Photodetector and its formation method
By forming holes in the waveguide layer of the photodetector and filling them with a light absorption layer to form a photonic crystal structure, the problem of bandwidth limitation due to increased absorption layer thickness and length is solved, thereby improving the responsivity and absorption efficiency of the photodetector.
Patent Information
- Application Number
- CN202510624244.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2025-05-14
- Publication Date
- 2026-11-17
AI Technical Summary
In existing photodetectors, increasing the thickness and length of the absorption layer to improve responsivity increases the transit time of charge carriers, thus limiting the device bandwidth.
Multiple holes are formed in the waveguide layer of the photodetector, and light absorption layers are filled in the holes to form a photonic crystal structure. This modulates the light field distribution, increases the effective contact area between the light absorption layer and the waveguide layer, and reduces reflection.
Without increasing the length of the light absorption layer, the responsivity and light absorption efficiency of the photodetector are improved, and light reflection is reduced.
Smart Images

Figure CN123124515A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of semiconductor manufacturing, and more particularly to a photodetector and a method for forming the same. Background Technology
[0002] Optical interconnects can overcome the problems of low bandwidth and high power consumption in electrical interconnects, which is beneficial to the development of technologies such as big data, cloud computing, and the Internet of Things. Silicon-based germanium photodetectors are important active devices for realizing optical interconnects. Growing germanium materials on silicon is compatible with mature complementary metal-oxide-semiconductor (CMOS) technology and expands the absorption range of infrared bands (such as C-band and O-band) for communication.
[0003] Currently, in order to improve the responsivity of devices, it is generally necessary to increase the thickness and length of the absorption layer to improve the light absorption rate. However, this also increases the transit time of charge carriers and limits the bandwidth of the device. Summary of the Invention
[0004] The problem solved by the embodiments of the present invention is to provide a photodetector and a method for forming the same, which is beneficial to improving the responsivity of the photodetector.
[0005] To address the aforementioned problems, embodiments of the present invention provide a photodetector, comprising: a substrate; a waveguide layer located on the substrate, the waveguide layer including an absorption region, wherein a plurality of holes are formed in a portion of the waveguide layer within the absorption region; and a light absorption layer covering the waveguide layer of the absorption region and filling the plurality of holes.
[0006] Optionally, multiple pores in the absorption region are arranged periodically.
[0007] Optionally, multiple holes may be arranged in an array within the absorption region.
[0008] Optionally, the aperture size is 40 nm to 80 nm.
[0009] Optionally, the spacing between adjacent holes is 20 nm to 60 nm.
[0010] Optionally, the depth of the holes can be from 80 nm to 120 nm.
[0011] Optionally, a first doped layer and a second doped layer are formed in the waveguide layers on both sides of the absorption region perpendicular to the direction of light propagation, with the doping types of the first doped layer and the second doped layer being opposite.
[0012] Optionally, a first interconnect via structure electrically connected thereto is formed on the first doped layer; and a second interconnect via structure electrically connected thereto is formed on the second doped layer.
[0013] Optionally, the waveguide layer may be made of silicon; the light-absorbing layer may be made of germanium.
[0014] Accordingly, embodiments of the present invention also provide a method for forming a waveguide structure, comprising: providing a substrate, on which a waveguide layer is formed, the waveguide layer including an absorption region; patterning a portion of the thickness of the waveguide layer of the absorption region to form a plurality of holes; and forming a waveguide layer covering the absorption region and filling the plurality of holes with a light absorption layer.
[0015] Optionally, in the step of forming multiple holes in a waveguide layer of partial thickness in the patterned absorption region, the multiple holes in the absorption region are arranged periodically.
[0016] Optionally, in the step of forming multiple holes in a waveguide layer of partial thickness in the patterned absorption region, multiple holes are arranged in an array in the absorption region.
[0017] Optionally, the step of patterning a portion of the waveguide layer with a patterned absorption region thickness to form multiple holes includes: forming a mask layer covering the waveguide layer, with multiple mask openings formed in the mask layer above the absorption region; patterning the waveguide layer along the mask openings to form multiple holes; and after forming multiple holes, further including: removing the mask layer.
[0018] Optionally, the step of forming a waveguide layer covering the absorption region and a light absorption layer filling multiple holes includes: forming a blocking layer covering the waveguide layer; removing the blocking layer above the absorption region to form a growth opening of the waveguide layer exposing the absorption region; and forming a waveguide layer covering the absorption region and a light absorption layer filling multiple holes in the growth opening.
[0019] Optionally, an epitaxial growth process is used to form a waveguide layer covering the absorption region, and a light absorption layer filled with multiple holes is also used.
[0020] Optionally, before forming the waveguide layer covering the absorption region and the light absorption layer filling the multiple holes, the forming method further includes: forming a first doped layer in the waveguide layer on one side of the absorption region perpendicular to the light propagation direction; and forming a second doped layer in the waveguide layer on the other side of the absorption region perpendicular to the light propagation direction, wherein the doping types of the first doped layer and the second doped layer are opposite.
[0021] Optionally, the step of forming a first doped layer in the waveguide layer on one side of the absorption region perpendicular to the light propagation direction includes: forming a first shielding layer on the waveguide layer, wherein the first shielding layer has a first opening exposing the top of the waveguide layer on the absorption region side; performing a first ion implantation process on the waveguide layer along the first opening to form the first doped layer; the step of forming a second doped layer in the waveguide layer on the other side of the absorption region perpendicular to the light propagation direction includes: forming a second shielding layer on the waveguide layer, wherein the second shielding layer has a second opening exposing the top of the waveguide layer on the other side of the absorption region; performing a second ion implantation process on the waveguide layer along the second opening to form the second doped layer, wherein the implanted ion types of the first ion implantation process and the second ion implantation process are opposite.
[0022] Optionally, before forming the first doped layer and the second doped layer, the method further includes: forming a protective layer that fills a plurality of holes and covers the waveguide layer; in the step of forming the first shielding layer on the waveguide layer, the first shielding layer is formed on the protective layer; in the step of forming the second shielding layer on the waveguide layer, the second shielding layer is formed on the protective layer.
[0023] Optionally, after forming a waveguide layer covering the absorption region and a light-absorbing layer filling multiple holes, the formation method further includes: forming a first interconnect via structure electrically connected thereto on a first doped layer; and forming a second interconnect via structure electrically connected thereto on a second doped layer.
[0024] Compared with the prior art, the technical solution of the embodiments of the present invention has the following advantages:
[0025] In the photodetector provided in this embodiment of the invention, a waveguide layer is located on a substrate. The waveguide layer includes an absorption region, and multiple holes are formed in a portion of the waveguide layer within the absorption region. A light absorption layer covers the waveguide layer of the absorption region and fills the multiple holes. In this embodiment of the invention, the light absorption layer covers the waveguide layer of the absorption region and fills the multiple holes. In the path of light absorption by the light absorption layer, the waveguide layer and the light absorption layer are alternately arranged to form a propagation medium composed of media with different refractive indices. That is, a photonic crystal structure is introduced into the photodetector. The introduction of the photonic crystal structure modulates the light field distribution in the light absorption layer, forming local field enhancement, confining the light within the photonic crystal, and increasing the volume ratio of the surface to the active device. This improves the responsivity of the photodetector without increasing the length of the light absorption layer. Moreover, the light absorption layer and the waveguide layer are in contact through the morphology of the holes, increasing the effective contact area between the light absorption layer and the waveguide layer, which is beneficial for improving the full absorption of light and reducing reflected light, thereby enhancing light absorption and improving the responsivity of the photodetector.
[0026] In the formation method provided by the embodiments of the present invention, a waveguide layer with a patterned absorption region thickness is formed to create multiple holes, forming a waveguide layer covering the absorption region and a light absorption layer filling the multiple holes. In the embodiments of the present invention, the light absorption layer covers the waveguide layer of the absorption region and fills the multiple holes. In the path of light absorption by the light absorption layer, the waveguide layer and the light absorption layer are alternately arranged to form a propagation medium composed of media with different refractive indices. That is, a photonic crystal structure is introduced into the photodetector. The introduction of the photonic crystal structure regulates the light field distribution in the light absorption layer, forming local field enhancement, confining the light within the photonic crystal, increasing the surface-to-volume ratio of the active device, thereby improving the responsivity of the photodetector without increasing the length of the light absorption layer. Moreover, the light absorption layer and the waveguide layer are in contact through the morphology of the holes, increasing the effective contact area between the light absorption layer and the waveguide layer, which is beneficial to improving the full absorption of light and reducing reflected light, thus enhancing light absorption and improving the responsivity of the photodetector. Attached Figure Description
[0027] Figure 1 This is a schematic diagram of the structure of one embodiment of the photodetector of the present invention;
[0028] Figures 2 to 20 This is a schematic diagram of the structure corresponding to each step in one embodiment of the method for forming the photodetector of the present invention. Detailed Implementation
[0029] As is known from the background technology, in order to improve the responsivity of photodetectors, it is generally necessary to increase the thickness and length of the light absorption layer to improve the light absorption rate. However, this also increases the transit time of charge carriers and limits the bandwidth of the photodetector.
[0030] To address the aforementioned technical problems, embodiments of the present invention provide a photodetector, comprising: a substrate; a waveguide layer located on the substrate, the waveguide layer including an absorption region, wherein a plurality of holes are formed in a portion of the thickness of the waveguide layer in the absorption region; and a light absorption layer covering the waveguide layer in the absorption region and filling the plurality of holes.
[0031] In this embodiment of the invention, the light absorption layer covers the waveguide layer of the absorption region and fills multiple holes. In the path of light absorption by the light absorption layer, the waveguide layer and the light absorption layer are alternately arranged to form a propagation medium composed of media with different refractive indices. That is, a photonic crystal structure is introduced into the photodetector. The introduction of the photonic crystal structure modulates the light field distribution in the light absorption layer, forming local field enhancement, confining the light within the photonic crystal, and increasing the surface-to-volume ratio of the active device. This can improve the responsivity of the photodetector without increasing the length of the light absorption layer. Moreover, the light absorption layer and the waveguide layer are in contact through the morphology of the holes, which increases the effective contact area between the light absorption layer and the waveguide layer, which is beneficial to improve the full absorption of light and reduce reflected light, thereby enhancing light absorption and improving the responsivity of the photodetector.
[0032] To make the above-mentioned objects, features and advantages of the present invention more apparent and understandable, specific embodiments of the present invention will be described in detail below with reference to the accompanying drawings.
[0033] Figure 1 This is a schematic diagram of the structure of one embodiment of the photodetector of the present invention.
[0034] refer to Figure 1 The photodetector includes: a substrate 100; a waveguide layer 200 located on the substrate 100, the waveguide layer 200 including an absorption region 100a, a plurality of holes 230 formed in a portion of the thickness of the waveguide layer 200 in the absorption region 100a; and a light absorption layer 300 covering the waveguide layer 200 in the absorption region 100a and filling the plurality of holes 230.
[0035] Substrate 100 provides the basis for the fabrication process of the photodetector.
[0036] In this embodiment, the substrate 100 includes a substrate 110 and an isolation layer 120 covering the substrate 110.
[0037] Specifically, in the photodetector manufacturing process, a silicon-on-insulator (SOI) substrate is used as substrate 100. The substrate 110 is a base silicon, which is usually thick and serves as a mechanical support. The isolation layer 120 is an insulating layer (Buried Oxide, BOX). Between the top silicon and the base silicon, there is usually a thin layer of silicon oxide (SiO2) which serves as an electrical isolation layer. The waveguide layer 200 is formed from the top silicon (Device Layer), which is the silicon layer used to form semiconductor devices.
[0038] The waveguide layer 200 is used as a channel for light propagation, wherein the absorption region 100a is the main region for light absorption.
[0039] Specifically, in this embodiment, the absorption region 100a is along the direction of light propagation (e.g., Figure 1 (Extended in the Y direction as shown)
[0040] In this embodiment, the waveguide layer 200 is made of silicon.
[0041] Using silicon as the waveguide layer 200 helps reduce light transmission loss.
[0042] In other embodiments, the waveguide layer may also be made of silicon nitride.
[0043] In this embodiment, a plurality of holes 230 are formed in a portion of the waveguide layer 200 in the absorption region 100a.
[0044] Multiple holes 230 are used to provide space for the formation of the light-absorbing layer 300.
[0045] In this embodiment, the light absorption layer 300 covers the waveguide layer 200 of the absorption region 100a and fills multiple holes 230. In the path of light absorption by the light absorption layer 300, the waveguide layer 200 and the light absorption layer 300 are alternately arranged to form a propagation medium composed of media with different refractive indices. That is, a photonic crystal structure is introduced into the photodetector. The introduction of the photonic crystal structure regulates the light field distribution in the light absorption layer 300, forming local field enhancement, confining the light within the photonic crystal, and increasing the surface-to-volume ratio of the active device. This can improve the responsivity of the photodetector without increasing the length of the light absorption layer. Moreover, the light absorption layer 300 and the waveguide layer 200 are in contact through the morphology of the holes 230, which increases the effective contact area between the light absorption layer 300 and the waveguide layer 200, which is beneficial to improve the full absorption of light and reduce reflected light, thereby enhancing light absorption and improving the responsivity of the photodetector.
[0046] In this embodiment, multiple pores 230 are arranged periodically in the absorption region 100a.
[0047] Multiple holes 230 are arranged periodically, that is, in the contact surface direction, the light absorption layer 300 and the waveguide layer 200 are arranged periodically, which can better form a photonic crystal structure. In the photonic crystal structure, the periodic change of the refractive index of light produces an optical bandgap structure, which increases the light absorption rate to a relatively high level.
[0048] In this embodiment, multiple holes 230 are arranged in an array in the absorption region 100a.
[0049] The array of multiple holes 230 results in good uniformity of hole arrangement in absorption region 100a. This is beneficial for light of a specific wavelength to form a relatively stable standing wave when it is reflected back and forth in the periodic structure. The waves superimposed on each other and enhanced, thus reaching a resonant state and improving the light absorption rate.
[0050] In this embodiment, the opening size of the hole 230 is 40nm to 80nm, which is beneficial to make the light resonate in the photonic crystal structure and enhance the light absorption effect. However, if the opening size of the hole 230 is too large or too small, it is easy to deviate from the resonant state, thereby weakening the strong light absorption effect.
[0051] Specifically, in the actual manufacturing process, the opening size of the hole 230 can be determined through simulation in order to obtain a better resonance effect in the photonic crystal structure.
[0052] In this embodiment, the spacing between adjacent holes 230 is 20nm to 60nm, which is beneficial for arranging a large number of holes 230 in the absorption region 100a, while not causing significant process difficulties in the formation of holes 230.
[0053] Specifically, in this embodiment, the sum of the opening size of the hole 230 and the spacing between adjacent holes 230 is taken as the period of the hole 230. In this embodiment, the period of the hole 230 is taken as an integer multiple of half the period of the incident light wavelength, thereby obtaining a better resonance effect and a better light absorption enhancement effect.
[0054] In this embodiment, the depth of the hole 230 is 80nm to 120nm, which is beneficial to increase the effective contact area between the light absorption layer 300 and the waveguide layer 200 while ensuring that the waveguide layer 200 still has sufficient thickness to guarantee the basic function of the photodetector.
[0055] In this embodiment, the hole 230 is cylindrical. In other embodiments, the hole may also be cuboid or triangular prism.
[0056] The light-absorbing layer 300 is used to absorb photons.
[0057] Specifically, in this embodiment, when photons are absorbed by the light-absorbing layer 300, electron-hole pairs are generated. Under the action of an applied electric field, these charge carriers drift and form a current, thereby converting the optical signal into an electrical signal.
[0058] In this embodiment, the material of the light-absorbing layer 300 includes germanium.
[0059] In other embodiments, the material of the light-absorbing layer may also be a germanium alloy.
[0060] As an example, in this embodiment, the photodetector is an evanescent waveguide-coupled silicon-based germanium (Ge-on-Si) photodetector. In the detector, the optical signal is transmitted through the silicon waveguide layer 200. Due to the refractive index distribution characteristics of the silicon waveguide layer 200, an evanescent field is generated when light propagates in the waveguide layer 200, which is an attenuation field near the surface of the waveguide layer 200. When a germanium light-absorbing layer 300 covers the waveguide layer 200, the evanescent field extends into the germanium light-absorbing layer 300, allowing the optical signal to couple into the germanium light-absorbing layer 300. When the optical signal is coupled into the germanium light-absorbing layer 300 through the evanescent field, photons are absorbed and excited electrons to jump to the conduction band, forming electron-hole pairs. Under the action of an applied reverse bias voltage, these charge carriers separate and drift under the action of an electric field, forming a photocurrent.
[0061] It should be noted that in this embodiment, the silicon waveguide layer 200 is used, which is based on a silicon platform and is compatible with CMOS technology, which is beneficial for the integration of photodetectors with other optoelectronic devices.
[0062] In this embodiment, the dimensions of the light absorption layer 300 can be obtained based on simulation. As an example, in this embodiment, the length of the light absorption layer 300 is 10μm, the width is 0.5μm, and the height is 0.16μm.
[0063] In this embodiment, perpendicular to the direction of light propagation (e.g.) Figure 1 In the X direction, a first doped layer 330 and a second doped layer 340 are formed in the waveguide layers 200 on both sides of the absorption region 100a, respectively. The doping types of the first doped layer 330 and the second doped layer 340 are opposite.
[0064] The first doped layer 330 and the second doped layer 340 have opposite doping types, forming a PIN-type photodetector.
[0065] Specifically, in this embodiment, the first doped layer 330 and the second doped layer 340 are heavily doped regions. The impurity concentration in the heavily doped regions is high, so the carrier concentration is also high, and the conductivity is significantly increased. Thus, the first doped layer 330 and the second doped layer 340 are used to form a low-resistance ohmic contact.
[0066] As an example, in this embodiment, the first doped layer 330 is an N-type heavily doped region, and the second doped layer 340 is a P-type heavily doped region.
[0067] In this embodiment, a first lightly doped layer 310 corresponding to the first doped layer 330 and a second lightly doped layer 320 corresponding to the second doped layer 340 are respectively formed in the waveguide layer 200 on both sides of the absorption region 100a in a direction perpendicular to the light propagation direction. The doping types of the first lightly doped layer 310 and the second lightly doped layer 320 are opposite.
[0068] Specifically, in this embodiment, the first lightly doped layer 310 and the second lightly doped layer 320 are lightly doped regions. The impurity concentration in the lightly doped regions is low, and therefore the carrier concentration is also low. This is used to form a low conductivity region, reduce parasitic effects, and improve device performance.
[0069] As an example, in this embodiment, the first lightly doped layer 310 is an N-type lightly doped region, and the second lightly doped layer 320 is a P-type lightly doped region.
[0070] In this embodiment, a first interconnect via structure 510 electrically connected to the first doped layer 330 is formed thereon; and a second interconnect via structure 520 electrically connected to the second doped layer 340 is formed thereon.
[0071] The first interconnect via structure 510 is used to realize the electrical connection between the first doped layer 330 and the outside, and the second via interconnect structure 520 is used to realize the electrical connection between the second doped layer 340 and the outside.
[0072] In this embodiment, the photodetector further includes a dielectric layer 400, which is located on the substrate 100 and covers the waveguide layer 200 and the light absorption layer 300.
[0073] The dielectric layer 400 is used to provide a process operation platform for the formation of the photodetector part structure.
[0074] In this embodiment, the material of the dielectric layer 400 includes silicon oxide.
[0075] Figures 2 to 20 This is a schematic diagram of the structure corresponding to each step in one embodiment of the method for forming the photodetector of the present invention.
[0076] refer to Figure 2 A substrate 100 is provided, on which a waveguide layer 200 is formed, the waveguide layer 200 including an absorption region 100a.
[0077] Substrate 100 provides the basis for the fabrication process of the photodetector.
[0078] In this embodiment, the substrate 100 includes a substrate 110 and an isolation layer 120 covering the substrate 110.
[0079] Specifically, in the photodetector manufacturing process, a silicon-on-insulator (SOI) substrate is used as substrate 100. The substrate 110 is a base silicon, which is usually thick and serves as a mechanical support. The isolation layer 120 is an insulating layer (Buried Oxide, BOX). Between the top silicon and the base silicon, there is usually a thin layer of silicon oxide (SiO2) which serves as an electrical isolation layer. The waveguide layer 200 is formed from the top silicon (Device Layer), which is the silicon layer used to form semiconductor devices.
[0080] The waveguide layer 200 is used as a channel for light propagation, wherein the absorption region 100a is the main region for light absorption.
[0081] Specifically, in this embodiment, the absorption region 100a is along the direction of light propagation (e.g., Figure 2 (Extended in the Y direction as shown)
[0082] In this embodiment, the waveguide layer 200 is made of silicon.
[0083] Using silicon as the waveguide layer 200 helps reduce light transmission loss.
[0084] In other embodiments, the waveguide layer may also be made of silicon nitride.
[0085] In this embodiment, during the step of providing the substrate 100, a first dielectric layer 130 covering the waveguide layer 200 is also formed on the substrate 100.
[0086] The first dielectric layer 130 is used to provide a process operation platform for subsequent processes.
[0087] In this embodiment, the material of the first dielectric layer 130 includes silicon oxide.
[0088] Reference Figures 3 to 4 A waveguide layer 200 with a partial thickness of patterned absorption region 100a forms multiple holes 230.
[0089] Multiple holes 230 are used to provide space for the formation of subsequent light-absorbing layers.
[0090] In this embodiment, the light absorption layer covers the waveguide layer 200 of the absorption region 100a and fills multiple holes 230. In the path of light absorption by the light absorption layer, the waveguide layer 200 and the light absorption layer are alternately arranged to form a propagation medium composed of media with different refractive indices. That is, a photonic crystal structure is introduced into the photodetector. The introduction of the photonic crystal structure modulates the light field distribution in the light absorption layer, forming local field enhancement, confining the light within the photonic crystal, and increasing the surface-to-volume ratio of the active device. This can improve the responsivity of the photodetector without increasing the length of the light absorption layer. Moreover, the light absorption layer and the waveguide layer 200 are in contact through the morphology of the holes 230, which increases the effective contact area between the light absorption layer and the waveguide layer 200, which is beneficial to improve the full absorption of light and reduce reflected light, thereby enhancing light absorption and improving the responsivity of the photodetector.
[0091] In this embodiment, in the step of forming multiple holes 230 in the waveguide layer 200 of the partial thickness of the patterned absorption region 100a, the multiple holes 230 in the absorption region 100a are arranged periodically.
[0092] Multiple holes 230 are arranged periodically, that is, the light absorption layer and the waveguide layer 200 are arranged periodically in the contact surface direction, so as to form a photonic crystal structure. In the photonic crystal structure, the periodic change of the refractive index of light produces an optical bandgap structure, which increases the light absorption rate to a relatively high level.
[0093] In this embodiment, in the step of forming multiple holes 230 in a waveguide layer 200 with a partial thickness of patterned absorption region 100a, multiple holes 230 are arranged in an array in absorption region 100a.
[0094] The array of multiple holes 230 results in good uniformity of hole arrangement in absorption region 100a. This is beneficial for light of a specific wavelength to form a relatively stable standing wave when it is reflected back and forth in the periodic structure. The waves superimposed on each other and enhanced, thus reaching a resonant state and improving the light absorption rate.
[0095] In this embodiment, the opening size of the hole 230 is 40nm to 80nm, which is beneficial to make the light resonate in the photonic crystal structure and enhance the light absorption effect. However, if the opening size of the hole 230 is too large or too small, it is easy to deviate from the resonant state, thereby weakening the strong light absorption effect.
[0096] Specifically, in the actual manufacturing process, the opening size of the hole 230 can be determined through simulation in order to obtain a better resonance effect in the photonic crystal structure.
[0097] In this embodiment, in the step of forming multiple holes 230 in the waveguide layer 200 of the patterned absorption region 100a, the spacing between adjacent holes 230 is 20nm to 60nm, which is beneficial to properly arrange more holes 230 in the absorption region 100a, while not causing great process difficulty to the formation of holes 230.
[0098] Specifically, in this embodiment, the sum of the opening size of the hole 230 and the spacing between adjacent holes 230 is taken as the period of the hole 230. In this embodiment, the period of the hole 230 is taken as an integer multiple of half the period of the incident light wavelength, thereby obtaining a better resonance effect and a better light absorption enhancement effect.
[0099] In this embodiment, in the step of forming multiple holes 230 in the waveguide layer 200 with a partial thickness of patterned absorption region 100a, the depth of the holes 230 is 80nm to 120nm. This is beneficial to increase the effective contact surface between the light absorption layer and the waveguide layer 200 while ensuring that the waveguide layer 200 still has sufficient thickness to guarantee the basic function of the photodetector.
[0100] In this embodiment, in the step of forming multiple holes 230 in the waveguide layer 200 with a partial thickness of the patterned absorption region 100a, the shape of the holes 230 is cylindrical. In other embodiments, the shape of the holes can also be cuboid or triangular prism.
[0101] Specifically, refer to Figure 3 The step of forming a plurality of holes 230 in a waveguide layer 200 with a partial thickness of patterned absorption region 100a includes: forming a mask layer 210 covering the waveguide layer 200, wherein a plurality of mask openings 220 are formed in the mask layer 210 above the absorption region 100a.
[0102] The mask layer 210 is used as an etching mask for the patterned waveguide layer 200.
[0103] Accordingly, in this embodiment, in the step of forming the mask layer 210 covering the waveguide layer 200, the mask layer 210 is located on the first dielectric layer 130.
[0104] refer to Figure 4 A waveguide layer 200 is patterned along the mask opening 220 to form multiple holes 230.
[0105] Accordingly, in this embodiment, in the step of patterning the waveguide layer 200 along the mask opening 220, the first dielectric layer 130 is also patterned along the mask opening 220.
[0106] refer to Figure 5 After forming multiple holes 230, the process also includes: removing the mask layer 210.
[0107] Remove the mask layer 210 to prepare for subsequent processes.
[0108] Accordingly, in this embodiment, the first dielectric layer 130 with a certain thickness is also removed in the step of removing the mask layer 210.
[0109] refer to Figure 6 Before the formation of the first doped layer and the second doped layer, the process also includes forming a protective layer 140 that fills multiple holes 230 and covers the waveguide layer 200.
[0110] The protective layer 140 is used to protect the waveguide layer 200 and to provide a process platform with better flatness for subsequent processes.
[0111] In this embodiment, the material of the protective layer 140 includes silicon oxide.
[0112] Reference Figures 7 to 8 Before the formation of the first doped layer and the second doped layer, the process also includes: [the process is described in the context of] perpendicular to the light propagation direction (e.g., ... Figure 7 On the X-direction (as shown), a first lightly doped layer 310 is formed in the waveguide layer 200 on one side of the absorption region 100a.
[0113] Specifically, refer to Figure 7 The step of forming a first lightly doped layer 310 in the waveguide layer 200 on the absorption region 100a side includes: forming a third shielding layer 150 on the waveguide layer 200, wherein a third opening 160 is formed in the third shielding layer 150 that exposes the top of the waveguide layer 200 on the absorption region 100a side.
[0114] The third shielding layer 150 serves as an ion implantation mask for the subsequent third ion implantation process.
[0115] Accordingly, in this embodiment, in the step of forming the third shielding layer 150 on the waveguide layer 200, the third shielding layer 150 is formed on the protective layer 140.
[0116] refer to Figure 8 A third ion implantation process is performed on the waveguide layer 200 along the third opening 160 to form a first lightly doped layer 310.
[0117] refer to Figure 9 After performing the third ion implantation process to form the first lightly doped layer 310, the process also includes: removing the third shielding layer 150.
[0118] Reference Figures 10 to 11 Before the formation of the first doped layer and the second doped layer, the process further includes: forming a second lightly doped layer 320 in the waveguide layer 200 on the other side of the absorption region 100a in a direction perpendicular to the light propagation direction. The doping type of the second lightly doped layer 320 is opposite to that of the first lightly doped layer 310.
[0119] Specifically, refer to Figure 10 The step of forming a second lightly doped layer 320 in the waveguide layer 200 on the other side of the absorption region 100a includes: forming a fourth shielding layer 170 on the waveguide layer 200, wherein a fourth opening 180 is formed in the fourth shielding layer 170 to expose the waveguide layer 200 on the other side of the absorption region 100a.
[0120] The fourth shielding layer 170 serves as an ion implantation mask for the subsequent fourth ion implantation process.
[0121] Accordingly, in this embodiment, in the step of forming the fourth shielding layer 170 on the waveguide layer 200, the fourth shielding layer 170 is formed on the protective layer 140.
[0122] refer to Figure 11 A fourth ion implantation process is performed on the waveguide layer 200 along the fourth opening 180 to form a second lightly doped layer 320.
[0123] refer to Figure 12 After performing the fourth ion implantation process to form the second lightly doped layer 320, the process also includes: removing the fourth shielding layer 170.
[0124] Specifically, in this embodiment, the first lightly doped layer 310 and the second lightly doped layer 320 are lightly doped regions. The impurity concentration in the lightly doped regions is low, and therefore the carrier concentration is also low. This is used to form a low conductivity region, reduce parasitic effects, and improve device performance.
[0125] As an example, in this embodiment, the first lightly doped layer 310 is an N-type lightly doped region, and the second lightly doped layer 320 is a P-type lightly doped region.
[0126] refer to Figure 13 Before the waveguide layer 200 covering the absorption region 100a and the light absorption layer filling the plurality of holes 230 are subsequently formed, the formation method further includes: forming a first doped layer 330 in the waveguide layer 200 on one side of the absorption region 100a perpendicular to the light propagation direction.
[0127] In this embodiment, the first doped layer 330 and the first lightly doped layer 310 have the same doping type.
[0128] Specifically, in this embodiment, the step of forming a first doped layer 330 in the waveguide layer 200 on the side of the absorption region 100a perpendicular to the light propagation direction includes: forming a first shielding layer 350 on the waveguide layer 200, wherein a first opening 360 is formed in the first shielding layer 350 that exposes the top of the waveguide layer 200 on the side of the absorption region 100a.
[0129] The first shielding layer 350 serves as an ion implantation mask for the subsequent first ion implantation process.
[0130] Accordingly, in this embodiment, in the step of forming the first shielding layer 350 on the waveguide layer 200, the first shielding layer 350 is formed on the protective layer 140.
[0131] Accordingly, in this embodiment, the waveguide layer 200 is subjected to a first ion implantation process along the first opening 360 to form a first doped layer 330.
[0132] refer to Figure 14 After performing the first ion implantation process to form the first doped layer 330, the process further includes: removing the first shielding layer 350.
[0133] refer to Figure 15 Before the waveguide layer 200 covering the absorption region 100a and the light absorption layer filling the plurality of holes 230 are subsequently formed, the formation method further includes: forming a second doped layer 340 in the waveguide layer 200 on the other side of the absorption region 100a perpendicular to the light propagation direction, wherein the doping type of the second doped layer 340 is opposite to that of the first doped layer 330.
[0134] In this embodiment, the second doped layer 340 and the second lightly doped layer 320 have the same doping type.
[0135] Specifically, in this embodiment, the step of forming a second doped layer 340 in the waveguide layer 200 on the other side of the absorption region 100a in a direction perpendicular to the light propagation direction includes: forming a second shielding layer 370 on the waveguide layer 200, wherein a second opening 380 is formed in the second shielding layer 370 to expose the top of the waveguide layer 200 on the other side of the absorption region 100a.
[0136] The second shielding layer 370 serves as an ion implantation mask for the subsequent second ion implantation process.
[0137] Accordingly, in this embodiment, in the step of forming the second shielding layer 370 on the waveguide layer 200, the second shielding layer 370 is formed on the protective layer 140.
[0138] Accordingly, in this embodiment, the waveguide layer 200 is subjected to a second ion implantation process along the second opening 380 to form a second doped layer 340.
[0139] refer to Figure 16 After performing the second ion implantation process to form the second doped layer 340, the process also includes: removing the second shielding layer 370.
[0140] In this embodiment, the first doped layer 330 and the second doped layer 340 have opposite doping types, forming a PIN-type photodetector.
[0141] Specifically, in this embodiment, the first doped layer 330 and the second doped layer 340 are heavily doped regions. The impurity concentration in the heavily doped regions is high, so the carrier concentration is also high, and the conductivity is significantly increased. Thus, the first doped layer 330 and the second doped layer 340 are used to form a low-resistance ohmic contact.
[0142] As an example, in this embodiment, the first doped layer 330 is an N-type heavily doped region, and the second doped layer 340 is a P-type heavily doped region.
[0143] Reference Figures 17 to 19 A waveguide layer 200 covering the absorption region 100a is formed, and a light absorption layer 300 filled with multiple holes 230 is formed.
[0144] The light-absorbing layer 300 is used to absorb photons.
[0145] Specifically, in this embodiment, when photons are absorbed by the light-absorbing layer 300, electron-hole pairs are generated. Under the action of an applied electric field, these charge carriers drift and form a current, thereby converting the optical signal into an electrical signal.
[0146] In this embodiment, the material of the light-absorbing layer 300 includes germanium.
[0147] In other embodiments, the material of the light-absorbing layer may also be a germanium alloy.
[0148] As an example, in this embodiment, the photodetector is an evanescent waveguide-coupled silicon-based germanium (Ge-on-Si) photodetector. In the detector, the optical signal is transmitted through the silicon waveguide layer 200. Due to the refractive index distribution characteristics of the silicon waveguide layer 200, an evanescent field is generated when light propagates in the waveguide layer 200, which is an attenuation field near the surface of the waveguide layer 200. When a germanium light-absorbing layer 300 covers the waveguide layer 200, the evanescent field extends into the germanium light-absorbing layer 300, allowing the optical signal to couple into the germanium light-absorbing layer 300. When the optical signal is coupled into the germanium light-absorbing layer 300 through the evanescent field, photons are absorbed and excited electrons to jump to the conduction band, forming electron-hole pairs. Under the action of an applied reverse bias voltage, these charge carriers separate and drift under the action of an electric field, forming a photocurrent.
[0149] It should be noted that in this embodiment, the silicon waveguide layer 200 is used, which is based on a silicon platform and is compatible with CMOS technology, which is beneficial for the integration of photodetectors with other optoelectronic devices.
[0150] In this embodiment, the dimensions of the light absorption layer 300 can be obtained based on simulation. As an example, in this embodiment, the length of the light absorption layer 300 is 10μm, the width is 0.5μm, and the height is 0.16μm.
[0151] Specifically, refer to Figure 17 The step of forming a waveguide layer 200 covering the absorption region 100a and a light absorption layer 300 filling multiple holes 230 includes: forming a blocking layer 190 covering the waveguide layer 200.
[0152] The barrier layer 190 provides a process platform for the formation of the light-absorbing layer 300.
[0153] In this embodiment, the material of the barrier layer 190 includes silicon oxide.
[0154] Accordingly, in this embodiment, in the step of forming the blocking layer 190 covering the waveguide layer 200, the blocking layer 190 covers the protective layer 140.
[0155] refer to Figure 18 Remove the blocking layer 190 above the absorption region 100a to form a growth opening 191 for the waveguide layer 200 that exposes the absorption region 100a.
[0156] The growth opening 191 provides space for the formation of the light absorption layer 300, and correspondingly, the sidewall of the growth opening 191 acts as a barrier during the formation of the light absorption layer 300.
[0157] Accordingly, in this embodiment, in the step of removing the blocking layer 190 above the absorption region 100a, the protective layer 140 covering the waveguide layer 200 of the absorption region 100a and filling the holes 230, as well as the first dielectric layer 130 in the absorption region 100a, are also removed to expose the surface of the waveguide layer 200 of the absorption region 100a.
[0158] In this embodiment, a wet etching process is used to remove the barrier layer 190 above the absorption region 100a, forming a growth opening 191 that exposes the waveguide layer 200 of the absorption region 100a.
[0159] Wet etching has the characteristics of isotropic etching, which makes it easy to remove the etching material cleanly. Furthermore, wet etching is easy to obtain a large etching selectivity, which helps to reduce damage to the waveguide layer 200 during the removal of the barrier layer 190 above the absorption region 100a.
[0160] refer to Figure 19 A waveguide layer 200 covering the absorption region 100a is formed in the growth opening 191, and a light absorption layer 300 filled with multiple holes 230 is formed.
[0161] In this embodiment, an epitaxial growth process is used to form a waveguide layer 200 covering the absorption region 100a, and a light absorption layer 300 filled with multiple holes 230 is formed.
[0162] The epitaxial growth process can easily obtain a light absorption layer 300 with good film quality. Since the waveguide layer 200 is made of silicon and the light absorption layer 300 is made of germanium, the light absorption layer 300 can be grown on the waveguide layer 200 using the epitaxial growth process.
[0163] It should be noted that in this embodiment, the silicon surface with multiple holes 230 forms a nanograting. When germanium is grown on the silicon surface with multiple holes 230, the nanograting can be used to limit the lateral size of germanium before growth, which is beneficial to reducing the dislocation density of germanium growth. Moreover, during the growth of germanium, germanium does not nucleate on the blocking layer 190 on the sidewall of the growth opening 191. The upward extension process of dislocations formed within the growth opening 191 is blocked by the sidewall of the blocking layer 190, which is also beneficial to reducing the dislocation density of germanium growth. This is beneficial to obtaining a light absorption layer 300 with better film quality.
[0164] Specifically, in this embodiment, in the step of forming the waveguide layer 200 covering the absorption region 100a using an epitaxial growth process, the epitaxial growth process includes chemical vapor deposition (CVD) epitaxy or molecular beam epitaxy (MBE).
[0165] refer to Figure 20 After forming a waveguide layer 200 covering the absorption region 100a and a light absorption layer 300 filling multiple holes 230, the formation method further includes: forming a first interconnect via structure 510 electrically connected thereto on the first doped layer 330; and forming a second interconnect via structure 520 electrically connected thereto on the second doped layer 340.
[0166] The first interconnect via structure 510 is used to realize the electrical connection between the first doped layer 330 and the outside, and the second via interconnect structure 520 is used to realize the electrical connection between the second doped layer 340 and the outside.
[0167] Specifically, in this embodiment, the steps of forming a first interconnect via structure 510 electrically connected to the first doped layer 330 and forming a second interconnect via structure 520 electrically connected to the second doped layer 340 include: forming a second dielectric layer 500 covering the blocking layer 190 and the light absorbing layer 300; patterning the second dielectric layer 500 to form a first via exposed to the top surface of the first doped layer 330 and a second via exposed to the top surface of the second doped layer 340; filling the first via to form the first interconnect via structure 510 and filling the second via to form the second interconnect via structure 520.
[0168] In this embodiment, the material of the second dielectric layer 500 includes silicon oxide.
[0169] While the present invention has been disclosed above, it is not limited thereto. Any person skilled in the art can make various modifications and alterations without departing from the spirit and scope of the invention; therefore, the scope of protection of the present invention should be determined by the scope defined in the claims.
Claims
1. A photodetector, characterized in that, include: Base; A waveguide layer is located on the substrate, the waveguide layer includes an absorption region, and a plurality of holes are formed in a portion of the thickness of the waveguide layer in the absorption region; A light-absorbing layer, a waveguide layer covering the absorption region, and filling the plurality of holes.
2. The photodetector as described in claim 1, characterized in that, In the absorption region, the multiple pores are arranged periodically.
3. The photodetector as described in claim 2, characterized in that, In the absorption region, a plurality of holes are arranged in an array.
4. The photodetector as described in claim 1, characterized in that, The opening size of the hole is 40 nm to 80 nm.
5. The photodetector as described in claim 1, characterized in that, The spacing between adjacent holes is 20 nm to 60 nm.
6. The photodetector as described in claim 1, characterized in that, The depth of the hole is 80nm to 120nm.
7. The photodetector as described in claim 1, characterized in that, A first doped layer and a second doped layer are formed in the waveguide layers on both sides of the absorption region perpendicular to the direction of light propagation, and the doping types of the first doped layer and the second doped layer are opposite.
8. The photodetector as described in claim 7, characterized in that, A first interconnect via structure electrically connected thereto is formed on the first doped layer; a second interconnect via structure electrically connected thereto is formed on the second doped layer.
9. The photodetector as described in claim 1, characterized in that, The waveguide layer is made of silicon; The material of the light-absorbing layer includes germanium.
10. A method for forming a photodetector, characterized in that, include: A substrate is provided on which a waveguide layer is formed, the waveguide layer including an absorption region; The waveguide layer of partial thickness in the absorption region is patterned to form multiple holes; A waveguide layer is formed covering the absorption region, and a light absorption layer is filled with multiple holes.
11. The method for forming a photodetector as described in claim 10, characterized in that, In the step of patterning a waveguide layer of a certain thickness in the absorption region to form multiple holes, the multiple holes in the absorption region are arranged periodically.
12. The method for forming a photodetector as described in claim 11, characterized in that, In the step of patterning a waveguide layer of partial thickness in the absorption region to form multiple holes, the multiple holes in the absorption region are arranged in an array.
13. The method for forming a photodetector as described in claim 10, characterized in that, The step of patterning a waveguide layer of a portion of the absorption region thickness to form multiple holes includes: forming a mask layer covering the waveguide layer, wherein multiple mask openings are formed in the mask layer above the absorption region; The waveguide layer is patterned along the opening of the mask to form a plurality of holes; After forming multiple holes, the process further includes: removing the mask layer.
14. The method for forming a photodetector as described in claim 10, characterized in that, The step of forming a waveguide layer covering the absorption region and a light-absorbing layer filling the plurality of holes includes: forming a blocking layer covering the waveguide layer; Remove the blocking layer above the absorption region to form a growth opening in the waveguide layer that exposes the absorption region; A waveguide layer covering the absorption region is formed in the growth opening, and a light absorption layer filling the plurality of holes is formed.
15. The method for forming a photodetector as described in claim 10 or 14, characterized in that, A waveguide layer covering the absorption region is formed using an epitaxial growth process, and a light absorption layer is filled with multiple holes.
16. The method for forming a photodetector as described in claim 11, characterized in that, Before forming a waveguide layer covering the absorption region and a light absorption layer filling the plurality of holes, the forming method further includes: forming a first doped layer in the waveguide layer on one side of the absorption region perpendicular to the light propagation direction; A second doped layer is formed in the waveguide layer on the other side of the absorption region, perpendicular to the direction of light propagation, wherein the doping type of the first doped layer is opposite to that of the second doped layer.
17. The method for forming a photodetector as described in claim 16, characterized in that, The step of forming a first doped layer in the waveguide layer on one side of the absorption region perpendicular to the light propagation direction includes: forming a first shielding layer on the waveguide layer, wherein the first shielding layer has a first opening that exposes the top of the waveguide layer on the absorption region side; The waveguide layer is subjected to a first ion implantation process along the first opening to form the first doped layer; The step of forming a second doped layer in the waveguide layer on the other side of the absorption region perpendicular to the light propagation direction includes: forming a second shielding layer on the waveguide layer, wherein a second opening is formed in the second shielding layer to expose the top of the waveguide layer on the other side of the absorption region; A second ion implantation process is performed on the waveguide layer along the second opening to form the second doped layer. The implanted ion types in the first ion implantation process and the second ion implantation process are opposite.
18. The method for forming a photodetector as described in claim 17, characterized in that, Before forming the first doped layer and the second doped layer, the method further includes: forming a protective layer that fills the plurality of holes and covers the waveguide layer; In the step of forming the first shielding layer on the waveguide layer, the first shielding layer is formed on the protective layer; In the step of forming the second shielding layer on the waveguide layer, the second shielding layer is formed on the protective layer.
19. The method for forming a photodetector as described in claim 16, characterized in that, After forming a waveguide layer covering the absorption region and a light absorption layer filling the plurality of holes, the forming method further includes: forming a first interconnect via structure electrically connected thereto on the first doped layer; and forming a second interconnect via structure electrically connected thereto on the second doped layer.