped region and the N-type doped region to obtain the photodetector.

[0067] Specifically, a positive resist is spin-coated onto the sample surface, and metal electrode openings are formed on the P-type ohmic contact area and the N-type ohmic contact area by electron beam lithography. The sample is then placed in a developer solution with an IPA / deionized water volume ratio of 7:3 for 30 seconds, rinsed in IPA for 30 seconds, and dried with N2.

[0068] Furthermore, a Ti / Au metal layer with a thickness of 10 / 100 nm is deposited using an ultra-high vacuum thermal evaporation device; subsequently, the resist and excess metal are removed by acetone immersion and stripping processes, and metal electrodes are formed on the P-type ohmic contact region and the N-type ohmic contact region, thus obtaining a low-concentration Te deep-level doped all-silicon-based room temperature micro-ring resonator photodetector for the communication band.

[0069] In this embodiment, incident light in the communication band is coupled into the input waveguide via a grating coupler and further coupled to a silicon microring resonator. When the incident light wavelength meets the microring resonance condition, the light circulates multiple times within the silicon microring resonator, thereby enhancing the effective interaction between the light and the low-concentration Te deep-level doped absorption region. Te introduces deep levels into the silicon bandgap, enabling photons in the communication band near 1550 nm to generate photogenerated carriers through subbandgap absorption. The P-type and N-type doped regions on both sides of the microring form a transverse built-in electric field, used to separate and collect photogenerated carriers, thus achieving all-silicon-based photodetection in the communication band at room temperature.

[0070] In this embodiment, the Te ions in S4 can be replaced with one or more deep-level impurity ions selected from Se, S, Au, and Ti. The technical solution of this invention is not limited to the Te-doped silicon system, but can also be applied to other impurity doping systems that can introduce deep levels into the silicon bandgap. By setting a low-concentration deep-level impurity doped absorption region in a silicon microring resonant cavity, this invention can utilize the resonant structure to reduce the deep-level impurity doping concentration required for effective photodetection in the communication band, making it suitable for room-temperature photodetectors in the communication band on an all-silicon substrate.

[0071] While the present invention has been disclosed above, its scope of protection is not limited thereto. Those skilled in the art can make various changes and modifications without departing from the spirit and scope of the present invention, and all such changes and modifications will fall within the scope of protection of the present invention.

Claims

1. A low-deep-level doped silicon-based microring photodetector, comprising an SOI substrate and an input waveguide, characterized in that, It also includes a silicon microring resonator, a deep-level impurity doping absorption region, a P-type doped region, an N-type doped region, and metal electrodes; The silicon microring resonant cavity is disposed in the top silicon layer of the SOI substrate and coupled to the input waveguide light to enable the communication band light to propagate multiple times in the top silicon layer, thereby extending the effective path of the communication band light in the deep energy level impurity doped absorption region. The deep-level impurity doped absorption region is disposed within the optical mode operating region of the silicon microring resonator, and is used to introduce deep levels in the silicon bandgap and realize subbandgap absorption of photons in the communication band. The doping concentration of the deep-level impurity in the deep-level impurity doped absorption region is lower than the solid solubility of the deep-level impurity in silicon. The P-type doped region is disposed on the inner side of the silicon microring resonator, and the N-type doped region is disposed on the outer side of the silicon microring resonator. The P-type doped region and the N-type doped region are used to form a transverse built-in electric field in the silicon microring resonator region to separate and collect photogenerated carriers generated by subbandgap absorption. The metal electrode is electrically connected to the P-type doped region and the N-type doped region, respectively.

2. The low-deep-level doped silicon-based microring photodetector according to claim 1, characterized in that, The deep-level impurities include one or more of Te, Se, S, Au, and Ti.

3. The low-deep-level doped silicon-based microring photodetector according to claim 2, characterized in that, The deep-level impurity is Te.

4. The low-deep-level doped silicon-based microring photodetector according to claim 1, characterized in that, The doping concentration of the deep-level impurity is at least an order of magnitude lower than its solid solubility in silicon.

5. The low-deep-level doped silicon-based microring photodetector according to claim 2, characterized in that, The doping concentration of the deep-level impurity is 10. 14 -10 17 cm -3 .

6. The low-deep-level doped silicon-based microring photodetector according to claim 1, characterized in that, The P-type doped region and the N-type doped region are respectively spaced apart from the silicon microring resonator to reduce the additional loss of the optical mode of the silicon microring resonator due to free carrier absorption; the P-type doped region is formed by boron ion implantation, and the N-type doped region is formed by phosphorus ion implantation or arsenic ion implantation; the resonant wavelength of the silicon microring resonator is located in the communication band, and the resonant wavelength is in the range of 1250-1600nm.

7. A method for fabricating a low-deep-level doped silicon-based microring photodetector according to any one of claims 1 to 6, characterized in that, include: Step 1: Obtain an SOI substrate, wherein the SOI substrate comprises a silicon substrate, a silicon dioxide buried oxide layer, and a top silicon layer; Step 2: An input waveguide and a silicon microring resonator are fabricated in the top silicon layer, and the input waveguide is optically coupled to the silicon microring resonator. Step 3: A P-type doped region is formed inside the silicon microring resonator, and an N-type doped region is formed outside the silicon microring resonator, so as to form a transverse built-in electric field in the silicon microring resonator region. Step 4: Introduce deep-level impurities into the optical mode operating region of the silicon microring resonator to form a deep-level impurity doped absorption region. The doping concentration of the deep-level impurities is lower than their solid solubility in silicon. Step 5: Prepare metal electrodes on the P-type doped region and the N-type doped region to obtain the photodetector.

8. The preparation method according to claim 7, characterized in that, In step two, the input waveguide and the silicon microring resonator are fabricated using electron beam lithography and reactive ion etching processes. A coupling gap exists between the input waveguide and the silicon microring resonator to couple incident light of the communication band into the silicon microring resonator.

9. The preparation method according to claim 7, characterized in that, In step three, the P-type doped region is formed by boron ion implantation, and the N-type doped region is formed by phosphorus ion implantation or arsenic ion implantation. The P-type dopant and N-type dopant are then activated by annealing. The P-type doped region and the N-type doped region maintain a preset distance from the silicon microring resonator to reduce the additional absorption loss of the optical mode of the silicon microring resonator by the heavily doped region.

10. The preparation method according to claim 7, characterized in that, In step four, the deep-level impurity is Te, which is introduced into the silicon microring resonator region through multi-energy staged ion implantation, so that the Te doping distribution at least partially overlaps with the optical mode action region of the silicon microring resonator. Step four is followed by annealing to repair some lattice damage caused by deep-level impurity implantation and activate deep-level doping centers.