An oxygen-absorbing thin film for use in perovskite photovoltaic devices and its preparation process

By using a two-dimensional Ruddlesden-Popper type phenylethylamine tin-iodine perovskite thin film as an active oxygen absorption layer in perovskite photovoltaic devices, the problems of irreversible damage and material degradation caused by oxygen permeation are solved, achieving long-term stability and efficient oxygen absorption.

CN123124581APending Publication Date: 2026-11-17CHANGSHU XINXIAN OPTOELECTRONICS TECHNOLOGY CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202611575330.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-12
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing perovskite photovoltaic device encapsulation cannot completely block oxygen permeation, leading to the accumulation of trace amounts of oxygen during long-term operation and causing irreversible damage. Current encapsulation technology lacks active oxygen removal capabilities, and tin-based perovskite materials are prone to irreversible oxidation under high oxygen concentrations. Furthermore, there is a lack of feasible solutions for integrating active oxygen-absorbing films into the encapsulation structure.

Method used

A two-dimensional Ruddlesden-Popper type phenylethylamine tin iodide perovskite (PEA2SnI4) film is used as an active oxygen absorption layer and is set between the inner side of the encapsulation cover and the light absorption layer. Through the synergistic effect of physical adsorption and irreversible chemical reaction, the oxygen concentration in the encapsulation cavity is controlled to be below 1.5 vol%, thus avoiding the degradation of the film itself.

Benefits of technology

It significantly extends the T80 lifetime of perovskite photovoltaic devices, controls the oxygen concentration to below 1.5 vol%, avoids irreversible damage, and achieves a balance between oxygen absorption capacity and long-term stability. The fabrication process is simple and low-cost.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123124581A_ABST
    Figure CN123124581A_ABST
Patent Text Reader

Abstract

This invention discloses an oxygen-absorbing thin film for use in perovskite photovoltaic devices and its fabrication process, belonging to the field of photovoltaic device packaging. The oxygen-absorbing thin film is disposed on the inner side of the encapsulation cover plate between the light-absorbing layer and the light-absorbing layer, without direct contact with the light-absorbing layer. It is composed of two-dimensional Ruddlesden-Popper type phenylethylamine tin iodide perovskite (PEA2SnI4) with a thickness of 30–80 nm. This oxygen-absorbing thin film utilizes Sn... 2+ The oxygen concentration depends on a multi-stage process to actively absorb oxygen within the encapsulation cavity: when the oxygen concentration is below 1.5 vol%, reversible physical adsorption and defect passivation are dominant; as the oxygen concentration increases, irreversible reactions occur to generate PEAI, SnO2, and I2, consuming oxygen and maintaining the oxygen concentration within the cavity below 1.5 vol% for an extended period. When used for encapsulating lead-based perovskite photovoltaic devices, the device's oxygen concentration in air at T... 80 The lifespan has been extended from 120 hours for the unsealed product to over 800 hours.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of photovoltaic device packaging technology, specifically relating to an oxygen-absorbing thin film for perovskite photovoltaic devices and its preparation process, and particularly to an active oxygen-absorbing thin film based on two-dimensional Ruddlesden-Popper type tin-based perovskite material. Background Technology

[0002] Perovskite solar cells have become a research hotspot in next-generation photovoltaic technology due to their excellent photoelectric performance, low cost, and solution-processability, with certified photoelectric conversion efficiencies exceeding 26%. However, perovskite materials (especially lead-based perovskites) are extremely sensitive to oxygen and moisture: in atmospheric environments, oxygen molecules easily penetrate the device and react with the perovskite light-absorbing layer, generating defect states such as superoxide radicals, accelerating material decomposition, and leading to a sharp decline in device efficiency. Research results show that unencapsulated perovskite solar cells exhibit significant efficiency degradation in humid air. 80 Lifetime (the time required for photoelectric conversion efficiency to decay to 80% of its initial value) is typically only a few hours to hundreds of hours (see De Rossi F. et al. Thermosetting polyurethane-based encapsulation of flexible perovskite solar cells. Materials Today Energy, 2025, 49: 101850). Therefore, encapsulation technology is crucial for the commercialization of perovskite photovoltaic devices.

[0003] Currently, common encapsulation solutions primarily employ physical barriers, such as epoxy resin, glass covers, or dense oxide layers deposited by atomic layer deposition, to isolate the device from external oxygen and moisture. However, these barrier layers cannot completely prevent oxygen penetration, especially for devices operating for extended periods, where the continuous accumulation of trace amounts of oxygen can still cause irreversible damage. Furthermore, existing encapsulation technologies lack the ability to actively remove residual oxygen from the encapsulation cavity. CN109560205A and CN109524554A disclose a dehumidification and oxygen removal encapsulation method for perovskite / silicon tandem solar cell modules. This method uses a vacuum heating drying process combined with dehumidification and oxygen removal materials to reduce residual water and oxygen in the encapsulation cavity. However, this method represents passive oxygen removal within the encapsulation process, only removing water and oxygen remaining in the cavity during encapsulation. It cannot continuously absorb the constantly penetrating oxygen during device operation. Moreover, its dehumidification and oxygen removal materials are mostly irreversibly consumable, losing their effectiveness once their oxygen absorption capacity is saturated, making it difficult to support the long-term operation of the device.

[0004] On the other hand, Sn in tin-based perovskite materials 2+ It has strong reducing properties and is easily oxidized to Sn.4+ While this characteristic is detrimental to the stability of tin-based perovskite solar cells, it can be utilized as an oxygen absorber: by making a thin film and placing it inside the encapsulation, it can preferentially absorb permeated oxygen, thereby protecting the main light-absorbing layer (such as lead-based perovskite) from oxidation. Ju Y., Wu X.-G., Huang S., Dai G., Song T., Zhong H. et al. (The Evolution of Photoluminescence Properties of PEA2SnI4 Upon Oxygen Exposure: Insight into Concentration Effects. Advanced Functional Materials, 2021, DOI: 10.1002 / adfm.202108296) systematically reported the evolution of photoluminescence properties of two-dimensional tin-based perovskite PEA2SnI4 films with oxygen concentration: at ultra-low oxygen concentrations (<1.5 vol%), photoluminescence enhancement and reversible photoluminescence quenching were observed; within the range of 1.5 vol% < [O2] < 21 vol%, photoluminescence could be partially recovered after the sample was returned to a nitrogen environment; when the oxygen concentration was further increased to 21–95 vol%, the photoluminescence was further enhanced. At vol%, the photoluminescence was significantly quenched and only slightly recovered after being moved back to a nitrogen environment, indicating that there is both physical adsorption and reversible / irreversible chemical reaction between PEA2SnI4 and oxygen.

[0005] However, the aforementioned studies considered oxygen as a detrimental factor leading to the instability of tin-based perovskites. Their research objective was to improve the inherent stability of PEA2SnI4 in oxygen environments, without proposing the use of PEA2SnI4 as an active oxygen-absorbing layer within the encapsulation, nor providing an integration scheme with the photovoltaic device encapsulation structure. Furthermore, the studies did not reveal how to utilize an oxygen concentration-dependent multi-stage mechanism to ensure that the oxygen-absorbing layer continuously consumes oxygen during long-term service while preventing its rapid irreversible degradation. Therefore, there is an urgent need for a functional thin film that can be placed inside the encapsulation cavity, actively and continuously absorbs oxygen during service, and possesses long-term operational stability. Summary of the Invention

[0006] In view of the above-mentioned shortcomings of the existing technology, the technical problem to be solved by the present invention is: (1) Existing perovskite photovoltaic device encapsulation relies solely on physical barriers, which cannot prevent oxygen permeation. Trace amounts of oxygen accumulate continuously during long-term operation of the device, causing irreversible damage. (2) Existing packaging technology lacks the function of actively removing residual oxygen in the packaging cavity. The dehumidification and deoxygenation scheme in the process cannot continuously absorb oxygen during service, and the oxygen-absorbing material will fail once it is saturated. (3) Although tin-based perovskite materials have strong oxygen absorption capacity, they will undergo irreversible oxidation degradation under high oxygen concentration. Directly using them as an oxygen absorption layer in the encapsulation makes it difficult to balance oxygen absorption capacity and long-term working stability. (4) There is a lack of feasible solutions to integrate active oxygen absorption films into the perovskite photovoltaic device packaging structure without affecting the device's optical path and interface.

[0007] To solve the above-mentioned technical problems, the present invention adopts the following technical solution: This invention provides an oxygen-absorbing film for use in perovskite photovoltaic devices. The oxygen-absorbing film is disposed between the inner side of the encapsulation cover plate of the photovoltaic device and the light-absorbing layer, and does not directly contact the light-absorbing layer. The oxygen-absorbing film is composed of two-dimensional Ruddlesden-Popper type phenylethylamine tin iodide perovskite (PEA2SnI4) and is used to absorb oxygen in the encapsulation cavity of the photovoltaic device.

[0008] Preferably, the thickness of the oxygen-absorbing film is 30–80 nm.

[0009] Preferably, the oxygen-absorbing film is disposed on the plane inside the encapsulation cover plate and is located between the metal electrode of the photovoltaic device and the encapsulation cover plate.

[0010] Preferably, a physical isolation layer or gap is provided between the oxygen-absorbing film and the light-absorbing layer.

[0011] Preferably, the encapsulation cover is a glass cover or a flexible transparent polymer cover, wherein the flexible transparent polymer cover is selected from polyethylene terephthalate (PET) or polyethylene naphthalate (PEN).

[0012] The present invention also provides a preparation process for the above-mentioned oxygen-absorbing film, comprising the following steps: S1, dissolving stannous iodide (SnI2) and phenylethyl ammonium iodide (PEAI) in a molar ratio of 1:2 in a mixed solvent of N,N-dimethylformamide (DMF) and dimethyl sulfoxide (DMSO) to prepare a precursor solution; S2, coating the precursor solution onto a substrate and annealing it to obtain the oxygen-absorbing film; S3, fixing the substrate with the oxygen-absorbing film to the inside of the encapsulation cover plate, with the oxygen-absorbing film facing the inside of the encapsulation cavity, applying encapsulating adhesive around the light-absorbing layer of the photovoltaic device, covering the photovoltaic device with the encapsulation cover plate with the oxygen-absorbing film, and completing the encapsulation by curing.

[0013] Preferably, the volume ratio of DMF to DMSO in the mixed solvent in step S1 is 4:1.

[0014] Preferably, the concentration of the precursor solution in step S1 is 0.25–0.35 mol / L; the coating in step S2 is spin coating, which adopts a two-step procedure: the first step is a spin speed of 1000 rpm for 10 s, the second step is a spin speed of 5000 rpm for 60 s, and an antisolvent is added dropwise in the last 10 s of the second step. The antisolvent is a mixed solution of toluene and 3-methylbutyric acid, the volume ratio of toluene to 3-methylbutyric acid is 1000:1, and the amount added is 200–350 μL.

[0015] Preferably, the annealing temperature in step S2 is 80–120 °C and the time is 10–30 min; the substrate is a transparent glass sheet or a transparent polymer film; the encapsulating adhesive in step S3 is a UV-curable epoxy resin, and the curing process is irradiation under a UV lamp for 20–30 s.

[0016] The present invention also provides the application of the above-mentioned oxygen-absorbing film in the encapsulation of lead-based perovskite photovoltaic devices.

[0017] The oxygen absorption mechanism of the oxygen-absorbing membrane of the present invention exhibits a significant oxygen concentration dependence, specifically comprising the following multi-stage mechanism (taking PEA2SnI4 as an example): (1) When the oxygen concentration inside the encapsulation cavity is below 1.5 vol%, oxygen is mainly physically adsorbed onto the amine cation sites on the surface of PEA2SnI4. Density functional theory (DFT) calculations show that oxygen has the lowest adsorption energy (approximately -0.32 eV) at the amine cation sites, making them the preferred adsorption sites. The adsorbed oxygen is converted into superoxide radicals (O2) through photoinduced electron transfer under light irradiation. - The superoxide radical occupies the iodine vacancy, passivates the defect state, and the photoluminescence exhibits a brightening phenomenon. Moreover, this process is completely reversible—the photoluminescence is completely restored after the film is returned to the nitrogen environment.

[0018] (2) When the oxygen concentration in the encapsulation cavity is between 1.5 vol% and 21 vol%, some oxygen occupies iodide ion sites, forming a metastable complex SnI2·2O2. - The reaction is reversible under low oxygen conditions, and the photoluminescence can be partially restored (recovery rate 40%–70%) after the film is returned to a nitrogen environment.

[0019] (3) When the oxygen concentration in the encapsulation cavity is higher than 21 vol%, oxygen further occupies iodine vacancies and initiates an irreversible chemical reaction: PEA2SnI4 + O2 → 2PEAI + SnO2 + I2, thereby irreversibly consuming oxygen. The PEAI, SnO2 and I2 generated by this reaction will not react further with oxygen.

[0020] Based on the above mechanism, the oxygen-absorbing membrane of the present invention maintains the oxygen concentration in the encapsulation cavity at an ultra-low level of less than 1.5 vol% for a long time through the synergistic effect of physical adsorption (reversible) and irreversible chemical consumption. At the same time, since the oxygen concentration in the encapsulation cavity is controlled below 1.5 vol%, the working state of the oxygen-absorbing membrane is mainly based on reversible physical adsorption and defect passivation, thereby avoiding the irreversible rapid degradation of the oxygen-absorbing membrane itself.

[0021] Compared with the prior art, the present invention has at least the following beneficial effects: (1) The present invention uses two-dimensional tin-based perovskite material as an active oxygen absorption film inside the package, realizing the transformation from passive barrier to active consumption. It can directly consume the residual oxygen in the package cavity and the oxygen that seeps in during service, overcoming the defects of physical barrier layers that cannot prevent oxygen penetration and the irreversible damage caused by long-term accumulation of trace oxygen.

[0022] (2) Based on a deep understanding of the interaction between PEA2SnI4 and oxygen concentration, this invention precisely controls the oxygen concentration in the encapsulation cavity to below 1.5 vol%, so that the oxygen absorption process is mainly based on reversible physical adsorption and defect passivation, avoiding the irreversible rapid degradation of the oxygen absorption film itself, and taking into account both oxygen absorption capacity and long-term working stability. In contrast, three-dimensional tin-based perovskites (such as CH3NH3SnI3) lack the layered barrier composed of long-chain organic cations and are mainly based on irreversible oxidative degradation of Sn(II)→Sn(IV), and do not have this reversible working characteristic.

[0023] (3) The oxygen-absorbing thin film preparation process provided by the present invention is highly compatible with the existing perovskite photovoltaic device process. It adopts solution spin coating and annealing, without the need to add complex equipment such as vacuum deposition, which is low in cost and easy to scale up.

[0024] (4) Experiments have shown that the lead-based perovskite photovoltaic device encapsulated with this oxygen-absorbing thin film exhibits good performance in an air environment (temperature 25±2 ℃, relative humidity 30±5%). 80 The lifespan was extended from 120 hours without encapsulation to over 800 hours, an improvement of more than 6 times. Furthermore, the oxygen concentration inside the encapsulation chamber remained below 1.5 vol% for 800 hours, demonstrating significant technical benefits. Attached Figure Description

[0025] Figure 1 This is a schematic diagram of the structure of an oxygen-absorbing thin film for a perovskite photovoltaic device provided in Embodiment 1 of this application; 1-encapsulation cover plate, 2-oxygen-absorbing thin film, 3-metal electrode, 4-hole transport layer, 5-perovskite light-absorbing layer, 6-electron transport layer, 7-transparent conductive substrate; Figure 2The color change of an oxygen-absorbing thin film used in a perovskite photovoltaic device according to Embodiment 1 of this application in air (oxygen concentration 20%); Figure 3 The in-situ photoluminescence time evolution of PEA2SnI4 thin film under 460 nm LED excitation; Figure 4 Photoluminescence spectra of PEA2SnI4 perovskite films exposed to different oxygen concentrations; Figure 5 The absorbance and integrated photoluminescence intensity of the PEA2SnI4 thin film at 607 nm are shown as the trend of oxygen concentration. Figure 6 To record the evolution of the photoluminescence spectrum of CH3NH3SnI3 thin film over time using a 460 nm LED as the excitation source; Figure 7 XPS Sn 3d spectra quantitatively revealed Sn 2+ / Sn 4+ Changes in proportion; original thin film Sn 2+ / Sn 4+ The atomic ratio was 3.4; it decreased to 0.9 after exposure to 50 vol% oxygen concentration and to 0.2 after exposure to 95 vol% oxygen concentration. Detailed Implementation

[0026] To make the objectives, technical solutions, and advantages of this disclosure clearer, the embodiments of this disclosure will be described in detail below with reference to the accompanying drawings. The implementation can be carried out in many different forms, and those skilled in the art will readily understand that the methods and content can be transformed into various forms without departing from the spirit and scope of this disclosure. Therefore, this disclosure should not be construed as limited to the contents described in the following embodiments. The technical solutions of the present invention will be further described below with reference to the accompanying drawings and specific embodiments.

[0027] As a specific embodiment of the present invention, a process for preparing an oxygen-absorbing thin film for use in perovskite photovoltaic devices is provided, such as... Figure 1As shown, the preparation process includes the following steps: Stannous iodide (SnI2) and phenylethyl ammonium iodide (PEAI) are dissolved in a mixed solvent of DMF and DMSO (volume ratio 4:1) at a molar ratio of 1:2, and stirred until completely dissolved to obtain a precursor solution. In a nitrogen glove box, the precursor solution is spin-coated onto a clean glass substrate using a two-step process: first, 1000 rpm for 10 s; second, 5000 rpm for 60 s, with the antisolvent (a mixture of toluene and 3-methylbutyric acid at a volume ratio of 1000:1) added dropwise in the last 10 s of the second step. The film is then placed on a hot plate and annealed at 90 °C for 20 minutes to obtain a dark brown PEA2SnI4 oxygen-absorbing film with a thickness of 30–80 nm. The oxygen-absorbing film, along with the substrate, is placed inside the encapsulation structure of the perovskite photovoltaic device, specifically in the cavity between the encapsulation cover and the device's light-absorbing layer, and sealed with UV-curable adhesive. The oxygen-absorbing film does not obstruct the light path and does not directly contact the light-absorbing layer.

[0028] Those skilled in the art will understand that the aforementioned performance tests, such as photoluminescence spectrum, absorbance, oxygen concentration, and device stability, can all be performed using conventional testing methods in the field: photoluminescence spectrum can be measured using steady-state fluorescence spectroscopy with a 460 nm excitation source and a fluorescence spectrophotometer; thin film absorbance can be measured using a UV-Vis spectrophotometer; oxygen concentration within the encapsulation cavity can be measured using an oxygen sensor or gas chromatography; device stability can be performed according to the ISOS stability testing protocol (see Khenkin MV et al. Consensus statement for stability assessment and reporting for perovskite photovoltaics based on ISOS procedures. Nature Energy, 2020, 5: 35-49), where T... 80 Lifetime is defined as the time required for the photoelectric conversion efficiency to decay to 80% of its initial value. All embodiments and comparative examples of this invention were tested under the same conditions to ensure the comparability of the results.

[0029] The present invention will be further described in detail below, but the following embodiments are merely examples of the present invention and do not represent or limit the scope of protection of the present invention. The scope of protection of the present invention shall be determined by the claims.

[0030] Example 1 This embodiment provides a method for preparing a PEA2SnI4 oxygen-absorbing film.

[0031] SnI₂ and PEAI were dissolved in a mixed solvent of DMF and DMSO (volume ratio 4:1) at a molar ratio of 1:2 to prepare a 0.3 mol / L precursor solution. The precursor solution was stirred overnight in a nitrogen glove box and filtered through a 0.22 μm polytetrafluoroethylene filter before use.

[0032] In a nitrogen glove box, the precursor solution was spin-coated onto a clean glass substrate using a two-step process: first, 1000 rpm for 10 s (acceleration 200 rpm / s), and second, 5000 rpm for 60 s (acceleration 800 rpm / s). During the last 10 s of the second step, 330 μL of antisolvent (a mixture of toluene and 3-methylbutyric acid at a volume ratio of 1000:1) was dropped onto the center of the substrate. After spin-coating, the film was placed on a hot plate and annealed at 90 °C for 20 min to obtain a dark brown PEA2SnI4 oxygen-absorbing film with a thickness of approximately 50 nm.

[0033] The obtained PEA2SnI4 film is dark brown and has a smooth surface under sunlight.

[0034] Comparative Example 1 This comparative example provides a method for preparing a three-dimensional tin-based perovskite CH3NH3SnI3 thin film, for comparison with the two-dimensional tin-based perovskite thin film of Example 1.

[0035] 0.372 g SnI₂ and 0.159 g CH₃NH₃I were dissolved in 1 mL of a mixed solvent of DMF:DMSO = 4:1, and 0.1 mol% SnF₂ was added as an additive. The mixture was stirred overnight. The solution was then spin-coated onto a clean glass slide at 4000 rpm for 30 s, with 200 μL of chlorobenzene added dropwise at the 10th s mark. After spin-coating, the film was annealed at 100 °C for 10 min to obtain the thin film.

[0036] The difference between this comparative example and Example 1 is that the three-dimensional tin-based perovskite CH3NH3SnI3 lacks the layered barrier formed by long-chain organic cations, allowing oxygen to directly contact the Sn in the inorganic framework. 2+ Therefore, the irreversible oxidative degradation of Sn(II) → Sn(IV) is the main process, and the low-oxygen physical adsorption and reversible passivation stages in PEA2SnI4 are absent. Figure 6 Using a 460 nm LED as the excitation source, the evolution of the photoluminescence (PL) spectrum of the CH3NH3SnI3 thin film over time was recorded in situ. At a low oxygen concentration of 1.5 vol%, the photoluminescence intensity decreased linearly with the extension of excitation time, while at a high oxygen concentration of 50 vol% and above, the photoluminescence decreased exponentially. Figure 7 XPS Sn 3d spectra quantitatively revealed Sn 2+ / Sn4+ Changes in proportion. Original thin film Sn 2+ / Sn 4+ The atomic ratio was 3.4. It decreased to 0.9 after exposure to 50 vol% oxygen concentration and to 0.2 after exposure to 95 vol% oxygen concentration.

[0037] Example 2 This embodiment provides oxygen absorption performance testing of PEA2SnI4 oxygen absorption membrane under different oxygen concentrations.

[0038] The PEA2SnI4 thin film prepared in Example 1 was placed in a self-made gas chamber, and mixed gases containing 1.5, 6.6, 10.5, 22.5, 35, 50, 80, and 95 vol% oxygen were introduced respectively (nitrogen balance). A 460 nm LED (power 0.8 W / cm²) was used. 2 Using 1000 sq.a. as the excitation source, the evolution of the photoluminescence (PL) spectrum of the thin film over time is recorded in situ.

[0039] The results show that ( Figure 3 At a low oxygen concentration of 1.5 vol%, the photoluminescence intensity showed an increasing brightness with prolonged excitation time, with the integrated intensity increasing by approximately 18%. At an oxygen concentration of 22.5 vol%, photoluminescence exhibited a linear decay. At high oxygen concentrations of 50 vol% and above, photoluminescence exhibited an exponential decay. Figure 4 It can be seen that the photoluminescence emission of the PEA2SnI4 film is quite sensitive to changes in oxygen concentration; as the oxygen concentration increases from 1 vol% to 85 vol%, the photoluminescence intensity of the film decreases significantly. To further elucidate the evolution of the optical properties of the PEA2SnI4 film with oxygen concentration, the absorbance and integrated photoluminescence intensity at 607 nm were plotted as a function of oxygen concentration (1–85 vol%). Figure 5 The results indicate that oxygen concentration is the key factor determining the interaction between PEA2SnI4 film and oxygen; the above results also show that PEA2SnI4 film mainly undergoes reversible adsorption at low oxygen concentrations, while irreversible oxygen consumption occurs at high oxygen concentrations.

[0040] Example 3 This embodiment provides stability testing of a lead-based perovskite photovoltaic device encapsulated with a PEA2SnI4 oxygen-absorbing thin film.

[0041] The structure of lead-based perovskite solar cells is: FTO / TiO2 dense layer (30 nm) / mesoporous TiO2 (200 nm) / CsO. 05 MA0. 15FA0.8PbI3 perovskite light absorption layer (500 nm) / Spiro-OMeTAD hole transport layer (150 nm) / Au electrode (80 nm).

[0042] The glass cover plate with a PEA2SnI4 oxygen-absorbing film prepared in Example 1 was encapsulated on top of the above-mentioned device using UV-cured epoxy resin. The control group consisted of an unencapsulated device and a conventionally encapsulated device using the same glass cover plate and UV-cured adhesive but without the oxygen-absorbing film.

[0043] Three sets of devices were placed in an air environment (temperature 25±2 ℃, relative humidity 30±5%), and device lifetime was measured. The lifetime of the unpackaged device was [not specified]. 80 Lifespan approximately 120 hours; T for conventionally packaged devices 80 Lifespan approximately 350 hours; Encapsulated device containing PEA2SnI4 oxygen-absorbing film T 80 Lifespan exceeds 800 hours. Monitoring by the internal oxygen sensor shows that the oxygen concentration inside the device cavity containing the oxygen-absorbing film remained below 1.5 vol% for 800 hours.

Claims

1. An oxygen-absorbing thin film for use in perovskite photovoltaic devices, characterized in that, The oxygen-absorbing film is disposed between the inner side of the encapsulation cover plate of the photovoltaic device and the light-absorbing layer, and does not directly contact the light-absorbing layer; the oxygen-absorbing film is composed of two-dimensional Ruddlesden-Popper type phenylethylamine tin iodide perovskite (PEA2SnI4), and is used to absorb oxygen in the encapsulation cavity of the photovoltaic device.

2. The oxygen-absorbing membrane according to claim 1, characterized in that, The thickness of the oxygen-absorbing film is 30–80 nm.

3. The oxygen-absorbing membrane according to claim 1, characterized in that, The oxygen-absorbing film is disposed on the plane inside the encapsulation cover plate and is located between the metal electrode of the photovoltaic device and the encapsulation cover plate.

4. The oxygen-absorbing membrane according to claim 1, characterized in that, A physical isolation layer or gap is provided between the oxygen-absorbing film and the light-absorbing layer.

5. The oxygen-absorbing membrane according to claim 1, characterized in that, The encapsulation cover is a glass cover or a flexible transparent polymer cover, wherein the flexible transparent polymer cover is selected from polyethylene terephthalate (PET) or polyethylene naphthalate (PEN).

6. A process for preparing an oxygen-absorbing thin film as described in any one of claims 1 to 5, characterized in that, Includes the following steps: S1. Prepare a precursor solution by dissolving stannous iodide (SnI2) and phenylethyl ammonium iodide (PEAI) in a molar ratio of 1:2 in a mixed solvent of N,N-dimethylformamide (DMF) and dimethyl sulfoxide (DMSO); S2. The precursor solution is coated onto a substrate and then annealed to obtain the oxygen-absorbing film. S3. Fix the substrate with the oxygen-absorbing film to the inside of the encapsulation cover plate, so that the oxygen-absorbing film faces the inside of the encapsulation cavity. Apply encapsulation adhesive around the light-absorbing layer of the photovoltaic device. Cover the photovoltaic device with the encapsulation cover plate with the oxygen-absorbing film and complete the encapsulation by curing.

7. The preparation process according to claim 6, characterized in that, In step S1, the volume ratio of DMF to DMSO in the mixed solvent is 4:

1.

8. The preparation process according to claim 6, characterized in that, The concentration of the precursor solution in step S1 is 0.25–0.35 mol / L; the coating in step S2 is spin coating, which adopts a two-step procedure: the first step is a spin speed of 1000 rpm for 10 s, the second step is a spin speed of 5000 rpm for 60 s, and an antisolvent is added dropwise in the last 10 s of the second step. The antisolvent is a mixed solution of toluene and 3-methylbutyric acid, the volume ratio of toluene to 3-methylbutyric acid is 1000:1, and the amount added is 200–350 μL.

9. The preparation process according to claim 6, characterized in that, The annealing process in step S2 is carried out at a temperature of 80–120 °C for 10–30 min; the substrate is a transparent glass sheet or a transparent polymer film; the encapsulating adhesive in step S3 is a UV-curable epoxy resin, and the curing process is performed by irradiation under a UV lamp for 20–30 s.

10. The application of the oxygen-absorbing thin film according to any one of claims 1 to 5 or the preparation process according to any one of claims 6 to 9 in the encapsulation of lead-based perovskite photovoltaic devices.

Citation Information

Patent Citations

  • Dehumidifying and deoxygenizing packaging method for perovskite / silicon laminated solar cell module

    CN109524554A

  • De-humidification and deoxidization package method of perovskite / silicon laminated solar cell module

    CN109560205A