Manufacturing method of reduced iron briquettes
By mixing low-grade and high-grade reduced iron in the manufacturing of reduced iron briquettes, the density and strength problems of low-grade ore are solved, and high-strength reduced iron briquettes are manufactured, suitable for marine transportation.
Patent Information
- Application Number
- CN202580029046.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2024-04-22
- Filing Date
- 2025-02-03
- Publication Date
- 2026-11-17
AI Technical Summary
Existing technologies for manufacturing reduced iron briquettes using low-grade ore suffer from reduced apparent density and strength, making it difficult to meet the requirements for maritime transport.
By mixing low-grade reduced iron and high-grade reduced iron at a specific mixing volume ratio to form a reduced iron aggregate, and then hot pressing it, the apparent density and strength of the reduced iron briquettes are ensured to meet the standards for marine transportation.
Even using low-grade ore, it is possible to produce reduced iron briquettes with a given apparent density and high strength, meeting the requirements for maritime transport.
Smart Images

Figure CN123125348A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to a method for manufacturing reduced iron blocks (hot-pressed iron blocks) for obtaining reduced iron blocks (hot-pressed iron blocks) by thermoforming. Background Technology
[0002] Hot-briquetted iron (HBI) has attracted considerable attention as a loading material capable of addressing both the challenges of high iron-to-feed ratio operation and CO2 emission reduction. HBI is a molded product manufactured by compressing directly reduced iron (DRI) in a hot state. DRI has a porous structure resulting from the removal of oxygen from the oxides (FexOy) within the material during the reduction reaction. Compared to its unreduced state, DRI has a higher T.Fe ratio and a larger specific surface area, resulting in higher reactivity. When stored in an oxygen atmosphere like atmospheric air, it reacts with oxygen, leading to heating and ignition due to oxidative heat. Therefore, when storing DRI, it is desirable to store it in an inert gas atmosphere (such as nitrogen), presenting storage challenges.
[0003] As a countermeasure to the problem of storing DRI, HBI (High-Performance Injection) can be cited. HBI reduces the specific surface area by compressing the internal pores of the DRI and the gaps between them, thus reducing reactivity and minimizing the risk of overheating and fire, within a hot temperature range that is easier to process than room temperature. Previously, the technology described in Patent Document 1 was known as an HBI manufacturing technique.
[0004] Patent Document 1 discloses a technique for manufacturing HBI with high strength and weather resistance suitable for charging raw materials into a blast furnace by setting the average C (Carbon) content of the surface and center portions to a given value.
[0005] Existing technical documents
[0006] Patent documents
[0007] Patent Document 1: Japanese Patent No. 5059379 Summary of the Invention
[0008] The problem that the invention aims to solve
[0009] However, the technology described in Patent Document 1 is a method for manufacturing HBI that is inexpensive and has high strength and weather resistance, and it limits the average C content of the surface and interior of DRI. On the other hand, there is currently a shortage of high-grade ore, and low-grade ore will be needed in the future, but the technology described in Patent Document 1 does not mention the use of low-grade ore for HBI. When using low-grade ore, there is a risk of a decrease in apparent density and strength due to the increase in gangue content.
[0010] The present invention was made in view of the above circumstances, and its object is to provide a method for manufacturing reduced iron briquettes that can improve apparent density and strength even when using low-grade ore in the hot forming of reduced iron briquettes.
[0011] Methods for solving problems
[0012] The method for manufacturing reduced iron briquettes of the present invention is a method for manufacturing reduced iron briquettes by hot pressing a reduced iron aggregate composed of reduced iron containing iron components. The reduced iron aggregate is a reduced iron aggregate containing high-grade reduced iron from high-grade ore mixed with low-grade reduced iron from low-grade ore at a mixing volume ratio determined according to the apparent density of the reduced iron briquettes.
[0013] It should be noted that, in the manufacturing method of the reduced iron block of the present invention as described above, the following approach can be considered a more preferred solution:
[0014] (1) The lower limit of the mixing volume ratio X of the above-mentioned high-grade reduced iron is determined based on the target apparent density of the above-mentioned reduced iron briquettes (HBI), the porosity of HBI, and the true density of low-grade and high-grade reduced iron, and satisfies the following formula (3).
[0015] X={(100×apparent density of target HBI) / (1-porosity of HBI / 100)-100ρa} / (ρb-ρa)···(3)
[0016] In the formula, ρa is the true density of low-grade reduced iron obtained by reducing low-grade ore, and ρb is the true density of high-grade reduced iron obtained by reducing high-grade ore.
[0017] (2) The above mixing volume ratio X is a value that satisfies the following equation (4).
[0018] X≥(625-100ρa) / (ρb-ρa)···(4);
[0019] (3) The T.Fe of the above-mentioned high-grade reduced iron is above 85 mass%, and the T.Fe of the above-mentioned low-grade reduced iron is less than 85 mass%.
[0020] (4) The above-mentioned reduced iron aggregate is formed by reducing low-grade ore and high-grade ore that have been mixed before being loaded into the reduction equipment based on the following mixing ratio, wherein the mixing ratio is determined by the mixing volume ratio X calculated using the true density of the expected reduced low-grade reduced iron and high-grade reduced iron in a manner that satisfies Equation (4).
[0021] The effects of the invention
[0022] According to the present invention, as a reduced iron aggregate for briquetting, a reduced iron aggregate containing high-grade reduced iron derived from high-grade ore is mixed with low-grade reduced iron derived from low-grade ore at a mixing volume ratio determined according to the target apparent density of the reduced iron briquettes. Thus, even using low-grade ore, reduced iron briquettes with a given apparent density suitable for sea transport and high strength can be obtained. Therefore, the method for manufacturing reduced iron briquettes according to the present invention is extremely useful in the utilization of low-grade ore. Attached Figure Description
[0023] Figure 1 This is a schematic diagram illustrating one embodiment of the apparatus configuration for implementing the method of manufacturing reduced iron briquettes according to the present invention.
[0024] Figure 2 This is a graph showing the experimental results of investigating the apparent density and / or strength of reduced iron briquettes relative to the true density of low-grade reduced iron and the mixed volume ratio of high-grade reduced iron.
[0025] Symbol Explanation
[0026] 1. Restoration equipment
[0027] 2. Hot Reduced Iron (DRI)
[0028] 3. Hopper feeder
[0029] 4 Double pressing rollers
[0030] 5. Reduced Iron Blocks (HBI)
[0031] 6. Crusher Detailed Implementation
[0032] The embodiments of the present invention will now be described in detail. It should be noted that the following embodiments exemplify apparatus and methods for embodying the technical concept of the present invention, and are not intended to limit their configuration to the manner described below. That is, the technical concept of the present invention can be modified in various ways within the scope of the claims.
[0033] <Development Objectives Regarding the Manufacturing Method of the Reduced Iron Block of the Present Invention>
[0034] In the method for manufacturing reduced iron briquettes of the present invention, as a reduced iron aggregate, a reduced iron aggregate containing high-grade reduced iron derived from high-grade ore is used, which is mixed with low-grade reduced iron derived from low-grade ore at a mixing volume ratio determined according to the target apparent density of the reduced iron briquettes. In the reduced iron briquettes as the final product, the mixing volume ratio of high-grade reduced iron to low-grade reduced iron is changed according to the target apparent density to produce a reduced iron aggregate capable of realizing the present invention. In the following description, the sea transport of reduced iron briquettes (HBI) will be described as an embodiment of the target apparent density for the reduced iron briquettes as the final product.
[0035] First, let's clarify the apparent density target to be achieved in HBI. For maritime transport of HBI, there are international regulations (IMSBC: International Maritime Solid Bulk Cargoes Code) requiring an apparent density of 5.0 g / cm³. 3 "The molding temperature is above 650℃." This is one of the important development indicators in establishing HBI technology.
[0036] The relationship between apparent density, true density and porosity of HBI is expressed by the following formula (1). As porosity decreases, apparent density increases.
[0037] HBI apparent density = HBI true density × (1 - HBI porosity / 100) ···(1)
[0038] Low-grade ore contains a large amount of gangue, and the low-grade reduced iron obtained by reducing low-grade ore has a low true density. As will be discussed later, it is impossible to achieve an apparent density of 5.0 g / cm³ when using only low-grade reduced iron. 3 Therefore, the inventors have discovered that by mixing high-grade reduced iron according to the true density of low-grade reduced iron, an apparent density of 5.0 g / cm³ for HBI can be achieved. 3 above.
[0039] <Regarding the mixing volume ratio of high-grade reduced iron>
[0040] When the mixing volume ratio of high-grade reduced iron is set as X (%), the apparent density of HBI is expressed by Equation (2) based on Equation (1). It should be noted that ρa is the true density of low-grade reduced iron obtained by reducing low-grade ore, and ρb is the true density of high-grade reduced iron obtained by reducing high-grade ore.
[0041] The apparent density of HBI is: {ρa×(1-X / 100)+ρb×(X / 100)}×(1-HBI porosity / 100)···(2)
[0042] Furthermore, based on equation (2), the lower limit of the apparent density mixing volume ratio X that can achieve the HBI target is expressed by equation (3).
[0043] X={(100×apparent density of target HBI) / (1-porosity of HBI / 100)-100ρa} / (ρb-ρa)···(3)
[0044] Here, the inventors conducted in-depth research, and as a result, from an operational perspective, the porosity of HBI is expected to be between 15% and 20%. In the case of manufacturing HBI with a porosity of less than 15%, for example, around 10%, it may promote wear and tear on the manufacturing apparatus itself. On the other hand, in the case of manufacturing HBI with a porosity exceeding 20%, for example, when it becomes HBI with a porosity of around 30%, it becomes brittle and easily breaks. Therefore, in this embodiment, in order to achieve the target apparent density, it can be assumed that the porosity is at most 20%, so that the apparent density reaches 5.0 g / cm³. 3 The manufacturing conditions for HBI are determined using the methods described above. Therefore, the following explanation assumes that the porosity of HBI is 20%.
[0045] When the porosity of HBI is set to 20%, an apparent density of 5.0 g / cm³ can be achieved. 3 The above conditions for X are calculated using equation (3), and are expressed as equation (4) below.
[0046] X≥(625-100ρa) / (ρb-ρa)···(4)
[0047] Here, low-grade reduced iron is preferably reduced iron whose T.Fe content is typically less than 85 mass% through reduction. The inventors conducted in-depth research and found that the true density of low-grade reduced iron is approximately 6.20 g / cm³. 3 Therefore, assuming only low-grade reduced iron is used, let X=0 and ρa=6.20 g / cm³. 3 The porosity of HBI is 20%, and its apparent density is 4.96 g / cm³ when calculated using formula (2). 3 The following cannot achieve the 5.0 g / cm³ required for HBI's maritime transport. 3 above.
[0048] Furthermore, the high-grade reduced iron is preferably reduced iron with a T.Fe content of 85% or higher obtained through reduction. The inventors conducted in-depth research and found that the true density of the high-grade reduced iron is approximately 6.30 g / cm³. 3 above.
[0049] Here, we consider a true density ρa of 6.20 g / cm³. 3 The low-grade reduced iron and the true density ρb are 7.00 g / cm³. 3 The case of high-grade reduced iron. When substituting into equation (4) for calculation, if the mixed volume of high-grade reduced iron is set to 6.25% or more, it is possible to produce an apparent density of 5.0 g / cm³. 3 The above refers to HBI. Thus, by mixing high-grade reduced iron with low-grade reduced iron, the apparent density of the manufactured HBI can be increased.
[0050] Furthermore, the strength of the manufactured high-grade reduced iron (HBI) can be improved by mixing high-grade reduced iron with low-grade reduced iron. The solid-bonding of Fe not only compresses the pores within the reduced iron but also facilitates the compression of the reduced iron atoms themselves, which is extremely important for strength improvement. However, the presence of gangue at the iron interface hinders solid-bonding. Therefore, low-grade reduced iron obtained from reducing low-grade ore with abundant gangue tends to impede solid-bonding, resulting in decreased HBI strength. Thus, high-grade reduced iron obtained by mixing with high-grade ore with less gangue can promote solid-bonding and improve the strength of HBI.
[0051] The aforementioned low-grade and high-grade reduced iron can be mixed in multiple ways. In this case, considering the true density of the mixed low-grade reduced iron and its mixing volume ratio, the average true density is calculated, and this value is taken as the true density ρa and ρb of the low-grade or high-grade reduced iron used.
[0052] It should be noted that the higher the proportion of high-grade reduced iron, the greater the apparent density and strength of the resulting HBI. Therefore, there is no specific upper limit, but from a cost perspective, it is preferable to set it below 95%.
[0053] <Methods for calculating true density>
[0054] True density can be determined by analyzing the composition of reduced iron and its proportions. It can be calculated using the following formula (5) based on the proportions of each component and the density of the substance.
[0055] True density [g / cm³] 3 ] = 100 / Σ(composition ratio of component x [mass%] / density of component x [g / cm³] 3 ])···(5)
[0056] Here, component x includes iron, gangue, carbon, and other components.
[0057] <Methods for determining T.Fe content>
[0058] The determination of T.Fe content is performed according to JIS M 8212 "Weight and volume analysis". Alternatively, other specifications / standards may be followed.
[0059] <Methods for determining the apparent density of HBI>
[0060] The apparent density of HBI is determined using the method described in "ISO 15968: Direct reduced iron - Determination of apparent density and water absorption of hot briquetted iron (HBI)". Alternatively, other specifications / standards may be followed.
[0061] <Regarding the manufacturing method and apparatus for the reduced iron briquettes of the present invention>
[0062] Figure 1 This is a schematic diagram illustrating one embodiment of the apparatus configuration for implementing the method of manufacturing reduced iron briquettes according to the present invention. Figure 1 One embodiment of the apparatus of the present invention shown consists of a reduction device 1, a hopper feeder 3, double pressing rollers of the same diameter 4, and a crusher 6.
[0063] The reduction equipment 1 is, for example, equivalent to a rotary hearth furnace or a direct reduction furnace. The hot reduced iron (DRI) 2 is, for example, heated to about 700°C. The hot reduced iron 2 is fed into the hopper feeder 3 as a reduced iron aggregate, and is supplied by being pushed into the double briquetting roller 4 by the rotation of the screw feeder provided by the hopper feeder 3.
[0064] The double-clamping roller 4 consists of a pair of forming rollers of the same diameter, with grooves shaped like the shaped material engraved on the outer surface of the forming rollers. Hot reduced iron 2 is sequentially filled into the grooves, and the forming rollers apply pressure to compress the hot reduced iron 2 through rotation. A continuous supply of raw materials and synchronous rotation of the forming rollers produce an amount of HBI corresponding to the production speed (forming roller rotation speed). Reduced iron briquettes (HBI) 5 are continuously manufactured at the forming roller exit side. The newly formed HBI 5 are not in a state of separate individual units, but rather are formed with the individual units connected to each other. Therefore, they are separated into individual units by a crusher 6. The crusher 6 separates the connected HBI 5 into small and easily handled sizes, such as approximately 100×50×30mm. The separated HBI can be used according to their purpose. For example, they can be fed to blast furnaces, electric furnaces, or melting furnaces via long-distance conveying.
[0065] In this invention, there is no particular limitation on the mixing method of the low-grade and high-grade ores used as raw materials. For example, the low-grade and high-grade ores can be mixed before being loaded into the reduction equipment. In this case, by conducting reduction tests that simulate actual reduction conditions in advance, the true densities of the reduced low-grade and high-grade reduced iron can be predicted. Therefore, using these true densities, the mixing volume ratio X is calculated according to equation (3). The mixing ratio of the low-grade and high-grade ores can be determined in a manner that makes the calculated mixing volume ratio X satisfy equation (4).
[0066] In this case, hot reduced iron 2 (reduced iron aggregate) is formed by reducing low-grade ore and high-grade ore, which have been mixed according to the mixing ratio determined above, before being loaded into the reduction equipment. Alternatively, reduction equipment for high-grade ore and reduction equipment for low-grade ore can be prepared, and the reduced iron discharged from each equipment can be mixed separately between the reduction equipment and the HBI manufacturing machine; the mixing method is not limited. However, in the latter example, the cost of the apparatus increases because both high-grade and low-grade ore reduction equipment are required. From this perspective, the former example is more preferable than the latter.
[0067] Example
[0068] use Figure 1 The apparatus for manufacturing reduced iron briquettes shown continuously operates by mixing low-grade and high-grade reduced iron at an outlet temperature of 700°C from the reduction equipment 1 to obtain a reduced iron aggregate, which is then used as hot reduced iron 2. The gap between the forming rollers of the double briquette rollers 4 is set to 1 mm, the rotation speed of the forming rollers is set to 7 rpm, and the forming pressure is set to 180 kN / cm.
[0069] As hot-state reduced iron 2, low-grade reduced iron was used [true density of 6.19, 6.11, 6.02, 5.93, 5.84, 5.76, 5.67 g / cm³]. 3 [A total of 7 types], high-grade reduced iron [true density 7.00 g / cm³] 3 These low-grade and high-grade reduced iron were mixed in various volumetric mixing ratios to produce HBI.
[0070] The apparent density of HBI was determined using the method described in ISO 15968. The apparent density of HBI was 5.0 g / cm³. 3 The above conditions are considered within the applicable range, and the value is less than 5.0 g / cm³. 3 Cases where the apparent density and compressive strength are both within the applicable range are considered outside the applicable range. The compressive strength was measured using an Amsler testing machine. A load was applied perpendicular to the compression direction of the HBI; cases with a value of 5.0 tonf or higher were considered within the applicable range, while cases with a value less than 5.0 tonf were considered outside the applicable range. Furthermore, cases where both apparent density and compressive strength are within the applicable range are used as examples of the present invention, while cases where both apparent density and compressive strength are outside the applicable range are used as comparative examples. The measurement results are shown in Table 1 below.
[0071] Figure 2 This is a graph showing the experimental results of investigating the apparent density and / or strength of reduced iron briquettes relative to the true density of low-grade reduced iron and the mixed volume ratio of high-grade reduced iron.
[0072] Based on the data in Table 1, the relationship between the mixing volume ratio of high-grade reduced iron and the true density of low-grade reduced iron is shown in the figure regarding apparent density. Furthermore, based on the data in Table 1, the relationship between the mixing volume ratio of high-grade reduced iron and the true density of low-grade reduced iron is shown in the figure regarding compressive strength. The apparent density of HBI is 5.0 g / cm³. 3 The above conditions are marked as "○", and the value is less than 5.0 g / cm³. 3 When the condition is set to "×", and when the condition of HBI compressive strength above 5.0 tonf is set to "○" and the condition of less than 5.0 tonf is set to "×", the following results were obtained: Figure 2 The results are shown.
[0073]
[0074] Based on the measurement results in Table 1, and the data in Table 1... Figure 2 The results show that the present invention, which uses a high-grade reduced iron mixed with low-grade reduced iron in a mixing volume ratio X according to the method satisfying equation (3), can produce an aggregate with an apparent density of 5.0 g / cm³. 3The above and high-intensity HBI.
[0075] It should be noted that in this embodiment, the outlet temperature of the reduction equipment 1 is set to 700℃, the gap between the forming rollers of the double pressing rollers 4 is 1mm, the rotation speed of the forming rollers is 7rpm, and the forming pressure is 180kN / cm. However, the implementation conditions of the present invention are not limited to this embodiment. For example, the present invention can be implemented by appropriately changing the outlet temperature of the reduction equipment 1 to 650~850℃, the gap between the forming rollers of the double pressing rollers 4 to 0.5~5mm, the rotation speed of the forming rollers to 1~12rpm, and the forming pressure to 150~250kN / cm.
Claims
1. A method for manufacturing reduced iron briquettes, comprising hot pressing a reduced iron aggregate containing iron to form briquettes, wherein... As the reduced iron aggregate, a reduced iron aggregate containing high-grade reduced iron derived from high-grade ore is used, with a mixing volume ratio determined according to the apparent density of the reduced iron briquettes, relative to the low-grade reduced iron derived from the reduction of low-grade ore.
2. The method for manufacturing reduced iron briquettes according to claim 1, wherein, The lower limit of the mixing volume ratio X of the high-grade reduced iron is determined based on the target apparent density of the reduced iron briquettes (HBI), the porosity of the HBI, and the true density of the low-grade and high-grade reduced iron, and satisfies the following formula (3). X={(100×apparent density of target HBI) / (1-porosity of HBI / 100)-100ρa} / (ρb-ρa)···(3) In the formula, ρa is the true density of low-grade reduced iron obtained by reducing low-grade ore, and ρb is the true density of high-grade reduced iron obtained by reducing high-grade ore.
3. The method for manufacturing reduced iron briquettes according to claim 2, wherein, The mixing volume ratio X is a value that satisfies the following equation (4). X≥(625-100ρa) / (ρb-ρa)···(4).
4. The method for manufacturing reduced iron briquettes according to claim 3, wherein, The high-grade reduced iron has a T.Fe content of 85 mass% or higher, while the low-grade reduced iron has a T.Fe content of less than 85 mass%.
5. The method for manufacturing reduced iron briquettes according to claim 3 or 4, wherein, The reduced iron aggregate is formed by reducing low-grade and high-grade ore that has been mixed before being loaded into the reduction equipment based on the following mixing ratio, which is determined by the mixing volume ratio X calculated using the true density of the desired reduced low-grade and high-grade reduced iron in a manner that satisfies equation (4).
Citation Information
Patent Citations
JP1975059379A