Improved VPO catalyst in shaped form and its preparation method

By introducing 0.05% to 7.0% ZnO into the VPO catalyst to form a cylindrical shape, the problems of insufficient mechanical strength and catalytic performance of existing catalysts are solved, and higher selectivity and stability are achieved, making it suitable for the oxidation of butane to maleic anhydride.

CN123125043APending Publication Date: 2026-11-17CLARIANT INT LTD
View PDF 16 Cites 0 Cited by

Patent Information

Application Number
CN202580028521.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2024-04-18
Filing Date
2025-04-16
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing VPO catalysts suffer from low catalytic performance, poor selectivity, and insufficient mechanical stability in the process of converting butane to maleic anhydride. In particular, when operating under pore diffusion-limited conditions, the mechanical strength of the molded body is insufficient, leading to high compressor costs and reduced throughput.

Method used

The VPO catalyst containing 0.05 wt% to 7.0 wt% ZnO was used. Transmission infrared spectroscopy analysis showed that the maximum absorption band was between 790 cm⁻¹ and 810 cm⁻¹. The shaped body was cylindrical with a height of 4 mm to 5 mm, an outer diameter of 5 mm to 6 mm, and a central axial opening of 2 mm to 4 mm. Combined with the powder X-ray diffraction peaks under Cu Kα radiation appearing at 31.7° to 36.4°, the mechanical strength and catalytic performance of the catalyst were increased.

Benefits of technology

It improves catalyst selectivity and mechanical strength, reduces wear, and has a lateral compressive strength greater than 15 N. It is suitable for layers or catalyst beds in tube bundle reactors, improving catalytic performance and stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123125043A_ABST
    Figure CN123125043A_ABST
Patent Text Reader

Abstract

This invention relates to a VPO catalyst in shaped form for the oxidation of hydrocarbons with molecular oxygen, particularly for the oxidation of butane to maleic anhydride with molecular oxygen, wherein the VPO catalyst contains 0.05 wt% to 7.0 wt% Zn partially present in the form of ZnO, and has a maximum value at 790 cm⁻¹ in the transmission infrared spectrum. ‑1 Up to 810 cm ‑1 The first absorption band, and may have a maximum value at 820 cm⁻¹. ‑1 Up to 840 cm ‑1 The second absorption band is characterized by the presence of only the first absorption band or the strength of the first absorption band being greater than the strength of the second absorption band, and the shaped body is a cylindrical shaped body having a height of 4 mm to 5 mm, an outer diameter of 5 mm to 6 mm, and a central axial opening with a diameter of 2 mm to 4 mm. The invention also relates to a method for preparing a VPO catalyst according to the invention, comprising the steps of: a) preparing a catalyst precursor containing vanadium hydroxide phosphate, b) shaping the catalyst precursor into a shaped body, and c) activating the shaped body to form a VPO phase, characterized in that, after step a), ZnO is mixed with the catalyst precursor.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] This invention relates to a VPO catalyst in shaped form for the oxidation of hydrocarbons with molecular oxygen, particularly for the oxidation of butane to maleic anhydride with molecular oxygen, wherein the VPO catalyst contains 0.05 wt% to 7.0 wt% Zn partially present in the form of ZnO, and exhibits a maximum value at 790 cm⁻¹ when analyzed by transmission infrared spectroscopy. -1 Up to 810cm -1 The first absorption band, and may show a maximum value at 820 cm⁻¹. -1 Up to 840 cm -1 The second absorbent band is characterized by the presence of only the first absorbent band or the strength of the first absorbent band being greater than the strength of the second absorbent band, and the molded body is a cylindrical molded body having a height of 4 mm to 5 mm, an outer diameter of 5 mm to 6 mm, and a central axial opening with a diameter of 2 mm to 4 mm.

[0002] The present invention also relates to a method for preparing a VPO catalyst according to the present invention, comprising the following steps:

[0003] a) Preparation of catalyst precursors containing vanadium hydrogen oxyphosphate.

[0004] b) The catalyst precursor is shaped into a molded body.

[0005] c) Activate the molded article to form the VPO phase.

[0006] The feature is that, after step a), ZnO is mixed with the catalyst precursor.

[0007] The present invention also relates to the use of solid-state Zn compounds for stabilizing particulate VPO catalysts of the present invention.

[0008] Maleic anhydride is a chemical intermediate of significant economic importance. It is used, for example, in the production of alkyd and polyester resins, either alone or in combination with other acids. Furthermore, it is a versatile intermediate in chemical synthesis, used for the production of γ-butyrolactone, tetrahydrofuran, and 1,4-butanediol, which can themselves be used as solvents or further processed into polymers such as polytetrahydrofuran or polyvinylpyrrolidone.

[0009] Maleic anhydride is typically produced in the gas phase by partial oxidation of n-butane with molecular oxygen or with a gas containing molecular oxygen in the presence of a vanadium-phosphorus oxide catalyst (VPO catalyst) containing vanadium pyrophosphate (VPP). Vanadium pyrophosphate contains vanadium in its pure form with a +4 valence and is particularly suitable for the production of maleic anhydride from unbranched saturated or unsaturated hydrocarbons having at least four carbon atoms. Both fixed-bed and fluidized-bed reactors are used.

[0010] VPO catalysts exhibit only low intrinsic activity in the conversion of n-butane to maleic anhydride. Therefore, large quantities of catalyst are required to achieve sufficient conversion. Furthermore, VPO catalysts are among the most expensive non-precious metal catalysts available, primarily due to the high cost of their raw materials. Therefore, the task is to improve the catalytic performance (activity and selectivity), lifetime, and mechanical stability of such catalysts. It is known from the prior art that the performance of VPO catalysts can be improved by adding foreign elements to the vanadium-phosphorus-oxide phase (VPO phase), for example, by adding molybdenum (Mo promoter or Mo dopant).

[0011] US 5,929,256 discloses the synthesis of an active molybdenum-modified vanadium-phosphorus catalyst for the production of maleic anhydride. In this method, a compound primarily containing pentavalent vanadium is reacted with a compound containing pentavalent phosphorus in an alcoholic medium suitable for reducing vanadium to an oxidation state below 5. In this method, molybdenum is introduced into the reaction product to form a solid molybdenum-modified precursor composition. The alcohol is removed to obtain a dried solid molybdenum-modified precursor composition. A molded article containing the dried solid molybdenum-modified precursor composition is formed. The dried and formed molybdenum-modified precursor composition is activated to convert it into an active catalyst.

[0012] US 5,070,060 discloses an improvement to an oxidation catalyst for the partial oxidation of n-butane containing a mixed oxide of vanadium and phosphorus, zinc and lithium. The improvement includes adding a molybdenum compound modifier, in an amount of about 0.005 to 0.025 / 1 Mo / V, to the catalyst during the reaction of the reduced vanadium compound with concentrated phosphoric acid. The addition of Mo produces a catalyst that is highly stable, represents a more active system, and has a longer lifetime than the unmodified catalyst.

[0013] US 3,980,585 discloses a catalyst complex suitable for converting C4 hydrocarbons to maleic anhydride in the gas phase, comprising vanadium, phosphorus, and copper, and one element selected from Te, Zr, Ni, Ce, W, Pd, Ag, Mn, Cr, Zn, Mo, Re, Sm, La, Hf, Ta, Th, Co, U, and Sn, preferably together with an alkali metal or alkaline earth metal.

[0014] US 4,056,487 discloses a catalyst suitable for the partial oxidation of alkanes to corresponding anhydrides, such as the gas-phase conversion of C4 hydrocarbons to maleic anhydride, comprising components vanadium, phosphorus and oxygen, Nb, Cu, Mo, Ni, Co, and Cr. Compositions containing one or more elements selected from Ce, Nd, Ba, Hf, U, Ru, Re, Li, or Mg are also preferred.

[0015] US 4,515,904 discloses a method for preparing phosphorus-vanadium catalysts and phosphorus-vanadium-co-metal catalysts for the preparation of maleic anhydride from butane, wherein the method comprises: reacting a vanadium compound with a phosphorus halide in an organic ether solvent having about 2 to about 10 carbon atoms at a temperature of about 0 °C to about 200 °C in the presence of water or an aliphatic alcohol having about 1 to about 8 carbon atoms; removing the solvent; and activating the catalyst by adding butane or another hydrocarbon feedstock and a phosphorus compound at a temperature of about 300 °C to about 500 °C.

[0016] US 5,158,923 discloses an improvement to an oxidation catalyst for the partial oxidation of n-butane containing a mixed oxide of vanadium and phosphorus, zinc and lithium. The improvement includes adding a molybdenum compound modifier in an amount of about 0.005 to 0.025 Mo / V to the catalyst during the decomposition and reduction of vanadium compounds by concentrated phosphoric acid. The addition of Mo produces a catalyst that is highly stable, represents a more active system, and has a longer lifetime than the unmodified catalyst.

[0017] US 5,262,548 discloses an improvement to an oxidation catalyst for the partial oxidation of n-butane containing a mixed oxide of vanadium and phosphorus, zinc and lithium. The improvement includes adding a molybdenum compound modifier in an amount of about 0.005 to 0.025 Mo / V to the catalyst during the decomposition and reduction of vanadium compounds by concentrated phosphoric acid. The addition of Mo produces a catalyst that represents a highly stable active system and has a longer lifetime than the unmodified catalyst.

[0018] WO 2013062919 A1 discloses a method for preparing a promoted VPO catalyst, wherein the catalyst comprises a mixed oxide of vanadium and phosphorus, and wherein the catalyst is promoted with at least one selected from niobium, cobalt, iron, zinc, molybdenum, or titanium. The method includes the steps of: (i) preparing a VPO catalyst comprising vanadium pyrophosphate as a major component and containing less than 5% by weight of vanadium phosphate; (ii) contacting the VPO catalyst with a solution comprising a compound as a metal source and containing at least one metal selected from niobium, cobalt, iron, zinc, molybdenum, or titanium to form a metal-impregnated VPO catalyst; and (iii) drying the metal-impregnated VPO catalyst to form a promoted VPO catalyst. In one embodiment, a niobium-activated VPO catalyst is prepared.

[0019] US 6,407,030 B1 discloses a method for preparing a catalyst that can be used to synthesize maleic anhydride by oxidation of saturated and / or unsaturated C4 hydrocarbons. A vanadium (V) compound is reacted with a mixture of phosphonic acid and phosphoric acid in a specific ratio in a solvent mixture containing a structure-forming agent and an entrainer, wherein reaction water is distilled off along with the entrainer, and the resulting precursor is calcined.

[0020] US 4,132,670 A discloses a method for preparing a compound with a molecular weight greater than 10m by reacting orthophosphoric acid with a vanadium(IV) oxide compound. 2 A method for preparing a crystalline vanadium(IV) phosphate composition with an intrinsic surface area of ​​ / g. The vanadium compound is suspended in a suitable organic medium containing hydroxyl groups, such as isobutanol, and contacted with an acid at a temperature of 20 °C to 210 °C until conversion is complete.

[0021] US 4,382,876 discloses a method for preparing a catalyst for oxidizing saturated or unsaturated hydrocarbons in the gas phase to maleic anhydride, comprising the steps of: (a) mixing a vanadium compound containing pentavalent vanadium with orthophosphoric acid in an alcohol selected from monobasic lower aliphatic alcohols having 2 to 8 carbon atoms, optionally in the presence of a combination of a promoter and a reducing agent of H3PO3 and the alcohol, wherein the total amount of H3PO3 and H3PO4 is controlled such that the atomic ratio of P to V is 1.0 to 1.2, and wherein H3PO3 is present in a concentration lower than stoichiometric ratio. The reducing agents are used in quantities sufficient to reduce vanadium to an oxidation state of only 4.2 to 4.4, and wherein the reducing agents are subsequently combined to further reduce vanadium to an oxidation state of 3.9 to 4.0 by heating to distill off any water present as an azeotrope with the alcohol; (b) titanium dioxide obtained by high-temperature cracking of titanium tetrahalide and optional additional promoters Ni, Fe, Li and Mg are added; (c) a catalyst that forms a precipitate in a known manner; and (d) the catalyst is activated in an oxidation reactor in the presence of an air-hydrocarbon stream at a temperature of about 450 °C to 510 °C for about 12 to 72 hours.

[0022] WO 9529006 A1 discloses a method for preparing an oxidation catalyst containing vanadium-phosphorus mixed oxides, comprising: contacting a phosphorus compound with a vanadium compound in an organic solvent, carrying out the process under conditions that allow for the preparation, recovery, and drying of the precursor and the time required to calcine the precursor at a temperature of 350 °C to 550 °C in an atmosphere containing air, steam, or an inert gas or a mixture thereof to obtain an active catalyst, and using the catalyst to prepare maleic anhydride by oxidation of aliphatic hydrocarbons.

[0023] US 5,185,455 discloses an improvement to a method for preparing maleic anhydride, wherein the method involves the catalytic oxidation of n-butane in a tubular reactor over a vanadium-phosphorus oxide fixed-bed catalyst in the presence of trimethyl phosphate. The trimethyl phosphate content in the gas entering the reactor is from about 0.9 N to about 1.1 N, where N is a specified concentration of trimethyl phosphate in ppm, determined by the following relationship: N = 5×C⁴ + 6×(H₂O₂⁻²⁴) + 0.75×-(CONV₂⁻¹ - c) + (SV / (25×P₂⁻¹)) in Where: C4 is the molar percentage of n-butane in the gas entering the reactor; H2O is the molar percentage of water in the gas entering the reactor; CONV = butane conversion percentage in the reactor; SV = gas hourly space velocity at the reactor inlet, converted to one atmosphere and 60 °F; P in = Pressure at reactor inlet (psig); and c = 84 × 0.05 [(SV × C4 ) / P in Regardless of how N is calculated, the trimethyl phosphate content is at least about 1 ppm.

[0024] US 5,280,003 discloses an improvement to an oxidation catalyst for the partial oxidation of n-butane and containing a mixed oxide of vanadium and phosphorus, zinc, lithium, and molybdenum. The improvement includes the preparation of the catalyst, wherein a crystallization step is carried out under static conditions that result in more uniform crystal growth. These static conditions are maintained during crystallization by heating the solvent under reflux.

[0025] US 4,251,390 discloses an improvement to an oxidative catalyst for the partial oxidation of n-butane, the catalyst containing a mixed oxide of vanadium and phosphorus, characterized in that a zinc compound is added to the catalyst in an amount of 0.15 to 0.001 Zn / V during the reaction of the reduced vanadium component with concentrated phosphoric acid. The addition of zinc produces a catalyst that is more easily activated and highly stable to the heat of the reaction system. Small amounts of lithium and silicon compounds also provide additional desired catalytic effects without diminishing the advantages of the zinc compound.

[0026] DE 10 2014 004786 A1 relates to a catalyst containing vanadium-phosphorus oxide and an alkali metal, wherein the alkali metal in the vanadium-phosphorus oxide is 10 to 400 ppm by weight, based on the total weight of the vanadium-phosphorus oxide, and also relates to a method for its preparation, and the use of said catalyst for the gas-phase oxidation of hydrocarbons, particularly for the preparation of maleic anhydride.

[0027] To prepare a VPO catalyst containing a VPP phase, vanadium pentoxide (V₂O₅) was reduced in an organic alcohol solvent in the presence of phosphoric acid using benzyl alcohol as a reducing agent, wherein vanadium hydroxide phosphate (VHP) was formed in addition to benzaldehyde. During this process, a redox reaction (“reduction”) occurs, in which vanadium (V(V)) in the oxidation state of V reacts to form the VHP phase, in which vanadium oxyphosphate species (V₂O₅) are present. 2+ Vanadium exists as an oxide in state IV (V(IV)), as shown below:

[0028]

[0029] In the subsequent activation step, the VHP phase is converted into the vanadium pyrophosphate phase by heat, while water is removed.

[0030]

[0031] When using VPO catalysts to catalytically convert butane to maleic anhydride, a challenge lies in the fact that the process must operate under pore-diffusion-limited conditions. Here, porosity directly impacts the catalytic yield. Therefore, care must be taken to ensure that the pore structure is not adversely affected during molding (e.g., tableting). However, this leads to decreased mechanical stability of the molded body. This stability must be sufficient to allow the tablets to remain intact during the filling process (falling into a reaction tube approximately 6 meters long). Otherwise, smaller fragments will result in excessively high dynamic pressures during the process, leading to high compressor costs or reduced throughput. Therefore, a technical task is to improve the mechanical strength of the molded body without adversely affecting the pore structure. Simultaneously, there is a need for VPO catalysts with improved performance, namely, improved activity, selectivity, and stability.

[0032] Therefore, the object of the present invention is to provide an improved VPO catalyst for the gas-phase oxidation of hydrocarbons, particularly for the production of maleic anhydride, which exhibits higher catalytic performance, particularly improved selectivity, compared with conventionally used catalysts, while also exhibiting significantly improved mechanical strength and greater wear resistance.

[0033] The task is accomplished by a VPO catalyst in the form of a molded prototyping medium, which is used for the oxidation of hydrocarbons with molecular oxygen, particularly for the oxidation of butane to maleic anhydride with molecular oxygen, wherein the VPO catalyst contains 0.05 wt% to 7.0 wt% Zn partially present as ZnO, and exhibits a maximum value at 790 cm⁻¹ when analyzed by transmission infrared spectroscopy. -1 Up to 810 cm -1 The first absorption band, and may show a maximum value at 820 cm⁻¹. -1 Up to 840 cm -1The second absorbent band is characterized in that only the first absorbent band exists or the strength of the first absorbent band is greater than the strength of the second absorbent band, and the molded body is a cylindrical molded body having a height of 4 mm to 5 mm, an outer diameter of 5 mm to 6 mm, and a central axial opening with a diameter of 2 mm to 4 mm.

[0034] The intensity of the absorption band is determined as follows: First, a line is drawn tangent to the spectrum immediately to the left and right of the band in question. Then, starting from the maximum value of the band, a second straight line is drawn along a direction where the wavelength remains constant and absorption decreases. The intersection point of the two lines is determined, where the width of the absorption band is defined as the distance between the maximum value and the intersection point. Preferably, the ratio of the width of the first absorption band to the width of the second absorption band is greater than 1.1, more preferably greater than 2.

[0035] The molded body of the present invention exhibits a lateral compressive strength greater than 15 N or 25 N, preferably 15 N to 200 N or 25 N to 200 N, wherein the lateral compressive strength is measured using a Zwick Z0.5 apparatus according to ASTM D4179 at a constant force rate of 20.0 N / s, wherein 100 pieces are individually placed and measured with their cylindrical axes parallel to the surface of the measuring claw to determine the average breaking force representing the lateral compressive strength.

[0036] When examined by powder X-ray diffraction using Cu Kα radiation, the VPO catalyst of the present invention exhibits peaks at 31.7° to 31.9°, 34.3° to 34.5°, and 36.2° to 36.4°.

[0037] The VPO catalyst of the present invention comprises, is composed of, or is substantially composed of the VPO phase. For example, based on the total weight of the VPO catalyst, the VPO catalyst of the present invention comprises the VPO phase in an amount greater than 70% by weight, preferably greater than 80% by weight, and more preferably greater than 90% by weight. Furthermore, the VPO catalyst may comprise VPP, dopants, and unreacted oxides of the starting material, such as vanadium pentoxide or phosphorus oxide.

[0038] Based on the total weight of the VPO catalyst, the VPO catalyst of the present invention may optionally contain, for example, 0.1% to 1% by weight, preferably 0.4% to 0.7% by weight of Mo.

[0039] The VPO catalyst of the present invention may also contain alkali metals such as Na and K, preferably 80 to 300 ppm of alkali metals. Furthermore, the VPO catalyst of the present invention may also contain carbon, for example in the form of graphite, in an amount of, for example, 3% to 5% by weight based on the total weight of the VPO catalyst. The graphite present may be used, for example, as a tableting aid.

[0040] The VPO catalyst of the present invention comprises ZnO, but may also contain other Zn compounds. In each case, the Zn content, based on the total weight of the catalyst and derived from the presence of ZnO and other possible Zn compounds, must be from 0.05 wt% to 7.0 wt% in the VPO catalyst, preferably from 0.1 wt% to 6.0 wt%, more preferably from 0.2 wt% to 4.0 wt%, and most preferably from 0.7 wt% to 3.0 wt% of Zn.

[0041] In each case, based on the total weight of the VPO catalyst, the VPO catalyst preferably has the following elemental composition:

[0042] - 0.05 wt% to 7 wt% Zn,

[0043] - 0 wt% to 0.7 wt% Mo,

[0044] - 26% to 31% V,

[0045] - 17% to 21% P,

[0046] - 3% to 5% by weight C

[0047] - The balance is oxygen.

[0048] The VPO catalyst according to the invention contains ZnO, and as long as the content of both phases is sufficiently high, the catalyst shows peaks of the ZnO phase in the XRD powder diffraction pattern recorded using Cu-Kα radiation. In particular, sharp peaks were detected at 31.7° to 31.9°, 34.3° to 34.5°, and 36.2° to 36.4°.

[0049] According to the present invention, the presence of ZnO stabilizes the catalyst particles, resulting in higher mechanical strength compared to the strength without ZnO. However, the presence of ZnO also improves the catalytic performance (i.e., activity, selectivity, and stability) of the catalyst particles, particularly enhancing selectivity.

[0050] The VPO catalyst of the present invention exists in the form of a molded body, the shape of which can be varied according to the contact time, flow rate, and pressure drop required during the catalytic reaction. The term "VPO catalyst in molded body form" refers to a molded body produced by a molding step such as tableting. Multiple molded bodies of the present invention form a layer or catalyst bed in a tube-buffered reactor, through which reactants butane, particularly n-butane, and air pass.

[0051] The molded body of the present invention is cylindrical. The cylinder has a height of 4 mm to 5 mm (length along the cylinder axis) and a generally circular base with an outer diameter of 5 mm to 6 mm. The cylinder has a central axial opening, which must have a diameter of 2 mm to 4 mm.

[0052] A central axial opening in a cylinder refers to a channel or cavity in the cylinder that extends from one generally circular base surface to the opposite generally circular base surface, i.e., in the axial direction. The central axial opening serves as a channel extending approximately from the center of the generally circular base surface to the center of the opposite generally circular base surface.

[0053] The molded body according to the invention is in the form of a cylinder with a central axial opening, preferably having a height of 4.5 mm to 4.8 mm, a substantially circular bottom surface with an outer diameter of 5.6 mm to 5.8 mm, and a central axial opening with a diameter of 2.2 mm to 3.5 mm.

[0054] The catalyst of the present invention is characterized by increased wear resistance, i.e., less debris (wear) is shed under friction and mechanical stress compared to conventional catalysts. In particular, the catalyst of the present invention is characterized in that, when wear is measured using an ERWEKATAR 120 apparatus, the molded body contains less than 1.5% by weight, preferably less than 1.0% by weight, and most preferably less than 0.5% by weight of wear based on the total weight of the catalyst, wherein approximately 25 g of the molded body is weighed and the wear measurement is performed at a speed of 25 rpm for 500 revolutions per minute.

[0055] The VPO catalyst or molded body according to the invention has a lateral compressive strength greater than 15 N, preferably from 15 N to 200 N. In particular, the preferred lateral compressive strength of the VPO catalyst or molded body is greater than 30 N to 150 N, and more preferably greater than 35 N to 100 N.

[0056] The VPO catalyst or cylindrical prototyping according to the invention has a lateral compressive strength greater than 15 N, preferably from 15 N to 50 N. Particularly preferred VPO catalysts or prototypings have a lateral compressive strength greater than 30 N to 45 N, more preferably from 35 N to 40 N.

[0057] The present invention also relates to a method for preparing a VPO catalyst according to the present invention, comprising the following steps:

[0058] a) Preparation of catalyst precursors containing vanadium hydrogen oxyphosphate.

[0059] b) The catalyst precursor is shaped into a molded body.

[0060] c) Activate the molded article to form the VPO phase.

[0061] The feature is that, after step a), ZnO is mixed with the catalyst precursor.

[0062] In process step a), a catalyst precursor containing vanadium hydroxide phosphate is prepared in a manner generally known. Typically, in the reaction mixture, during the reduction step, the V(V) compound in solution is reduced using a reducing agent in the presence of the P(V) compound and optionally the Mo compound. For example, the reaction mixture may consist of 45 wt% to 90 wt% solvent, 5 wt% to 15 wt% reducing agent, 5 wt% to 15 wt% V(V) compound, at most 1 wt% Mo compound, and 5 wt% to 25 wt% P(V) compound. More specifically, in each case, based on the total weight of the reaction mixture, for example, 60 wt% to 70 wt% isobutanol, 5 wt% to 15 wt% benzyl alcohol, 5 wt% to 15 wt% vanadium pentoxide, 0.05 wt% to 0.2 wt% (NH4)2Mo2O7, and 10 wt% to 20 wt% phosphoric acid may be provided as the reaction mixture.

[0063] The V(V) compound used as a starting material in the reaction mixture for preparing vanadium hydroxide phosphate is a compound containing vanadium in its oxidation state, preferably V₂O₅. The P(V) compound used as a starting material in the reaction mixture for preparing vanadium hydroxide phosphate is a compound containing phosphorus in its oxidation state, preferably phosphoric acid or a phosphate such as Na₃PO₄. If phosphoric acid (H₃PO₄) is used, the phosphoric acid is preferably anhydrous phosphoric acid (100% phosphoric acid) or phosphoric acid containing only a small amount of water, i.e., a concentration of 98% to 100%, preferably 99% to 100% (this description refers to the weight percentage of pure phosphoric acid relative to the weight of a water-phosphoric acid mixture, as generally given). Alternatively, in preparing the reaction mixture for producing vanadium hydroxide phosphate, phosphoric acid with a concentration greater than 100% can be used, which immediately reacts with any water initially present in the reaction mixture to form a phosphoric acid concentration of 98% to 100%, preferably 99% to 100%, most preferably 100%, such that there is no phosphoric acid concentration greater than 100% in the reaction mixture, while the remaining water in the reaction mixture is no more than 0.2% by weight based on the weight of the reaction mixture.

[0064] Optionally, the Mo compound used as a starting material in the reaction mixture for the preparation of vanadium hydroxide phosphate can be any molybdenum-containing compound, such as molybdenum trioxide, ammonium heptamolybdate ((NH4)6Mo7O 24 (NH4)6Mo7O2*4H2O), ammonium molybdate ((NH4)6Mo7O2*4H2O), metamolybdate, molybdic acid (H2MoO4), and their salts such as (NH4)2MoO4, Na2MoO4, K2MoO4 or (NH4)2Mo2O7.

[0065] The reducing agent present in the reaction mixture for preparing vanadium hydroxide phosphate can be any reducing agent capable of reducing compound V(V) to at least partially generate vanadium hydroxide phosphate. Preferably, the reducing agent is an organic reducing agent, such as ethanol, isobutanol, or aromatic alcohols, particularly benzyl alcohol.

[0066] The solvent present in the reaction mixture for preparing vanadium hydroxide phosphate is preferably an alcohol, more preferably a high-boiling aliphatic alcohol, especially isobutanol, or ethanol or isopropanol.

[0067] The starting material is placed in a suitable reaction vessel for a reduction step to obtain vanadium hydroxide phosphate, the catalyst precursor. The reaction mixture is heated to above room temperature, for example, to 100 °C. Since the reduction is preferably carried out under stirring during a reflux step, the reaction vessel preferably includes a reflux condenser and a device for stirring the reaction mixture. Optionally, the reaction vessel is equipped with a device that allows water generated during reduction to be removed from the reaction mixture, i.e., a water separator, such as a Dean-Stark water separator.

[0068] The reduction to vanadium hydroxide phosphate is preferably carried out under reflux at atmospheric pressure; during this process, the temperature increases according to the boiling point of the solvent used, and preferably only a single reflux step is performed in the method of the present invention. The catalyst precursor preferably contains vanadium hydroxide phosphate as its main phase, or may even consist essentially of the vanadium hydroxide phosphate phase. Molybdenum, which may also be present in the catalyst precursor, may exist as a dopant in the vanadium hydroxide phosphate phase, thus "molybdenum doping" means that molybdenum is either incorporated into the vanadium hydroxide phosphate phase or exists on its surface. However, in addition to the vanadium hydroxide phosphate phase, other vanadium-phosphorus mixed oxides may be formed during the reduction, wherein vanadium has oxidation states IV or even III. The reduction need not be complete, so that some V(V) compounds and P(V) compounds remain in the catalyst precursor. However, the catalyst precursor typically has an average vanadium oxidation state of 3.8 to 4.2.

[0069] Water generated during reduction can be removed from the reaction mixture during the reduction process. Water removal during reduction is carried out physically in the prior art, such as using a water separator, or chemically, using water-binding compounds, such as desiccants or acid anhydrides, such as phosphoric acid with a concentration exceeding 100%. The reaction mixture may, for example, contain acid anhydrides that react with water and bind water; in particular, the reaction mixture may contain phosphoric acid with a concentration exceeding 100%.

[0070] The suspension obtained after the reduction step can be filtered, for example, in an inert gas atmosphere, such as nitrogen or a rare gas. In this case, an inert gas is any gas that does not react with the catalyst precursor under any given filtration conditions but simultaneously displaces oxygen in the air, thereby minimizing the risk of explosion. Filtration is performed in a manner known to those skilled in the art, typically using a filter press, decanter, or suction filter. Filtration produces an uncalcined catalyst precursor that is still wetted by the solvent.

[0071] The catalyst precursor obtained by filtration (from the solid residue of the filter) can then be dried, typically at temperatures above room temperature, such as at up to 150 °C under reduced pressure, vacuum, or an inert gas atmosphere, to obtain a dried catalyst precursor. In this case, an inert gas refers to any gas that does not react with the catalyst precursor under drying conditions but simultaneously displaces oxygen in the air, thereby minimizing the risk of explosion; examples include nitrogen or rare gases. Preferably, the drying process is carried out under reduced pressure or vacuum at 50 °C to 150 °C, more preferably 90 °C to 140 °C.

[0072] Alternatively or optionally, calcination may be performed after the drying step to obtain the catalyst precursor. The calcination is carried out at a higher temperature of 150°C to 350°C, preferably 230°C to 290°C, under an inert gas atmosphere. In this case, the inert gas refers to any gas that does not react with the catalyst precursor under calcination conditions but displaces oxygen from the air, thereby minimizing the risk of explosion; such gases include nitrogen or rare gases.

[0073] Optionally, graphite may be incorporated into the dried catalyst precursor to facilitate shaping in step b). The dried catalyst precursor may also be compacted and / or granulated to obtain a compacted or granulated dried catalyst precursor. In this process, a roller press may be used to compact the precursor into a sheet at a contact pressure of 190 bar, a gap width of 0.60 mm, and a roller speed of 7 rpm, followed by granulation through a 1 mm sieve.

[0074] In step b), the obtained catalyst precursor is shaped into a catalyst prototyping body, which can be done, for example, by tableting. In this process, the particles are pressed into the desired tablet shape and size, for example, using a rotary tablet press.

[0075] In subsequent process step c), the resulting catalyst profile is activated at a temperature above 200 °C. This activation is typically carried out in a gas mixture consisting of air, an inert gas, and water vapor, whereby any gas that does not react with the catalyst profile under given activation conditions can be used as the inert gas; nitrogen or a rare gas is particularly preferred. Alternatively, the activation can also be carried out in a process gas, i.e., in a gas mixture containing air and butane. The activation is carried out at a temperature of 300 °C to 500 °C, preferably 350 °C to 450 °C. After activation, the finished VPO catalyst is obtained as the product of the process. The tableted VPO catalyst typically has a lateral compressive strength higher than 15 N, typically 15 N to 200 N.

[0076] The method for preparing VPO catalyst in shaped form according to the present invention is characterized in that, after process step a), ZnO is added to or mixed with the catalyst precursor. In this process, the ZnO, i.e., zinc(II) oxide, is used as a powdered solid. The addition of ZnO to the catalyst precursor can also be performed using a metering device and a mixer. Typically, sufficient ZnO is added to obtain the catalyst of the present invention. For example, based on the weight of the dried catalyst precursor (excluding ZnO), 0.5 wt% to 7.0 wt%, preferably 1.0 wt% to 5.0 wt%, more preferably 1.5 wt% to 3.5 wt% of solid ZnO can be added.

[0077] The ZnO is added to the catalyst precursor, i.e., after preparation in process step a), for example by a reduction step, but before the formation of the catalyst body in process step c). Preferably, the ZnO is added to a dried catalyst precursor, and particularly preferably to a dried and calcined catalyst precursor.

[0078] In another preferred embodiment, in addition to the ZnO, another solid metal compound, preferably in powder form, is added. Preferably, a solid Mg compound such as MgO is also included in the binder.

[0079] The present invention also relates to the use of ZnO for stabilizing VPO catalysts in the form of molded articles according to the present invention, and the use of ZnO as a binder in VPO catalysts in the form of molded articles according to the present invention.

[0080] The present invention also relates to a method for producing maleic anhydride by catalytic oxidation of n-butane, wherein a feed gas containing oxygen and n-butane is passed through a reaction tube containing a VPO catalyst according to the present invention.

[0081] The VPO catalyst bed in the reaction tube consists of the VPO catalyst or molded body of the present invention, which is added to the reaction tube and stacked on top of each other to form the bed. The reaction tube is preferably part of a plurality of reaction tubes in a tubular reactor, as is known to those skilled in the art for the industrial production of maleic anhydride. During the reaction, the VPO catalyst bed is maintained at a temperature of 300 °C to 420 °C. The feed gas may, for example, contain 0.2 to 10 vol% n-butane and 5 to 50 vol% oxygen, and is subjected to a reaction at a rate of 1100 h⁻¹. -1 Up to 2500 h -1 1300 h preferred -1 up to 2000 h -1 The space velocity passes through the reaction tube.

[0082] Figure 1 : Dimensions of the manufactured molded body

[0083] Figure 2 IR spectra of samples from Examples 1 and 2.

[0084] Figure 3 Catalytic experiments used to determine catalyst activity: Comparison of Example 1 with Examples 3 to 5 of the present invention.

[0085] Figure 4 Catalytic experiments for determining catalyst selectivity: Comparison of Example 1 with Examples 3 to 5 of the present invention.

[0086] Figure 5 Catalytic experiments used to determine catalyst activity: Comparison of Example 1 with Examples 6 to 8 of the present invention.

[0087] Figure 6 Catalytic experiments used to determine catalyst selectivity: Comparison of Example 1 with Examples 6 to 8 of the present invention.

[0088] Figure 7 XRD diffraction patterns of VPO catalysts from Examples 1 and 2.

[0089] The numbers in parentheses in the figure refer to the samples prepared according to the corresponding embodiments. Example

[0090] Example 1 (Comparative)

[0091] Devices used

[0092] A heating mantle is placed on a laboratory lift platform, inside which a 2 L four-necked flask is placed. A crescent-shaped stirrer and a matching stirrer plug are installed in the center opening of the flask; the stirrer is connected to a stirring drive via a stirrer coupling. A thermometer is inserted into the right opening, and a riser tube leading to the reflux condenser is inserted into the left opening. The front center opening is used for adding chemicals; nitrogen purging is then connected at this point. The entire apparatus can also be filled with nitrogen. To do this, nitrogen is first introduced into the apparatus through a gas scrubbing bottle and then discharged from the top of the condenser through another gas scrubbing bottle.

[0093] Preparation of catalyst precursors

[0094] First, 1069.5 g of isobutanol and 156.0 g of benzyl alcohol were added. Then, 150 g of V₂O₅ was added with stirring. After the addition of V₂O₅, 2.52 g of ammonium dimolybdate was added. Subsequently, 232.50 g of phosphoric acid (100%, anhydrous) was added to the suspension, and the mixture was heated under reflux at N₂ for 10 h.

[0095] filter

[0096] After cooling the suspension containing the catalyst precursor as a solid, it is transferred from the four-necked flask to a suction filter and the liquid is removed by suction. The wet filter cake is then pressed dry overnight in a press at 14 to 18 bar.

[0097] Drying / Calcination

[0098] The pressed filter cake was placed into the evaporation flask of a rotary evaporator. Under water-jet vacuum, the filter cake was dried overnight at 110 °C. The powder dried in this manner was then placed in a suitable calcination crucible in a furnace and calcined at 200 °C to 300 °C for 9 hours in a N2 atmosphere.

[0099] Compaction / Tableting

[0100] Prior to compaction / tableting, 5% by weight of graphite was added to the calcined powdered catalyst precursor and mixed uniformly using a drum mixer. The powder was then compacted into tablets using a roller press at a contact pressure of 190 bar, a gap width of 0.60 mm, and a roller speed of 7 rpm, and then granulated through a 1 mm sieve.

[0101] The granules are compressed into the desired tablet shape using a rotary tablet press, which is 5.6 × 5.6 × 2.3 mm [height × outer diameter × inner diameter].

[0102] Activated to pyrophosphate

[0103] Activation for the formation of vanadium pyrophosphate was carried out under controlled conditions in a reaction vessel installed in a programmable furnace. Calcined flakes were uniformly loaded into the reaction vessel and then tightly sealed. The catalyst was then activated under the following conditions: first at above 300 °C for 5 h in a humid air-nitrogen mixture (50% relative humidity), followed by activation at above 400 °C for 9 h.

[0104] Example 2 (Comparative)

[0105] The VPO catalyst was prepared in the same manner as in Example 1, except that 2.0 g of calcined catalyst precursor powder (Example 2) was simultaneously mixed with graphite per 100 g. This produced a calcined precursor powder containing 2.0 wt% ZnO (Example 2).

[0106] The VPO catalysts of Examples 1 and 2 were tested for fracture strength before and after activation. Furthermore, XRD diffraction patterns of the VPO catalysts were generated, and their catalytic selectivity was tested.

[0107] The results showed that adding ZnO after the calcination step did not lead to a systematic increase in the lateral compressive strength (LCS) when measured immediately after tableting. However, surprisingly, this was indeed the case after the subsequent activation step of the VPO catalyst tablets. Here, a systematic and very significant increase in the lateral compressive strength of the particles was observed with the addition of ZnO.

[0108] The VPO catalyst was also characterized by infrared spectral features. Conventional non-inventive VPO catalysts without ZnO showed a 790 cm⁻¹ spectral density in the IR spectrum. -1 Up to 810 cm -1 The maximum value (first absorption band) and 820 cm -1 Up to 840 cm -1 The second maximum value (second absorption band), where the second absorption band is stronger than the first absorption band. Figure 2 Example 1). It has been found that the addition of ZnO also resulted in 790 cm⁻¹ -1 Up to 810 cm -1 The intensity of the first absorption band at 820 cm increases. -1 Up to 840 cm -1 The intensity of the peak (second absorption band) decreases, making the intensity of the first absorption band in the sample stronger than that of the second absorption band, or the intensity of the second absorption band even decreases to a level that is no longer detectable. Figure 2 (Example 2). In the latter case, the VPO catalyst is characterized by exhibiting only a first absorption band.

[0109] Furthermore, it was also shown that the VPO catalyst exhibited the following characteristics, which could be observed by XRD diffraction ( Figure 7 ):

[0110] 31.7 to 31.9° (sharp peak, ZnO)

[0111] 34.3 to 34.5° (sharp peak, ZnO)

[0112] 36.2 to 36.4° (sharp peak, ZnO)

[0113] These characteristics become more pronounced with increasing ZnO content and are well consistent with ZnO (in wurtzite structure or as zincite).

[0114] The wear resistance of the VPO catalyst according to Example 2 was tested after activation, and the result was a wear loss of 2.3% by weight (based on the total weight of the catalyst used in the test).

[0115] Examples 3 to 5 (based on Test 1 according to the present invention)

[0116] The molded articles of the present invention according to Examples 3 to 5 were prepared in the same manner as the VPO catalyst according to Example 2 (i.e., with the addition of 2% by weight of ZnO), but were each molded into different tablet shapes using a rotary tablet press. The dimensions of the molded articles are as follows:

[0117] Example 3: (Outer) diameter 5.6 mm, height 4.5 mm, inner diameter 2.2 mm

[0118] Example 4: (Outer) diameter 5.6 mm, height 4.8 mm, inner diameter 2.8 mm

[0119] Example 5: (Outer) diameter 5.6 mm, height 4.5 mm, inner diameter 3.4 mm

[0120] Examples 6 to 8 (Test 2 according to the present invention)

[0121] The molded articles of the present invention according to Examples 6 to 8 were prepared in the same manner as the VPO catalyst according to Example 2 (i.e., with the addition of 2% by weight ZnO), but were each molded into different tablet shapes using a rotary tablet press. The dimensions of the molded articles are as follows:

[0122] Example 6: (Outer) diameter 5.6 mm, height 4.1 mm, inner diameter 2.2 mm

[0123] Example 7: (Outer) diameter 5.6 mm, height 4.2 mm, inner diameter 2.8 mm

[0124] Example 8: (Outer) diameter 5.6 mm, height 4.1 mm, inner diameter 3.4 mm

[0125] Table 1 shows that, despite the thinner walls of the molded body geometry according to the invention, favorable lateral compressive strength can still be maintained.

[0126] Example 9 (Comparative)

[0127] The molded articles according to the invention described in Example 9 were prepared in the same manner as the VPO catalyst described in Example 1 (i.e., without the addition of ZnO); however, they were each molded into different tablet shapes using a rotary tablet press.

[0128] Example 9: (Outer) diameter 5.6 mm, height 4.2 mm, inner diameter 3.36 mm

[0129] Figures 3 to 6 The results show that improved catalytic performance is achieved by utilizing the geometry of the molded body according to the invention, i.e., having thinner cylindrical walls. Table 1 shows that favorable lateral compressive strength is maintained despite the thinner walls of the molded body geometry according to the invention.

[0130] Table 1

[0131]

[0132] method

[0133] Infrared spectroscopy (IR)

[0134] The catalyst was characterized using infrared transmission spectroscopy (IR). In this method, the intensity (I) of the infrared radiation (I0) after passing through the sample is measured according to the wavelength. The infrared radiation undergoes wavelength-dependent attenuation due to absorption of the IR radiation and the resulting excitation of vibrational modes in the material under study. The spectrum is obtained by plotting the absorption calculated as log(I0 / I) against the wavenumber.

[0135] Measurements were performed using a Nicolet Nexus 470 FTIR spectrometer equipped with a liquid nitrogen-cooled mercury cadmium telluride (MCT) detector, an "IR Source Everglo" as the IR source, and a HeNe laser for frequency calibration. To prepare the samples, flakes of each catalyst were finely ground in a mortar and pressed into thin pellets with a diameter of 11 mm using a manual pellet press with approximately 10 mg of material. These pellets were then placed in a vacuum chamber with a KBr window and positioned in the optical path. The samples were subsequently subjected to temperature and humidity control at 200°C and 10°C. -4 Pretreatment at mbar pressure for 2 h was performed to remove adsorbed water. For measurements, the vacuum chamber containing the sample was cooled to 77 K using liquid nitrogen and then subjected to 10 mbar pressure. -4 At mbar pressure with 2 cm-1 The spectral density was 72 Hz, the aperture was 72 Hz, and the optical speed was 0.64 Hz.

[0136] Determination of the maximum IR absorption value

[0137] The maximum values ​​are 790 cm. -1 Up to 810 cm -1 and 820 cm -1 Up to 840 cm -1 The intensities of the two absorption bands correspond to the absorption intensity of the maximum region of the band relative to the spectral background. To determine the absorption intensity of the maximum region, an initial straight line is established as a linear baseline, tangent to the spectra immediately to the left and right of the band in question, i.e., the spectral background (i.e., the frequency range up to the adjacent absorption band). Next, a line is drawn vertically downwards from the maximum value (S0) of the band, i.e., along a direction where the wavelength remains constant and absorption decreases, and the intersection point (S1) of this line with the linear background is determined. The intensity of the absorption band is defined as the length of the line segment from S0 to S1.

[0138] Fracture strength test

[0139] To measure the fracture strength of the molded specimens, the force required to fracture them was determined using a Zwick Z0.5 machine. Measurements were performed according to standard ASTM D4179. To dry the molded specimens prior to measurement, they were stored in a drying oven at 100°C for at least 3 hours, and subsequent fracture strength measurements were performed at most 1 hour after drying. The instrument was operated at a constant force rate of 20.0 N / s according to ASTM D4179. For each embodiment, 100 pieces were individually placed with their cylindrical axes parallel to the surface of the measuring jaws (referred to as “radial crushing” in ASTM D4179) and measured sequentially. The average value was then determined from the 100 individual values ​​representing the force required to fracture each test specimen, corresponding to the average fracture force of the test specimen. All data regarding lateral crush strength in this application refer to lateral crush strength obtained using the methods described herein.

[0140] Abrasion resistance test

[0141] Wear of the molded body was measured using an ERWEKA TAR120 measuring device. For each embodiment, approximately 25 g of the molded body was weighed and placed into the drum of the testing device, which was then installed. For the abrasion resistance measurement, 500 revolutions were performed at a speed of 25 revolutions per minute. This resulted in a measurement time of 20 minutes. After completion, the drum was automatically emptied into a collection tray placed below it. After separating the worn material from the intact pieces using a sieve, the intact pieces were weighed. The worn material was then determined by the ratio of the difference between the initial weight and the weight of the intact piece after the abrasion test to the initial weight.

[0142] Wear percentage = (Initial weight – Number of intact pieces after wear) / Initial weight * 100%

[0143] All data regarding wear in this application pertain to the method described herein.

[0144] X-ray powder diffraction (XRD)

[0145] The catalyst was characterized using X-ray powder diffraction (XRD). In this process, X-rays diffracted at various angles in the crystalline region of the sample. The diffraction angles were measured or plotted at 2θ. Characteristic peaks varying with the diffraction angle appeared, depending on the present phase. These diffraction patterns were matched with known parameters using a database.

[0146] Measurements were performed using a Bruker AXS D4 Endeavor with Cu-Kα radiation and a LYNXEYE detector. Diffraction patterns were recorded using a fixed divergence aperture of 0.3° in 0.02° steps and 1.5 s exposure times within a 2θ range of 5° to 50°. For the measurements, the sample was finely ground in a mortar and pressed into a sample holder. The diffraction angle was varied by tilting the sample within the instrument. All data regarding XRD peaks in this application refer to XRD peaks obtained using this method.

[0147] To improve the comparability of diffraction patterns, they were each normalized. To do this, the data point with the lowest intensity value was first determined for each diffraction pattern. This value was then subtracted from all intensity values ​​of the corresponding diffraction pattern. Next, the maximum intensity of the (024) peak (2θ value located at 28.4–28.5°) in the corresponding diffraction pattern was measured. Subsequently, all intensity values ​​of the corresponding diffraction pattern were divided by this maximum intensity.

[0148] Catalytic test reaction

[0149] To determine catalyst performance, after complete catalyst preparation (reflux, filtration, vacuum drying, calcination, compaction, tableting, and activation), its catalytic performance was tested in a Bench-Scale reactor in a diluted catalyst bed (a 1:9 mixture of catalyst and ceramic inert rings) with 1.5 mol% butane in air. To determine catalyst activity, butane conversion was plotted against corrected residence time (the ratio of catalyst mass to inlet volumetric flow rate—contact time, as conventional methods cannot be used here, is measured on a diluted catalyst bed). Selectivity for maleic anhydride (MA) was measured at a reaction temperature of 410 °C (salt bath) by varying mass-based GHSV from 1300 L / kg / h to 5500 L / kg / h.

Claims

1. A VPO catalyst in the form of a molded body for oxidizing hydrocarbons with molecular oxygen, particularly for oxidizing butane to maleic anhydride with molecular oxygen, wherein the VPO catalyst contains 0.05 wt% to 7.0 wt% Zn partially present in the form of ZnO, and exhibits a maximum value at 790 cm⁻¹ when analyzed by transmission infrared spectroscopy. -1 Up to 810 cm -1 The first absorption band, and optionally showing a maximum value at 820 cm⁻¹. -1 Up to 840 cm -1 The second absorption band, characterized in that The first absorbent band is present only, or the strength of the first absorbent band is greater than the strength of the second absorbent band, and the molded body is a cylindrical molded body having a height of 4 mm to 5 mm, an outer diameter of 5 mm to 6 mm, and a central axial opening with a diameter of 2 mm to 4 mm.

2. The VPO catalyst according to claim 1, characterized in that, The intensity of the absorption band is determined by the following method: First, a first straight line is drawn so that it is tangent to the spectrum immediately to the left and right of the corresponding band. Then, a second straight line is drawn starting from the maximum value of the band along the direction where the wavelength remains constant and the absorption decreases, and the intersection of the two straight lines is determined. The intensity of the absorption band is defined as the length between the maximum value and the intersection.

3. The VPO catalyst according to claim 1 or 2, characterized in that, The ratio of the intensity of the first absorption band to the intensity of the second absorption band is greater than 1.1, preferably greater than 2.

4. The VPO catalyst according to any one of the preceding claims, characterized in that, In each case, based on the total weight of the VPO catalyst, the VPO catalyst contains 0.1% to 1% Mo, preferably 0.4% to 0.7% Mo.

5. The VPO catalyst according to any one of the preceding claims, characterized in that, Based on the total weight of the VPO catalyst, the VPO catalyst contains 0.1 wt% to 6 wt%, preferably 0.2 wt% to 4 wt%, and more preferably 0.5 wt% to 3.5 wt% of Zn.

6. The VPO catalyst according to any one of the preceding claims, characterized in that, In each case, based on the total weight of the VPO catalyst, the VPO catalyst has the following elemental composition: - 0.5% to 7% by weight of Zn, - 0% to 0.7% by weight of Mo, - 26% to 31% V, - 17% to 21% by weight of P, - 3% to 5% C by weight The rest is oxygen.

7. The VPO catalyst according to any one of the preceding claims, characterized in that, The molded body has a lateral compressive strength greater than 15 N, preferably from 15 N to 200 N, wherein the lateral compressive strength is measured using a Zwick Z0.5 apparatus according to ASTM D4179 at a constant force rate of 20.0 N / s, wherein 100 pieces are individually placed and measured with their cylindrical axes parallel to the surface of the measuring claw to determine the average breaking force representing the lateral compressive strength.

8. The VPO catalyst according to any one of the preceding claims, characterized in that, When detected by powder X-ray diffraction using a Bruker AXS D4 Endeavor with Cu-Kα radiation and a LYNXEYE detector, the VPO catalyst exhibited peaks at 31.7° to 31.9°, 34.3° to 34.5°, and 36.2° to 36.4°, with the diffraction pattern recorded using a fixed divergence aperture of 0.3° in 0.02° steps and 1.5 s exposure time per step within a 2θ range of 5° to 50°.

9. The VPO catalyst according to any one of claims 1 to 8, characterized in that, The molded body has a cylindrical shape, with a height of 4.5 mm to 4.8 mm, a generally circular bottom surface with an outer diameter of 5.6 mm to 5.8 mm, and a central axial opening with a diameter of 2.2 mm to 3.5 mm.

10. The VPO catalyst according to any one of claims 1 to 9, characterized in that, When abrasion is measured using an ERWEKA TAR120 apparatus, the VPO catalyst has abrasion of less than 1.5% by weight, preferably less than 1.0% by weight, based on the total weight of the catalyst, wherein about 25 g of the molded body is weighed and the abrasion is measured at 500 revolutions per minute at a speed of 25 revolutions per minute.

11. A method for preparing a VPO catalyst according to any one of claims 1 to 10, comprising the following steps: a) Preparation of catalyst precursors containing vanadium hydrogen oxyphosphate. b) The catalyst precursor is shaped into a molded body. c) Activate the molded article to form the VPO phase. The feature is that, after step a), ZnO is mixed with the catalyst precursor.

12. The method for preparing a VPO catalyst according to claim 11, characterized in that, The preparation of the catalyst precursor containing vanadium hydroxide phosphate in step a) is carried out by reducing the V(V) compound with an organic reducing agent in the presence of the P(V) compound during a reflux step in an organic solvent at atmospheric pressure.

13. The method for preparing a VPO catalyst according to claim 11 or 12, characterized in that, The catalyst precursor obtained in step a) is filtered in step a1) and dried and / or calcined in step a2) at a temperature not exceeding 300 °C.

14. The method for preparing a VPO catalyst according to claim 13, characterized in that, Step a2) is carried out in two steps. In the first step, the product is dried in a vacuum at a temperature of 90 °C to 140 °C for 1 h to 24 h, and in the second step, it is calcined in nitrogen at a temperature of 230 °C to 290 °C for 1 h to 24 h.

15. The method for preparing a VPO catalyst according to claims 11 to 14, characterized in that, The activation step is carried out in a gas mixture consisting of air, inert gas and water vapor at a temperature of 300 °C to 500 °C, preferably 350 °C to 450 °C, for 1 hour to 24 hours.

16. The method for preparing a VPO catalyst according to any one of claims 11 to 15, characterized in that, After step a), the catalyst precursor is further mixed with a Mg compound, preferably MgO.

17. A method for preparing maleic anhydride by catalytic oxidation of n-butane, wherein a feed gas containing oxygen and n-butane is passed through a reaction tube containing a bed of VPO catalyst according to any one of claims 1 to 10.

18. The method according to claim 17, characterized in that, The VPO catalyst bed in the reaction tube is maintained at a temperature of 300 °C to 420 °C.

19. The method according to any one of claims 17 or 18, characterized in that, The feed gas contains 0.2% to 10% by volume n-butane and 5% to 50% by volume oxygen, and is discharged at 1100 h⁻¹. -1 Up to 2500 h -1 1300 h preferred -1 Up to 1600 h -1 The air velocity passes through the reaction tube.

Citation Information

Patent Citations

  • Alkali metal-modified vanadium phosphorus oxide (VPO) catalyst

    DE102014004786A1

  • Catalyst and process for preparing maleic anhydride from C{HD 4 {B hydrocarbons

    US3980585A

  • Vanadium phosphorus oxygen oxidation catalysts useful for preparing anhydrides from alkanes

    US4056487A

  • Method of preparing vanadium (IV) phosphate composition with high intrinsic surface area

    US4132670A

  • Partial oxidation catalyst

    US4251390A