Recycling methods for heterojunction solar cells

By employing steps such as laser etching, hydrochloric acid dissolution, nitric acid treatment, and electrolysis, the problem of incomplete separation of electrodes and indium tin oxide films in heterojunction solar cells has been solved. This enables the efficient recovery of high-purity valuable metals such as silver, copper, indium, and tin, ensuring the cleanliness of silicon wafers and reducing energy consumption and costs.

CN123124769APending Publication Date: 2026-11-17JINNENG PHOTOVOLTAIC TECH LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611253850.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-18
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

In existing methods for recycling heterojunction solar cells, it is difficult to completely separate the electrodes and indium tin oxide film. Monocrystalline silicon wafers are easily contaminated by metal ions and amorphous silicon films. Valuable metals such as silver, copper, indium, and tin have low recovery rates and it is difficult to obtain high-purity metals separately. The recycling process has high energy consumption and processing costs.

Method used

The copper electrode is removed by laser physical etching, the indium tin oxide film is dissolved by hydrochloric acid and the electrode on the silicon wafer is dissolved by nitric acid, and the amorphous silicon film is removed by cleaning with a mixed solution of ozone and hydrochloric acid. Silver and copper are recovered by electrolysis, and indium and tin are separated by adjusting the pH value of the hydrochloric acid solution, thus achieving efficient separation and recovery of each metal.

Benefits of technology

This technology enables complete separation of silicon wafers from electrodes and indium tin oxide films in heterojunction solar cells, improving the recovery rate and purity of valuable metals such as silver, copper, indium, and tin, reducing energy consumption and cost in the recycling process, and ensuring that the cleanliness of silicon wafers meets the requirements for reprocessing.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123124769A_ABST
    Figure CN123124769A_ABST
Patent Text Reader

Abstract

This invention relates to the recycling of heterojunction solar cells, specifically providing a method for recycling heterojunction solar cells, aiming to solve the problem of incomplete separation of electrodes and indium tin oxide (ITO) films in existing heterojunction solar cell recycling processes. To this end, the method for recycling heterojunction solar cells of this invention includes the following steps: processing the heterojunction solar cell to separate the silicon wafer, electrodes, and ITO film. This invention, by processing the heterojunction solar cell to separate the silicon wafer, electrodes, and ITO film, enables the separation of the silicon wafer from the electrodes and ITO film, addressing the multilayer structure of heterojunction solar cells. This provides a foundation for the subsequent separate recycling of monocrystalline silicon wafers and valuable materials such as silver, copper, indium, and tin. Compared to existing recycling methods, this method reduces cross-contamination between different materials and improves resource recycling efficiency.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the recycling of heterojunction solar cells, and specifically provides a method for recycling heterojunction solar cells. Background Technology

[0002] With the rapid development of photovoltaic power generation, crystalline silicon cells have captured a significant market share due to their technological maturity. Heterojunction solar cells, as a representative of the next generation of crystalline silicon cells, use N-type monocrystalline silicon wafers as substrates. Amorphous silicon films, transparent conductive oxide (TCO) films, and silver, silver-clad copper, or copper electrodes are sequentially formed on both sides of the monocrystalline silicon wafer. The TCO film typically contains indium tin oxide, and the electrodes contain metals such as silver and copper. As early photovoltaic modules gradually enter their retirement cycle, and due to batch defects, inefficient cells, and debris generated during mass production, there is an urgent need to recycle and reuse high-value materials such as monocrystalline silicon wafers, silver, copper, indium, and tin in heterojunction solar cells.

[0003] Existing recycling methods for heterojunction solar cells typically employ chemical dissolution, thermal treatment, or metal replacement to recover the electrodes, TCO film, and silicon wafers separately. However, due to the low-temperature manufacturing process and multi-layered ultra-thin structure of heterojunction solar cells, the electrodes and TCO film are tightly bonded, and a thin amorphous silicon film remains on the surface of the monocrystalline silicon wafer. This leads to problems such as incomplete removal of the electrodes and TCO film, low recovery rates and purity of metals like silver, difficulty in further recovering high-purity indium, copper, and other valuable metals, and residual amorphous silicon film and metal ion contamination on the surface of the recovered silicon wafer, resulting in insufficient cleanliness and minority carrier lifetime to meet the requirements for re-fabrication of heterojunction solar cells. Furthermore, some recycling processes require high-temperature, strong acid, or strong alkali treatment, resulting in high energy consumption and costs, making it difficult to simultaneously achieve the reuse of monocrystalline silicon wafers and the efficient recovery of multiple valuable metals.

[0004] Therefore, there is an urgent need in the field for a method to recycle heterojunction solar cells to solve the above problems. Summary of the Invention

[0005] The present invention aims to solve the above-mentioned technical problems, namely, to solve the problems in the existing heterojunction solar cell recycling process, such as the difficulty in completely separating the electrodes and indium tin oxide film, the susceptibility of monocrystalline silicon wafers to contamination by metal ions and amorphous silicon films, the low recovery rate of valuable metals such as silver, copper, indium, and tin and the difficulty in obtaining high-purity metals separately, as well as the high energy consumption and processing cost of the recycling process.

[0006] In a first aspect, the present invention provides a method for recycling a heterojunction solar cell, the method comprising the following steps: The heterojunction solar cell is processed to separate the silicon wafer, electrodes, and indium tin oxide film.

[0007] In a specific embodiment of the above recycling method, for the heterojunction solar cell having copper electrodes, the recycling method includes the following steps: The copper electrode on the heterojunction solar cell is removed by laser physical etching. The heterojunction solar cell, after the copper electrodes with the copper grid lines removed, is placed in a hydrochloric acid solution to dissolve the indium tin oxide film, thereby obtaining the silicon wafer.

[0008] In a specific embodiment of the above recycling method, for the heterojunction solar cell having a silver electrode or a silver-clad copper electrode, the recycling method includes the following steps: The heterojunction solar cell is placed in a hydrochloric acid solution to dissolve the indium tin oxide film and peel off the electrodes to obtain the silicon wafer; The silicon wafer is placed in a nitric acid solution to dissolve the remaining electrodes on the silicon wafer.

[0009] In a specific embodiment of the above recycling method, the recycling method further includes the following steps: The silicon wafer is placed in a mixed solution of nitric acid and hydrofluoric acid to remove the amorphous silicon film on the silicon wafer; The silicon wafer after the amorphous silicon film is removed is cleaned with a mixed solution of ozone and hydrochloric acid to obtain a monocrystalline silicon wafer.

[0010] In a specific embodiment of the above recycling method, "washing the silicon wafer after removing the amorphous silicon film with a mixed solution of ozone and hydrochloric acid to obtain a monocrystalline silicon wafer" includes the following steps: The silicon wafer was cleaned with a mixed solution of ozone and hydrochloric acid at an ambient temperature of 25°C for a time ranging from 3 to 5 minutes. The silicon wafer is cleaned again at room temperature by a mixed solution of ozone and hydrochloric acid for 3 to 5 minutes. The silicon wafer was cleaned with deionized water. The silicon wafer is dried to obtain a single-crystal silicon wafer.

[0011] In a specific embodiment of the above recycling method, the recycling method further includes the following steps: Electrolysis of a nitric acid solution containing silver ions yields metallic silver. Copper oxide is obtained by heating a nitric acid solution containing copper ions.

[0012] In a specific embodiment of the above recycling method, the recycling method further includes the following steps: A hydrochloric acid solution containing indium and tin ions is treated to separate and recover metallic indium and metallic tin.

[0013] In a specific implementation of the above-mentioned recovery method, "treating the hydrochloric acid solution containing indium ions and tin ions to separate and recover metallic indium and metallic tin" includes the following steps: The pH of a hydrochloric acid solution containing indium and tin ions is adjusted to recover tin hydroxide precipitate. Electrolysis of hydrochloric acid solution containing indium ions yields metallic indium.

[0014] By employing the above-mentioned technical solution, this invention processes heterojunction solar cells to separate silicon wafers, electrodes, and indium tin oxide films. This enables the separation of silicon wafers from electrodes and indium tin oxide films in the multilayer structure of heterojunction solar cells, providing a basis for the subsequent separate recycling of monocrystalline silicon wafers and valuable materials such as silver, copper, indium, and tin. Compared with existing recycling methods, this reduces cross-contamination between different materials and improves resource recycling efficiency.

[0015] Furthermore, this invention targets heterojunction solar cells with copper electrodes. First, the copper electrodes are removed by laser physical etching, and then the indium tin oxide film is dissolved by hydrochloric acid. This separates the copper electrodes and the indium tin oxide film in different ways, which can prevent a large amount of copper from entering the subsequent wet processing solution and causing contamination to the silicon wafer. At the same time, copper powder can be recovered by laser etching, which is beneficial to obtaining clean silicon wafers and improving the recycling rate of copper resources.

[0016] Furthermore, this invention targets heterojunction solar cells with silver electrodes or silver-coated copper electrodes. It utilizes hydrochloric acid to simultaneously dissolve the indium tin oxide film and strip off part of the electrodes, and then uses nitric acid to dissolve the remaining electrodes on the silicon wafer, so that the electrodes can be completely removed. This reduces the impact of residual metal electrodes on subsequent monocrystalline silicon wafer processing and provides a metal-containing nitric acid solution for further separation and recovery of metals such as silver and copper.

[0017] Furthermore, the present invention places the silicon wafer in a mixed solution of nitric acid and hydrofluoric acid to remove the amorphous silicon film, and further cleans it with a mixed solution of ozone and hydrochloric acid. This can further remove the amorphous silicon film, impurity ions and foreign matter on the surface of the silicon wafer, thereby reducing the residue of amorphous silicon film and metal contaminants on the surface of the silicon wafer, improving the surface cleanliness of the recycled monocrystalline silicon wafer, and enabling it to meet the requirements for re-fabrication of heterojunction solar cells.

[0018] Furthermore, this invention uses a mixed solution of ozone and hydrochloric acid at an ambient temperature of 25°C for cleaning, followed by a second cleaning at room temperature, deionized water cleaning, and drying. This allows for further fine cleaning of the silicon wafer, removing impurity ions and foreign matter from the surface of the silicon wafer. While avoiding damage to the silicon wafer from high-temperature processing, this improves the cleanliness of the recycled monocrystalline silicon wafer, which is beneficial for the reuse of the recycled monocrystalline silicon wafer in the fabrication of heterojunction solar cells.

[0019] Furthermore, this invention electrolyzes a nitric acid solution containing silver ions, causing the silver ions to precipitate at the cathode to form metallic silver. Copper oxide is obtained by heating a nitric acid solution containing copper ions, thereby enabling the separate recovery of silver and copper, reducing the mutual entrainment and contamination between different metals, and improving the recovery rate of silver and copper resources and the utilization value of the recovered products. In the embodiments, the silver recovery rate can reach 93.5%, and the copper recovery rate can reach 82%.

[0020] Furthermore, this invention treats hydrochloric acid solutions containing indium and tin ions to recover metallic indium and metallic tin separately. This avoids the problem of traditional methods that mix and recover indium and tin, making them difficult to further utilize. It achieves the separation and recovery of rare metal resources in heterojunction solar cells, improves the utilization value of indium and tin resources, and enables the recycling of carrier and anti-adhesion cleaning solutions generated in the TCO coating process, reducing the waste of indium and tin resources.

[0021] Furthermore, this invention adjusts the pH value of a hydrochloric acid solution containing indium and tin ions to convert tin ions into tin hydroxide precipitate and separate them. Then, the remaining hydrochloric acid solution containing indium ions is electrolyzed to obtain metallic indium. This invention utilizes the separation characteristics of indium and tin under different processing conditions to achieve the gradual separation and recovery of the two metals, thereby obtaining metallic tin and high-purity metallic indium. This reduces the problem of traditional metal substitution methods forming indium-tin alloys that are difficult to purify separately. Attached Figure Description

[0022] The preferred embodiments of the present invention are described below with reference to the accompanying drawings, in which: Figure 1 This is a detailed flowchart of a method for recycling a heterojunction solar cell provided by the present invention. Detailed Implementation

[0023] Preferred embodiments of the present invention will now be described with reference to the accompanying drawings. Those skilled in the art should understand that these embodiments are merely illustrative of the technical principles of the present invention and are not intended to limit the scope of protection of the present invention.

[0024] It should be noted that in the description of this invention, terms such as "upper," "lower," "left," "right," "inner," and "outer," indicating directional or positional relationships, are based on the directional or positional relationships shown in the accompanying drawings. These are merely for ease of description and do not indicate or imply that the device or element must have a specific orientation, or be constructed and operated in a specific orientation; therefore, they should not be construed as limitations on this invention. Furthermore, the terms "first" and "second" are used for descriptive purposes only and should not be construed as indicating or implying relative importance.

[0025] Furthermore, it should be noted that, in the description of this invention, unless otherwise explicitly specified and limited, the terms "installation," "setting," and "connection" should be interpreted broadly. For example, they can refer to a fixed connection, a detachable connection, or an integral connection; they can refer to a direct connection, an indirect connection through an intermediate medium, or a connection within two components. Those skilled in the art can understand the specific meaning of the above terms in this invention according to the specific circumstances.

[0026] To address the problems in existing heterojunction solar cell recycling processes, such as the difficulty in completely separating electrodes and indium tin oxide films, the susceptibility of monocrystalline silicon wafers to metal ion and amorphous silicon film contamination, the low recovery rate of valuable metals like silver, copper, indium, and tin, and the difficulty in obtaining high-purity metals separately, as well as the high energy consumption and processing costs of the recycling process, this embodiment discloses a method for recycling heterojunction solar cells. This recycling method includes the following steps: Heterojunction solar cells are processed to separate the silicon wafer, electrodes, and indium tin oxide film.

[0027] Reference Figure 1 The recycling method classifies heterojunction solar cells into heterojunction solar cells with copper electrodes, heterojunction solar cells with silver electrodes, and heterojunction solar cells with silver-clad copper electrodes.

[0028] For heterojunction solar cells with copper electrodes, the recycling method includes the following steps S001 to S002: S001, copper electrodes on heterojunction solar cells are removed via laser physical etching. Specifically, the laser is a high-energy-density ultraviolet pulsed laser with a wavelength of 355 nm, a power range of 50 kW to 100 kW, and a frequency range of 10 kHz to 20 kHz. The laser can shatter the copper electrodes into nanoscale fragments. These fragments are then recovered as copper powder using a cyclone separator.

[0029] S002, the heterojunction solar cell after removing the copper electrode is placed in a hydrochloric acid solution to dissolve the indium tin oxide film, obtaining a silicon wafer. The concentration of the hydrochloric acid solution ranges from 5 mol / L to 7 mol / L. The reaction temperature for this step is controlled between 25°C and 30°C, and the reaction time ranges from 5 minutes to 10 minutes.

[0030] Then, the silicon wafer and the hydrochloric acid solution containing indium ions and tin ions were processed separately.

[0031] For heterojunction solar cells with silver electrodes and silver-clad copper electrodes, the recycling method includes the following steps: S011, the heterojunction solar cell is placed in a hydrochloric acid solution to dissolve the indium tin oxide film and strip the electrodes to obtain a silicon wafer. The concentration of the hydrochloric acid solution ranges from 5 mol / L to 7 mol / L. The reaction temperature for this step is controlled between 25°C and 30°C, and the reaction time ranges from 5 minutes to 10 minutes.

[0032] S012, the silicon wafer is placed in a nitric acid solution to dissolve the remaining electrodes on the silicon wafer. The concentration of the nitric acid solution ranges from 3 mol / L to 5 mol / L. The reaction time for this step ranges from 10 minutes to 20 minutes.

[0033] Subsequently, silicon wafers, hydrochloric acid solutions containing indium and tin ions, and nitric acid solutions containing electrode metals were processed separately.

[0034] The processing method for the silicon wafer produced in step S002 is the same as that for the silicon wafer produced in step S012. The silicon wafer processing method includes the following steps: S021, the silicon wafer is placed in a mixed solution of nitric acid and hydrofluoric acid to remove the amorphous silicon film on the wafer. The initial concentration of nitric acid is 70%, and the initial concentration of hydrofluoric acid is 48%, prepared using the pickling tank of a texturing equipment. The volume ratio of nitric acid to hydrofluoric acid is 98:2. The temperature in this step is controlled at 25°C, and the reaction time ranges from 3 to 5 minutes.

[0035] S022, the silicon wafer after removing the amorphous silicon film is cleaned with a mixed solution of ozone and hydrochloric acid to obtain a monocrystalline silicon wafer. The ozone concentration in the mixed solution is 30 ppm, and the hydrochloric acid concentration is 2% to 3%. The cleaning time for this step ranges from 3 to 5 minutes. Cleaning effectively removes impurity ions and foreign matter from the surface of the silicon wafer.

[0036] S023, clean the monocrystalline silicon wafer with deionized water.

[0037] S024, the monocrystalline silicon wafer is dried to obtain a monocrystalline silicon wafer with a cleanliness level suitable for battery fabrication.

[0038] The treatment method for the hydrochloric acid solution containing indium and tin ions produced in step S002 is the same as the treatment method for the hydrochloric acid solution containing indium and tin ions produced in step S011. The treatment method for the hydrochloric acid solution containing indium and tin ions includes the following steps: S031, adjust the pH of the hydrochloric acid solution containing indium and tin ions to recover tin hydroxide precipitate. The target pH range is 2 to 3.5. Within this pH range, tin ions in the hydrochloric acid solution can be converted into tin hydroxide precipitate. Subsequently, metallic tin can be obtained from the tin hydroxide precipitate through a conventional reduction smelting purification process; the specific steps of which are not detailed here.

[0039] S032 involves electrolyzing a hydrochloric acid solution containing indium ions to obtain metallic indium. Specifically, one graphite electrode is used as the anode, and another graphite electrode as the cathode. A direct current power supply is applied to both the anode and cathode to electrolyze the hydrochloric acid solution. The current density applied to the electrodes is in the range of 100 A / m. 2 Up to 120A / m 2 The electrolysis time ranges from 20 to 40 minutes. After electrolysis, metallic indium can be recovered from the cathode.

[0040] Furthermore, for the carrier plates that are periodically replaced in the TCO coating process and the anti-sticking plates in the magnetron sputtering equipment during the heterojunction solar cell production process, the following treatment methods can be used: S041, Clean the indium tin oxide on the carrier plate and / or the anti-attachment plate in hydrochloric acid solution. The concentration of the hydrochloric acid solution ranges from 5 mol / L to 7 mol / L. Specifically, immerse the carrier plate and / or the anti-attachment plate in hydrochloric acid solution at room temperature. After immersion cleaning for 24 hours, rinse the carrier plate and the anti-attachment plate with a high-pressure water gun to remove any remaining indium tin oxide.

[0041] S042, adjust the pH of the hydrochloric acid solution containing indium and tin ions to recover tin hydroxide precipitate. The target pH range is 2 to 3.5. Within this pH range, tin ions in the hydrochloric acid solution can be converted into tin hydroxide precipitate. Subsequently, metallic tin can be obtained from the tin hydroxide precipitate through a conventional reduction smelting purification process; the specific steps of which are not detailed here.

[0042] The hydrochloric acid solution after step S042 can be combined with the hydrochloric acid solution after step S031 and processed according to step S032 to recover metallic indium.

[0043] The method for treating the nitric acid solution containing electrode metal produced in step S012 includes the following steps: S051 describes the electrolysis of a nitric acid solution containing silver ions to obtain metallic silver. Specifically, graphite is used as the anode, and a titanium plate as the cathode. A DC power supply is applied to both the anode and cathode to electrolyze the nitric acid solution. The current density applied to the electrodes is in the range of 200 A / m. 2 Up to 400A / m 2 The electrolysis time ranges from 5 to 20 minutes. After electrolysis, dense granular or dendritic metallic silver forms on the titanium plate cathode, facilitating the recovery of metallic silver.

[0044] S052, heating a nitric acid solution containing copper ions to obtain copper oxide. Specifically, the nitric acid solution is heated to 200°C to evaporate the nitric acid solution, yielding insoluble copper oxide.

[0045] The following examples and comparative cases illustrate the specific steps and technical effects of the recycling method for heterojunction solar cells.

[0046] Example 1 The battery in this embodiment features silver electrodes. It utilizes an N-type monocrystalline silicon wafer with dimensions of 166 mm * 166 mm, a resistivity ranging from 0.3 Ω·cm to 2.1 Ω·cm, and a thickness of 130 μm. The battery underwent key fabrication steps including texturing and cleaning, deposition of intrinsic and doped silicon thin films, deposition of a TCO thin film, screen printing, and electrical performance testing. Batteries with mass-produced efficiencies exceeding 0.5% of the standard efficiency were selected as the subjects for the recycling experiments.

[0047] The recycling method for this heterojunction solar cell includes the following steps: The batteries are mounted onto a specialized basket on the texturing and cleaning equipment. This basket serves as a carrier for transporting silicon wafers and batteries. A 5 mol / L hydrochloric acid solution is prepared in the pickling tank of the texturing equipment, and the temperature is controlled at 25°C. The basket immerses the batteries in the pickling tank for 5 minutes. Afterward, the basket removes the batteries from the pickling tank, and the solution is filtered to collect the silver electrodes that have detached from the batteries. Subsequently, the batteries in the basket, the detached silver electrodes, and the solution in the pickling tank are processed separately.

[0048] The pH of the solution in the pickling tank is adjusted to 2.5 to convert tin ions in the solution into tin hydroxide precipitate. The tin hydroxide precipitate is then separated from the solution by filtration. The tin hydroxide and the solution are then processed separately. For the tin hydroxide, metallic tin is obtained through a conventional reduction solution purification process. For the solution, one graphite electrode is used as the anode, and another graphite electrode as the cathode. A DC power supply is applied to both the anode and cathode to electrolyze the solution. The current density applied to the electrodes is in the range of 100 A / m. 2 The electrolysis time is 40 minutes. After electrolysis, metallic indium can be recovered from the cathode.

[0049] A 3 mol / L nitric acid solution was prepared in another pickling tank of the texturing equipment, and the temperature in the pickling tank was controlled at 25℃. The previously treated battery and the detached silver electrode were placed in the nitric acid solution, and the reaction time was 20 minutes to completely dissolve the residual silver electrode on the battery, forming a silicon wafer. Afterwards, the silicon wafer was removed from the pickling tank using a basket. Then, the silicon wafer in the basket and the solution in the pickling tank were processed separately. For the solution in the pickling tank, graphite was used as the anode and a titanium plate as the cathode, and a DC power supply was applied to both the anode and cathode to electrolyze the solution. The current density applied to the electrodes was in the range of 200 A / m. 2The electrolysis time ranges from 20 minutes. After electrolysis, dense granular or dendritic metallic silver forms on the titanium plate cathode, facilitating the recovery of metallic silver.

[0050] For silicon wafers, a mixed solution of nitric acid and hydrofluoric acid is prepared in one pickling tank of the texturing equipment, while a mixed solution of ozone and hydrochloric acid is prepared in another tank. Specifically, the initial concentration of nitric acid is 70%, the initial concentration of hydrofluoric acid is 48%, and the volume ratio of nitric acid to hydrofluoric acid is 98:2. The ozone concentration in the mixed solution of ozone and hydrochloric acid is 30 ppm, and the hydrochloric acid concentration is 2%. The silicon wafer is then immersed in the mixed solution of nitric acid and hydrofluoric acid, with the temperature of the pickling tank controlled at 25°C and the reaction time at 3 minutes, to remove the amorphous silicon film from the wafer. The silicon wafer with the amorphous silicon film removed is then placed in the mixed solution of ozone and hydrochloric acid and cleaned at room temperature for 5 minutes to further remove impurity ions and foreign matter from the surface of the silicon wafer. Afterward, the silicon wafer is cleaned with deionized water. Finally, the silicon wafer is dried with hot air to obtain a monocrystalline silicon wafer with a cleanliness level meeting the requirements for battery fabrication.

[0051] Subsequently, the monocrystalline silicon wafers were fabricated into heterojunction solar cells. After testing, the cell efficiency was only 0.05% lower than the standard. This verified the feasibility of this recycling method for recovering monocrystalline silicon to fabricate high-efficiency cells again.

[0052] Example 2 The battery in this embodiment features a silver-coated copper electrode. The battery uses an N-type monocrystalline silicon wafer with dimensions of 166 mm x 166 mm, a resistivity ranging from 0.3 Ω·cm to 2.1 Ω·cm, and a thickness of 130 μm. The battery underwent key fabrication steps including texturing and cleaning, deposition of intrinsic and doped silicon thin films, deposition of a TCO thin film, screen printing, and electrical performance testing. Batteries with mass-produced efficiencies exceeding 0.5% of the standard efficiency were selected as the subjects for the recycling experiment.

[0053] The recycling method for heterojunction solar cells includes the following steps: The batteries are mounted onto a specialized basket on the texturing and cleaning equipment. This basket serves as a carrier for transporting silicon wafers and batteries. A 5 mol / L hydrochloric acid solution is prepared in the pickling tank of the texturing equipment, and the temperature is controlled at 25°C. The basket immerses the batteries in the pickling tank for 5 minutes. Afterward, the basket removes the batteries from the pickling tank, and the solution is filtered to collect the silver-coated copper electrodes that have detached from the batteries. Subsequently, the batteries in the basket, the detached silver-coated copper electrodes, and the solution in the pickling tank are processed separately.

[0054] The pH of the solution in the pickling tank is adjusted to 2.5 to convert tin ions in the solution into tin hydroxide precipitate. The tin hydroxide precipitate is then separated from the solution by filtration. The tin hydroxide and the solution are then processed separately. For the tin hydroxide, metallic tin is obtained through a conventional reduction solution purification process. For the solution, one graphite electrode is used as the anode, and another graphite electrode as the cathode. A DC power supply is applied to both the anode and cathode to electrolyze the solution. The current density applied to the electrodes is in the range of 100 A / m. 2 The electrolysis time is 40 minutes. After electrolysis, metallic indium can be recovered from the cathode.

[0055] A 3 mol / L nitric acid solution was prepared in another pickling tank of the texturing equipment, and the temperature in the pickling tank was controlled at 25℃. The previously treated battery and the detached silver-coated copper electrode were placed in the nitric acid solution, and the reaction time was 20 minutes to completely dissolve the residual silver-coated copper electrode on the battery, forming a silicon wafer. Afterwards, the silicon wafer was removed from the pickling tank using a basket. Then, the silicon wafer on the basket and the solution in the pickling tank were processed separately. For the solution in the pickling tank, graphite was used as the anode and a titanium plate as the cathode, and a DC power supply was applied to both the anode and cathode to electrolyze the solution. The current density applied to the electrodes was in the range of 200 A / m. 2 The electrolysis time is 20 minutes. After electrolysis, dense granular or dendritic metallic silver forms on the titanium plate cathode, facilitating the recovery of metallic silver. The remaining solution is then heated to 200°C to obtain copper oxide.

[0056] For silicon wafers, a mixed solution of nitric acid and hydrofluoric acid is prepared in one pickling tank of the texturing equipment, while a mixed solution of ozone and hydrochloric acid is prepared in another tank. Specifically, the initial concentration of nitric acid is 70%, the initial concentration of hydrofluoric acid is 48%, and the volume ratio of nitric acid to hydrofluoric acid is 98:2. The ozone concentration in the mixed solution of ozone and hydrochloric acid is 30 ppm, and the hydrochloric acid concentration is 2%. The silicon wafer is then immersed in the mixed solution of nitric acid and hydrofluoric acid, with the temperature of the pickling tank controlled at 25°C and the reaction time at 3 minutes, to remove the amorphous silicon film from the wafer. The silicon wafer with the amorphous silicon film removed is then placed in the mixed solution of ozone and hydrochloric acid and cleaned at room temperature for 5 minutes to further remove impurity ions and foreign matter from the surface of the silicon wafer. Afterward, the silicon wafer is cleaned with deionized water. Finally, the silicon wafer is dried with hot air to obtain a monocrystalline silicon wafer with a cleanliness level meeting the requirements for battery fabrication.

[0057] Subsequently, the monocrystalline silicon wafers were fabricated into heterojunction solar cells. After testing, the cell efficiency was only 0.05% lower than the standard. This verified the feasibility of this recycling method for recovering monocrystalline silicon to fabricate high-efficiency cells again.

[0058] Example 3 The battery in this embodiment has copper electrodes. The battery uses an N-type monocrystalline silicon wafer with dimensions of 166 mm * 166 mm, a resistivity ranging from 0.3 Ω·cm to 2.1 Ω·cm, and a thickness of 130 μm. The battery underwent key fabrication steps including texturing and cleaning, deposition of intrinsic and doped crystalline silicon thin films, deposition of a TCO thin film, screen printing, and electrical performance testing. Batteries with mass-produced efficiencies more than 0.5% lower than the standard efficiency were selected as the experimental subjects for the recycling experiment.

[0059] The recycling method for heterojunction solar cells includes the following steps: The copper electrodes on the battery are broken into nanoscale fragments by impacting them with a high-energy ultraviolet pulsed laser. These fragments are then collected in a cyclone separator to recover copper powder. Specifically, the laser wavelength is 355 nm, the laser power ranges from 50 kW to 100 kW, and the laser frequency ranges from 10 kHz to 20 kHz.

[0060] Next, the batteries are mounted onto a special basket on the texturing and cleaning equipment. This basket serves as a carrier for transporting silicon wafers and batteries. A 5 mol / L hydrochloric acid solution is prepared in the pickling tank of the texturing equipment, and the temperature inside the tank is controlled at 25°C. The basket immerses the batteries in the pickling tank for 5 minutes. Afterward, the basket removes the batteries from the pickling tank. Subsequently, the batteries in the basket and the solution in the pickling tank are treated separately.

[0061] The pH of the solution in the pickling tank is adjusted to 2.5 to convert tin ions in the solution into tin hydroxide precipitate. The tin hydroxide precipitate is then separated from the solution by filtration. The tin hydroxide and the solution are then processed separately. For the tin hydroxide, metallic tin is obtained through a conventional reduction solution purification process. For the solution, one graphite electrode is used as the anode, and another graphite electrode as the cathode. A DC power supply is applied to both the anode and cathode to electrolyze the solution. The current density applied to the electrodes is in the range of 100 A / m. 2 The electrolysis time is 40 minutes. After electrolysis, metallic indium can be recovered from the cathode.

[0062] For silicon wafers, a mixed solution of nitric acid and hydrofluoric acid is prepared in one pickling tank of the texturing equipment, while a mixed solution of ozone and hydrochloric acid is prepared in another tank. Specifically, the initial concentration of nitric acid is 70%, the initial concentration of hydrofluoric acid is 48%, and the volume ratio of nitric acid to hydrofluoric acid is 98:2. The ozone concentration in the mixed solution of ozone and hydrochloric acid is 30 ppm, and the hydrochloric acid concentration is 2%. The silicon wafer is then immersed in the mixed solution of nitric acid and hydrofluoric acid, with the temperature of the pickling tank controlled at 25°C and the reaction time at 3 minutes, to remove the amorphous silicon film from the wafer. The silicon wafer with the amorphous silicon film removed is then placed in the mixed solution of ozone and hydrochloric acid and cleaned at room temperature for 5 minutes to further remove impurity ions and foreign matter from the surface of the silicon wafer. Afterward, the silicon wafer is cleaned with deionized water. Finally, the silicon wafer is dried with hot air to obtain a monocrystalline silicon wafer with a cleanliness level meeting the requirements for battery fabrication.

[0063] Subsequently, the monocrystalline silicon wafers were fabricated into heterojunction solar cells. After testing, the cell efficiency was only 0.06% lower than the standard. This verifies the feasibility of this recycling method for recovering monocrystalline silicon to fabricate high-efficiency cells again.

[0064] Example 4 This embodiment includes the following steps: A 5 mol / L hydrochloric acid solution was prepared in the carrier cleaning equipment. The carrier plate for the TCO coating process and the anti-attachment plate from the magnetron sputtering equipment were placed in the hydrochloric acid solution and immersed in it at room temperature for 24 hours. Afterward, the carrier plate, anti-attachment plate, and solution were treated separately.

[0065] Next, clean the carrier board and anti-stick plate with a high-pressure water gun to remove any remaining indium tin oxide. Then, dry the carrier board and anti-stick plate. The carrier board and anti-stick plate are then ready for reuse.

[0066] For the solution, the pH was adjusted to 2.5 to convert tin ions into tin hydroxide precipitate. The tin hydroxide precipitate was then separated from the solution by filtration. The tin hydroxide and solution were then processed separately. For the tin hydroxide, metallic tin was obtained through a conventional reduction solution purification process. For the solution, electrolysis was performed using one graphite electrode as the anode and another as the cathode, with a DC power supply applied to both electrodes. The current density applied to the electrodes ranged from 100 A / m. 2 The electrolysis time is 60 minutes. After electrolysis, metallic indium can be recovered from the cathode.

[0067] Comparative Example This embodiment selects a heterojunction solar cell with a mass-produced efficiency more than 0.5% lower than the standard efficiency as the experimental subject. This cell has silver electrodes.

[0068] The recycling method for this heterojunction solar cell includes the following steps: The batteries are mounted onto a specialized basket on the texturing and cleaning equipment. This basket serves as a carrier for transporting silicon wafers and batteries. A 3 mol / L hydrochloric acid solution is prepared in the alkaline washing tank of the texturing equipment, and the temperature is controlled at 90°C. The basket immerses the batteries in the alkaline washing tank for 8 minutes. After alkaline washing, the silver electrodes of the batteries completely detach. The basket then removes the batteries from the alkaline washing tank, and the solution is filtered to collect the detached silver electrodes. Subsequently, the batteries in the basket, the detached silver electrodes, and the solution in the alkaline washing tank are processed separately.

[0069] For the silver electrode, high-temperature pyrolysis is performed to obtain silver powder.

[0070] For the batteries, a 4 mol / L sulfuric acid solution is prepared in the pickling tank of the texturing equipment, and the temperature in the pickling tank is controlled at 95℃. A basket is used to immerse the batteries in the pickling tank, and the reaction time is 5 minutes to remove the indium tin oxide film and amorphous silicon film from the batteries, forming silicon wafers. Afterwards, the basket removes the batteries from the pickling tank. Subsequently, the silicon wafers on the basket and the solution in the pickling tank are processed separately.

[0071] Iron powder is added to the solution in the pickling tank to displace the indium-tin alloy.

[0072] The silicon wafers are cleaned with deionized water. They are then dried with hot air to obtain monocrystalline silicon wafers that can be used to fabricate cells again.

[0073] A new battery was fabricated from a monocrystalline silicon wafer. Testing showed that the efficiency of this battery was 0.3% lower than that of a standard battery. Compared to Examples 1-3, this battery exhibited poorer electrical performance, and contaminants were detected by electroluminescence, indicating that the removal of metal ions and the amorphous silicon film was incomplete during the monocrystalline silicon wafer recycling process.

[0074] The experimental results of Examples 1-4 and the comparative examples are shown in the table below:

[0075] Based on the results of the above experiments, the method for recycling monocrystalline silicon and rare metals silver, indium, and tin in heterojunction solar cells according to the present invention is feasible for industrialization. The efficiency of the cells reconstituted from the recycled monocrystalline silicon is 0.05% lower than the standard 25.5%, but 0.45% higher than the efficiency of the cells before recycling, thus improving the efficiency and yield of heterojunction cells. The recovery rate of rare metals can reach over 90% during the cell recycling, carrier plate, and anti-sticking plate cleaning processes. This invention can accurately and thoroughly peel each thin film layer and silver electrode from the silicon wafer while avoiding damage to the substrate. It also avoids incomplete separation and residual indium, silver, and other metals contaminating the silicon substrate, preventing it from meeting the cleanliness requirements of heterojunction solar cell silicon substrates. Furthermore, this step utilizes existing equipment and chemicals in heterojunction solar cell mass production lines, using hydrometallurgy combined with a highly efficient room-temperature electrochemical method to overcome the limitations of high energy consumption and environmentally harmful technologies in traditional rare metal recycling. This provides a new approach for efficient and environmentally friendly silver and indium-tin recycling and purification, offering new ideas for cost reduction and efficiency improvement for photovoltaic enterprises.

[0076] The technical solution of the present invention has been described above with reference to the preferred embodiments shown in the accompanying drawings. However, it will be readily understood by those skilled in the art that the scope of protection of the present invention is obviously not limited to these specific embodiments. Without departing from the principles of the present invention, those skilled in the art can make equivalent changes or substitutions to the relevant technical features, and the technical solutions after such changes or substitutions will all fall within the scope of protection of the present invention.

Claims

1. A method for recycling heterojunction solar cells, characterized in that, Includes the following steps: The heterojunction solar cell is processed to separate the silicon wafer, electrodes, and indium tin oxide film.

2. The method for recycling a heterojunction solar cell according to claim 1, characterized in that, For the heterojunction solar cell with copper electrodes, the recycling method includes the following steps: The copper electrode on the heterojunction solar cell is removed by laser physical etching. The heterojunction solar cell, after the copper electrodes with the copper grid lines removed, is placed in a hydrochloric acid solution to dissolve the indium tin oxide film, thereby obtaining the silicon wafer.

3. The method for recycling a heterojunction solar cell according to claim 1, characterized in that, For the heterojunction solar cell having a silver electrode or a silver-clad copper electrode, the recycling method includes the following steps: The heterojunction solar cell is placed in a hydrochloric acid solution to dissolve the indium tin oxide film and peel off the electrodes to obtain the silicon wafer; The silicon wafer is placed in a nitric acid solution to dissolve the remaining electrodes on the silicon wafer.

4. A method for recycling a heterojunction solar cell according to claim 2 or 3, characterized in that, The recycling method further includes the following steps: The silicon wafer is placed in a mixed solution of nitric acid and hydrofluoric acid to remove the amorphous silicon film on the silicon wafer; The silicon wafer after the amorphous silicon film is removed is cleaned with a mixed solution of ozone and hydrochloric acid to obtain a monocrystalline silicon wafer.

5. The method for recycling a heterojunction solar cell according to claim 4, characterized in that, "The process of cleaning the silicon wafer after removing the amorphous silicon film using a mixed solution of ozone and hydrochloric acid to obtain a monocrystalline silicon wafer" includes the following steps: The silicon wafer was cleaned with a mixed solution of ozone and hydrochloric acid at an ambient temperature of 25°C for a time ranging from 3 to 5 minutes. The silicon wafer is cleaned again at room temperature by a mixed solution of ozone and hydrochloric acid for 3 to 5 minutes. The silicon wafer was cleaned with deionized water. The silicon wafer is dried to obtain a single-crystal silicon wafer.

6. The method for recycling a heterojunction solar cell according to claim 3, characterized in that, The recycling method further includes the following steps: Electrolysis of a nitric acid solution containing silver ions yields metallic silver. Copper oxide is obtained by heating a nitric acid solution containing copper ions.

7. A method for recycling a heterojunction solar cell according to claim 2 or 3, characterized in that, The recycling method further includes the following steps: A hydrochloric acid solution containing indium and tin ions is treated to separate and recover metallic indium and metallic tin.

8. The method for recycling a heterojunction solar cell according to claim 7, characterized in that, "Treatment of hydrochloric acid solutions containing indium and tin ions to separate and recover metallic indium and metallic tin" includes the following steps: The pH of a hydrochloric acid solution containing indium and tin ions is adjusted to recover tin hydroxide precipitate. Electrolysis of hydrochloric acid solution containing indium ions yields metallic indium.