High-precision wafer manufacturing method based on temporary bonding

By depositing a dielectric film layer on the back of the carrier wafer and then grinding and planarizing it, the problem of uneven wafer thinning caused by the non-uniformity of the temporary bonding adhesive thickness was solved, achieving precise wafer thinning and improving the accuracy of subsequent processes.

CN123124737APending Publication Date: 2026-11-17BEIJING XINLI TECH INNOVATION CENT CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611100772.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2025-07-30
Filing Date
2026-07-23
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

The non-uniformity of the thickness of existing temporary bonding adhesives leads to non-uniform thickness after wafer thinning, affecting the accuracy of subsequent processes, especially photolithography and etching.

Method used

A dielectric film layer is deposited on the back side of the carrier wafer and then ground and planarized to eliminate temporary bonding adhesive thickness deviations, ensuring that the overall thickness of the stacked wafers is consistent. Then, the device wafer is thinned.

Benefits of technology

It improves the thickness uniformity of device wafers, ensures the accuracy of subsequent processes such as photolithography, bonding and etching, and extends the lifespan of carrier wafers.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123124737A_ABST
    Figure CN123124737A_ABST
Patent Text Reader

Abstract

The application provides a high-precision wafer manufacturing method based on temporary bonding, comprising the following steps: temporarily bonding a device wafer and a carrier wafer by using a temporary bonding process to form a temporary bonding stacked wafer, wherein the temporary bonding comprises the following steps: coating temporary bonding glue on the device wafer and the carrier wafer respectively, and heat curing the temporary bonding glue; the thickness of the device wafer is less than 100 um, the thickness of the coated temporary bonding glue is not more than 20 um, and the thickness deviation is not more than 5 um; the device wafer is located at the bottom, the carrier wafer is located at the top, a dielectric film layer is deposited on the back surface of the carrier wafer to eliminate the thickness difference caused by the coated temporary bonding glue, and the flattening treatment of the back surface side of the carrier wafer is completed by grinding the dielectric film layer; and the carrier wafer is separated from the device wafer and removed by using a debonding process. By using the application, the thickness uniformity of the stacked wafer after temporary bonding is good, and the processing accuracy of the subsequent process is reliably ensured.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of semiconductor manufacturing technology, and in particular relates to a high-precision wafer manufacturing method based on temporary bonding. Background Technology

[0002] In existing temporary bonding and thinning processes, standard carrier wafers typically possess excellent thickness uniformity. However, the core reason for the poor thickness uniformity of the final device wafer after thinning is mainly due to the thickness deviation introduced by the temporary bonding adhesive coating process.

[0003] Uneven thickness of this adhesive layer can cause stress and morphological fluctuations within the bonded stacked wafers. Since subsequent back-side thinning processes on the device wafer use the back side of the carrier wafer as the mechanical reference plane, thickness deviations in the temporary bonding adhesive will eventually accumulate and be directly transferred to the device wafer. When the total thickness of the bottom support structure is uneven, the equipment cannot achieve precise thinning of the device wafer. Summary of the Invention

[0004] Therefore, the present invention provides a high-precision wafer manufacturing method based on temporary bonding, comprising: Step S1: Temporary bonding process is used to temporarily bond the device wafer and the carrier wafer to form a temporary bonded stacked wafer. The temporary bonding includes: coating temporary bonding adhesive on the device wafer and the carrier wafer respectively, and thermally curing the temporary bonding adhesive. The thickness of the device wafer is less than 100 μm, the thickness of the temporary bonding adhesive coating is not more than 20 μm, and the thickness deviation is not more than 5 μm. Step S2: Place the device wafer at the bottom and the carrier wafer at the top. Deposit a dielectric film layer on the back side of the carrier wafer to eliminate the thickness difference caused by the coating of temporary bonding adhesive. The planarization process of the back side of the carrier wafer is completed by grinding the dielectric film layer, so that the thickness of the temporary bonding stack wafer is consistent in different areas. Specifically, the consistency of thickness in different areas means that the surface of the entire back side of the dielectric film layer deposited on the temporary bonding stack wafer is flat and there are no unevenness. Step S3: Flip the temporary bonding stacked wafers so that the carrier wafer is at the bottom and the device wafer is at the top. Then, thin the device wafer from the top. Use a wet etching process to thin the dielectric film layer on the back of the carrier wafer to not less than 1 μm. The wet etching solution for removing the dielectric film layer on the back of the carrier wafer is a dilute hydrofluoric acid solution prepared by mixing hydrofluoric acid and deionized water in a volume ratio of 1:50 to 1:100, or a buffer oxide etching solution prepared by mixing hydrofluoric acid and ammonium fluoride in a volume ratio of 6:1. Step S4: Separate and remove the carrier wafer from the device wafer through a debonding process, and then complete the bonding and patterning process between the device wafers; Step S5: Detect the thickness of the separated and removed carrier wafer. If the thickness of the carrier wafer is insufficient to support the mechanical strength of the device wafer, after repeated use and temporary bonding with the next round of device wafers, place the device wafer at the bottom and the carrier wafer at the top, and continue to deposit a dielectric film layer on the back of the carrier wafer so that it can still have sufficient mechanical strength to support the device wafer when the carrier wafer is reused and its thickness is reduced.

[0005] Furthermore, preferably, in the high-precision wafer manufacturing method of the present invention, the temporary bonding adhesive is a thermosetting polymer adhesive with high thermal stability.

[0006] Furthermore, preferably, in the high-precision wafer manufacturing method of the present invention, in step S4, the debonding process is achieved by one or a combination of thermal debonding, chemical dissolution, mechanical stripping and laser debonding.

[0007] Furthermore, preferably, in the high-precision wafer manufacturing method of the present invention, in step S5, the thickness of the carrier wafer that has been separated and removed is detected. If the thickness of the carrier wafer is insufficient to support the mechanical strength of the device wafer, after repeated use and temporary bonding with the device wafer of the next round, the device wafer is placed at the bottom and the carrier wafer is placed at the top, and an additional film layer of a certain thickness is deposited on the back of the carrier wafer.

[0008] Furthermore, preferably, in the high-precision wafer manufacturing method of the present invention, the additional film layer is PEOX and / or TEOS.

[0009] Furthermore, preferably, in the high-precision wafer manufacturing method of the present invention, the grinding of the carrier wafer and the thinning of the device wafer are mechanical grinding, chemical mechanical grinding, or a combination of both.

[0010] Furthermore, preferably, in the high-precision wafer manufacturing method of the present invention, the change in surface tension characteristics is used to accurately determine the etching endpoint of the wet etching process. When the dielectric layer on the back of the carrier wafer is present, its surface is hydrophilic; when the dielectric layer is completely removed and the silicon substrate is exposed, the silicon surface is hydrogen-terminated and exhibits strong hydrophobicity.

[0011] Furthermore, preferably, in the high-precision wafer manufacturing method of the present invention, if the solution or rinsing water film instantly disappears on the back of the carrier wafer, the etching endpoint is immediately determined and the wet etching process is stopped.

[0012] Before thinning the device wafer, this invention first performs planarization on the overall support structure consisting of "carrier wafer + temporary bonding adhesive," that is, it specifically performs planarization on the "carrier wafer side." By performing a physical planarization process on the carrier wafer side (i.e., locally thinning the carrier wafer body or thinning the dielectric film layer on its back side), it reverses and precisely compensates for the morphological deviations caused by the uneven thickness of the temporary bonding adhesive.

[0013] After leveling the carrier wafer side, the total thickness of the support structure consisting of the carrier wafer and temporary bonding adhesive achieves perfect uniformity. Eliminating the interference of the bonding adhesive, subsequent thinning and measurement of the device wafer ensures that the overall thickness of the stacked wafers is consistent, meaning the final thickness of the device wafer itself is absolutely uniform. This significantly improves the thickness uniformity of the device wafer, thereby guaranteeing the accuracy of subsequent critical processes such as photolithography, hybrid bonding, and etching.

[0014] Using this invention, the grinding and leveling process on the back side of the carrier wafer stops within the dielectric film layer, leaving a certain amount of dielectric film remaining without touching the silicon on the back side of the carrier wafer. This prevents any loss of the Si thickness on the carrier wafer, theoretically allowing for greater reuse. Furthermore, the subsequent removal of the dielectric film layer on the back side of the carrier wafer uses a solution with high Si etching selectivity, ensuring precise removal of the dielectric film layer without causing additional damage to the Si on the back side of the carrier wafer, thus maximizing the reusability of the carrier wafer.

[0015] The high-precision wafer manufacturing method of the present invention can achieve the following effects: the thickness uniformity of the stacked wafers after temporary bonding is good, the thickness of the final device wafer and carrier wafer after temporary bonding is uniform, and the processing accuracy of subsequent processes is reliably guaranteed. Attached Figure Description

[0016] Figure 1 This is a schematic diagram illustrating the process flow for common temporary bond debonding.

[0017] Figure 2 This is a schematic diagram illustrating the temporary bonding wafer thinning process.

[0018] Figure 3 This is a schematic diagram illustrating the alignment deviation caused by wafer unevenness.

[0019] Figure 4 This is a schematic diagram showing the morphology of the lateral etching defect at the bottom notch of TSV Si.

[0020] Figure 5 This is a schematic diagram showing the morphology of TSV Si etching defects caused by uneven wafer thickness.

[0021] Figure 6 This is a schematic diagram of a process flow including direct grinding and planarization of a carrier wafer according to an embodiment of the present invention.

[0022] Figure 7 This is a schematic diagram of a process flow including the deposition of a sacrificial film compensation on the back side of a carrier wafer according to an embodiment of the present invention. Detailed Implementation

[0023] The technical solutions of the embodiments of this application will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only a part of the embodiments of this application, and not all of the embodiments. Other embodiments or modifications obtained by those skilled in the art based on the embodiments of this application without creative effort are all within the scope of protection of this application.

[0024] In advanced packaging processes, vertical stacking of wafers is frequently involved. After vertical stacking, to reduce the final chip size, the stacked wafers need to be thinned, and subsequent fine circuitry needs to be fabricated on the thinned wafer. When the wafer thickness is reduced to a certain level (less than 100µm), its mechanical strength is insufficient to sustain subsequent processes independently. Therefore, it needs to be bonded to a carrier wafer before the thinning process, using bonding to the carrier wafer to improve its mechanical strength. Once the thinned wafer has completed the relevant processes or has been bonded to another wafer and achieved sufficient mechanical strength, the carrier wafer needs to be debonded and removed. The above involves wafer bonding and debonding processes. Because this type of wafer bonding does not require permanent bonding and the carrier wafer needs to be removed later, it is also called temporary bonding and debonding process.

[0025] The specific process flow of a substrate-type temporary bonding according to one embodiment of the present invention is as follows: Figure 1 As shown. Specifically includes: Temporary bonding adhesive is applied to both the device wafer and the carrier. Perform heat curing; Bonding the device wafer and the carrier; When the carrier wafer is no longer needed, we remove it by debonding. Common methods include thermal debonding, chemical dissolution, mechanical exfoliation, and laser debonding.

[0026] The above temporary bonding scheme has the following disadvantages: 1. The intermediate medium consists of organic materials such as temporary bonding adhesive. Its biggest disadvantage is that it has flow characteristics and cannot guarantee a completely flat surface, resulting in uneven thickness of the temporary bonding adhesive in different areas; 2. At the same time, during the bonding process, a certain amount of pressure is also applied to the wafer. Although the temporary bonding adhesive has undergone a thermosetting process and its hardness has been enhanced, the temporary bonding adhesive will also deform, resulting in differences in the thickness of the temporary bonding adhesive in different areas.

[0027] The aforementioned disadvantages can lead to uneven thickness of the temporary bonding adhesive between wafers after bonding, resulting in differences in the absolute height of stacked wafers in different areas, which affects subsequent processes. Specific examples are given below.

[0028] Wafer thinning: After the device wafer is temporarily bonded to the carrier wafer, the device wafer needs to be thinned. However, the inconsistent thickness of the temporary bonding adhesive in different areas within the wafer can interfere with the wafer thinning process and thickness measurement, resulting in poor uniformity of the final thinned thickness. Specific problems include... Figure 2 As shown.

[0029] Alignment deviations caused by wafer unevenness: Due to the poor flatness of the temporary bonding adhesive, the flatness of the wafers bonded to it is also poor. The final grinding result is that the overall thickness of different locations on the wafer is consistent, i.e., all at the same horizontal level. However, due to the uneven thickness of the intermediate temporary bonding adhesive, the final thickness of the wafers requiring thinning is uneven. This causes discrepancies between the alignment marks and the original design positions, leading to problems in subsequent photolithography, bonding, and other processes involving alignment with the alignment marks. This results in decreased overlay accuracy and may even prevent the processes from proceeding normally. Specific problems include... Figure 3 As shown.

[0030] TSV Si etching deviations caused by wafer unevenness: TSV Si etching typically uses the Bosch process. Its process window is small, therefore it's necessary to ensure consistent etching rates across different regions. Consistent Si thickness across different regions is also required. This ensures that the Si material is etched completely during the TSV Si etching process. After TSV Si etching is complete, the underlying dielectric oxide layer continues to be etched. Because the oxide layer cannot conduct away the plasma charge, the plasma continues to etch the Si material on the bottom sidewalls, resulting in a defect morphology with a notch at the bottom of the TSV Si. Specific issues are as follows... Figure 4 As shown.

[0031] In summary, after employing this wafer thinning process, due to the uneven Si thickness on the wafer, even if the etching rate of Si at different locations is consistent, several situations can occur simultaneously during the TSV Si etching process: Si not completely etched, Si just completely etched, and over-etching after Si etching, resulting in a bottom notch morphology. Specific problems are as follows... Figure 5 As shown.

[0032] The carrier wafer in this approach is reusable, but each debonding (e.g., thermal debonding, chemical dissolution, mechanical peeling) applies a certain force to the carrier wafer, causing deformation and reducing its flatness. This is similar to the poor flatness of temporary bonding adhesives. Poor flatness of the carrier wafer, after temporary bonding, will also introduce the aforementioned process problems for stacking wafers.

[0033] In summary, the existing technology uses temporary bonding adhesive and reusable carrier wafers for temporary bonding and debonding of wafers. The biggest problem it faces is the poor thickness uniformity of the stacked wafers after temporary bonding. This results in uneven thickness between the final device wafer and the carrier wafer after temporary bonding, which affects the accuracy of subsequent processes.

[0034] This solution does not require special optimization of existing temporary bonding and debonding methods. Existing temporary bonding and debonding methods can be used, and by adding some common process flows, precise wafer thinning can be achieved, thereby significantly improving the accuracy of subsequent photolithography, bonding, etching, and other processes.

[0035] Currently, the overall thickness uniformity after bonding is mainly improved by optimizing temporary bonding adhesive and carrier wafer materials, as well as the temporary bonding and debonding processes. However, since temporary bonding adhesive is an organic material, it inherently has a certain degree of fluidity. Furthermore, debonding inevitably applies a certain force to the carrier wafer, causing it to deform. Therefore, existing solutions cannot fundamentally solve the problem of final bonding thickness uniformity, thus hindering precise wafer thinning for subsequent device applications and ultimately leading to the aforementioned problems in photolithography, bonding, and etching. This invention does not rely on optimizations of existing temporary bonding and debonding schemes. Instead, it incorporates some common process flows to compensate for the problems arising from temporary bonding processes using temporary bonding adhesive, thereby achieving precise wafer thinning for subsequent device applications.

[0036] According to one embodiment of the present invention, the following detailed scheme is adopted, including: Existing processes are used to coat the device wafer and the carrier wafer with temporary bonding adhesive, followed by thermal curing and temporary bonding. This forms a stacked wafer. The device wafer is placed at the bottom, and the carrier wafer is placed at the top. The back side of the carrier wafer is ground and planarized. This ultimately ensures that the thickness of different areas of the stacked wafers is consistent. The stacked wafers are flipped so that the carrier wafer is at the bottom and the device wafer is at the top, and the device wafer is thinned.

[0037] Because the stacked wafers have excellent flatness and good thickness uniformity across different regions, the final thickness uniformity of the device wafer is very good. This achieves precise wafer thinning while also ensuring the accuracy of subsequent processes such as photolithography, bonding, and etching.

[0038] The reason why existing solutions cannot achieve thinning is that the flatness of the temporary bonding adhesive and the carrier wafer is poor, which ultimately leads to poor flatness of the stacked wafers and uneven overall thickness, making it impossible to achieve precise thinning of the device wafer.

[0039] Therefore, in the embodiments of the present invention, after bonding, the carrier wafer is first ground and planarized to level the entire stacked wafer, so as to achieve uniformity of flatness and thickness in different areas of the device wafer, and eliminate the errors introduced by temporary bonding adhesive and carrier wafer. Then, the device wafer is thinned, and the uniformity of the final thinning thickness of the device wafer and the flatness are greatly improved, and the accuracy of subsequent photolithography, bonding, etching and other processes can also be guaranteed.

[0040] According to a preferred embodiment of the present invention, as the carrier wafer is reused, its thickness will become thinner and thinner. When the thickness of the carrier wafer is insufficient to support the mechanical strength of the device wafer, it will no longer be usable.

[0041] In advanced packaging processes, vertical stacking interconnects of wafers are one of the core technologies. After wafer stacking is completed, in order to reduce the size and thickness of the final chip, the stacked wafers need to be thinned on the back side, and fine circuit structures or exposed TSVs are fabricated on the thinned wafer surface. When the thickness of the device wafer is reduced to below 100μm, its mechanical strength is insufficient to independently support subsequent processes. Therefore, the device wafer must first be temporarily bonded to a carrier wafer to improve mechanical strength with the support of the carrier wafer. After the thinned wafer has completed the corresponding processes or has been permanently bonded to another wafer to obtain sufficient strength, the carrier wafer is removed through a debonding process. The above process is called temporary bonding and debonding.

[0042] A typical existing wafer-based temporary bonding process flow is as follows: Figure 1 As shown, it specifically includes: (1) Spin-coat temporary bonding adhesive onto the bonding surfaces of the device wafer and the carrier wafer respectively; (2) Perform thermosetting treatment on the temporary bonding adhesive; (3) Bond the device wafer and the carrier wafer under certain temperature and pressure to bond the two layers of adhesive; (4) When the carrier wafer support is no longer needed, the carrier wafer is removed by means of thermal bonding, chemical dissolution, mechanical stripping or laser debonding.

[0043] The existing solutions described above have the following fundamental flaws: First, the uniformity of the thickness of temporary bonding adhesive cannot be guaranteed. Temporary bonding adhesive is an organic polymer material with inherent fluidity. Although its viscosity increases significantly after thermosetting, the pressure applied during bonding can still cause uncontrollable deformation of the adhesive layer. Furthermore, the spin coating process itself is affected by multiple factors such as the precision of the coating equipment, the viscosity of the adhesive, and the ambient temperature and humidity, making it difficult to achieve absolute uniformity of the adhesive layer thickness across the entire wafer. Experimental data shows that even with process optimization, the thickness deviation of temporary bonding adhesive typically reaches ±2~5μm or even greater, which is unacceptable for advanced applications where the target thickness is only a few micrometers to tens of micrometers.

[0044] Secondly, uneven thickness of the temporary bonding adhesive directly leads to a deterioration in the thickness uniformity of the device wafer after thinning. For example... Figure 2 As shown, since the thinning process typically uses the back side of the carrier wafer as the mechanical reference plane, when the thickness of the temporary bonding adhesive varies in different regions of the wafer, the remaining thickness of the device wafer after the thinning equipment reduces the entire stacked wafer to the target total thickness is not equal in each region. Specifically, in areas with thicker adhesive layers, the device wafer is thinned more; in areas with thinner adhesive layers, the remaining thickness of the device wafer is greater. This device wafer thickness error introduced by adhesive layer thickness variation cannot be corrected by conventional thinning processes.

[0045] Third, uneven wafer thickness leads to photolithography alignment errors. For example... Figure 3 As shown, the uneven surface of the device wafer after thinning causes the alignment marks to deviate from their designed positions in the vertical direction (i.e., the optical axis direction). In photolithography, the depth of focus (DoF) of the projection lens is usually small. When the vertical position deviation of the alignment marks exceeds the depth of focus range, the alignment system cannot obtain a clear alignment signal in all areas of the entire wafer, resulting in deterioration of overlay accuracy or even alignment failure.

[0046] Fourth, uneven wafer thickness leads to defects in TSV etching. TSV silicon etching typically uses the Bosch process, which has a narrow process window, requiring consistent etching rates and thicknesses across different regions. Figure 4 and Figure 5As shown, when the silicon thickness of a device wafer is uneven, several situations may occur simultaneously within the same etching time: (a) the thicker areas have not yet been etched through; (b) the moderately thick areas have just been etched; (c) the thinner areas have been etched through and exposed the underlying dielectric layer, and continued over-etching causes the plasma to laterally etch the silicon on the bottom sidewall of the TSV, forming notching defects. The coexistence of these situations on the same wafer will directly lead to substandard electrical performance of the TSV and a significant decrease in process yield.

[0047] Fifth, the repeated use of carrier wafers leads to a gradual deterioration in flatness. In existing solutions, carrier wafers are typically designed to be reusable. However, whether through thermal bonding, chemical dissolution, or mechanical peeling, each debonding process applies thermal stress or mechanical force to the carrier wafer, causing minute but irreversible plastic deformation. With increasing reuse, the flatness of the carrier wafer gradually decreases, further exacerbating the aforementioned problems.

[0048] Existing technologies in this field mainly focus on optimizing the material formulation of temporary bonding adhesives, improving coating and curing processes, and enhancing the precision of bonding and debonding equipment. However, due to the inherent fluidity of temporary bonding adhesives as organic materials and the unavoidable external forces during the debonding process, these optimization methods can only alleviate the problem to a certain extent, and cannot fundamentally solve the problem of thickness uniformity in stacked wafers after temporary bonding. In other words, existing technical solutions have the limitation of "treating the symptoms but not the root cause."

[0049] This invention is based on a deep understanding of the shortcomings of the prior art. Instead of relying on optimization of the temporary bonding adhesive material and bonding process itself, this invention fundamentally eliminates the impact of temporary bonding adhesive thickness deviation on the uniformity of device wafer thickness by performing active planarization on the back side of the carrier wafer before device wafer thinning.

[0050] The core concept of this invention lies in actively leveling the overall support structure consisting of the "carrier wafer + temporary bonding adhesive" before thinning the device wafer. Specifically, a dielectric film layer is deposited on the back side of the carrier wafer, followed by planarization through grinding, ensuring that the total thickness of the "carrier wafer + temporary bonding adhesive + dielectric film layer" is consistent across the entire wafer. At this point, even if the temporary bonding adhesive itself still has thickness variations, these variations are compensated for by the thickness differences in the dielectric film layer. After thinning the device wafer based on this support structure with consistent total thickness, the remaining thickness of the device wafer naturally remains consistent across the entire wafer.

[0051] The total thickness of the support structure is uniform across the entire wafer. Therefore, as long as the total thickness of the thinned stacked wafer is uniform across the entire wafer, the thickness of the device wafer will necessarily be uniform. In this way, the "interference factor" of temporary bonding adhesive thickness deviation is completely excluded from the thickness control of the device wafer.

[0052] Therefore, after temporary bonding, we can place the device wafer at the bottom and the carrier wafer at the top, and use CVD process to deposit a film layer (PEOX, TEOS, etc.) of a certain thickness on the back of the carrier wafer. Then, we can use a grinding and planarization process to level the stacked wafers and improve their flatness and thickness uniformity.

[0053] The thickness of the carrier wafer does not decrease with the number of times it is reused, which can significantly increase the number of times the carrier wafer can be reused, thereby reducing costs.

[0054] For carrier wafer grinding, planarization, and device wafer thinning processes, mechanical grinding (grinding), chemical mechanical polishing (CMP), and other related processes or combinations of these processes can be used.

[0055] Furthermore, it should be noted that, preferably, the final device wafer thickness reduction should be within ±10%. For example, if the target thickness of the final device wafer is 3µm, then the silicon thickness at all locations should be between 2.7-3.3µm; if the final device wafer thickness is 50µm, then the silicon thickness at all locations should be between 49.5-50.5µm. Therefore, preferably, the deviation in thickness of the initial carrier wafer plus the temporary bonding film layer is within ±10% of the final device wafer thickness. First, TSV etching has pre-defined etching standards, and it is necessary to consider, for example, a ±10% range of Si thickness. If the Si thickness is too thick, for example, exceeding 10%, incomplete etching will occur, resulting in electrical conduction failure. If the Si thickness is too thin, after Si etching, since the bottom is a dielectric film layer, that is, an insulator, charge accumulation will occur. In this case, the charge will move towards the silicon around the bottom, that is, it will etch away the bottom silicon, creating a gap morphology, which will lead to abnormal TSV morphology. Photolithography works similarly. The focal length can only cover ±10% of the thickness of the top wafer. This ensures that the morphology of the photoresist after development is vertical; otherwise, exposure failure or non-vertical morphology after photoresist development will occur. Abnormal photoresist morphology will lead to abnormal etching morphology.

[0056] Furthermore, it should be noted that, preferably, the combined thickness of the bottom carrier wafer and the bonding material meets the aforementioned thickness deviation. Then, as long as subsequent processes proceed normally, the thickness of the top wafer thinning can be maintained within ±10%. If the final top wafer thinning thickness is not within ±10%, the consequences are the same as described above.

[0057] Furthermore, it should be noted that, preferably, the temporary bonding adhesive used in this invention can be, for example, the following products: 1. Brewer Science: WaferBOND® Series: Organic polymer coating, BrewerBOND® 305: High-performance organic bond-free coating; 2. 3M™ liquid UV curable adhesives (such as the LC-3200 / LC-4200 / LC-5200 series): 3M UV liquid adhesive + LTHC layer with laser release, The LC-3200, LC-4200, and LC-5200 series are based on 100% solid acrylic UV-curable adhesives. The LTHC layer is a 3M Light-To-Heat Conversion coating; 3. TOK TBDB A series: A4012-1, A4017, A4035, A4007, A4030H, etc. It belongs to the category of thermosetting polymer adhesives with high thermal stability.

[0058] Before thinning the device wafer, the device wafer is placed at the bottom and the carrier wafer at the top. First, the back side of the carrier wafer is planarized by grinding to improve the flatness and thickness uniformity of the stacked wafers. Then, the stacked wafers are flipped so the carrier wafer is at the bottom and the device wafer at the top for the device wafer thinning process. To increase the lifespan of the carrier wafer and prevent it from becoming thinner with repeated use, we deposit a film layer on the back side of the carrier wafer. The deposited film layer is a common fab material, such as PEOX or TEOS, and the deposition process is CVD. We cannot use furnace tubes to grow polysilicon because furnace tube processes grow polysilicon not only on the back side of the carrier wafer but also on the surface of the device wafer, requiring subsequent removal of the polysilicon from the device surface, adding an extra process step. After depositing the film layer on the back side of the carrier wafer, the back side of the carrier wafer is then planarized by grinding, and the device wafer surface undergoes a precise thinning process.

[0059] like Figure 6 As shown, according to one embodiment of the present invention, Scheme 1 includes a process flow for direct grinding and planarization of the carrier wafer, comprising: 1. Using existing processes, temporary bonding adhesive is applied to the device wafer and the carrier wafer, followed by thermal curing and temporary bonding to form stacked wafers; 2. Place the device wafer at the bottom and the carrier wafer at the top. Grind the back of the carrier wafer and planarize it to make the thickness of different areas of the stacked wafers uniform. 3. Flip the stacked wafers, placing the carrier wafer at the bottom and the device wafer at the top, and then thin the device wafer. Because the stacked wafers have excellent flatness and uniform thickness across different regions, the final thickness uniformity of the thinned device wafer is very good. This achieves precise thinning of the device wafer and ensures the accuracy of subsequent processes such as photolithography, bonding, and etching. 4. Using a debonding process, the device wafer and the carrier wafer are debonded and separated. The carrier wafer can be reused, and the device wafer can be processed according to the requirements.

[0060] Research has found that the reason existing methods ultimately fail to achieve thinning is the poor flatness of the temporary bonding adhesive, which leads to poor flatness of the stacked wafers and uneven overall thickness, preventing precise thinning of the device wafer. Therefore, this method first grinds and planarizes the carrier wafer after bonding. This initial planarization of the entire stacked wafer aims to ensure a highly uniform overall structure formed by the carrier wafer and temporary bonding adhesive. At this point, during the thinning and measurement of the device wafer, the unevenness originates entirely from the carrier wafer. The final device wafer thickness is calculated by subtracting the thickness of the uniformly thick carrier wafer and temporary bonding adhesive from the overall thickness of the device wafer during thinning and measurement, thus eliminating the influence of uneven temporary bonding adhesive thickness. When the overall thickness is consistent across different regions, the final device wafer thickness is also consistent. This significantly improves the uniformity of device wafer thickness, ensuring the accuracy of the aforementioned photolithography, bonding, and etching processes.

[0061] The drawback of the above approach is that each backside planarization of the carrier wafer results in some wear and tear. As the carrier wafer is reused and its thickness is reduced further, its strength may become insufficient to support the final thinned device wafer. Therefore, it is necessary to monitor the thickness of the carrier wafer as it is reused to ensure that its thickness can support the final thinned wafer. If it cannot support the wafer, it must be discarded promptly.

[0062] In Option 1, the thickness of the temporary bonding adhesive is ≤20µm, and the thickness uniformity is ≤5µm. As the carrier wafer is continuously consumed and its thickness decreases, when the final thickness of the device wafer plus the temporary bonding adhesive plus the carrier wafer is ≤350µm, the overall strength is insufficient. At this point, the carrier wafer needs to be scrapped and cannot be reused; a new carrier wafer needs to be replaced.

[0063] In addition, in order to overcome the problem of continuous wear and tear on the carrier wafer in the aforementioned scheme, a preferred process route that is almost lossless and can realize the unlimited recycling of the carrier wafer is proposed.

[0064] like Figure 7 As shown, according to one embodiment of the present invention, Scheme 2 includes a process flow for depositing a sacrificial film compensation on the back side of a carrier wafer, comprising: 1. Using existing processes, temporary bonding adhesive is applied to the device wafer and the carrier wafer, followed by thermal curing and temporary bonding to form stacked wafers; 2. A dielectric film layer (PEOX, TEOS, etc.) of a certain thickness is deposited on the back side of the carrier wafer using CVD to compensate for the thickness difference of the temporary bonding adhesive and prepare for subsequent thickness reduction. 3. Thinning the back side of the carrier wafer. Since a dielectric film layer is deposited on the back side, we only need to grind a portion of the dielectric film layer without contacting the carrier wafer itself. This ensures good uniformity in the thickness of the remaining dielectric film layer in different areas, plus the carrier wafer and temporary bonding adhesive, preparing for subsequent device wafer thinning. 4. Flip the stacked wafers, placing the carrier wafer at the bottom and the device wafer at the top, and then thin the device wafer. Based on the same principle, the final device wafer exhibits excellent uniformity in thickness reduction. 5. Using a wet etching process, taking advantage of its high etching selectivity for dielectric film and silicon, the remaining dielectric film on the back side of the carrier wafer is removed, and finally the etching stops on the silicon on the back side of the carrier wafer. 6. Using a debonding process, the device wafer and the carrier wafer are debonded and separated. The carrier wafer can be reused, and the device wafer can be processed according to the requirements.

[0065] Compared to Option 1, the advantage of this option is that the overall thickness of the carrier wafer is not affected after going through this series of processes, and it can be used almost without damage and indefinitely.

[0066] In Scheme 2, a dielectric film layer is deposited on the back of the carrier wafer. Because the thickness difference of the bonding adhesive is on the order of several micrometers, the stress on SiN is relatively high. Therefore, we choose to deposit SiO2 material, such as PEOX or TEOS. To cover the thickness difference of the bonding adhesive on the order of several micrometers, we use CVD instead of furnace tube process for depositing SiO2 material.

[0067] Similar to Scheme 1, in Scheme 2, the thickness of the temporary bonding adhesive is ≤20µm, and the thickness uniformity is ≤5µm. The subsequent SiO2 deposition thickness must be ≥6µm. This means that after step 3, the remaining SiO2 thickness on the back side of the carrier wafer is ≥1µm. During the grinding and leveling process on the back side of the carrier wafer in step 3, the SiO2 remains, ensuring it does not touch the silicon on the back side of the carrier wafer. Therefore, unlike Scheme 1, the Si thickness of the carrier wafer is not lost, theoretically allowing for greater recycling and reuse.

[0068] Option 2 involves using a wet etching solution with a high selectivity for Si etching to remove SiO2 from the back of the carrier wafer. This ensures that the SiO2 on the back of the carrier wafer is completely removed without causing additional damage to the Si on the back of the carrier wafer, thus maximizing the reuse of the carrier wafer.

[0069] The wet etching solution of this invention selects the following two schemes: Option A: Use dilute hydrofluoric acid (DHF) solution. • Composition: It is prepared by mixing hydrofluoric acid (HF) and deionized water (H2O) in a certain proportion, such as 1:50 or 1:100 by volume.

[0070] • Reaction Mechanism: HF can specifically break polar Si-O bonds (chemical reaction formula: SiO2 + 6HF → H2SiF6 + 2H2O), but cannot break nonpolar Si-Si covalent bonds in the pure silicon lattice of the carrier wafer. Therefore, this solution has an extremely high etching selectivity for SiO2 and pure Si.

[0071] • Process advantages: The etching rate is relatively slow, making it easy to precisely control the etching thickness. The solution does not contain strong oxidants, ensuring that the etching process stops perfectly on the bare silicon surface of the carrier wafer, without damaging the carrier wafer substrate.

[0072] Option B: Use buffered oxide etching solution (BOE or BHF) • Composition: A buffer solution prepared by mixing hydrofluoric acid (HF) and ammonium fluoride (NH4F), with a commonly used volume ratio of, for example, 6:1.

[0073] • Process advantages: In a pure HF solution, rapid consumption of fluoride ions can lead to a decrease in etching rate and affect etching uniformity. The NH4F added in this solution acts as a buffer, continuously providing a stable source of fluoride ions and maintaining the stability of the etching solution's pH.

[0074] • Applicable scenarios: While maintaining an extremely high etching selectivity (without damaging the underlying Si), it can maintain a constant and relatively high etching rate, which is particularly suitable for the rapid removal of thick SiO2 additional films on the back of the carrier wafer (such as CVD-grown PEOX or TEOS), thus improving the output efficiency of the equipment.

[0075] Furthermore, according to a preferred embodiment of the present invention, a method for determining the process endpoint is also provided: when performing any of the above-described wet etching schemes, the etching endpoint can be accurately determined by utilizing changes in surface tension characteristics. When the SiO2 layer on the back side of the carrier wafer is present, its surface is hydrophilic; when the SiO2 is completely removed and the pure Si substrate is exposed, the silicon surface is hydrogen-terminated, exhibiting strong hydrophobicity. At this time, the solution or rinsing water film can be observed to instantly recede on the back side of the carrier wafer, which serves as the optimal endpoint determination criterion for determining that SiO2 has been completely removed without damaging the carrier wafer.

[0076] As can be seen from the above description of the specific embodiments, the present invention has the following significant advantages compared with the prior art: 1. It fundamentally solves the problem of wafer thinning accuracy caused by uneven thickness of temporary bonding adhesive.

[0077] This invention breaks away from the traditional approach of "passively optimizing" temporary bonding adhesive and the carrier wafer itself, creatively proposing a strategy of actively planarizing the back side of the carrier wafer before thinning the device wafer. By depositing a dielectric film layer on the back side of the carrier wafer and then grinding and leveling it, this invention achieves a high degree of uniformity in the total thickness of the support structure composed of "carrier wafer + temporary bonding adhesive + dielectric film layer" across the entire wafer. While the temporary bonding adhesive in the support structure still exhibits uneven thickness, its thickness deviation is compensated for by the thickness of the dielectric film layer. When the total thickness of the entire stacked wafer is uniform across the entire wafer, the thickness of the device wafer naturally becomes uniform after thinning. In other words, this invention completely eliminates the "interference factor" of temporary bonding adhesive thickness deviation from the device wafer thickness control equation, achieving precise control over the device wafer thickness.

[0078] 2. Significantly improved the processing accuracy and yield of subsequent key processes such as photolithography, bonding, and etching.

[0079] Because the thickness uniformity of the device wafer is significantly improved after thinning, its surface flatness is also correspondingly improved. The vertical position of the alignment marks remains consistent across the entire wafer, and the focal plane of the photolithography equipment can perfectly cover all areas, fundamentally ensuring overlay accuracy. At the same time, due to the guaranteed uniformity of silicon thickness, the TSV etching process no longer suffers from issues such as incomplete etching in some areas or bottom gaps in others on the same wafer. The consistency of TSV morphology and process yield are significantly improved.

[0080] 3. It enables near-lossless reuse of carrier wafers, significantly reducing production costs.

[0081] In a preferred embodiment of the invention, the grinding and leveling process on the back side of the carrier wafer always stops within the deposited dielectric film layer, and the grinding process does not touch the silicon material of the carrier wafer itself. After debonding, the dielectric film layer is completely removed by wet etching, restoring the carrier wafer to its original thickness. Therefore, the thickness of the carrier wafer does not gradually decrease due to repeated use, and its mechanical strength remains unchanged. This allows the carrier wafer to be reused an unlimited number of times, greatly reducing the procurement cost of the carrier wafer and the overall process cost, resulting in significant economic benefits.

[0082] 4. It has good compatibility with existing mainstream equipment and processes, and is easy to promote in industrial applications.

[0083] This invention does not require major modifications to existing temporary bonding and debonding processes. It only requires adding conventional semiconductor manufacturing steps such as PECVD / CVD deposition and wet etching to the process flow. These processes are standardized processes well-known to semiconductor manufacturers, with mature equipment and stable processes. No additional hardware investment or complex process development is required, making industrial promotion extremely easy.

[0084] It should be noted that, in this document, relational terms such as "first" and "second" are used only to distinguish one entity or operation from another, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Furthermore, the terms "comprising," "including," or any other variations thereof are intended to cover non-exclusive inclusion, such that a process, method, article, or apparatus that comprises a list of elements includes not only those elements but also other elements not expressly listed, or elements inherent to such a process, method, article, or apparatus. Without further limitations, an element defined by the phrase "comprising one..." does not exclude the presence of other identical elements in the process, method, article, or apparatus that includes said element.

[0085] The various embodiments in this specification are described in a related manner. For the same or similar parts between the various embodiments, please refer to each other. Each embodiment focuses on describing the differences from other embodiments.

[0086] The above description is merely a specific embodiment of the present invention, but the scope of protection of the present invention is not limited thereto. Any variations or substitutions that can be easily conceived by those skilled in the art within the technical scope disclosed in the present invention should be included within the scope of protection of the present invention. Therefore, the scope of protection of the present invention should be determined by the scope of the claims.

[0087] The above embodiments of the present invention are merely examples for clearly illustrating the present invention and are not intended to limit the implementation of the present invention. Those skilled in the art will recognize that other variations or modifications can be made based on the above description. It is neither necessary nor possible to exhaustively describe all possible implementations here. Any modifications, equivalent substitutions, and improvements made within the spirit and principles of the present invention should be included within the scope of protection of the claims of the present invention.

Claims

1. A high-precision wafer manufacturing method based on temporary bonding implementation, characterized in that, include: Step S1: Temporary bonding process is used to temporarily bond the device wafer and the carrier wafer to form a temporary bonded stacked wafer. The temporary bonding includes: coating temporary bonding adhesive on the device wafer and the carrier wafer respectively, and thermally curing the temporary bonding adhesive. The thickness of the device wafer is less than 100 μm, the thickness of the temporary bonding adhesive coating is not more than 20 μm, and the thickness deviation is not more than 5 μm. Step S2: Place the device wafer at the bottom and the carrier wafer at the top. Deposit a dielectric film layer on the back side of the carrier wafer to eliminate the thickness difference caused by the coating of temporary bonding adhesive. Complete the planarization process of the back side of the carrier wafer by grinding the dielectric film layer, so that the thickness of the temporary bonding stacked wafers is consistent in different areas. Step S3: Flip the temporary bonding stacked wafers so that the carrier wafer is at the bottom and the device wafer is at the top. Then, thin the device wafer from the top. Use a wet etching process to thin the dielectric film layer on the back of the carrier wafer to not less than 1 μm. The wet etching solution for removing the dielectric film layer on the back of the carrier wafer is a dilute hydrofluoric acid solution prepared by mixing hydrofluoric acid and deionized water in a volume ratio of 1:50 to 1:100, or a buffer oxide etching solution prepared by mixing hydrofluoric acid and ammonium fluoride in a volume ratio of 6:

1. Step S4: Separate and remove the carrier wafer from the device wafer through a debonding process, and then complete the bonding and patterning process between the device wafers; Step S5: Detect the thickness of the separated and removed carrier wafer. If the thickness of the carrier wafer is insufficient to support the mechanical strength of the device wafer, after repeated use and temporary bonding with the next round of device wafers, place the device wafer at the bottom and the carrier wafer at the top, and continue to deposit a dielectric film layer on the back of the carrier wafer so that it can still have sufficient mechanical strength to support the device wafer when the carrier wafer is reused and its thickness is reduced.

2. The high-precision wafer manufacturing method according to claim 1, characterized in that, The temporary bonding adhesive is a thermosetting polymer adhesive with high thermal stability.

3. The high-precision wafer manufacturing method according to claim 1, characterized in that, In step S4, the debonding process is achieved by one or a combination of thermal debonding, chemical dissolution, mechanical exfoliation, and laser debonding.

4. The high-precision wafer manufacturing method according to claim 1, characterized in that, The additional film layer is PEOX and / or TEOS.

5. The high-precision wafer manufacturing method according to claim 1, characterized in that, In step S2, the grinding of the carrier wafer and the thinning of the device wafer are performed by mechanical grinding, chemical mechanical grinding, or a combination of both.

6. The high-precision wafer manufacturing method according to claim 1, characterized in that, By utilizing changes in surface tension properties, the etching endpoint of a wet etching process can be accurately determined. When a dielectric layer is present on the back side of the carrier wafer, the surface is hydrophilic. When the dielectric layer is completely removed and the silicon substrate is exposed, the silicon surface is hydrogen-terminated and exhibits strong hydrophobicity.

7. The high-precision wafer manufacturing method according to claim 6, characterized in that, If the solution or rinsing water film disappears instantly on the back of the carrier wafer, the etching endpoint is immediately determined, and the wet etching process is stopped.