A diamond composite semiconductor wafer with adjustable coefficient of thermal expansion and its fabrication method
By controlling the thermal expansion coefficient of diamond composite semiconductor wafers, the heat dissipation bottleneck and interface mismatch problem of traditional semiconductor wafers are solved, achieving efficient heat dissipation and improved stability, which facilitates large-scale production.
Patent Information
- Application Number
- CN202611449504.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-17
- Publication Date
- 2026-11-17
AI Technical Summary
Traditional semiconductor wafers such as Si, GaN, SiC, GaAs, and InP have limited thermal conductivity, making it difficult to meet the rapid heat dissipation requirements of high-power semiconductor chips. Furthermore, the mismatch in thermal expansion coefficients between diamond and semiconductor materials leads to residual stress at the interface, which limits the large-scale industrial application of diamond-based epitaxial wafers.
By combining a matrix phase with a high coefficient of thermal expansion with diamond with a low coefficient of thermal expansion, adjusting the volume fraction of the two, and combining ion implantation lift-off process, surface activation bonding and interface protection technology, diamond composite semiconductor wafers with adjustable coefficient of thermal expansion are prepared, which are suitable for large-scale epitaxial growth by MOCVD.
This method achieves thermal expansion coefficient matching between diamond composite substrates and semiconductor wafers, reduces thermal stress, improves interface bonding performance and structural stability, enhances the heat dissipation capacity and device operation stability of semiconductor chips, and facilitates mass production.
Smart Images

Figure CN123124802A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of advanced thermal management technology for semiconductor devices, specifically to a diamond composite semiconductor wafer with adjustable coefficient of thermal expansion and its preparation method. Background Technology
[0002] Semiconductor materials such as Si, GaN, SiC, GaAs, and InP are widely used in the fabrication of semiconductor chips, including lasers, optical communication devices, and photodetectors. Among them, MOCVD has become an important technology for the epitaxial growth and fabrication of related semiconductor chips due to its advantages such as high epitaxial crystal quality, easy control of material composition and thickness, and suitability for large-size wafer epitaxial growth.
[0003] As semiconductor chips become increasingly miniaturized and integrated, the heat dissipation bottleneck caused by high heat flux density is becoming increasingly prominent. Traditional semiconductor wafers such as Si, GaN, SiC, GaAs, and InP have limited thermal conductivity, making it difficult to meet the rapid heat dissipation requirements of high-power semiconductor chips. Excessively high device operating temperatures can lead to decreased luminous efficiency, wavelength drift, reduced device reliability, and shortened lifespan.
[0004] Diamond possesses extremely high thermal conductivity (approximately 2000-2200 W / m·K), making it an ideal high-end heat dissipation material. Using diamond as a substrate material for semiconductor epitaxial wafers can effectively improve the heat dissipation capabilities of semiconductor chips. However, diamond's coefficient of thermal expansion is significantly lower than that of semiconductor materials such as GaAs, AlN, InP, and GaSb. If diamond is directly used as a substrate for heterogeneous integration with semiconductor wafers, the mismatch in thermal expansion coefficients will generate huge residual stress at the interface, leading to problems such as epitaxial layer cracking, wafer warping, and decreased interface bonding performance, thus limiting the large-scale industrial application of diamond-based epitaxial wafers.
[0005] Therefore, there is an urgent need to develop a diamond composite semiconductor epitaxial wafer with an adjustable coefficient of thermal expansion that is compatible with large-scale MOCVD epitaxial growth and its preparation method, in order to solve the above-mentioned technical problems. Summary of the Invention
[0006] To address the shortcomings of existing technologies, this invention provides a diamond composite semiconductor wafer with an adjustable coefficient of thermal expansion and its fabrication method. By combining a matrix phase with a high coefficient of thermal expansion with diamond with a low coefficient of thermal expansion, and adjusting the volume fraction of both, the coefficient of thermal expansion of the diamond composite substrate can be adjusted. Combining ion implantation lift-off process, surface activation bonding, and interface protection techniques, scalable MOCVD epitaxial growth substrates adaptable to wafers of different sizes are fabricated. The resulting substrates possess both excellent thermal conductivity and structural stability.
[0007] This invention discloses a diamond composite semiconductor wafer with adjustable thermal expansion coefficient, comprising, from bottom to top: a diamond composite substrate, a transition layer, a protective layer, a semiconductor seed layer, and a semiconductor wafer; wherein, the transition layer and the protective layer are used to improve the interface bonding performance and block the diffusion of matrix phase elements; The diamond composite substrate is prepared by a consolidation molding process of diamond particles and matrix phase, and the thermal expansion coefficient of the diamond composite substrate is matched with that of the semiconductor seed layer. The surface of the diamond composite substrate is selectively etched to form a matrix phase nanogroove structure; The transition layer is deposited on the surface of a diamond composite substrate after selective etching and fills the matrix phase nanogroove structure; The protective layer is disposed between the transition layer and the semiconductor seed layer; The semiconductor seed layer is obtained by ion implantation and thermal annealing peeling of a substrate wafer bonded to the surface of the protective layer. The semiconductor wafer is obtained by MOCVD epitaxial growth on the surface of the semiconductor seed layer.
[0008] As a further improvement of the present invention, the substrate phase is any one of silver, aluminum, copper, tantalum nitride or ceramic, and the substrate wafer and semiconductor wafer are any one of silicon, silicon carbide, gallium nitride, gallium arsenide or indium phosphide.
[0009] As a further improvement of the present invention, the consolidation forming process is any one of high-temperature hot pressing sintering, vacuum hot pressing, powder metallurgy sintering, spark plasma sintering, or liquid phase melting infiltration.
[0010] As a further improvement of the present invention, the diameter of the diamond composite substrate and the semiconductor wafer is 2-12 inches. After the diamond composite substrate is solidified and formed, the substrate thickness is reduced to 0.6-1.2 mm by chemical mechanical polishing (CMP) process, and its surface roughness is less than 0.5 nm.
[0011] The aforementioned diamond composite substrate is formed using a consolidation process, which ensures a uniform distribution of the matrix phase within the diamond particles to create a composite structure. Therefore, the thermal expansion coefficient of the diamond composite substrate can be controlled by adjusting the volume fraction of the diamond particles to the matrix phase, depending on the specific application requirements. After consolidation, the substrate thickness is reduced using chemical mechanical polishing (CMP) to accommodate different sizes and thermal management needs.
[0012] The aforementioned semiconductor wafer is grown by MOCVD epitaxy based on a semiconductor seed layer. Therefore, the aforementioned semiconductor wafer can be customized according to different application requirements to obtain the required diamond composite semiconductor wafer.
[0013] As a further improvement of the present invention, the selective etching adopts wet chemical etching or dry plasma etching process, and after etching, a groove structure with a depth of 5-100nm is formed on the surface of the substrate phase.
[0014] The aforementioned selective etching etches only the matrix phase while retaining the diamond particles, thereby forming a matrix phase micro-recessed morphology on the surface of the diamond composite substrate. During the deposition of the transition layer, the transition material fills into the micro-recessed structure, thereby enhancing the mechanical interlocking ability of the interface and improving the stability of the interfacial bonding.
[0015] As a further improvement of the present invention, the transition layer is any one of titanium, tungsten, chromium, nickel or molybdenum, the thickness of the transition layer is 5-100 nm, and the deposition method of the transition layer is any one of magnetron sputtering, electron beam evaporation, molten salt bath plating, electroplating or atomic layer deposition (ALD).
[0016] The aforementioned transition layer serves as an interfacial bonding layer, used to improve the interfacial bonding ability between the diamond composite substrate and the protective layer, and to enhance the stability of the interface under high temperature or cooling conditions through interfacial chemical reactions, mechanical interlocking or diffusion, thereby preventing interface detachment.
[0017] As a further improvement of the present invention, the protective layer is any one of aluminum nitride, aluminum oxide, silicon nitride, single-crystal lithium niobate or pure diamond film, and the protective layer is prepared by any one of atomic layer deposition (ALD), chemical vapor deposition (CVD) or physical vapor deposition (PVD) process. The deposition thickness of the protective layer is 1-2 μm, and the thickness of the protective layer is reduced to 100-1000 nm by chemical mechanical polishing (CMP) process, and its surface roughness is less than 0.5 nm.
[0018] The aforementioned protective layer acts as a diffusion barrier for the matrix phase, preventing elemental diffusion from the matrix phase into the semiconductor layer under the high-temperature environment of MOCVD. Simultaneously, this protective layer serves as a transition layer for the coefficient of thermal expansion between the diamond composite substrate and the semiconductor seed layer, improving interface stability. Therefore, the coefficient of thermal expansion of the protective layer must match that of the semiconductor wafer. The aforementioned surface roughness limitation helps improve the surface smoothness of the protective layer, enhances the bonding uniformity between the protective layer and the substrate wafer, reduces interface voids and localized debonding, and ultimately improves the yield of diamond composite semiconductor wafers.
[0019] As a further improvement of the present invention, the implanted ion is either hydrogen ion or helium ion, the ion implantation depth of the substrate wafer is 200nm-1.1μm, the thickness of the substrate wafer to be transferred is 200nm-1.1μm, and the surface roughness of the ion implantation surface is less than 0.5nm.
[0020] This invention also discloses a method for preparing a diamond composite semiconductor wafer with an adjustable coefficient of thermal expansion, comprising the following steps: Step 1: Based on the coefficient of thermal expansion (CTE) of the target single-crystal semiconductor wafer, determine the volume ratio of diamond to the matrix phase according to the thermal expansion mixing law, prepare the diamond composite substrate through a consolidation molding process, and clean it. Step 2: Selectively etch the bonding surface of the diamond composite substrate to make the substrate phase slightly recessed relative to the diamond particles, and then deposit a transition layer. Step 3: A protective layer is formed on the surface of a diamond composite substrate with a transition layer deposited using low-temperature deposition, followed by polishing and cleaning. Step 4: Ion implantation is performed on the substrate wafer, followed by pre-annealing at a temperature below 500°C. Step 5: Under a high vacuum environment, plasma activation and bonding are performed on the surface of the protective layer and the ion implantation surface of the substrate wafer to obtain a bonded composite wafer. Step 6: Anneal the bonded composite wafer and peel off the semiconductor seed layer of the target thickness; Step 7: Polish and clean the semiconductor seed layer, and grow a semiconductor wafer using MOCVD process on the cleaned sample to obtain the desired diamond composite semiconductor wafer.
[0021] As a further improvement of the present invention, in step 4, the pre-annealing temperature is 180-500℃ and the pre-annealing time is 1-36h.
[0022] The pre-annealing temperature and time mentioned above are determined according to the type of substrate wafer and the ion implantation process. This allows the stress in the substrate wafer to be fully released, which is conducive to improving the bonding strength. It can also avoid the reintroduction of internal stress or damage to the crystallization of the substrate wafer, so as to obtain a high-quality bonded composite wafer.
[0023] As a further improvement of the present invention, in step 6, the annealing step is divided into two-step gradient annealing, with an annealing temperature of 120-600℃ and a holding time of 2-40h. The substrate wafer after stripping can be recycled and reused after surface polishing.
[0024] The temperature and time for the two-step annealing process described above are determined based on the type of substrate wafer and the ion implantation process. This annealing process allows for the gradual release of stress in the bonded composite wafer, improving the stability of the interfacial bonding. Furthermore, at this temperature, the substrate wafer can be gradually peeled off, resulting in a damage-free semiconductor seed layer. Simultaneously, it avoids introducing thermal stress into the diamond composite substrate, yielding a high-quality diamond composite semiconductor wafer. After ion implantation and peeling, the substrate wafer surface can be polished and recycled for industrial production.
[0025] Compared with the prior art, the beneficial effects of the present invention are as follows: This invention achieves adjustable thermal expansion coefficients (TEC) of the composite substrate by combining a high thermal expansion coefficient matrix phase with a low thermal expansion coefficient diamond, and by adjusting the composition ratio of the two. This allows the TEC of the composite substrate to match that of the upper semiconductor wafer, reducing thermal stress caused by thermal expansion mismatch during MOCVD epitaxial growth and minimizing wafer warping, cracking, and interface failure. The high thermal conductivity of the diamond composite substrate also enhances the heat dissipation capacity of the semiconductor wafer, reducing localized heat accumulation during semiconductor chip operation and improving device stability. By selectively etching the matrix phase of the diamond composite substrate and then depositing a transition layer and a protective layer, the interfacial bonding between the diamond composite substrate and the upper substrate wafer is strengthened, and the diffusion of the matrix phase under the high-temperature environment of MOCVD is blocked, improving the structural stability of the semiconductor wafer during epitaxial growth. After obtaining the semiconductor seed layer using ion implantation lift-off, surface activation bonding, and thermal annealing lift-off processes, the desired semiconductor wafer is fabricated on its surface via MOCVD epitaxy. The lift-off substrate wafer can be reused after surface treatment, which helps reduce material consumption and manufacturing costs. This invention is applicable to the fabrication of wafers of different sizes, which helps to realize heat dissipation applications in high-power semiconductor devices and facilitates large-scale mass production. Attached Figure Description
[0026] Figure 1 This is a schematic diagram of the overall structure of a diamond composite semiconductor wafer with an adjustable coefficient of thermal expansion disclosed in this invention. Figure 2 This is a process flow diagram of the fabrication process of diamond composite semiconductor wafers with adjustable thermal expansion coefficient disclosed in this invention; Figure 3 The curves showing the change in thermal expansion coefficient and thermal conductivity of the diamond composite substrate prepared in Example 1 of this application as a function of copper volume fraction are shown. Figure 4 The curves showing the change in thermal expansion coefficient and thermal conductivity of the diamond composite substrate prepared in Example 3 of this application as a function of aluminum volume fraction are shown.
[0027] In the picture: 1. Diamond composite substrate; 2. Transition layer; 3. Protective layer; 4. Substrate wafer; 5. Semiconductor seed layer; 6. Semiconductor wafer. Detailed Implementation
[0028] To make the objectives, technical solutions, and advantages of the embodiments of the present invention clearer, the technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of the present invention, not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.
[0029] The present invention will now be described in further detail with reference to the accompanying drawings: Example 1
[0030] This case study focuses on the epitaxial fabrication of GaN chips, where the coefficient of thermal expansion of the GaN chip is 5.6 × 10⁻⁶. -6 K -1 The diamond composite substrate 1 uses copper as the matrix phase, with copper powder particle size of 5-20 μm (purity of 99.999%) and a coefficient of thermal expansion of 16.5 × 10⁻⁶. - 6 K -1 The transition layer 2 is made of Ti, and the protective layer 3 is made of AlN. In this embodiment, a diamond-copper composite substrate 1 is first prepared by vacuum hot pressing sintering; then, a Ti transition layer 2 and an AlN protective layer 3 are sequentially deposited on the substrate surface; next, a diamond composite semiconductor seed layer 5 is obtained by ion implantation lift-off and surface activation bonding processes; finally, a diamond composite GaN-based wafer 6 is prepared by MOCVD homoepitaxial growth, with the structure as shown in the figure. Figure 1 As shown. Figure 2 The preparation process corresponding to this embodiment includes the following steps: Step 1: First, use ethanol to ultrasonically clean the diamond particles for 15-30 minutes, then use dilute nitric acid to clean the diamond particles in a water bath at 60℃ for 15-30 minutes, and finally rinse with deionized water for 2-3 minutes and blow dry with N2 gas.
[0031] Step 2: A 50 nm thick Ti layer was deposited on the surface of the diamond particles using radio frequency magnetron sputtering. The sputtering target was a Ti target (99.999% purity), the sputtering gas was Ar gas (99.995% purity), the gas flow rate was 30 sccm, the sputtering power was 100 W, and the sputtering time was 30 min. During the deposition process, the diamond particles were placed in a rotating disk to ensure uniform coating, thus obtaining Ti-coated diamond particles.
[0032] Step 3: Using a wet mixing process, the structure prepared in Step 2 is mixed with copper powder. Based on the thermal expansion coefficient of GaN chips (5.6 × 10⁻⁶),... -6 K -1 ,refer to Figure 3The volume fraction ratio of diamond particles to copper was controlled at 7:3, and 10% ethanol was added to the diamond-copper composite powder. After mixing, the mixture was subjected to high vacuum conditions (1×10⁻⁶). -4 Pa) removes alcohol from the pre-compressed composite powder.
[0033] Step 4: Prepare a diamond-copper composite substrate using a vacuum hot-pressing sintering process. Place the structure prepared in Step 3 into a high-temperature vacuum furnace and evacuate the furnace until the pressure inside the furnace is ≤1×10⁻⁶. -3 The furnace temperature was raised to 850℃ at a heating rate of 5-10℃ / min and held for 2-4 hours. Then, the furnace temperature was lowered to 300-500℃ at a cooling rate of ≤3℃ / min, and then allowed to cool naturally to room temperature under inert protection before removal. The prepared diamond-copper composite material was placed under high vacuum conditions (1×10⁻⁶). -4 A diamond-copper composite substrate was prepared by heating at 700-800℃ for 1-2 hours (Pa).
[0034] Step 5: Polish and clean the structure prepared in Step 4 to remove surface impurities, and dry it with N2 gas. Clean the substrate surface in a water bath using propanol and isopropanol (IPA) at 60℃ for 15-30 minutes, followed by rinsing with deionized water for 2-3 minutes. Finally, immerse the substrate surface in hydrofluoric acid for 30-45 seconds, rinse with deionized water, and dry with N2 gas.
[0035] Step 6: Selectively etch copper using electrochemical etching on the structure prepared in Step 5. Seal the back of the sample prepared in Step 5 with insulating adhesive and place it in an electrolyte containing H2SO4 and CuSO4, maintaining the electrolyte temperature at 25℃. Apply a constant current at a current density of 0.1 mA / cm². 2 Using the sample as the anode and a platinum sheet as the cathode, dissolve for 1-2 minutes to make the copper substrate recessed 30 nm relative to the diamond particles. After etching, remove the sample and rinse according to step 5.
[0036] Step 7: The structure prepared in Step 6 is deposited with a Ti layer of 50 nm and an AlN layer of 50 nm on its surface using Step 2. After the coating is completed, polishing and rinsing are performed according to Step 5 to make the surface roughness of the AlN protective layer less than 0.5 nm.
[0037] Step 8: Perform H2S on the GaN substrate wafer + Ion implantation, implantation dose 2 × 10 16 ions / cm 2 The implantation depth was 100 nm. After ion implantation, the wafer underwent pre-annealing at 200 °C for 36 h. Subsequently, the implantation surface of the GaN substrate wafer was polished and cleaned to achieve a surface roughness of less than 0.5 nm.
[0038] Step 9: Surface activation and bonding are performed on the surface of the AlN protective layer of the structure prepared in Step 7 and the ion implantation surface of the structure prepared in Step 8 to obtain a bonded composite wafer.
[0039] Step 10: The structure prepared in Step 9 is subjected to a two-step gradient annealing process, first held at 180℃ for 20 h, and then held at 280℃ for 20 h, to obtain a 100 nm diamond-copper composite GaN semiconductor seed layer. The surface is then polished and cleaned using the method described in Step 5 to achieve a surface roughness of less than 0.5 nm.
[0040] Step 11: Place the structure prepared in Step 10 into the MOCVD reaction chamber, introduce H2 and NH3 gases into the chamber, heat the chamber to 1000℃, hold for 10 min, and then clean the surface of the seed layer. Maintain the reaction chamber temperature at 1000℃ and the pressure at 100 Torr, introduce NH3 gas as the nitrogen source and Ga(CH3)3 as the gallium source, control the molar ratio of NH3 gas to Ga(CH3)3 inlet gas to be 2000, and homoepitaxially grow GaN wafers on the surface of the GaN-based seed layer until the GaN wafer thickness is 20 μm. Stop supplying Ga(CH3)3, but continue to introduce NH3 gas, cooling the temperature to 800℃ at a cooling rate of ≤3℃ / min, then switch to N2 gas, cooling to room temperature at a cooling rate of ≤5℃ / min, finally obtaining a diamond-copper composite GaN-based wafer. Example 2
[0041] This case study focuses on the epitaxial fabrication of Si chips, where the coefficient of thermal expansion of the Si chip is 2.6 × 10⁻⁶. -6 K -1 The diamond composite substrate 1 uses aluminum as the matrix phase, with aluminum powder particle size of 5-20 μm (purity of 99.999%) and a coefficient of thermal expansion of 23 × 10⁻⁶. -6 K -1 The transition layer 2 is made of W, and the protective layer 3 is made of pure diamond film. In this embodiment, a diamond-aluminum composite substrate 1 is first prepared by vacuum hot pressing sintering; then, a W transition layer 2 and a pure diamond film protective layer 3 are sequentially deposited on the substrate surface; next, a diamond composite semiconductor seed layer 5 is obtained by ion implantation lift-off and surface activation bonding processes; finally, a diamond composite Si-based wafer 6 is prepared by MOCVD homoepitaxial process, with the structure as shown in the figure. Figure 1 As shown. Figure 2 The preparation process corresponding to this embodiment includes the following steps: Step 1: First, use ethanol to ultrasonically clean the diamond particles for 15-30 minutes, then use dilute nitric acid to clean the diamond particles in a water bath at 60℃ for 15-30 minutes, and finally rinse with deionized water for 2-3 minutes and blow dry with N2 gas.
[0042] Step 2: A 50 nm thick W layer was deposited on the surface of the diamond particles using radio frequency magnetron sputtering. The sputtering target was a W target (99.999% purity), the sputtering gas was Ar gas (99.995% purity), the gas flow rate was 30 sccm, the sputtering power was 100 W, and the sputtering time was 30 min. During the deposition process, the diamond particles were placed in a rotating disk to ensure uniform coating, thus obtaining W-coated diamond particles.
[0043] Step 3: Using a wet mixing process, the structure prepared in Step 2 is mixed with aluminum powder. Based on the thermal expansion coefficient of GaN chips (5.6 × 10⁻⁶),... -6 K -1 ,refer to Figure 4 The volume fraction ratio of diamond particles to aluminum was controlled at 92:7, and 10% ethanol was added to the diamond-aluminum composite powder. After mixing, the mixture was subjected to high vacuum conditions (1×10⁻⁶). -4 Pa) removes alcohol from the pre-compressed composite powder.
[0044] Step 4: Prepare a diamond-aluminum composite substrate using a vacuum hot-pressing sintering process. Place the structure prepared in Step 3 into a high-temperature vacuum furnace and evacuate the furnace until the pressure inside the furnace is ≤1×10⁻⁶. -3 The furnace temperature was raised to 600℃ at a heating rate of 5-10℃ / min and held for 2-4 hours. Then, the furnace temperature was lowered to 300-500℃ at a cooling rate of ≤3℃ / min, and then allowed to cool naturally to room temperature under inert protection before removal. The prepared diamond-aluminum composite material was placed under high vacuum conditions (1×10⁻⁶ Pa). -4 A diamond-aluminum composite substrate was prepared by heating at 500℃ for 1-2 hours (Pa).
[0045] Step 5: Polish and clean the structure prepared in Step 4 to remove surface impurities, and dry it with N2 gas. Clean the substrate surface in a water bath using propanol and isopropanol (IPA) at 60℃ for 15-30 minutes, followed by rinsing with deionized water for 2-3 minutes. Finally, immerse the substrate surface in hydrofluoric acid for 30-45 seconds, rinse with deionized water, and dry with N2 gas.
[0046] Step 6: Selectively etch the aluminum using ICP dry etching on the sample prepared in Step 5. Place the sample in the ICP chamber and temporarily fix it, then evacuate the furnace until the pressure inside the furnace is ≤1×10⁻⁶. -4At 1 Pa, BCl3 gas was introduced at a flow rate of 40 sccm, with a bias power of 100 W and an etching time of 1 min. Subsequently, BCl3 gas was continued to be introduced, followed by Cl2 gas, maintaining a BCl3 to Cl2 gas molar ratio of 5:2. The chamber pressure was 2 Pa, the bias power was 100 W, the chamber temperature was 60 °C, and the etching time was 2 min. The BCl3 gas flow was maintained while the Cl2 gas flow rate was reduced, and the etching time was 30 s, causing the aluminum substrate to be recessed 30 nm relative to the diamond particles. After etching, Ar gas was switched to purge the chamber for 3 min, followed by N2 gas to refill to atmospheric pressure. The sample was removed and rinsed according to step 5.
[0047] Step 7: Deposit a 50nm W layer on the surface of the structure prepared in Step 6 using magnetron sputtering. After deposition, polish and rinse according to the process in Step 5 to ensure the surface roughness of the W transition layer is less than 0.5nm. Deposit a diamond film on the W transition layer surface using MPCVD: Place the sample on the MPCVD chamber sample stage and evacuate to a furnace pressure ≤1×10⁻⁶. -4 At a pressure of 5 kPa, H2 and CH4 gases were introduced at a flow rate of 300 sccm and 20 sccm, respectively. The deposition rate was 0.4 μm / h, and the deposition time was 10 min, resulting in a pure diamond film with a thickness of 50 nm. After deposition, H2 gas was continued to be introduced, while the CH4 gas flow rate was gradually reduced to 5 sccm and maintained for 5 min. The H2 gas flow was maintained while the sample was cooled to below 200 °C. The H2 flow was then stopped, and N2 gas was switched to backfill the chamber pressure to atmospheric pressure. The sample was then removed. The sample was polished and rinsed to ensure that the surface roughness of the pure diamond film protective layer was less than 0.5 nm.
[0048] Step 8: Perform H-processing on the Si substrate wafer + Ion implantation, implantation dose 2 × 10 16 ions / cm 2 The implantation depth was 100 nm. After ion implantation, the wafer underwent pre-annealing at 200 °C for 36 h. Subsequently, the implantation surface of the Si substrate wafer was polished and cleaned to achieve a surface roughness of less than 0.5 nm.
[0049] Step 9: Surface activation and bonding are performed on the surface of the pure diamond thin film protective layer of the structure prepared in Step 7 and the ion implantation surface of the structure prepared in Step 8 to obtain a bonded composite wafer.
[0050] Step 10: The structure prepared in Step 9 is subjected to a two-step gradient annealing process, first held at 180℃ for 20 h, and then held at 280℃ for 20 h, to obtain a 100 nm diamond-aluminum composite-based Si semiconductor seed layer. The surface is then polished and cleaned using the method described in Step 5 to achieve a surface roughness of less than 0.5 nm.
[0051] Step 11: Place the structure prepared in Step 10 into the MOCVD reaction chamber, introduce H2 and NH3 gases into the chamber, heat the chamber to 1000℃, hold for 10 min, and then clean the surface of the seed layer. Maintain the reaction chamber temperature at 1000℃ and the pressure at 100 Torr, introduce SiH4 gas as the silicon source and H2 as the carrier gas, and homoepitaxially grow a Si wafer on the surface of the Si-based seed layer until the Si wafer thickness reaches 20 μm. Stop supplying SiH4, but continue to introduce H2 gas, cooling the temperature to 800℃ at a cooling rate of ≤3℃ / min, then switch to N2 gas, cooling to room temperature at a cooling rate of ≤5℃ / min, finally obtaining a diamond-aluminum composite Si-based wafer.
[0052] The above are merely preferred embodiments of the present invention and are not intended to limit the present invention. Various modifications and variations can be made to the present invention by those skilled in the art. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the scope of protection of the present invention.
Claims
1. A diamond composite on semiconductor wafer with adjustable coefficient of thermal expansion, characterized in that, From bottom to top, it includes: a diamond composite substrate, a transition layer, a protective layer, a semiconductor seed layer, and a semiconductor wafer; among which, The diamond composite substrate is prepared by a consolidation molding process of diamond particles and matrix phase, and the thermal expansion coefficient of the diamond composite substrate is matched with that of the semiconductor seed layer. The surface of the diamond composite substrate is selectively etched to form a matrix phase nanogroove structure; The transition layer is deposited on the surface of a diamond composite substrate after selective etching and fills the matrix phase nanogroove structure; The protective layer is disposed between the transition layer and the semiconductor seed layer; The semiconductor seed layer is obtained by ion implantation and thermal annealing peeling of a substrate wafer bonded to the surface of the protective layer. The semiconductor wafer is obtained by MOCVD epitaxial growth on the surface of the semiconductor seed layer.
2. The diamond composite based semiconductor wafer of claim 1, wherein, The substrate phase is any one of silver, aluminum, copper, tantalum nitride, or ceramic, and the substrate wafer and semiconductor wafer are any one of silicon, silicon carbide, gallium nitride, gallium arsenide, or indium phosphide.
3. The diamond composite based semiconductor wafer of claim 1, wherein, The consolidation forming process is any one of high-temperature hot pressing sintering, vacuum hot pressing, powder metallurgy sintering, spark plasma sintering, or liquid phase melting infiltration.
4. The diamond composite based semiconductor wafer of claim 1, wherein, The diamond composite substrate and the semiconductor wafer have a diameter of 2-12 inches. After the diamond composite substrate is solidified and formed, the substrate thickness is reduced to 0.6-1.2 mm by chemical mechanical polishing process, and its surface roughness is less than 0.5 nm.
5. The diamond composite based semiconductor wafer of claim 1, wherein, The selective etching employs wet chemical etching or dry plasma etching processes, resulting in a groove structure with a depth of 5-100 nm formed on the substrate surface after etching.
6. The diamond composite based semiconductor wafer of claim 1, wherein, The transition layer is any one of titanium, tungsten, chromium, nickel or molybdenum, the thickness of the transition layer is 5-100 nm, and the deposition method of the transition layer is any one of magnetron sputtering, electron beam evaporation, molten salt bath plating, electroplating or atomic layer deposition.
7. The diamond composite based semiconductor wafer of claim 1, wherein, The protective layer is any one of aluminum nitride, aluminum oxide, silicon nitride, single-crystal lithium niobate, or pure diamond film. The protective layer is prepared by any one of atomic layer deposition, chemical vapor deposition, or physical vapor deposition. The thickness of the protective layer is 1-2 μm, and the thickness is reduced to 100-1000 nm by chemical mechanical polishing. Its surface roughness is less than 0.5 nm.
8. The diamond composite based semiconductor wafer of claim 1, wherein, The ion implantation uses either hydrogen or helium ions. The ion implantation depth of the substrate wafer is 200 nm to 1.1 μm, corresponding to a thickness of 200 nm to 1.1 μm for the substrate wafer to be transferred. The surface roughness of the ion implantation is less than 0.5 nm.
9. A method of producing a diamond composite-based semiconductor wafer according to any one of claims 1 to 8, characterized by, Includes the following steps: Step 1: Based on the thermal expansion coefficient of the target single-crystal semiconductor wafer, determine the volume ratio of diamond to the matrix phase according to the thermal expansion mixing law, prepare the diamond composite substrate through a consolidation molding process, and clean it. Step 2: Selectively etch the bonding surface of the diamond composite substrate to make the substrate phase slightly recessed relative to the diamond particles, and then deposit a transition layer. Step 3: A protective layer is formed on the surface of a diamond composite substrate with a transition layer deposited using low-temperature deposition, followed by polishing and cleaning. Step 4: Ion implantation is performed on the substrate wafer, followed by pre-annealing at a temperature below 500°C. Step 5: Under a high vacuum environment, plasma activation and bonding are performed on the surface of the protective layer and the ion implantation surface of the substrate wafer to obtain a bonded composite wafer. Step 6: Anneal the bonded composite wafer and peel off the semiconductor seed layer of the target thickness; Step 7: Polish and clean the semiconductor seed layer, and grow a semiconductor wafer using MOCVD process on the cleaned sample to obtain the desired diamond composite semiconductor wafer.
10. The preparation method according to claim 9, characterized in that, In step 4, the pre-annealing temperature is 180-500℃, and the pre-annealing time is 1-36h; In step 6, the annealing step is divided into two-step gradient annealing, with an annealing temperature of 120-600℃ and a holding time of 2-40h. The substrate wafer after stripping can be recycled and reused after surface polishing.