Back contact solar cells, battery modules and photovoltaic systems
By setting a heterogeneous insert sublayer in the back-contact solar cell to form an anti-hot spot structure, high photoelectric conversion efficiency is maintained while avoiding cell damage, thus solving the problem of hot spot effect.
Patent Information
- Application Number
- CN202611407672.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-10
- Publication Date
- 2026-11-17
AI Technical Summary
Existing back-contact solar cells are prone to hot spot effects when partially shaded, leading to cell damage. Existing bypass diode designs struggle to find a balance between avoiding reduced cell conversion efficiency and reverse breakdown damage.
Multiple heterojunction sublayers are set in the back contact solar cell to form a hot spot resistant structure. The heterojunction sublayers have different reverse activation voltages, and the reverse bias is clamped step by step through a graded start-up mechanism to avoid reverse breakdown.
It effectively suppresses the hot spot effect, reduces the risk of battery damage, and maintains high photoelectric conversion efficiency, while preventing individual anti-hot spot structures from burning out due to excessive current.
Smart Images

Figure CN123124503A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of battery technology, and more specifically, to a back-contact solar cell, a battery module, and a photovoltaic system. Background Technology
[0002] Back-contact solar cells are widely used due to their advantages such as no grid lines obstructing the front side and high conversion efficiency. However, in practical applications, when a portion of the cell is shaded, the shaded area experiences reverse bias in the series circuit. When the reverse bias reaches the reverse breakdown voltage, the PN junction in that area enters a reverse breakdown state. The reverse breakdown current generates a large amount of heat, causing the temperature in that area to rise and forming a hot spot effect. If the heat continues to accumulate, it can lead to cell damage or even a fire.
[0003] In related technologies, a scheme utilizing the unidirectional conductivity of diodes is proposed, namely, constructing a bypass diode between the P-type and N-type regions of the back-contact solar cell. When the reverse bias voltage across the shaded region reaches the forward conduction threshold of the diode, the bypass diode conducts forward, providing a discharge path for the reverse breakdown current. This clamps the reverse bias voltage of the PN junction in that region within a safe range, preventing it from entering the reverse breakdown state, thereby suppressing the hot spot effect and reducing the risk of battery damage due to overheating.
[0004] However, a drawback is that if the effective conduction area of the bypass diode is designed to be too large, although it can effectively reduce the reverse bias voltage, the increased leakage area will lead to a decrease in the parallel resistance of the battery, thereby reducing the battery's conversion efficiency. Conversely, if the effective conduction area of the bypass diode is designed to be too small, the reverse bias voltage will be too high, which can easily cause avalanche breakdown, resulting in PN junction damage and ultimately battery failure. Summary of the Invention
[0005] The present invention aims to solve at least one of the technical problems existing in the prior art, and provides a back-contact solar cell, battery module and photovoltaic system that can effectively suppress hot spot effect while avoiding reducing the conversion efficiency of the battery.
[0006] In a first aspect, the present invention provides a back-contact solar cell, comprising:
[0007] A silicon substrate having a first surface;
[0008] Multiple first doped sublayers and multiple second doped sublayers are alternately disposed on the first surface, the polarities of the first doped sublayers and the second doped sublayers being opposite; there is a spacer region between adjacent first doped sublayers and second doped sublayers;
[0009] A plurality of heterogeneous insertion sublayers are disposed on the first surface, at least a portion of the heterogeneous insertion sublayers are located in the spacer region, and are respectively connected to the adjacent first doped sublayer and second doped sublayer;
[0010] The hetero-inserted sublayer, the first doped sublayer connected to the hetero-inserted sublayer, and the second doped sublayer constitute at least one hot spot resistance structure, and the reverse activation voltage corresponding to at least one hot spot resistance structure is greater than or equal to 10V.
[0011] In some embodiments, the plurality of heterogeneous insert sublayers are divided into multiple groups, and the heterogeneous insert sublayers in different groups have different projected areas on the first surface, and the reverse activation voltages between the first doped sublayer and the second doped sublayer corresponding to the heterogeneous insert sublayers in different groups are different.
[0012] In some embodiments, the magnitude of the reverse activation voltage is positively correlated with the projected area of the heterogeneous insert sublayers in different groups on the first surface.
[0013] In some embodiments, the material of the heterogeneous insert sublayer includes one or more of silicon oxide, silicon nitride, aluminum oxide, hafnium oxide, zirconium oxide, tantalum oxide, titanium oxide, barium strontium titanate, and lead zirconate titanate.
[0014] In some embodiments, the percentage of the number of anti-hot spot structures corresponding to each reverse activation voltage range is as follows: 40% to 50% for voltages greater than or equal to 2V and less than 4V; 20% to 30% for voltages greater than or equal to 4V and less than 7V; 10% to 15% for voltages greater than or equal to 7V and less than 10V; 5% to 10% for voltages greater than or equal to 10V and less than 12V; and less than 5% for voltages greater than or equal to 12V.
[0015] In some embodiments, the material of the heterojunction sublayer is silicon oxide, and the thickness range and number proportion of the heterojunction sublayer corresponding to each reverse activation voltage range are as follows:
[0016] 2V or higher and less than 4V: thickness 1nm to 1.4nm, quantity accounting for 40% to 50%;
[0017] 4V or higher and less than 7V: thickness 1.41nm to 1.8nm, quantity accounting for 20% to 30%;
[0018] 7V or higher and less than 10V: thickness 1.81nm to 2.2nm, quantity percentage 10% to 15%;
[0019] 10V or higher and less than 12V: thickness 2.21nm to 2.6nm, quantity percentage 5% to 10%;
[0020] 12V or higher: thickness 2.61nm to 3.0nm, quantity percentage less than 5%;
[0021] The heterojunction insert sublayer includes a first surface and a second surface disposed opposite to each other. The first surface is connected to the adjacent first doped sublayer, and the second surface is connected to the adjacent second doped sublayer. The thickness of the heterojunction insert sublayer is the distance between the first surface and the second surface.
[0022] In some embodiments, the heterojunction sublayer includes a first portion and a second portion connected together, the first portion being located in the spacer region, and the second portion being located on the side of at least one of the first doped sublayer and the second doped sublayer away from the silicon substrate.
[0023] In some embodiments, the second portion is located on the side of at least one of the first doped sublayer and the second doped sublayer away from the silicon substrate, and overlaps with the other of the first doped sublayer and the second doped sublayer.
[0024] In some embodiments, the projected area of the second part on the first surface is less than or equal to half of the projected area of the first doped sublayer or the second doped sublayer on the first surface.
[0025] In some embodiments, the spacer region is filled with an insulating material.
[0026] In some embodiments, a passivation layer is provided on the side of the first doped sublayer and the second doped sublayer close to the silicon substrate, and the hetero-inserted sublayer is connected to the side of the passivation layer away from the silicon substrate;
[0027] Alternatively, the heterogeneous insert sublayer may pass through the passivation layer and connect to the silicon substrate.
[0028] In a second aspect, the present invention provides a battery assembly comprising a plurality of back-contact solar cells as described in any one of the embodiments of the first aspect.
[0029] Thirdly, the present invention provides a photovoltaic system comprising a battery module as described in any one of the embodiments of the second aspect.
[0030] The present invention has the following beneficial effects:
[0031] This invention provides a back-contact solar cell, battery module, and photovoltaic system. By incorporating at least one anti-hot spot structure on the cell, each anti-hot spot structure corresponds to a reverse activation voltage. As the reverse bias voltage of the shaded area gradually increases, it first reaches the minimum reverse activation voltage. At this minimum voltage, the anti-hot spot structure corresponding to the minimum reverse activation voltage is activated, providing a discharge path for the reverse breakdown current. Since each anti-hot spot structure has different current-limiting characteristics after conduction, the reverse bias voltage can continue to rise, thereby sequentially triggering anti-hot spot structures corresponding to higher reverse activation voltages. Through this graded activation mechanism, the reverse bias voltage of the PN junction in the shaded area can be clamped within a safe range step by step, preventing it from entering an uncontrollable reverse breakdown state, thus effectively suppressing the hot spot effect and reducing the risk of battery damage due to overheating. Attached Figure Description
[0032] Figure 1 A plan view of a first structure of a solar cell provided in an embodiment of the present invention;
[0033] Figure 2 A plan view of a second structure of a solar cell provided in an embodiment of the present invention;
[0034] Figure 3 A plan view of a third structure of a solar cell provided in an embodiment of the present invention;
[0035] Figure 4 A cross-sectional view of a solar cell with a first structure including a heterogeneous intercalation sublayer provided in an embodiment of the present invention;
[0036] Figure 5 A cross-sectional view of a solar cell with a second structure including a heterogeneous intercalation sublayer provided in an embodiment of the present invention;
[0037] Figure 6 A cross-sectional view of a solar cell with a third structure including a heterogeneous intercalation sublayer provided in an embodiment of the present invention;
[0038] Figure 7 A cross-sectional view of a solar cell with a fourth structure including a heterogeneous intercalation sublayer provided in an embodiment of the present invention;
[0039] Figure 8 A cross-sectional view of a solar cell with a fifth structure including a heterogeneous intercalation sublayer provided in an embodiment of the present invention;
[0040] Figure 9 A cross-sectional view of a solar cell with a sixth structure including a heterogeneous intercalation sublayer provided in an embodiment of the present invention;
[0041] Figure 10 A cross-sectional view of a solar cell with a seventh structure including a heterogeneous insert sublayer, provided in an embodiment of the present invention. Detailed Implementation
[0042] To make the objectives, technical solutions, and advantages of this invention clearer, the invention will be further described in detail below with reference to the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are merely illustrative and not intended to limit the invention. All other embodiments obtained by those skilled in the art based on the embodiments of this invention without inventive effort are within the scope of protection of this invention.
[0043] It should be noted that although functional modules are divided in the device schematic diagram and the logical order is shown in the flowchart, in some cases, the steps shown or described may be executed in a different order than the module division in the device or the order in the flowchart. In the description of this invention, "several" means one or more, "multiple" means two or more, "greater than," "less than," and "exceeding" are understood to exclude the number itself, while "above," "below," and "within" are understood to include the number itself. The use of "first" and "second" is merely for distinguishing technical features and should not be construed as indicating or implying relative importance, or implicitly indicating the number of indicated technical features, or implicitly indicating the order of the indicated technical features. Unless otherwise expressly specified and limited, the terms "installation," "connection," "linking," "setting," and "arrangement," etc., should be interpreted broadly. For example, they can refer to a fixed connection, a detachable connection, or an integral connection; a mechanical connection or an electrical connection; a direct connection or an indirect connection through an intermediate medium; or a connection within two components. Those skilled in the art can understand the specific meaning of the above terms in this invention based on the specific circumstances.
[0044] Firstly, such as Figures 1 to 10 As shown, the back-contact solar cell provided in this embodiment of the invention includes:
[0045] Silicon substrate 1, having a first surface;
[0046] Multiple first doped sublayers 3 and multiple second doped sublayers 6 are alternately disposed on the first surface, the polarities of the first doped sublayers 3 and the second doped sublayers 6 are opposite; there is a spacer region 12 between adjacent first doped sublayers 3 and second doped sublayers 6;
[0047] Multiple heterojunction sublayers 4 are disposed on the first surface, at least a portion of the heterojunction sublayers 4 are located in the spacer region 12, and are respectively connected to the adjacent first doped sublayer 3 and second doped sublayer 6.
[0048] Among them, the hetero-inserted sublayer 4, the first doped sublayer 3 connected to the hetero-inserted sublayer 4, and the second doped sublayer 6 constitute at least one hot spot resistance structure, and the reverse activation voltage corresponding to at least one hot spot resistance structure is greater than or equal to 10V.
[0049] In this embodiment, the first doped sublayer 3 and the second doped sublayer 6 have opposite polarities. For example, the first doped sublayer 3 is a P-type doped layer and the second doped sublayer 6 is an N-type doped layer. Alternatively, the first doped sublayer 3 is an N-type doped layer and the second doped sublayer 6 is a P-type doped layer.
[0050] In this embodiment, the first surface is the back side of the battery. The heterojunction sublayer 4, the first doped sublayer 3 connected to the heterojunction sublayer 4, and the second doped sublayer 6 form at least one hot spot resistance structure on the back side of the battery. The hot spot resistance structure is distributed in multiple regions on the first surface, and each of the at least one hot spot resistance structure corresponds to a reverse activation voltage. The reverse activation voltage refers to the critical voltage value that can cause significant avalanche breakdown or tunnel breakdown inside the battery when it is in a reverse bias state. The range of reverse activation voltage can be divided, for example, greater than or equal to 2V and less than 4V, greater than or equal to 4V and less than 7V, greater than or equal to 7V and less than 10V, greater than or equal to 10V and less than 12V, and greater than or equal to 12V.
[0051] The test method for the reverse activation voltage corresponding to the hot spot resistance structure is as follows: A white light source is set up to irradiate the back-contact solar cell, and the voltage across the cell is measured to obtain a first voltage value. Then, a predetermined area on the cell is shaded with a shader to form a hot spot in that area. At this time, the voltage across the cell is measured again to obtain a second voltage value. The absolute value of the difference between the first voltage value and the second voltage value is taken as the reverse activation voltage of the hot spot resistance structure.
[0052] As the reverse bias voltage in the shaded area gradually increases, it first reaches the minimum reverse activation voltage. At this minimum voltage, the anti-hot spot structure is activated, providing a discharge path for the reverse breakdown current. Because each anti-hot spot structure has different current-limiting characteristics after conduction, the reverse bias voltage can continue to rise, thereby sequentially triggering anti-hot spot structures corresponding to higher reverse activation voltages. Through this graded activation mechanism, the reverse bias voltage of the PN junction in the shaded area can be clamped within a safe range step by step, preventing it from entering an uncontrollable reverse breakdown state. This effectively suppresses the hot spot effect and reduces the risk of battery damage due to overheating.
[0053] It should be noted that the total number of anti-heat spot structures and their distribution on the first surface can be adjusted according to the actual situation, which will not be elaborated here.
[0054] In some specific embodiments of the present invention, such as Figure 1 and Figure 2As shown, a heterogeneous insert sublayer 4 is disposed at a portion of the spacer region 12. The heterogeneous insert sublayer 4 is connected to the adjacent first doped sublayer 3 and second doped sublayer 6 to form a hot spot resistant structure. When the projected area of the heterogeneous insert sublayer 4 on the first surface is large (e.g., Figure 2 (Region 10 within the red dashed box in the image) This heat-resistant structure corresponds to a high reverse activation voltage, for example, 12V. When the projected area of the heterojunction sublayer 4 on the first surface is small (e.g., ... Figure 2 The red dashed box area 11 in the diagram represents the area with a low reverse activation voltage, for example, 2V, corresponding to the anti-hot spot structure. The remaining areas within the spacer region 12 are not filled, thus creating spatial isolation between the first doped sublayer 3 and the second doped sublayer 6, which are not connected to the heterojunction sublayer 4.
[0055] In some embodiments, the remaining locations within the spacer region 12 may also be filled with an insulating material (not shown in the figures). Exemplarily, the insulating material may be silicon oxide or the like. While achieving isolation between the first doped sublayer 3 and the second doped sublayer 6, the insulating material can also optimize and improve the mechanical strength and load-bearing capacity of the spacer region 12, preventing damage to the battery structure due to mechanical stress.
[0056] In some specific embodiments of the present invention, such as Figure 3 As shown, heterogeneous insert sublayers 4 can also be filled in all the spacer regions 12. The heterogeneous insert sublayers 4 are connected to the adjacent first doped sublayers 3 and second doped sublayers 6 to form a hot spot resistant structure.
[0057] In some specific embodiments of the present invention, the material of the heterogeneous insert sublayer 4 includes one or more of silicon oxide (SiO2), silicon nitride (Si3N4), aluminum oxide (Al2O3), hafnium oxide (HfO2), zirconium oxide (ZrO2), tantalum oxide (Ta2O5), titanium oxide (TiO2), barium strontium titanate (BST), and lead zirconate titanate (PZT).
[0058] It should be noted that silicon oxide is a low-k dielectric; silicon nitride and aluminum oxide are medium-k dielectrics; hafnium oxide, zirconium oxide, and tantalum oxide are high-k dielectrics; and titanium oxide, barium strontium titanate, and lead zirconate titanate are ultra-high-k dielectrics. k represents the relative permittivity: k≈3.9 for silicon oxide, k≈7 for silicon nitride, k≈9 for aluminum oxide, k≈25 for hafnium oxide, zirconium oxide, and tantalum oxide, k≈80 for titanium oxide, k≈200–500 for barium strontium titanate, and k≈1000 for lead zirconate titanate.
[0059] When the heterogeneous insert sublayer 4 is made of multiple materials, such as silicon oxide and silicon nitride, silicon oxide layers and silicon nitride layers can be prepared sequentially to form a stacked heterogeneous insert sublayer 4.
[0060] In some specific embodiments of the present invention, the percentage of the number of anti-hot spot structures corresponding to each reverse activation voltage range is as follows: 40% to 50% for voltages greater than or equal to 2V and less than 4V; 20% to 30% for voltages greater than or equal to 4V and less than 7V; 10% to 15% for voltages greater than or equal to 7V and less than 10V; 5% to 10% for voltages greater than or equal to 10V and less than 12V; and less than 5% for voltages greater than or equal to 12V.
[0061] It should be noted that the percentage of anti-hot spot structures corresponding to each reverse activation voltage range refers to the ratio of the number of anti-hot spot structures corresponding to each reverse activation voltage range to the total number of anti-hot spot structures on the first surface.
[0062] In this embodiment, the number of anti-hot spot structures corresponding to different reverse activation voltage ranges can be the same or different. This ensures that as the reverse bias voltage gradually increases, a sufficient number of anti-hot spot structures in each reverse activation voltage range are simultaneously turned on to disperse the current and prevent individual anti-hot spot structures from burning out or failing due to excessive current. Reasonably allocating the number of anti-hot spot structures in different reverse activation voltage ranges can provide sufficiently strong anti-hot spot capability and maintain high photoelectric conversion efficiency.
[0063] For example, the probability of a slightly shaded area (low reverse bias) is relatively high, requiring a smaller discharge current. Therefore, the number of anti-hotspot structures in the low reverse activation voltage range can be appropriately reduced to decrease additional leakage current under normal operating conditions. The probability of a heavily shaded area (high reverse bias) is low, but the damage is extremely significant, requiring more anti-hotspot structures for rapid response. Therefore, the number of anti-hotspot structures in the high reverse activation voltage range can be appropriately increased.
[0064] For example, when the material of the heterojunction sublayer 4 is silicon oxide, the thickness range and number proportion of the heterojunction sublayer 4 corresponding to each reverse activation voltage range are as follows:
[0065] 2V or higher and less than 4V: thickness 1nm to 1.4nm, quantity accounting for 40% to 50%;
[0066] 4V or higher and less than 7V: thickness 1.41nm to 1.8nm, quantity accounting for 20% to 30%;
[0067] 7V or higher and less than 10V: thickness 1.81nm to 2.2nm, quantity percentage 10% to 15%;
[0068] 10V or higher and less than 12V: thickness 2.21nm to 2.6nm, quantity percentage 5% to 10%;
[0069] 12V or higher: thickness 2.61nm to 3.0nm, quantity percentage less than 5%.
[0070] It should be noted that, as Figure 4 and Figure 5 As shown, the heterojunction sublayer 4 includes a first surface 41 and a second surface 42 disposed opposite to each other. The first surface 41 is connected to the adjacent first doped sublayer 3, and the second surface 42 is connected to the adjacent second doped sublayer 6. The thickness of the heterojunction sublayer 4 is the distance between the first surface 41 and the second surface 42.
[0071] In some specific embodiments of the present invention, the thickness of the heterojunction sublayer 4 corresponding to each reverse activation voltage range can be derived from the Fowler-Nordheim tunneling formula.
[0072] The Fowler-Nordheim tunnel formula is as follows:
[0073]
[0074] In the formula, This represents the tunneling current density (unit: A / cm²). Represents the amount of electron charge, for example ; This represents the electric field strength perpendicular to the potential barrier (unit: V / m). This represents the effective Schottky barrier height on the cathode side (in eV), such as that of an alumina dielectric layer. Approximately 2.8 eV; It represents the effective mass of an electron in an insulating medium (unit: kg), and is usually taken as 0.2 to 0.4 times the mass of a free electron (including the endpoint value). Describe the reduced Planck constant, for example ; To represent Planck's constant, for example .
[0075] According to the Fowler-Nordheim tunneling formula above, the tunneling current density can be determined. With electric field strength It exhibits an exponential relationship. This is due to the voltage across sublayer 4, which is inserted into the heterogeneous material. Approximately equal to electric field strength With thickness Therefore, in order to achieve conduction at a specific reverse activation voltage, the required heterojunction sublayer thickness can be calculated in reverse using the tunneling formula described above. The specific calculation process is existing technology and will not be elaborated here. Based on this principle, the present invention achieves a stepped distribution design of the reverse activation voltage of the battery by setting the heterogeneous insertion sublayer 4 to different thicknesses and setting a corresponding proportion of heterogeneous insertion sublayer 4 for each thickness.
[0076] In some specific embodiments of the present invention, the shape of the heterogeneous insert sublayer 4 includes various types.
[0077] For example, such as Figures 6 to 10 As shown, the heterogeneous insertion sublayer 4 includes a first part 43 and a second part 44 connected together. The first part 43 is located in the spacer region 12, and the second part 44 is located on the side of at least one of the first doped sublayer 3 and the second doped sublayer 6 away from the silicon substrate 1.
[0078] For example, such as Figure 6 and Figure 10 As shown, the second part 44 is located on the side of the first doped sublayer 3 away from the silicon substrate 1, and the first part 43 and the second part 44 form an L-shaped structure. Figure 7 and Figure 9 As shown, the second part 44 is located on the side of the second doped sublayer 6 away from the silicon substrate 1, and the first part 43 and the second part 44 form an L-shaped structure. The L-shaped structure effectively increases the contact area between the heterojunction sublayer 4 and the first doped sublayer 3 or the second doped sublayer 6, so that under the same electric field strength... The hot spot-resistant structure has more electron tunneling channels, which helps to reduce local current density and reduce the risk of battery breakdown caused by current concentration, thereby achieving reverse activation conduction more efficiently.
[0079] For example, such as Figure 8 As shown, a portion of the second part 44 is located on the side of the first doped sublayer 3 away from the silicon substrate 1, and another portion is located on the side of the second doped sublayer 6 away from the silicon substrate 1. The first part 43 and the second part 44 form a T-shaped structure. The T-shaped structure can ensure that there is a uniform distribution of heterogeneous inserted sublayers 4 at the junction of the first doped sublayer 3 and the second doped sublayer 6 and in the surrounding area, which can effectively eliminate edge effects and make the voltage blocking characteristics of the entire cell more uniform.
[0080] For example, such as Figure 6 and Figure 7 As shown, the second part 44 is located on the side of at least one of the first doped sublayer 3 and the second doped sublayer 6 away from the silicon substrate 1, and overlaps with the other of the first doped sublayer 3 and the second doped sublayer 6.
[0081] For example, such as Figure 6As shown, the second part 44 is located on the side of the first doped sublayer 3 away from the silicon substrate 1, and the first part 43 and the second part 44 form an L-shaped structure. A portion of the second doped sublayer 6 is located on the side of the second part 44 away from the silicon substrate 1. Figure 7 As shown, the second part 44 is located on the side of the second doped sublayer 6 away from the silicon substrate 1, and the first part 43 and the second part 44 form an L-shaped structure, with a portion of the first doped sublayer 3 located on the side of the second part 44 away from the silicon substrate 1. This arrangement enables directional guidance of the carrier transport path. It not only effectively shields the edges of the first doped sublayer 3 or the second doped sublayer 6 to reduce the peak electric field intensity and prevent edge breakdown, but also, the first part 43 located in the spacer region 12 can effectively passivate the silicon substrate 1, thereby optimizing the battery's voltage withstand characteristics and surface recombination performance while ensuring high reverse activation efficiency.
[0082] For example, the projected area of the second part 44 on the first surface is less than or equal to half the projected area of the first doped sublayer 3 or the second doped sublayer 6 on the first surface. This configuration achieves a balance between battery conductivity and voltage withstand capability, while also considering the feasibility of the manufacturing process and structural reliability.
[0083] In some specific embodiments of the present invention, the multiple heterogeneous insert sublayers 4 are divided into multiple groups, and the heterogeneous insert sublayers 4 in different groups have different orthogonal projection areas on the first surface. The reverse activation voltage of the anti-hot spot structure formed by the heterogeneous insert sublayers 4 in different groups and the corresponding first doped sublayers 3 and second doped sublayers 6 is different.
[0084] Furthermore, the magnitude of the reverse activation voltage is positively correlated with the projected area of the heterogeneous insert sublayer 4 on the first surface in different groups.
[0085] For example, the total area of the orthographic projection of all heterogeneous inserted sublayers 4 on the first surface is S, the total area of the first surface is M, and the value range of S / M is, for example, 9.272 × 10⁻⁶. -10 Up to 47.28×10 -10 .
[0086] For example, the orthographic projection area of the heterogeneous insert sublayer 4 in different groups on the first surface includes a first area interval, a second area interval, a third area interval, a fourth area interval, and a fifth area interval; the total orthographic projection areas of the heterogeneous insert sublayer 4 belonging to the first area interval, the second area interval, the third area interval, the fourth area interval, and the fifth area interval on the first surface are S1, S2, S3, S4, and S5, respectively.
[0087] The range of values for S1 / M is, for example, 2.86 × 10⁻⁶. -11 Up to 6.01×10 -10The range of values for S2 / M is, for example, 4.01 × 10⁻⁶. -11 Up to 7.73×10 -10 The range of values for S3 / M is, for example, 5.15 × 10⁻⁶. -11 Up to 9.44×10 -10 The range of values for S4 / M is, for example, 6.3 × 10⁻⁶. -11 Up to 1.12×10 -9 The range of values for S5 / M is, for example, 7.44 × 10. -10 Up to 1.29×10 -9 .
[0088] In some specific embodiments of the present invention, such as Figures 4 to 10 As shown, a passivation layer 2 is disposed on the side of the first doped sublayer 3 and the second doped sublayer 6 near the silicon substrate 1. For example, as... Figure 4 As shown, the heterogeneous insertion sublayer 4 is connected to the side of the passivation layer 2 away from the silicon substrate 1. Alternatively, as... Figures 5 to 10 As shown, the heterogeneous insert sublayer 4 passes through the passivation layer 2 and is connected to the silicon substrate 1.
[0089] In some specific embodiments of the present invention, such as Figures 4 to 10 As shown, the first doped sublayer 3 is connected to a first metal electrode 31 on the side away from the silicon substrate 1, and the second doped sublayer 6 is connected to a second metal electrode 61 on the side away from the silicon substrate 1.
[0090] In some specific embodiments of the present invention, a field-effect passivation layer 7 and a buffer layer 9 are sequentially disposed on the first surface along a direction away from the silicon substrate 1. The silicon substrate 1 also has a second surface (the front side of the battery, i.e., the light-receiving surface) disposed opposite to the first surface, such as... Figures 4 to 10 As shown, a field-effect passivation layer 7, an anti-reflection layer 8, and a buffer layer 9 are sequentially disposed on the second surface along the direction away from the silicon substrate 1 to maximize light absorption. For example, the field-effect passivation layer 7 may be made of aluminum oxide with a thickness less than or equal to 6 nm. The anti-reflection layer 8 may be made of silicon nitride with a thickness less than or equal to 60 nm. The buffer layer 9 may be made of silicon oxide with a thickness less than or equal to 20 nm.
[0091] The fabrication process of the aforementioned back-contact solar cell includes the following steps:
[0092] S1. Provide a silicon substrate, and sequentially prepare a first passivation layer and a first polysilicon layer on its first surface in a direction away from the silicon substrate, wherein the first passivation layer and the first polysilicon layer cover the entire first surface.
[0093] S2. Doping diffusion is performed on the first polysilicon layer to form a first doped layer, which covers the entire first passivation layer.
[0094] S3. Deposit a first doped silicon glass layer on the first doped layer, the first doped silicon glass layer covering the entire first doped layer.
[0095] S4. Laser removal of the first doped silicon glass layer, the first doped layer, the first polycrystalline silicon layer, and the first passivation layer located in the first designated region, forming multiple spaced-apart first doped sublayers. The first designated region includes the area to be prepared for the second doped sublayer, and the spacer region between the first and second doped sublayers.
[0096] S5. A heterojunction layer of maximum thickness is prepared on the side of the retained first doped silicon glass layer away from the silicon substrate, and the heterojunction layer covers the entire first surface.
[0097] S6. The hetero-insertion layer located on the first doped silicon glass layer and the hetero-insertion layer located in the region to be prepared in the second doped sublayer are removed by laser, while the hetero-insertion layer located in the spacer region is retained, forming multiple hetero-insertion sublayers located in the spacer region. At the same time, the thickness of the multiple hetero-insertion sublayers is corrected by laser to obtain multiple hetero-insertion sublayers of different thicknesses.
[0098] S7. On the side of the heterojunction sublayer away from the silicon substrate, along the direction away from the silicon substrate, a second passivation layer and a second polysilicon layer are sequentially prepared, with the second passivation layer and the second polysilicon layer covering the entire first surface.
[0099] S8. Doping diffusion is performed on the second polysilicon layer to form a second doped layer, which covers the entire second passivation layer.
[0100] S9. Deposit a second doped silicon glass layer on the second doped layer, the second doped silicon glass layer covering the entire second doped layer.
[0101] S10: Laser removal of the second doped silicon glass layer, second doped layer, second polysilicon layer, and second passivation layer located in the second designated region. While forming multiple spaced second doped sublayers, this process exposes multiple first doped sublayers formed in step S4, as well as the spacer region formed in step S6 and multiple heterogeneous insertion sublayers located within the spacer region. The second designated region includes the area containing the multiple first doped sublayers and the spacer region between the first and second doped sublayers.
[0102] In this embodiment, taking an N-type silicon substrate as an example, before performing step S1, the silicon substrate needs to be cleaned to remove the damaged layer, surface dirt, organic matter, etc.
[0103] In steps S1 and S7, the materials of the first passivation layer and the second passivation layer can be one of silicon oxide, intrinsic polycrystalline silicon, and intrinsic hydrogenated microcrystalline silicon.
[0104] In step S2, boron diffusion is performed on the first polysilicon layer to form a first doped layer (P-type).
[0105] In step S3, the first doped silicon glass layer is a borosilicate glass layer (BSG).
[0106] Before performing step S7 and after step S10, a polishing process is required to remove any residue left by the laser.
[0107] In step S8, phosphorus diffusion is performed on the second polysilicon layer to form a second doped layer (N-type).
[0108] In step S9, the second doped silicon glass layer is a phosphorosilicate glass layer (PSG).
[0109] In some specific embodiments of the present invention, after the preparation of each film layer on the first surface (back side) is completed, a cleaning step on the second surface (front side) is further included: using a wet etching process to remove the diffusion- or deposition-formed wrap-around layer and deposited layer on the second surface, so that the second surface is restored to a clean silicon substrate surface. This cleaning step may use tetramethylammonium hydroxide solution (TMAH) or potassium hydroxide solution (KOH) to remove the wrap-around polycrystalline silicon layer and other deposited layers.
[0110] In some specific embodiments of the present invention, after cleaning the second surface, the first doped silicon glass layer and the second doped silicon glass layer are removed by dilute hydrofluoric acid solution (HF), and then the second surface is texturized with alkaline solution to form an anti-reflective textured surface.
[0111] In some specific embodiments of the present invention, after preparing an antireflective textured surface on the second surface, a field-effect passivation layer 7 is first deposited on the first and second surfaces using atomic layer deposition (ALD). Next, an antireflective layer 8 is deposited on the second surface using plasma-enhanced chemical vapor deposition (PECVD). Finally, a buffer layer 9 is deposited on the first and second surfaces using PECVD.
[0112] In some specific embodiments of the present invention, after depositing buffer layers 9 on the first and second surfaces, a first metal electrode and a second metal electrode are respectively prepared on the side of the first and second doped sublayers on the first surface away from the silicon substrate by means of printing combined with an infrared belt sintering furnace or by means of electroplating. The materials of the first metal electrode and the second metal electrode include one or more of gold, silver, copper, tin, and nickel.
[0113] It is understood that the steps involved in the fabrication process of the back-contact solar cell described above are merely exemplary and not exhaustive or in a fixed order. In actual processes, some steps may be combined, adjusted, or omitted.
[0114] Secondly, the battery assembly provided in the embodiments of the present invention includes multiple back-contact solar cells as described in any of the embodiments of the first aspect.
[0115] Thirdly, the photovoltaic system provided in the embodiments of the present invention includes the battery module as described in the second aspect embodiment.
[0116] It is understood that the above embodiments are merely exemplary implementations used to illustrate the principles of the present invention, and the present invention is not limited thereto. For those skilled in the art, various modifications and improvements can be made without departing from the spirit and essence of the present invention, and these modifications and improvements are also considered to be within the scope of protection of the present invention.
Claims
1. A back-contact solar cell, characterized in that, include: A silicon substrate having a first surface; Multiple first doped sublayers and multiple second doped sublayers are alternately disposed on the first surface, wherein the polarities of the first doped sublayers and the second doped sublayers are opposite; There is a spacer region between adjacent first and second doped sublayers; A plurality of heterogeneous insertion sublayers are disposed on the first surface, at least a portion of the heterogeneous insertion sublayers are located in the spacer region, and are respectively connected to the adjacent first doped sublayer and second doped sublayer; The hetero-inserted sublayer, the first doped sublayer connected to the hetero-inserted sublayer, and the second doped sublayer constitute at least one hot spot resistance structure, and the reverse activation voltage corresponding to at least one hot spot resistance structure is greater than or equal to 10V.
2. The back-contact solar cell according to claim 1, characterized in that, The heterogeneous insert sublayers are divided into multiple groups. The heterogeneous insert sublayers in different groups have different projected areas on the first surface. The reverse activation voltages between the first doped sublayer and the second doped sublayer corresponding to the heterogeneous insert sublayers in different groups are different.
3. The back-contact solar cell according to claim 2, characterized in that, The magnitude of the reverse activation voltage is positively correlated with the projected area of the heterogeneous inserted sublayers in different groups on the first surface.
4. The back-contact solar cell according to claim 1, characterized in that, The material of the heterogeneous insert sublayer includes one or more of silicon oxide, silicon nitride, aluminum oxide, hafnium oxide, zirconium oxide, tantalum oxide, titanium oxide, barium strontium titanate, and lead zirconate titanate.
5. The back-contact solar cell according to claim 4, characterized in that, The percentage of the number of anti-hot spot structures corresponding to each reverse activation voltage range is as follows: 40% to 50% for voltages greater than or equal to 2V and less than 4V; 20% to 30% for voltages greater than or equal to 4V and less than 7V; 10% to 15% for voltages greater than or equal to 7V and less than 10V; 5% to 10% for voltages greater than or equal to 10V and less than 12V; and less than 5% for voltages greater than or equal to 12V.
6. The back-contact solar cell according to claim 4, characterized in that, The heterojunction sublayer is made of silicon oxide, and according to the reverse activation voltage range, the thickness range and number proportion of the heterojunction sublayer corresponding to each range are as follows: 2V or higher and less than 4V: thickness 1nm to 1.4nm, quantity accounting for 40% to 50%; 4V or higher and less than 7V: thickness 1.41nm to 1.8nm, quantity accounting for 20% to 30%; 7V or higher and less than 10V: thickness 1.81nm to 2.2nm, quantity percentage 10% to 15%; 10V or higher and less than 12V: thickness 2.21nm to 2.6nm, quantity percentage 5% to 10%; 12V or higher: thickness 2.61nm to 3.0nm, quantity percentage less than 5%; The heterojunction insert sublayer includes a first surface and a second surface disposed opposite to each other. The first surface is connected to the adjacent first doped sublayer, and the second surface is connected to the adjacent second doped sublayer. The thickness of the heterojunction insert sublayer is the distance between the first surface and the second surface.
7. The back-contact solar cell according to any one of claims 1 to 6, characterized in that, The heterojunction sublayer includes a first part and a second part connected together, the first part being located in the spacer region, and the second part being located on the side of at least one of the first doped sublayer and the second doped sublayer away from the silicon substrate.
8. The back-contact solar cell according to claim 7, characterized in that, The second part is located on the side of at least one of the first doped sublayer and the second doped sublayer away from the silicon substrate, and overlaps with the other of the first doped sublayer and the second doped sublayer.
9. The back-contact solar cell according to claim 7, characterized in that, The projected area of the second part on the first surface is less than or equal to half of the projected area of the first doped sublayer or the second doped sublayer on the first surface.
10. The back-contact solar cell according to any one of claims 1 to 6, characterized in that, The spacer area is filled with an insulating material.
11. The back-contact solar cell according to any one of claims 1 to 6, characterized in that, A passivation layer is provided on the side of the first doped sublayer and the second doped sublayer close to the silicon substrate, and the hetero-inserted sublayer is connected to the side of the passivation layer away from the silicon substrate; Alternatively, the heterogeneous insert sublayer may pass through the passivation layer and connect to the silicon substrate.
12. A battery assembly, characterized in that, It includes multiple back-contact solar cells as described in any one of claims 1 to 11.
13. A photovoltaic system, characterized in that, Includes the battery assembly as described in claim 12.