Low phonon scattering substrates / substrates and their applications in thermal management of high-power semiconductor devices
By controlling the type and size of diamond particles and optimizing reaction process parameters, the residual Si content is reduced, and a reaction-bonded SiC composite material with high thermal conductivity is prepared. This solves the problem of residual Si affecting thermal conductivity and is suitable for thermal management of high-power semiconductor devices.
Patent Information
- Application Number
- CN202610664595.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2026-05-07
- Filing Date
- 2026-05-14
- Publication Date
- 2026-11-17
AI Technical Summary
In existing technologies for preparing reactive bonded SiC composites with high diamond content, the presence of residual Si phase limits their thermal conductivity and performance in high-temperature applications, leading to reduced thermal management efficiency.
By controlling the type and size of diamond particles and optimizing reaction process parameters, especially by using RVD and MBD diamond powders, combined with high packing density and appropriate impregnation time, the residual Si content is reduced, and low or ultra-low Si reactive bonded diamond-SiC composite materials are formed.
A composite material with high thermal conductivity (>700 W/mk or >800 W/mk) has been developed, which is suitable for thermal management of high-power semiconductor devices and improves thermal management efficiency.
Smart Images

Figure FT_1 
Figure FT_2 
Figure FT_3
Abstract
Description
[0001] Cross-reference to related applications / incorporation by reference
[0002] This application is a continuation-in-part of U.S. Application 19 / 430,220, filed December 22, 2025, and claims the benefit and priority of U.S. Provisional Application 63 / 805,757, filed May 14, 2025, the disclosure of which is incorporated herein by reference in its entirety. Technical Field
[0003] Various aspects of this disclosure relate to reaction-bonded composites and the phonon scattering properties of such composites. Background Technology
[0004] Modern semiconductor devices can generate significant amounts of heat due to their density and / or operating frequency. Therefore, thermal management and materials suitable for dissipating this heat are necessary to maintain the peak operating efficiency of these devices.
[0005] Further limitations and disadvantages of such methods will become apparent to those skilled in the art by comparing them with aspects of this disclosure as set forth with reference to the accompanying drawings in the remainder of this application. Summary of the Invention
[0006] Reactively bonded composite materials with low phonon scattering properties are disclosed. Such low-phonon-scattering composite materials can be used in thermal management components for high-power semiconductor devices. Furthermore, systems and methods for manufacturing such reactively bonded composite materials are disclosed. Such systems and / or methods may include reactive bonding of diamond and / or other high thermal conductivity particle preforms, as shown substantially in at least one of the figures and / or described in combination with at least one of the figures, and as set forth more fully in the claims.
[0007] These and other advantages, aspects and novel features of this disclosure, as well as details of the illustrative embodiments thereof, will be more fully understood from the following description and accompanying drawings. Attached Figure Description
[0008] Figure 1 This is a schematic diagram of a reaction-bonded diamond / SiC / Si composite material according to an exemplary embodiment of the present disclosure.
[0009] Figure 2 An example conventionally reactive bonded diamond composite material according to an example embodiment of the present disclosure is shown.
[0010] Figures 3A to 3BModeling of the thermal conductivity of reactively bonded diamond / SiC / Si composites is shown, where Figure 3A The calculated thermal conductivity of diamond / SiC as a function of diamond content is shown, and Figure 3B The effect of residual Si on the calculated thermal conductivity of diamond / SiC / Si according to an example embodiment of this disclosure is shown.
[0011] Figures 4A to 4E Results for various diamond particle sizes and ratios of MBD powder are shown. According to an example embodiment of this disclosure, Figure 4A Using 95 µm MBD powder, which has a packing density of approximately 60% and a volumetric residual Si of approximately 24%; Figure 4B Using 40 µm MBD powder, which has a packing density of about 52% and a residual Si of about 15% by volume; Figure 4C Using 25 µm MBD powder, which has a packing density of about 48% and a residual Si of about 10% by volume; Figure 4D Using a 95 / 25 µm MBD powder mixture 80 / 20, which has a packing density of about 62% and a volumetric residual Si of about 12%; Figure 4E Using a 95 / 25 µm MBD powder mixture 60 / 40, which has a packing density of approximately 62% and a volumetric residual Si of approximately 7%.
[0012] Figures 5A to 5D Results for various diamond particle sizes and ratios of RVD powder are shown. According to an example embodiment of this disclosure, Figure 5A Using 65 µm RVD powder, which has approximately 47% diamond and approximately 18% by volume of residual Si; Figure 5B Using 12 µm RVD powder, which has approximately 38% diamond and approximately 1% by volume residual Si; Figure 5C Using a 65 / 12 μm RVD powder mixture 80 / 20, which has approximately 50% diamond and approximately 8% by volume of residual Si; Figure 5D The RVD powder mixture 60 / 40 with 65 / 12 µm has approximately 58% diamond and approximately 0.3% by volume of residual Si.
[0013] Figures 6A to 6C Results based on the packing method are shown. According to an example implementation of this disclosure, Figure 6A Using a 65 / 12µm RVD powder mixture 60 / 40, which has approximately 58% diamond and approximately 0.5% by volume of residual Si; Figure 6BUsing a 65 / 12 µm RVD powder mixture 60 / 40, which has approximately 60% diamond and approximately 0.5 vol% residual Si; Figure 6C The RVD powder mixture 60 / 40 with a size of 65 / 12 µm was used, which has approximately 62% diamond and approximately 0.05% by volume of residual Si.
[0014] Figures 7A to 7E Results based on infiltration time are shown. According to an example embodiment of this disclosure, Figure 7A and Figure 7B The density and elastic modulus of samples with different impregnation times (15 minutes, 1 hour, 10 hours) are shown; Figures 7C to 7E The microstructures of these examples with various infiltration times are shown.
[0015] Figure 8 An example process for fabricating low phonon scattering boules and / or substrates is described.
[0016] Figure 9 An example packaged semiconductor chip or semiconductor device is depicted, comprising a signal distribution structure having a low phonon scattering substrate, a reactively bonded diamond / SiC composite substrate, and / or a reactively bonded diamond / SiC / Si substrate.
[0017] Figure 10 An example cooling system is depicted, comprising a cooling plate having a low phonon scattering substrate, a reactively bonded diamond / SiC composite substrate, and / or a reactively bonded diamond / SiC / Si substrate.
[0018] Figure 11 Depicting suitable for Figure 10 Example embodiments of the cooling system include a low phonon scattering substrate, a reactively bonded diamond / SiC composite substrate, and / or a reactively bonded diamond / SiC / Si substrate. Detailed Implementation
[0019] Various aspects of this disclosure relate to reactively bonded composite materials and reactively bonded composite materials having low phonon scattering properties suitable for thermal management of high-power semiconductor devices.
[0020] The accompanying drawings illustrate a general manner of construction. Descriptions and details of well-known features and techniques may be omitted to avoid unnecessarily obscuring this disclosure. Furthermore, elements in the drawings are not necessarily drawn to scale. For example, the dimensions of some elements in the figures may be exaggerated relative to others to aid in understanding the examples discussed in this disclosure. The same reference numerals in different figures denote the same elements.
[0021] The term "and / or" refers to any one or more items in a list connected by "and / or". As an example, "x and / or y" refers to any element in the three-element set {(x), (y), (x, y)}. In other words, "x and / or y" means "one or both of x and y". As another example, "x, y and / or z" refers to any element in the seven-element set {(x), (y), (z), (x, y), (x, z), (y, z), (x, y, z)}. In other words, "x, y and / or z" means "one or more of x, y, and z".
[0022] The terms “comprises”, “comprising”, “includes”, and / or “including” are “open-ended” terms and specify the presence of the stated feature but do not exclude the presence or addition of one or more other features.
[0023] The terms “first,” “second,” etc., may be used herein to describe various elements, and these elements should not be limited by these terms. These terms are used only to distinguish one element from another. Thus, for example, a first element discussed in this disclosure may be referred to as a second element without departing from the teachings of this disclosure.
[0024] Unless otherwise stated, the term "coupled" can be used to describe two elements that are in direct contact with each other, or to describe two elements that are indirectly connected through one or more other elements. For example, if element A is coupled to element B, then element A can be in direct contact with element B, or indirectly connected to element B through an intermediate element C. Similarly, the terms "on top of" or "on" can be used to describe two elements that are in direct contact with each other, or to describe two elements that are indirectly connected through one or more other elements.
[0025] Furthermore, any numerical ranges listed herein are intended to include all subranges contained therein. For example, the range “1 to 10” is intended to include any and all subranges between and including the listed minimum value 1 and the listed maximum value 10, that is, all subranges that begin with a minimum value equal to or greater than 1 and end with a maximum value equal to or less than 10, and all subranges in between, such as 1 to 6.3, or 5.5 to 10, or 2.7 to 6.1.
[0026] Reactively bonded silicon carbide (RB-SiC) ceramic components are important in various industries. Diamond can be used as a carbon source to produce materials with desired properties. In one embodiment, the diamond is in the form of particles. In other embodiments, the diamond can be in other forms, such as a coating on SiC particles.
[0027] Reactively bonded SiC (RB-SiC or SiSiC) possesses many positive properties. Compared to conventionally processed SiC (sintering, hot pressing, chemical vapor deposition (CVD)), RB-SiC can be fabricated into complex shapes (without shrinkage) and large sizes, can be customized (properties, grain size, added phases), can be produced in high purity, and can offer attractive process economics (e.g., relatively low process temperatures and smaller equipment due to the absence of process shrinkage). However, due to the infiltration process employed, RB-SiC often contains residual Si phase. The presence of Si phase limits its use in various applications (such as those at high temperatures) and can negatively impact some properties such as thermal conductivity.
[0028] Traditional methods for forming high-diamond-content composites include sintering, hot pressing, and / or CVD. These methods are limited in many ways, including diamond content, cost, size and shape capability, purity, grain size, and properties. Reactively bonded diamond-SiC composites (e.g., reactive-bonded diamond or RB-diamond) offer attractive size and shape capability, cost, purity, and customizability. However, the presence of residual Si phase reduces their thermal conductivity and limits applications in areas such as high temperatures, corrosion, direct polishing, armor, and wear.
[0029] "Si-free" versions of reactive-bonded composites (e.g., with little or no residual Si phase) will be valuable in many markets that require attractive cost, large size and complex shape forming capabilities, and properties provided by the pure SiC microstructure.
[0030] Conventional RB-SiC (diamond) typically contains residual Si that reduces its thermal conductivity. As disclosed herein, composites are produced where the Si + diamond SiC reaction occurs in high volumetric yield, thereby providing composites with low or ultra-low Si content, where the low Si content is less than about 2% and the ultra-low Si content is less than about 0.5%. Methods for producing low or ultra-low Si include controlling the type of diamond particles (e.g., RVD (crushed) vs. MBD (sphericalized) diamond powder); smaller particle size (i.e., larger surface area for the reaction); particle size blends (higher diamond particle packing, leaving less volume for the Si / SiC matrix phase); and / or optimized process times to maximize the Si + diamond SiC reaction. Materials developed as discussed herein exhibit low or ultra-low residual Si, achieving high thermal conductivity (> 700 W / mK) or ultra-high thermal conductivity (> 800 W / mK). In some implementations, high thermal conductivity can be > 700 W / mk, or about 700 to 800 W / mk, or about 700 to 750 W / mk, and ultra-high thermal conductivity can be > 800 W / mk, or about 800 to 900 W / mk, or 800 to 850 W / mk.
[0031] In the disclosed example methods, a preform comprising diamond powder is manufactured. In some embodiments, the preform consists solely of diamond powder of one or more particle sizes. The preform can be a loose mixture of dry diamond powder or a consolidated body formed by casting, pressing, or other methods. Additionally, the reactive bonding can occur under a vacuum (which removes any oxygen or residual moisture such as from room humidity). In other embodiments, the reaction can be carried out under an inert atmosphere such as Ar or He.
[0032] Preforms can be made into green parts using various methods, such as using only dry powder (or a loose mixture of dry powders), pressing into a green body, or by preparing a slurry with water (or other solvents) and shaping the slurry in a mold (or casting it into a brick for subsequent green machining). The slurry is then frozen, dried, or both to remove the solvent and allow the green body to solidify. A drying / carbonization process is then performed; this can occur under an inert atmosphere, such as nitrogen. In some embodiments, the temperature range for this step can be from about 500°C to about 700°C. A carbon-based organic binder can also be used. During the carbonization process, the organic binder decomposes and transforms into carbon (pyrolytic). In some embodiments, the organic binder content is from about 1% to 10% by weight. In other embodiments, the organic binder content is from about 1% to 8% by weight, 1% to 6% by weight, or 1% to 4% by weight.
[0033] This disclosure presents a method for producing RB-SiC ceramics with low, ultra-low, or nominally zero residual Si by utilizing diamond powder in a preform. The process steps include: (1) producing a preform of ceramic and diamond particles (or 100% diamond particles), (2) the preform may contain carbon in forms other than diamond, such as pyrolytic polymers or carbon particles, (3) reactively infiltrating the preform with molten Si (also known as reactive bonding) at a nominal temperature of 1410°C (the melting point of Si) to 1600°C, wherein the Si+CSiC reaction (silicon reacts with carbon to form silicon carbide) occurs, and (4) holding the preform in the furnace for a longer time than required for complete infiltration to allow residual Si in the microstructure to react with diamond to form SiC, until nominally all elemental Si is removed from the microstructure. Typical holding times at the temperature used for standard reactive bonding are 0.5 to 2 hours. Additional time is added when Si reacts with diamond (i.e., infiltration, and then reaction). In the case of diamond, the total time at this temperature can be 1 to 5 hours or 2 to 5 hours. The preform is a sponge with interconnecting channels for Si. Therefore, for diamond, this is a two-step process of (1) filling the sponge (impregnation) and (2) allowing the Si + diamond SiC reaction to occur to remove elemental Si. In some embodiments, the temperature can be increased during / after impregnation to allow the reaction to occur more rapidly.
[0034] This disclosure discloses a method for manufacturing a diamond-SiC composite material with low residual Si phase (e.g., nominally "Si-free") reactive bonding by utilizing diamond powder in a preform. The low residual Si content results in a component due to the very high expansion when diamond reacts to form SiC. Standard reactive-bonded SiC without diamond in the preform can be produced with a minimum residual Si content in the range of 8% to 10%. However, for this disclosure utilizing diamond in the preform, the residual Si content can be 5% or less silicon by volume; in some embodiments, the Si content is 3% or less silicon by volume, 2% or less silicon by volume, 1% or less silicon by volume, 0.5% or less silicon by volume, or 0.1% or less silicon by volume. In some embodiments, the residual Si content is 0.5% or less by volume. In other embodiments, the residual Si is 1% to 0% by volume; 0.5% to 0% by volume; or 0.1% to 0% by volume. In some implementations, there may be no detectable residual Si. Changing the diamond content of the preform, the diamond grit size, the processing time and temperature, and other variables can produce different results.
[0035] In one embodiment, the preform comprises 100% diamond particles (the preform contains only particles nominally 100% diamond). In another embodiment, the diamond particles are used in a particulate slurry comprising particles, a solvent, and optionally a dispersant / binder. In some embodiments, diamond powder of a specified size is used in the preform. Possible diamond particles that can be used herein are disclosed below.
[0036] The diamond particles (powder) used can have various particle sizes. In some embodiments, the diamond particle size ranges from about 3 μm to about 95 μm. The diamond particles (powder) can have two (or more) different particle sizes, one being coarse and the other fine. In some embodiments, larger (coarse) particles with a particle size of about 95 to 60 μm are used. In other embodiments, smaller (fine) particles with a particle size of about 12 to 30 μm are used. In other embodiments, very small diamond particles (ultrafine, about 3 to 10 μm) are used to enhance the reaction between silicon and diamond to form SiC (small, high-surface-area particles react more strongly). Two or more sizes of diamond particles can be used to maximize packing efficiency. Small particles are coupled between larger particles in a particle array to enhance the overall packing in the preform. In some embodiments, two different sizes of diamond particles are used; in other embodiments, three different sizes of diamond particles are used; four different sizes of diamond particles are used; or five or more different sizes of diamond particles are used.
[0037] In one embodiment, a method for manufacturing a reactively bonded diamond-SiC composite material with low residual Si is disclosed, the method comprising: producing a preform containing diamond particles having two different sizes; impregnating the preform with molten Si to produce an impregnated preform; and reacting the molten Si with the diamond particles in the impregnated preform to form a reactively bonded diamond-SiC composite material.
[0038] In some embodiments, the ratio of larger (coarse) particles to smaller (fine / ultrafine) particles falls within a specific range. In one embodiment, two different sizes of diamond particles are used, having a larger particle to smaller particle ratio in the range of about 80-60:20-40. In some embodiments, the blend of coarse diamond particles:fine diamond particles is between about 80:20 and 60:40. In other embodiments, the blend may be about 75:25; 70:30 or 65:35. Particle size measurement may include measurement of particle size, particle size and / or size distribution.
[0039] Particle size measurement can be performed according to ASTM D4464, which is a method for measuring particle size distribution using laser scattering; or by other methods such as laser diffraction. Particle size can be described using values such as D10, D50, and D90. These are particle size values that can be determined from a particle size distribution curve and indicate the size at which 10%, 50%, or 90% of all particles can be found that are smaller than that value. D50 in the particle size distribution is the median particle size, meaning it is the size at which 50% of the particles (by volume or by weight) are smaller and 50% of the particles are larger. It is used as a key indicator of the average particle size of a powder or material. The particle size described in this article is the D50 value.
[0040] The amount of diamond reacting with SiC during this process depends on the diamond grain size and the packing density in the preform. See Figure 4. For example, a preform containing approximately 70% by volume diamond particles can be reacted during the process described herein, leaving approximately 65% by volume diamond and approximately <2% (by volume) residual Si in the composite. In other embodiments, diamonds with a higher surface area in the preform (i.e., through higher packing density and / or finer particles) and / or a longer reaction time can be used, potentially leaving <1% (by volume); <0.5% (by volume); or <0.1% (by volume). If held at this temperature for a sufficiently long time, the diamond can react until all the Si is depleted (no residual Si remains).
[0041] In the disclosed materials, a low final volume percentage of Si (low residual Si phase) in the "Si-free" material is associated with 10% or less Si remaining by volume, with a lower limit of 0% Si (undetectable). In some embodiments, the remaining Si is 9% or less by volume; 8% or less by volume; 7% or less by volume; 6% or less by volume; 5% or less by volume; 4% or less by volume; 3% or less by volume; 2% or less by volume; 1% or less by volume; 0.5% or less by volume; or 0.1% or less by volume. In some embodiments, there is no detectable Si (0% residual).
[0042] Figure 1This is a schematic diagram of a conventional reactive-bonded diamond composite material produced by reactively infiltrating molten Si into a preform of diamond particles. After infiltration, the molten Si reacts with the diamond to form SiC (Si + C → SiC), bonding the structures together. A typical final composite material can consist of (1) the remaining original diamond, (2) the reactively formed SiC, and (3) residual Si. One problem limiting the thermal conductivity of this material is the presence of the residual Si phase, which has been demonstrated both through modeling and experimentation. The residual Si phase is an artificial product of the reactive bonding process (also known as the Si infiltration process). It should be noted that during the reaction, a halo of SiC forms around each diamond particle. This halo can partially or completely encapsulate the diamond particle. This halo consumes volume and thus reduces the space available for the elemental Si phase.
[0043] In the fabrication of reactive-bonded silicon carbide (RB-SiC) ceramic materials, preforms are frequently used. Many different preform processes exist (casting, molding, pressing, etc.). In some embodiments, such as the method described herein, diamond powder of a specified size can be used in the preform.
[0044] Carbon can exist in several forms, such as carbon black, graphite, pyrolytic carbon, and diamond. Diamond is a high-density form of carbon and contains more moles of carbon relative to other forms of carbon at a given specific volume. Because diamond is a high-molecular-weight "carbon," the Si + diamond → SiC reaction is highly expansive (i.e., the SiC formed by the reaction can fill voids in the preform). Furthermore, because diamond is a high-molecular-weight carbon, the Si + diamond → SiC reaction is slow, thus allowing infiltration of the preform followed by the reaction. If the starting diamond powder in the preform has a small particle size, it can react completely to SiC during the process, resulting in "Si-free" reactively bonded SiC.
[0045] Available diamond materials include, but are not limited to, RVD (resin-vitrified diamond) powder and / or MBD (metal-bonded diamond) powder. RVD powder has crushed, irregular, and angular diamond particles, while MBD powder has blocky and more rounded particles. MBD has a more uniform crystal shape and higher mechanical strength, wear resistance, and toughness. RVD powder has an irregular and angular shape and is more brittle / brittle. Due to its irregular shape, RVD powder has a higher surface area and is therefore more readily reacted with molten Si. In other embodiments, diamond can be added to the preform in other forms, such as a diamond coating on SiC particles. In such embodiments, the preform is manufactured to include diamond-coated SiC particles, which are then impregnated with molten Si to produce an impregnated preform, and then the molten Si is reacted with the diamond coating.
[0046] When diamond is added to a preform in the form of diamond-coated SiC particles, the SiC particles can have a particle size of approximately 10 to 100 micrometers and a diamond coating thickness of approximately 10 to 50 micrometers. Using diamond-coated ceramic particles offers a cost advantage over using 100% diamond particles and places high-molecular-weight carbon material at the desired location on the particle surface for the Si + diamond → SiC reaction, aiming to significantly reduce residual Si content.
[0047] Figure 2 An example of conventionally reactive bonded diamond composite material is shown. Figure 2 In the image, the microstructure on the left shows diamond (black); SiC (gray); and residual Si (red). This material has a preform composition containing two sizes of diamond particles: approximately 60% 65 μm diamond and approximately 20% 22 μm diamond; and also contains 20% 12 μm SiC, resulting in a final composite material with a diamond content of 55% by volume. The residual Si content of this material is approximately 8% by volume. Typical properties of such materials are... Figure 2 The right side is shown. Due to the presence of residual Si, this version of the material has a relatively low thermal conductivity of 550 W / W / mK.
[0048] As shown above, conventional RB-SiC (diamond) typically contains residual Si that reduces its thermal conductivity. As disclosed herein, composite materials are produced that allow the reaction of silicon and carbon (diamond) to form SiC (Si + diamond → SiC) to occur in high yields, thus providing composite materials with ultra-low Si content. Methods for producing low and ultra-low residual Si include controlling the type of diamond particles (RVD (crushed) vs. MBD (sphericalized) diamond powder); smaller particle size (i.e., larger surface area for the reaction); particle size blends (higher diamond packing, leaving less volume for the Si / SiC matrix phase); and / or optimized process times to maximize the Si + diamond → SiC reaction. The materials discussed herein have near-zero residual Si, achieving high (> 700 W / mK) or ultra-high (> 800 W / mK) thermal conductivity.
[0049] Figures 3A to 3B Modeling of the thermal conductivity of a reaction-bonded diamond / SiC / Si composite material according to an example embodiment of the present disclosure is shown, wherein Figure 3A The calculated thermal conductivity of diamond / SiC as a function of diamond content is shown, and Figure 3B The effect of residual Si on the calculated thermal conductivity of diamond / SiC / Si is shown. Figure 3A The modeling results shown are for a diamond content of 65 vol% and indicate that < 0.5 vol% residual Si is required to achieve an ultra-high thermal conductivity of > 800 W / mk. Figure 3B The presence of residual Si is shown to significantly reduce the thermal conductivity of the material. For example, when the material has 65 vol% diamond and 5 vol% residual Si, the thermal conductivity decreases from the theoretical 812 W / mk to 677 W / mk (a decrease of approximately 17%).
[0050] Therefore, to obtain ultra-high thermal conductivity, it is crucial to increase the packing density of the diamond preform and reduce the residual Si content to a very low level (< about 0.5%). This disclosure illustrates that ultra-low residual Si (< about 0.5%) can be achieved by utilizing one or more of the following methods: controlling diamond particle size and ratio; packing; and / or infiltration parameters.
[0051] Bulk density can be measured by the green density of a preform. One method for this measurement is to produce a cylindrical or rectangular preform, measure its mass, measure its volume (depending on the dimensions), and calculate its density (i.e., weighing and measurement method). Other methods include Archimedes' principle with a sealed surface (according to ASTM B328) or the helium specific gravity bottle method.
[0052] The amount of diamond was measured by analyzing the microstructure after infiltration (using image analysis from the open-source image processing program ImageJ). Due to the halos of SiC on each diamond particle, the amount of diamond after infiltration was less than that in the preform (see [link to image analysis]). Figure 1 In some implementations, the preform filling can be as high as 70%, resulting in a final diamond content of 65%.
[0053] Figures 4A to 4E The microstructure of a reaction-bonded diamond composite material using MBD powder manufactured according to this disclosure is shown. The microstructure shows diamond (black); SiC (grey); and residual Si (red). Figure 4A Using 95 µm MBD powder, which has a packing density of about 60%, results in about 24 vol% residual Si. Figure 4B Using 40 µm MBD powder, which has a packing density of 52%, results in approximately 15 vol% residual Si. Figure 4C Using 25 µm MBD powder, which has a packing density of approximately 48%, results in approximately 10 vol% residual Si. For 4A to 4C: finer diamond powder with a higher surface area provides a larger Si+CSiC reaction and thus provides less residual Si. Figure 4D Using 95 / 25 µm MBD powder mixed with 80% 95 µm diamond particles and 20% 25 µm diamond particles, it has a packing density of about 62% and results in about 12% by volume of residual Si. Figure 4E Using 95 / 25 µm MBD powder mixed with 60% 95 µm diamond particles and 40% 25 µm diamond particles, it has a packing density of approximately 62% and results in approximately 7% by volume of residual Si. Figures 4D to 4E Diamond particle size blends offer higher packing density (higher diamond content) and less residual Si. More fine particles in the blend contribute to lower Si content (larger surface area available for the reaction).
[0054] Finer diamond powders have a larger surface area for the Si+CSiC reaction, thus reducing the residual Si content. Furthermore, the particle size blends pack better to provide a higher final diamond content.
[0055] Figures 5A to 5D The microstructure of a reaction-bonded diamond composite material using RVD powder manufactured according to this disclosure is shown. The microstructure shows diamond (black); reaction-formed SiC (gray); and residual Si (red). Figure 5AUsing 65 µm RVD powder, a composite material with approximately 47% diamond and approximately 18 vol% residual Si was produced (bulk density < 60%). Figure 5B Using 12 μm RVD powder, a composite material with approximately 38% diamond and approximately 1 vol% residual Si was produced (bulk density < 60%). Figure 5C A 65 / 12 μm RVD powder mixture of 80 / 20 was used to produce a composite material with approximately 50% diamond and approximately 8 vol% residual Si (bulk density < 60%). Figure 5D A 60 / 40 mixture of 65 / 12 µm RVD powder was used to produce a composite material with approximately 58% diamond and approximately 0.3 vol% residual Si (bulk density > 65%). Increasing the bulk density allows for a reduction in residual Si (see below). Furthermore, the amount of diamond after infiltration was measured in the microstructure. Due to the halos of SiC grown on each diamond particle, the amount of diamond after infiltration was less than that in the preform (see below). Figure 1 ).
[0056] Figures 5A to 5C It has a bulk density of < 60%. Figure 5D It has a bulk density of >65%. Due to the more irregular shape of RVD (crushed crystal) diamond powder, RVD has a higher surface area than MBD diamond powder of similar size. Mixtures with a high content of small RVD particles (e.g., 40% 12 µm) can achieve high bulk density (>65%) and low residual Si (<0.5%). As discussed above, the bulk density can be measured in preforms by green density, and for impregnated parts, the bulk density can be measured by image analysis of the microstructure. In some embodiments, the bulk density is >65%, >70%, or about 60% to 80% (see also below).
[0057] Figures 6A to 6C Images of the microstructure of the final impregnated materials using different powder deposition methods are shown. Figure 6A A composite material with approximately 58% diamond and approximately 0.5% by volume of residual Si was obtained by mixing 65 / 12 µm RVD powder at a ratio of 60% 65 µm and 40% 12 µm. This material has a bulk density of >65%. The preform is a dried powder in a graphite mold and has a thermal conductivity of 670 W / mK. Figure 6BA composite material with approximately 60% diamond and approximately 0.5% vol% residual Si was obtained by mixing 65 / 12 µm RVD powder at a ratio of 60% / 40%. This material has a bulk density of >65%. The preform was made from the powder slurry in a graphite mold and has a thermal conductivity of 710 W / mK. Figure 6C Using RVD powder mixed at a ratio of 60% / 40% with 65 / 12 µm, a composite material with approximately 62% diamond and approximately 0.05 vol% residual Si was obtained. This material has a bulk density of >70%. The preform was made from the powder slurry in a rubber mold, which allows for higher particle packing than in a graphite mold (due to reduced interaction between the mold wall and the preform); and has a thermal conductivity of 750 W / mK.
[0058] As discussed above, Figure 6A It is a material made from dried powder in a graphite mold. Figure 6B It is a material made from powder slurry in a graphite mold, and Figure 6C It is a material made from a powder slurry in a rubber mold. The powder slurry is made with a solvent such as water. Dispersants / binders may also be used in the slurry, including but not limited to Tamol. ® It is a condensation product of naphthalenesulfonic acid. In the example above, using a powder slurry to produce the preform gives a high thermal conductivity, and further using a rubber mold to produce the preform gives the highest packing density of the preform, which leads to the highest thermal conductivity of the impregnated material.
[0059] Therefore, as discussed in this paper, the thermal conductivity of diamond / SiC composites can reach 750 W / mK and above by developing deposition methods (such as casting using slurry and rubber molds). Particle deposition in preforms can be increased by using particle shape (the rounder the better), particle size distribution (better mixing of sizes), and optimized preform processing (an example being casting in rubber molds versus graphite molds, which reduces interactions with the particles (such as mold wall friction)).
[0060] Figures 7A to 7E Results are shown based on the impregnation time of 65 / 12 µm VD powder mixed in a 60% / 40% ratio using a powder slurry in a vacuum atmosphere at 1500°C. Figure 7A and Figure 7B The density and elastic modulus of samples with various impregnation times (15 minutes, 1 hour, 10 hours) are shown. Figures 7C to 7E The microstructures of these examples with various infiltration times are shown. Figure 7C The results show an infiltration time of 15 minutes and approximately 0.08% residual Si. Figure 7DThe results show an infiltration time of 1 hour and approximately 0.05% residual Si. Figure 7E The diagram illustrates an infiltration time of 10 hours and the onset of graphitization of the diamond particles. Initially, increasing the infiltration time reduces the residual Si content via the Si + diamond → SiC reaction, resulting in higher thermal conductivity. However, too long a time at approximately 1500°C may initiate diamond degradation via conversion to graphite, which could adversely affect thermal conductivity. Therefore, in some embodiments, the infiltration time can be approximately 1 hour, or 1 to 10 hours; 1 to 8 hours; 1 to 6 hours; 1 to 4 hours; or 1 to 2 hours.
[0061] Now for reference Figure 8 An example process 800 for fabricating a low phonon scattering substrate is shown. Generally, example process 800 can be implemented in a manner similar to the method described above for forming Si-free diamond-SiC composite materials. Specifically, as explained above, a suitable high thermal conductivity ceramic powder can be selected at 810, formed into a preform at 820, and impregnated with silicon at 830. Specifically, at 810, process 800 may include selecting various high thermal conductivity ceramic powders, such as silicon carbide particles, diamond particles, silicon carbide-coated diamond particles, boron nitride particles, and / or other high thermal conductivity ceramic powders. Furthermore, the selected high thermal conductivity ceramic can possess any of the properties of the aforementioned particles. In particular, a blend of fine and coarse particles can be selected to obtain a closely packed preform.
[0062] At 820, process 800 may include forming a preform from a selected high thermal conductivity ceramic powder. Specifically, process 800 may use any of the aforementioned preform techniques to form the preform, including forming dry powder preforms and green part preforms. In embodiments utilizing boron nitride particles, process 800 may form a green part preform, subsequently carbonizing the binder material in the green part preform. Such carbonization may coat the boron nitride with carbon to improve its wettability and subsequent infiltration with molten silicon.
[0063] Similar to the process described above, the Si-infiltrated preform can be heated at 840°C to allow the high thermal conductivity ceramic powder to react with molten Si and form a reactively bonded composite material. In a manner similar to the method disclosed above, the Si-infiltrated preform can be heated for a sufficient duration to allow the molten Si to react completely or substantially with the high thermal conductivity ceramic powder, producing a low phonon scattering (LPS) substrate or ingot.
[0064] At 850°, the LPS substrate or ingot can be further processed. Specifically, the LPS substrate or ingot can be sliced to provide one or more LPS wafers, and these wafers can be further fabricated to meet semiconductor standards. For example, the thickness and / or edges of each LPS wafer can be processed. Specifically, the upper main surface and / or lower main surface of each LPS wafer can be ground to reduce the thickness of each LPS wafer to a desired thickness. Furthermore, the side surfaces and / or edges of each LPS wafer can be trimmed and / or ground to provide notched or flat edge structures.
[0065] The upper and / or lower surfaces of an LPS wafer can undergo finishing processes. For example, such surfaces can be achieved by depositing a layer of material such as SiC, Si, etc. The thickness of such finishing layer can range from a few micrometers to several hundred micrometers. Furthermore, such finishing layer can be applied to only one of the upper and / or lower main surfaces, or it can be applied to both the upper and lower main surfaces. In addition, such finishing layer can create an interface that provides a reduced thermal boundary resistance (TBR).
[0066] Furthermore, the top, bottom, and / or side surfaces of an LPS wafer can undergo grinding and / or planarization to prepare LPS wafers for semiconductor and / or optical applications. For example, such preparation can include chemical mechanical planarization (CMP); plasma treatment, such as steam plasma treatment; CMP using selective CMP slurries; selective additives: amino acid or protein-related derivatives; nucleoside or DNA / RNA base derivatives; and / or laser and / or ion beam planarization of the surface.
[0067] As a result of the above process, LPS substrates can meet semiconductor substrate standards: 12” (300 mm), 8” (200 mm), 6” (150 mm), 4” (100 mm), etc. Such LPS substrates are also suitable for other industrial applications and can be in non-circular shapes and / or other geometries.
[0068] The various properties of the prepared example LPS substrates, including the corresponding phonon scattering properties, are presented in Table 1 below.
[0069] <![CDATA[ powder ]]> <![CDATA[ Example 1 ]]> <![CDATA[ Example 2 ]]> <![CDATA[ Example 3 ]]> <![CDATA[ Example 4 ]]> Young's modulus (Pa) <![CDATA[8.26 × 10 11 ]]> <![CDATA[3.73 × 10 11 ]]> <![CDATA[4.01 × 10 11 ]]> <![CDATA[4.42 × 10 11 ]]> <![CDATA[4.53 × 10 11 ]]> <![CDATA[Density (kg / m 3 )]]> 3390 3020 3090 3170 3180 Speed of sound (m / s) 15610 11113 11392 11808 11935 Diamond (volume %) 60% 0% 0.2% 1.3% 2.9% Si (volume %) 0% 22% 13.4% 4.1% 2.9% SiC (volume %) 40% 78% 86.4% 94.6% 94.2% Theoretical thermal conductivity of composite materials (W / mK) 1048 319 341 375 397 The measured thermal conductivity of the composite material (W / mK) 720 255 255 281 282 Apparent phonon scattering limit (%) 31% 20% 25% 25% 29%
[0070] Table 1
[0071] In Table 1, the apparent phonon scattering limit is equal to 1 – C, expressed as a percentage. m / C t C m It is the measured thermal conductivity of the composite material; and where C is... tThis is the theoretical thermal conductivity of the composite material. Furthermore, the theoretical thermal conductivity is calculated under the following conditions: assuming no scattering and linearity per volume percentage for all materials, using the thermal conductivity of diamond powder (1,500 W / mK), SiC (370 W / mK), and Si (140 W / mK).
[0072] According to Table 1, low-diamond-content (i.e., less than about 3% by volume) LPS substrates, hereinafter referred to as (LDC-LPS) substrates, can have phonon scattering limits of less than about 40%, less than about 38%, less than about 36%, less than about 34%, or less than about 32%. Furthermore, LDC-LPS substrates can have thermal conductivity greater than about 200 W / mK, greater than about 250 W / mK, greater than about 260 W / mK, greater than about 270 W / mK, greater than about 280 W / mK, or greater than about 290 W / mK. Furthermore, high-diamond-content (i.e., greater than about 55% by volume, greater than about 60% by volume, or greater than about 65% by volume) LPS substrates, hereinafter referred to as (HDC-LPS) substrates, can have thermal conductivity greater than about 600 W / mK, greater than about 650 W / mK, greater than about 700 W / mK, greater than about 750 W / mK, or greater than about 800 W / mK.
[0073] In some implementations, regardless of the diamond content, the LPS substrate may have a coefficient of thermal expansion (CTE) mismatch with silicon of less than about 100%, less than about 90%, less than about 80%, less than about 70%, or less than about 60%. Specifically, the CTE mismatch is equal to 1 - |CTE – CTE (expressed as a percentage). LPS | / CTE, where CTE corresponds to the CTE of silicon, which is 2.6 ppm at 25°C, and where CTE LPS The CTE corresponds to the LPS substrate of interest. When the LPS substrate is coupled to semiconductors, optics, electronic heating devices, etc., the packaged CTE may be much higher than that of silicon, possibly as high as 8 to 9 ppm.
[0074] Regardless of diamond content, LPS substrates can have a variety of geometries. That is, LPS substrates can have aspect ratios (e.g., diameter relative to thickness) greater than about 3, about 10, about 20, about 50, about 100, or about 150. Furthermore, LPS substrates can have wafer diameters greater than about 23 mm, about 48 mm, about 98 mm, about 148 mm, about 198 mm, or about 298 mm. LPS substrates can have wafer thicknesses less than about 2 mm, less than about 1.5 mm, less than about 1.0 mm, and less than about 0.85 mm.
[0075] Such LPS substrates, as well as the reactive-bonded diamond / SiC composites and reactive-bonded diamond / SiC / Si composites disclosed above, are suitable for a variety of applications. For example, such substrates are suitable for semiconductor device packaging. That is, such substrates are suitable for implementing printed circuit boards, laminates, interposers, and / or signal distribution structures on which one or more semiconductor chips of the packaged semiconductor device can be mounted.
[0076] More specifically, such as Figure 9 As shown, the semiconductor device 90 may include a signal distribution structure 94 and one or more semiconductor chips 94 mounted to the signal distribution structure 94. In various embodiments, the signal distribution structure 94 may be implemented as a printed circuit board, a laminated substrate, an interposer, or other signal distribution structure. For this purpose, the signal distribution structure 94 may include an LPS substrate, a reactive-bonded diamond / SiC composite substrate, or a reactive-bonded diamond / SiC / Si composite substrate. Furthermore, the signal distribution structure 94 may include one or more conductive structures (e.g., through-vias, conductive traces, etc.) to route power, ground, data, and / or other electrical signals between the one or more semiconductor chips 94 mounted to the signal distribution structure 94.
[0077] As shown, in some embodiments, the semiconductor device 90 may be implemented as a semiconductor package that further includes external interconnect structures 96 (e.g., solder balls, pins, pads, etc.) along the bottom side of the signal distribution structure 92 and an encapsulant 98 covering the top side of one or more semiconductor chips 94 and the signal distribution structure 94. However, in other embodiments, the semiconductor device 90 may be implemented as a motherboard, motherboard, daughterboard, etc., of a computing device or another electronic device.
[0078] Such substrates are also suitable for cooling systems, which are used to extract heat from heat-generating devices. Specifically, such as... Figure 10 As shown, the cooling system 101 for the heat-generating device 120 may include a cooling plate 100, which includes an LPS substrate, a reactively bonded diamond / SiC composite substrate, or a reactively bonded diamond / SiC / Si composite substrate 110; a manifold 130; and a fluid distribution system 140.
[0079] The bottom side of the cooling plate 100 can be mounted to the heat-generating device 120. The heat-generating device 120 may include a graphics processing unit (GPU), a tensor processing unit (TPU), a central processing unit (CPU), optical components, electronic components, quantum computing components, etc. Furthermore, the manifold 130 can couple the fluid distribution system 140 to the top side of the cooling plate 100 via a fluid delivery conduit 142. In various embodiments, the fluid distribution system 140 can circulate fluid (e.g., gas or liquid) through the manifold 130 via the fluid delivery conduit 142 to transfer heat energy from the heat-generating device 120 to the fluid distribution system 140 via the cooling plate 100.
[0080] In some embodiments, the cooling plate 100 can be mounted to the heating device 120 via a thermal interface material, such as a paste, phase change medium, and / or thermally conductive liquid (e.g., liquid metal). In such embodiments, the cooling plate 100 can be further secured to the heating device 120 via a clamping mechanism. In other embodiments, the cooling plate 100 can be mounted to the heating device 102 using an adhesive such as an organic or inorganic glue, wherein the O-rings or recesses of the cooling plate 100 can be filled (or unfilled) with a filler material. In yet another embodiment, the cooling plate 100 can be directly bonded to the heating device 102 via a bonding process involving surface activation. In still other embodiments, the cooling plate 100 can be mounted to the heating device 120 by brazing or soldering the bottom side of the cooling plate 100 to the heating device 120. In such embodiments, the bottom side of the cooling plate 100 can be metallized to provide an adhesion layer. Such adhesive layers may include carbide-forming elements of Group IVA (such as Si and Ge), Group IVB (such as Ti, Zr and Hf), Group VB (V, Nb and Ta), and Group VIB (such as Cr, Mo and W). Furthermore, such adhesive layers may include barrier layers comprising metallic elements, insulating elements, and / or semiconductor elements.
[0081] Similarly, manifold 130 can be mounted to cooling plate 100 in various ways. In some embodiments, manifold 130 can be mounted to cooling plate 100 via a thermal interface material, such as a paste, phase change medium, and / or thermally conductive liquid (e.g., liquid metal). In such embodiments, manifold 130 can be further secured to heating device 120 via a clamping mechanism. In other embodiments, manifold 130 can be mounted to cooling plate 100 using an adhesive such as an organic or inorganic glue. In some embodiments, manifold 130 can be secured to the top side of cooling plate 100 via an O-ring. In such embodiments, manifold 130 can be further secured to cooling plate 100 via a clamping mechanism.
[0082] In another embodiment, manifold 130 may be directly bonded to cooling plate 100 via an adhesive process involving surface activation. In various embodiments, manifold 130 may be mounted to cooling plate 100 via brazing or soldering. In such embodiments, one or more surfaces of cooling plate 100 may be metallized with an adhesive layer. Such an adhesive layer may include carbide-forming elements of Group IVA (such as Si and Ge), Group IVB (such as Ti, Zr, and Hf), Group VB (V, Nb, and Ta), and Group VIB (such as Cr, Mo, and W). Furthermore, such an adhesive layer may include a barrier layer comprising metallic elements, insulating elements, and / or semiconductor elements.
[0083] Now for reference Figure 11 Further details regarding various implementations of the cooling plate 100 are presented. Specifically, Figure 11 Cooling plates 100A, 100B, 100C, and 100D are depicted, each of which can be used for similar purposes. Figure 10 The cooling system 101 is in the cooling system.
[0084] As shown, the cooling plate 100A can be implemented as a bare LPS substrate, a diamond / SiC composite substrate, or a diamond / SiC / Si composite substrate 110. As shown, the substrate 110 can have a lateral side or short geometry A and a top side or long geometry B. The ratio of the top side B to the lateral side A (B / A) can be greater than about 5, greater than about 20, greater than about 50, or greater than about 100. Furthermore, the top side B can be greater than about 15 mm, greater than about 24 mm, greater than about 49 mm, greater than about 99 mm, or greater than or equal to 149 mm. Furthermore, the lateral side A can be less than about 15 mm, less than about 10 mm, less than about 5 mm, and less than about 2 mm. Additionally, one or more outer sides of the substrate 110 can be lapped and / or polished.
[0085] Cooling plate 100B can be implemented using substrate 110 in a similar manner to cooling plate 100A. However, substrate 110 of cooling plate 100B may be further coated or covered with cladding layer 112 on one or more outer surfaces of substrate 110. Cladding layer 112 may include one or more insulating materials, such as, for example, oxides, nitrides, carbides, borides, arsenides, silicides, phosphides, etc. Alternatively or additionally, cladding layer 112 may contain one or more layers of semiconductor material, such as silicon, germanium, etc. Furthermore, such semiconductor materials may be doped. Alternatively or additionally, cladding layer 112 may contain one or more metal and / or transition metal materials, such as, for example, Group 3A, Group 4A, Group 5A metal materials and / or Group 3B to Group 10B transition metal materials.
[0086] In some embodiments, the cladding layer 112 may cover all cladding surfaces of the substrate 110 with the same material. In other embodiments, one or more outer surfaces of the substrate 110 may be covered with a different material than the material used to cover one or more other outer surfaces of the substrate 110. Finally, in some embodiments, one or more outer surfaces of the cladding layer 112 may be ground and / or polished.
[0087] Cooling plate 100C can be implemented in a similar manner to cooling plate 100B, employing substrate 110 and cladding layer 112. However, cooling plate 100C may further include a capping layer 114 that coats or covers one or more outer surfaces of cladding layer 112 and / or substrate 110. Generally, capping layer 114 can be implemented in a similar manner to cladding layer 112. However, in various embodiments, capping layer 114 can be made of high-purity materials (e.g., contamination levels less than about 5 × 10⁻⁶). 11 / cm 2 Less than approximately 1 × 10 10 / cm 2 or less than about 2 × 10 10 / cm 2 The capping layer 114 may be implemented using materials such as oxides, nitrides, carbides, borides, arsenides, silicides, phosphides, etc. Alternatively or additionally, the capping layer 114 may contain one or more layers of high-purity semiconductor materials, such as silicon, germanium, etc. Furthermore, such high-purity semiconductor materials may be doped. Alternatively or additionally, the capping layer 114 may contain one or more high-purity metals and / or high-purity transition metal materials, such as, for example, Group 3A, Group 4A, Group 5A metals and / or Group 3B to Group 10B transition metals.
[0088] In some embodiments, the cover layer 114 may be provided with the same cover material on all covered surfaces of the cover layer 112 and / or the substrate 110. In other embodiments, one or more outer surfaces of the cover layer 112 and / or the substrate 110 may be covered with a material different from the material used to cover one or more other outer surfaces of the cover layer 112 and / or the substrate 110. Finally, in some embodiments, one or more outer surfaces of the cover layer 114 may be ground and / or polished.
[0089] Cooling plate 100D can be implemented in a manner similar to cooling plate 100C, employing substrate 110, cladding layer 112, and capping layer 114. However, cooling plate 100D may further include a metal layer 116 that further coats or covers one or more outer surfaces of capping layer 114, cladding layer 112, and / or substrate 110. Generally, metal layer 116 can be implemented in a manner similar to capping layer 114. In some embodiments, metal layer 116 may provide a carbide-forming metal, such as Group 3A and Group 4A metals, and / or transition metals, such as Si, Ge, Cr, Ta, W, Mo, etc. Such carbide-forming metals can effectively provide an adhesion layer for cooling plate 100D, suitable for adhesion to heat-generating devices via reactive bonding or other processes. In other embodiments, metal layer 116 may include one or more metals from Groups IIIA, IVA, VA, and IB to VIIB, such as Ni, Au, Pt, Cu, etc. In such embodiments, the metal layer 116 can provide a metal barrier for the cooling plate 100D.
[0090] In some embodiments, the metal layer 116 may be provided with the same metallic material on all covered surfaces of the capping layer 114, the cladding layer 112, and / or the substrate 110. In other embodiments, one or more outer surfaces of the capping layer 114, the cladding layer 112, and / or the substrate 110 may be covered with a different material than the material used to cover one or more other outer surfaces of the capping layer 114, the cladding layer 112, and / or the substrate 110. Finally, in some embodiments, one or more outer surfaces of the metal layer 116 may be ground and / or polished.
[0091] This disclosure uses a reactive bonding process to produce Si-free diamond-SiC composites, wherein the composites are "Si-free" (e.g., with little or no residual Si phase) and exhibit high thermal conductivity. Conventional reactive-bonded ceramic materials (such as those described above) exhibit poor properties in some applications (such as those exposed to high temperatures, those exposed to corrosion, and / or those requiring ultra-high thermal conductivity), at least in part, due to the presence of residual Si. Therefore, in one embodiment of this disclosure, a preform comprising diamond particles of a specific size is produced, which is reactively infiltrated with molten Si. Diamond and Si react to form SiC (Si + C SiC), which consumes the residual Si from the infiltration process, resulting in a composite with very low (near-zero) residual Si.
[0092] In the fabrication of reactively bonded diamond-SiC composites as described herein, one or more of the following are utilized: RVD (crushed) and MBD (spherical) diamond powders; smaller diamond particle size (i.e., larger surface area for the reaction); particle size blends (higher diamond packing, leaving less volume for the Si / SiC matrix phase); and / or optimized processing time (to maximize the Si + diamond-SiC reaction).
[0093] Si-free versions of diamond-SiC composites (e.g., RB-diamond) will be valuable in many markets that demand attractive cost, large size and complex shape forming capabilities, and properties provided by the diamond / SiC microstructure. Diamond-SiC composites, as described herein, can be used to manufacture a wide variety of parts. Example parts include, but are not limited to, thermal management applications (data center microcoolers, power electronics heat sinks, semiconductor detector chucks, etc.); armor tiles; industrial wear and fire-resistant parts; corrosion applications (semi-focusing and RTP rings, chemical processing parts, mining, etc.); and high-temperature aerospace parts.
[0094] This paper discloses a method for producing RB-diamond ceramics using diamond particles, which have low, ultra-low, or nominally zero residual Si and high or ultra-high thermal conductivity. In some embodiments, at least some of the diamond particles have a high surface area (i.e., fine size) to enhance reactivity. In some embodiments, the diamond particles are a blend of various sizes to enhance particle packing. In other embodiments, the diamond particles are crushed (RVD) rather than rounded (MBD).
[0095] In one embodiment, various methods are used to achieve a high packing density in the preform. In other embodiments, infiltration parameters are used to achieve low residual Si content and minimal thermal degradation of the diamond particles.
[0096] In one embodiment, diamond / SiC components with low, ultra-low, or nominally zero residual Si reactive bonding after processing are produced, wherein the components include, but are not limited to, thermal management components (microcoolers, heat sinks); armor plate components and parts; and / or semiconductor applications (focusing rings, RTP rings, etc.).
[0097] While the invention has been described with reference to certain embodiments, those skilled in the art will understand that various changes and substitutions can be made without departing from the scope of the invention. Furthermore, many modifications can be made to adapt particular situations or materials to the teachings of the invention without departing from the scope of the invention. Therefore, it is intended that the invention be limited to the specific embodiments disclosed, but rather that the invention encompass all embodiments falling within the scope of the appended claims.
Claims
1. A low-phonon scattering substrate, comprising: The composite material comprises silicon carbide reactive bonds between thermally conductive particles; and The composite material described therein has a phonon scattering limit of less than about 40%.
2. The low phonon scattering substrate according to claim 1, wherein the composite material has a phonon scattering limit of less than about 38%.
3. The low phonon scattering substrate according to claim 1, wherein the composite material has a phonon scattering limit of less than about 36%.
4. The low phonon scattering substrate according to claim 1, wherein the composite material has a phonon scattering limit of less than about 34%.
5. The low phonon scattering substrate according to claim 1, wherein the composite material has a phonon scattering limit of less than about 32%.
6. The low phonon scattering substrate of claim 1, wherein the composite material comprises more than about 55% by volume diamond.
7. The low phonon scattering substrate of claim 1, wherein the composite material comprises more than about 60% by volume diamond.
8. The low phonon scattering substrate of claim 1, wherein the composite material comprises more than about 65% by volume diamond.
9. The low phonon scattering substrate of claim 6, wherein the composite material comprises a blend with diamond particle size.
10. The low phonon scattering substrate of claim 9, wherein the diamond particle size blend comprises two different sizes having a ratio of larger particles to smaller particles in the range of about 80-60:20-40.
11. The low phonon scattering substrate of claim 6, wherein the composite material has a thermal conductivity greater than about 600 W / mk.
12. The low phonon scattering substrate according to claim 6, wherein the composite material has a thermal conductivity greater than about 650 W / mk.
13. The low phonon scattering substrate of claim 6, wherein the composite material has a thermal conductivity greater than about 700 W / mk.
14. The low phonon scattering substrate of claim 6, wherein the composite material has a thermal conductivity greater than about 750 W / mk.
15. The low phonon scattering substrate of claim 6, wherein the composite material has a thermal conductivity greater than about 800 W / mk.
16. The low phonon scattering substrate of claim 1, wherein the composite material comprises less than about 3% by volume of diamond.
17. The low phonon scattering substrate of claim 16, wherein the composite material has a thermal conductivity greater than about 250 W / mk.
18. The low phonon scattering substrate of claim 16, wherein the composite material has a thermal conductivity greater than about 270 W / mk.
19. The low phonon scattering substrate of claim 16, wherein the composite material has a thermal conductivity greater than about 290 W / mk.
20. The low phonon scattering substrate of claim 1, wherein the thermally conductive particles comprise boron nitride particles.
21. The low phonon scattering substrate according to claim 1, comprising: Diameter and thickness; and The ratio of the diameter to the thickness is greater than about 3, greater than about 10, greater than about 20, greater than about 50, greater than about 100, or greater than about 150.
22. The low phonon scattering substrate of claim 1, comprising a diameter greater than about 23 mm, greater than about 48 mm, greater than about 98 mm, greater than about 148 mm, greater than about 198 mm, or greater than about 298 mm.
23. The low phonon scattering substrate according to claim 1, comprising a thickness of less than about 2 mm, less than about 1.5 mm, less than about 1.0 mm, and less than about 0.85 mm.
24. A cooling plate, comprising: The low phonon scattering substrate according to claim 1; and A coating layer that covers one or more outer surfaces of the low phonon scattering substrate.
25. The cooling plate of claim 24, comprising a high-purity capping layer covering one or more outer surfaces of the cladding layer and / or the low-phonon scattering substrate.
26. The cooling plate of claim 25, comprising a metal layer covering one or more outer surfaces of the cover layer, the cladding layer, and / or the low phonon scattering substrate.
27. A cooling system for a heat-generating device, the cooling system comprising: The cooling plate according to claim 24, wherein the cooling plate is coupled to the heat-generating device; and A fluid distribution system coupled to the cooling plate.
28. A packaged device, comprising: A signal distribution structure, the signal distribution structure comprising the low phonon scattering substrate according to claim 1; and One or more semiconductor chips, optical devices, and / or electronic devices are mounted to the signal distribution structure.