Surface-treated metal plates for batteries
By controlling the crystal orientation index ratio of the metal substrate and the tin layer, the surface-treated metal plate for batteries formed can effectively suppress hydrogen generation in a high-concentration alkaline electrolyte environment, solving the problem of insufficient durability in the prior art and improving the stability and safety of the battery.
Patent Information
- Application Number
- CN202580027632.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2024-04-18
- Filing Date
- 2025-04-17
- Publication Date
- 2026-11-17
AI Technical Summary
In the presence of high-concentration alkaline electrolytes, the tin-plated metal negative electrode current collector cannot effectively suppress hydrogen generation and has insufficient durability, leading to reduced battery performance and safety hazards.
A surface-treated metal plate for batteries is formed by tin plating, using a combination of a metal substrate and a tin layer, controlling the crystal orientation index ratio of the metal substrate and the tin layer to be above 1.1 and the crystal orientation index of the tin layer to be below 2.95.
In a high-concentration electrolyte environment, hydrogen production is significantly suppressed, battery durability is improved, metal substrate surface is prevented from being exposed, and battery performance stability and safety are ensured.
Smart Images

Figure CN123125701A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to a surface-treated metal plate for batteries that has a gas generation suppression effect and excellent durability. Background Technology
[0002] Nickel-cadmium (NiCd) batteries and nickel-metal hydride (NiMH) batteries, which are types of secondary batteries whose electrolyte is an alkaline aqueous solution, are widely known and have been put into practical use. In addition, among alkaline secondary batteries, air batteries and nickel-zinc batteries (which use nickel hydroxide in the positive electrode, zinc in the negative electrode active material, and an alkaline aqueous solution in the electrolyte) have been extensively studied as next-generation batteries.
[0003] The advantages of nickel-zinc batteries include: as an aqueous battery, they have high electromotive force and high energy density; zinc is inexpensive; they use less rare metals; both nickel and zinc are recyclable metals; and because they use an aqueous electrolyte, they are safer than lithium-ion batteries; etc.
[0004] On the other hand, one of the issues for the practical application of air-zinc batteries and nickel-zinc batteries as secondary batteries is the generation of hydrogen gas (hereinafter also referred to as gas generation) during charging and discharging (including natural discharge). If excessive hydrogen gas is generated, it may cause a decrease in battery performance, an increase in internal pressure, and battery leakage. These problems may be particularly pronounced in batteries in which zinc participates in the battery reaction.
[0005] It is known that the aforementioned hydrogen generation problem can be solved by applying a material with high hydrogen overvoltage to the negative electrode current collector. For example, Patent Document 1 discloses a nickel-zinc battery in which the negative electrode current collector is made of a tin-plated metal material with high hydrogen overvoltage.
[0006] Existing technical documents
[0007] Patent documents
[0008] Patent Document 1: Japanese Patent Application Publication No. 2019-139986 Summary of the Invention
[0009] The problem the invention aims to solve
[0010] However, as described in Patent Document 1, when the concentration of potassium hydroxide in the electrolyte is set to a high concentration of 20% by weight or more in order to achieve full battery performance of the alkaline secondary battery, the technology described in Patent Document 1 has a problem that gas generation cannot always be adequately prevented depending on the state of the tin plating. Furthermore, in the aforementioned high-concentration electrolyte environment, repeated charging and discharging can cause the tin to dissolve, exposing a portion of the tin-plated metal material in the electrolyte, potentially increasing gas generation and resulting in low durability.
[0011] The problem to be solved by the present invention is to provide a surface-treated metal plate for batteries, which has excellent suppression effect on gas generation during the charging and discharging of alkaline secondary batteries and excellent durability in the high-concentration electrolyte environment described above.
[0012] Solution for solving the problem
[0013] In order to achieve the above-mentioned objectives, the inventors conducted in-depth research and found that the above-mentioned objectives can be achieved by using a surface-treated metal plate for batteries that has a metal substrate and a tin layer disposed on at least one side of the metal substrate and controls the crystal orientation index of the metal substrate and the tin layer respectively, thereby completing the present invention.
[0014] [1] According to Embodiment 1 of the present invention, a surface-treated metal plate for a battery is provided, comprising: a metal substrate; and a tin layer disposed on at least one side of the metal substrate, wherein the ratio of the crystal orientation index MI (200) of the (200) side of the metal substrate to the crystal orientation index MI (211) of the (211) side of the metal substrate (MI (200) / MI (211)) is 1.1 or more, and the crystal orientation index Sn (200) of the (200) side of the tin layer is 2.95 or less.
[0015] [2] According to embodiment 2 of the present invention, a surface-treated metal plate for a battery according to embodiment 1 is provided, wherein the aforementioned metal substrate is an iron-based metal substrate.
[0016] [3] According to embodiment 3 of the present invention, a surface-treated metal plate for a battery of embodiment 2 is provided, wherein the aforementioned iron-based metal substrate is a steel plate.
[0017] [4] According to embodiment 4 of the present invention, a surface-treated metal plate for a battery of embodiment 3 is provided, wherein the aforementioned steel plate is low-carbon steel or very low-carbon steel.
[0018] [5] According to embodiment 5 of the present invention, a surface-treated metal plate for a battery is provided according to any one of embodiments 1 to 4, wherein the thickness of the aforementioned metal substrate is 0.01 mm to 1.2 mm.
[0019] [6] According to embodiment 6 of the present invention, a surface metal plate for a battery according to any one of embodiments 1 to 5 is provided, wherein the amount of tin adhering in the aforementioned tin layer is 1.0 g / m 2 Above and 35.0g / m 2 the following.
[0020] [7] According to embodiment 7 of the present invention, a surface-treated metal plate for a battery according to any one of embodiments 1 to 6 is provided, wherein the thickness of the aforementioned tin layer is 0.15 μm or more and 5.00 μm or less.
[0021] [8] According to embodiment 8 of the present invention, the surface-treated metal plate for battery according to any one of embodiments 1 to 7, wherein the ratio of the crystal orientation index Sn(200) of the (200) face of the aforementioned tin layer to the thickness (μm) of the aforementioned tin layer (Sn(200) / thickness (μm) of the tin layer) is 6.00 or less.
[0022] [9] According to embodiment 9 of the present invention, a surface-treated metal plate for a battery is provided according to any one of embodiments 1 to 8, wherein the ratio of the crystal orientation index Sn(200) of the (200) face of the aforementioned tin layer to the thickness (μm) of the aforementioned tin layer (Sn(200) / thickness (μm) of the tin layer) is 3.00 or less.
[0023] The effects of the invention
[0024] According to the present invention, a surface-treated metal plate for batteries with gas generation suppression effect and excellent durability can be provided. Attached Figure Description
[0025] Figure 1 This is a cross-sectional view of a surface-treated metal plate for batteries according to an embodiment of the present invention. Detailed Implementation
[0026] The surface-treated metal plate for batteries of the present invention is a surface-treated metal plate used for battery applications, such as current collectors for negative electrodes, battery tab / lead materials, and battery containers for housing power generation elements of batteries. There are no particular limitations on the type of battery; examples include aqueous batteries such as nickel-cadmium batteries, nickel-metal hydride batteries, zinc-air batteries, and nickel-zinc batteries, as well as non-aqueous batteries such as lithium-ion batteries, which use alkaline electrolytes. However, the surface-treated metal plate for batteries of the present invention is suitable for use in aqueous batteries, and is particularly suitable for use as a current collector and battery container in aqueous batteries (e.g., nickel-zinc batteries) where zinc participates in the battery reaction. It should be noted that the present invention can be applied to either primary or secondary batteries as long as they are aqueous batteries. The surface-treated metal plate for batteries in this embodiment is particularly suitable for use in alkaline secondary batteries where a high concentration of electrolyte environment (e.g., the concentration of potassium hydroxide in the electrolyte is 20% by weight or more) is required.
[0027] Hereinafter, an embodiment of the present invention will be described with reference to the accompanying drawings.
[0028] Figure 1 This is a cross-sectional view of the surface-treated metal plate 10 for batteries according to an embodiment of the present invention. Figure 1 As shown, the surface-treated metal plate 10 for batteries in this embodiment has tin layers 30 disposed on both sides of the metal substrate 20.
[0029] Figure 1 The example illustrates a method of forming tin layers 30 on both sides of the metal substrate 20, but the configuration of the surface-treated metal plate 10 for batteries is not particularly limited to this. In the surface-treated metal plate 10 for batteries, the tin layer 30 only needs to be formed on at least one side of the metal substrate 20. In addition, in this embodiment, the tin layer 30 only needs to be formed on the side where gas generation is required to be suppressed. For example, when the surface-treated metal plate 10 for batteries of this embodiment is used as a current collector for the negative electrode (e.g., as a current collector for the negative electrode of a nickel-zinc battery), a lead material, or a tab material, the tin layer 30 can be formed on both sides of the metal substrate 20. In addition, when the surface-treated metal plate 10 for batteries of this embodiment is used as a battery container such as a container or an electrode canister, the tin layer 30 can be formed on the side of the metal substrate 20 that becomes the inner surface of the battery. There is no particular limitation on the side that becomes the outer surface of the battery; the tin layer 30 can be formed or not formed.
[0030] <Metal Substrate 20>
[0031] In the metal substrate 20, the ratio of the crystal orientation index MI(200) of the (200) facet to the crystal orientation index MI(211) of the (211) facet (MI(200) / MI(211)) is 1.1 or higher. By making the ratio of the crystal orientation index MI(200) of the (200) facet to the crystal orientation index MI(211) of the (211) facet of the metal substrate 20 (MI(200) / MI(211)) 1.1 or higher, the surface-treated metal plate 10 for batteries in this embodiment exhibits excellent durability when used for battery applications. That is, according to the surface-treated metal plate 10 for batteries in this embodiment, gas generation can be suppressed for a long period of time. It should be noted that in this embodiment, in order to further improve durability, the ratio of crystal orientation indices (MI(200) / MI(211)) is preferably 1.3 or higher, and more preferably 1.5 or higher. The upper limit of the ratio of the crystal orientation index of the (200) facet to the crystal orientation index of the (211) facet of the aforementioned metal substrate (MI(200) / MI(211)) is not particularly limited, but is usually below 5.0.
[0032] The crystal orientation index MI(200) of the (200) facet and the crystal orientation index MI(211) of the (211) facet of the metal substrate 20 can be calculated as follows. It should be noted that the following explanation is based on the case where low-carbon steel or very low-carbon steel is used as the metal substrate 20.
[0033] First, the crystal orientation index MI(200) of the (200) plane of the metal substrate 20 can be determined by measuring the diffraction intensity of each crystal plane on the surface of the metal substrate 20 using an X-ray diffraction apparatus with CuKα as the X-ray source, and then by using the obtained diffraction intensity of iron and the diffraction intensity of standard iron powder, it can be calculated using the method of Willson and Rogers (“KSWillson and JARogers; Tech. Proceeding Amer. Electroplaters Soc., 51, 92 (1964)”). It can be calculated based on the following equation (1). It should be noted that the diffraction intensity data used are the data of the (110) plane, (200) plane, and (211) plane that appear in the diffraction angle (2θ) range of 30~90° when the X-ray source is CuKα.
[0034] The crystal orientation index MI(200) of the (200) facet of the metal substrate 20 can be calculated based on the following equation (1).
[0035] MI(200)=IF(200) / IFR(200) (1)
[0036] The IF(200) and IFR(200) in equation (1) above can be calculated based on equations (2) and (3) below, respectively.
[0037] IF(200)=I(200) / [I(110)+I(200)+I(211)] (2)
[0038] IFR(200)=IR(200) / [IR(110)+IR(200)+IR(211)] (3)
[0039] In equation (1) above, IF(hkl) (where h, k, and l are integers) represents the X-ray diffraction intensity ratio from the (hkl) plane, and IFR(hkl) represents the X-ray diffraction intensity ratio from the (hkl) plane of the standard iron powder. In equation (2) above, I(hkl) represents the X-ray diffraction intensity from the (hkl) plane. In equation (3) above, IR(hkl) represents the X-ray diffraction intensity from the (hkl) plane recorded in the ICDD PDF-2 2014 database of the standard iron powder, 03-065-4899. The same applies to equations (4) to (6) below.
[0040] The crystal orientation index MI(211) of the (211) plane of the metal substrate 20 can be calculated based on the following equation (4) using the measurement results of the diffraction intensity of each crystal plane of the surface of the metal substrate 20 obtained by using an X-ray diffraction device.
[0041] MI(211)=IF(211) / IFR(211) (4)
[0042] The IF(211) and IFR(211) in equation (4) above can be calculated based on equations (5) and (6) below, respectively.
[0043] IF(211)=I(211) / [I(110)+I(200)+I(211)] (5)
[0044] IFR(211)=IR(211) / [IR(110)+IR(200)+IR(211)] (6)
[0045] As described above, by calculating the crystal orientation indices MI(200) and MI(211) of the (200) and (211) planes of the metal substrate 20 respectively, the ratio of the crystal orientation index MI(200) of the (200) plane to the crystal orientation index MI(211) of the (211) plane (MI(200) / MI(211)) can be calculated.
[0046] As for the metal substrate 20, as long as the ratio of the crystal orientation index MI(200) of the (200) facet to the crystal orientation index MI(211) of the (211) facet (MI(200) / MI(211)) is 1.1 or higher, the type of metal is not particularly limited. For example, a metal plate based on iron, copper, or nickel is preferred. Specifically, steel plates, copper plates, and nickel plates can be used as the metal substrate 20. Among these, iron is preferred from the viewpoint that it is easy to properly control the crystal orientation index MI(200) of the (200) facet and the crystal orientation index MI(211) of the (211) facet of the metal substrate 20. By setting the metal type to iron, it is easy to control the crystal orientation indices of the (200) facet and the (211) facet, it is possible to appropriately suppress defects generated when forming the tin layer 30 described later, and it is also possible to appropriately control the strength of the metal substrate 20.
[0047] As the metal substrate 20, when it is an iron-based metal substrate, steel plate is preferred. As the steel plate, low-carbon steel (carbon content 0.01~0.15 wt%), ultra-low-carbon steel (carbon content less than 0.01 wt%), and non-aging ultra-low-carbon steel formed by adding Ti, Nb, etc. to ultra-low-carbon steel can be used. Furthermore, as the metal substrate 20, electrolytic foil formed from a pure metal selected from iron, copper, and nickel (electrolytic foil containing 99.9% or more of one of iron, copper, and nickel), and electrolytic foil formed from an alloy containing two or more of iron, copper, and nickel can be used. Additionally, when the surface-treated metal plate 10 for the battery of this embodiment is used as a current collector for the negative electrode, the metal substrate 20 can be a perforated plate or a perforated foil with through holes.
[0048] It should be noted that when using a metal plate based on a metal other than iron, such as copper or nickel, as the metal substrate 20, the crystal orientation index of each facet can be determined by the above method, just as when using a steel plate as the metal substrate 20. For example, when using a nickel plate as the metal substrate 20, the crystal orientation index of each facet can be determined based on the above equations (1) to (6) using the X-ray diffraction intensity data of standard nickel powder and the measurement results of the diffraction intensity of each crystal facet of the surface of the metal substrate 20 obtained by using an X-ray diffraction device.
[0049] The thickness of the metal substrate 20 is not particularly limited, but is preferably 0.005 to 2.0 mm, more preferably 0.01 to 1.0 mm. For example, when used as a current collector, it is preferably 0.01 to 0.3 mm, more preferably 0.01 to 0.2 mm, and particularly preferably 0.01 to 0.1 mm. Furthermore, when used as a battery container or battery tab / lead material, it is preferably 0.1 to 1.2 mm, more preferably 0.1 to 1.0 mm, and particularly preferably 0.15 to 0.5 mm. It should be noted that, as described later, the metal substrate 20 can be prepared by cold rolling a metal sheet, but the thickness of the cold-rolled metal substrate 20 is preferably within the above-mentioned range. The thickness of the metal substrate 20 is preferably measured using cross-sectional observation based on an optical microscope or a scanning electron microscope (SEM). Additionally, as a thickness measurement before surface treatment, i.e. before forming the tin layer 30 described later, a thickness measurement using a micrometer can be applied.
[0050] In the metal substrate 20, the ratio of the crystal orientation index MI(200) of the (200) surface to the crystal orientation index MI(211) of the (211) surface (MI(200) / MI(211)) is at least 1.1.
[0051] <Tin Layer 30>
[0052] like Figure 1 As shown, the surface-treated metal plate 10 for batteries in this embodiment includes a tin layer 30 formed on the surface of a metal substrate 20. The tin layer 30 can be formed by tin plating the metal substrate 20.
[0053] The crystal orientation index Sn(200) of the (200) plane of the tin layer 30, determined by X-ray diffraction, is 2.95 or less, preferably 2.80 or less, more preferably 2.50 or less, and particularly preferably 2.00 or less. The lower limit of the crystal orientation index Sn(200) of the (200) plane of the tin layer 30 is not particularly limited, but is generally 0.01 or more. It should be noted that Sn(200) refers to the crystal orientation index of the (200) plane of the tin layer 30.
[0054] The crystal orientation index Sn(200) of the (200) plane of the tin layer 30 can be obtained in the same way as the method described above for obtaining the crystal orientation index of the metal substrate 20. That is, after measuring the diffraction intensity of each crystal plane of the surface of the tin layer 30 using an X-ray diffraction apparatus with CuKα as the X-ray source, the index can be calculated using the diffraction peaks of the obtained tin and the diffraction peaks of the standard tin powder, by the method of Willson and Rogers. The diffraction intensity data used are those of the (200), (101), (220), (211), (301), (112), (400), (321), (420), (411), (312), and (501) planes that appear in the diffraction angle (2θ) range of 30 to 90° when the X-ray source is CuKα. The crystal orientation index Sn(200) can be calculated using Wilson and Rogers' method based on the following equation (7).
[0055] Sn(200)=IF(200) / IFR(200)…(7)
[0056] In equation (7) above, IF(200) can be obtained by equation (8) below.
[0057] IF(200)=I(200) / [I(200)+I(101)+I(220)+I(211)+I(301)+I(112)+I(400)+I(321)+I(420)+I(411)+I(312)+I(501)]…(8)
[0058] In equation (7) above, IFR(200) can be obtained by equation (9) below.
[0059] IFR(200)=IR(200) / [IR(200)+IR(101)+IR(220)+IR(211)+IR(301)+IR(112)+IR(400)+IR(321)+IR(420)+IR(411)+IR(312)+IR(501)]…(9)
[0060] In equation (7) above, IF(200) represents the X-ray diffraction intensity ratio from the (200) plane; in equation (8) above, I(hkl) represents the X-ray diffraction intensity from the (hkl) plane; and in equation (9) above, IR(hkl) represents the X-ray diffraction intensity from the (hkl) plane as recorded in the ICDDPDF-2 2014 database of standard tin powder, 00-004-0673.
[0061] The preferred tin content in tin layer 30 is 1.0 g / m². 2 The above, more preferably 2.0 g / m 2 The above is further preferred to be 3.0 g / m 2 The above, especially preferred, is 5.0 g / m 2 The above applies. There is no particular limit to the upper limit of the amount of tin adhering to the tin layer 30, but it is preferably 35.0 g / m². 2 The following is more preferably 25.0 g / m 2 The following is a further preferred value of 20.0 g / m 2 The following is particularly preferred: 15.0 g / m 2 The following measures can effectively suppress gas generation during charging and discharging by setting the amount of tin adhering to the tin layer 30 within the above-mentioned range. Specifically, by controlling the amount of tin adhering to the tin layer 30 to 5.0 g / m³... 2 The above range allows for appropriate control of the crystal orientation index Sn(200) of the (200) facet of the tin layer 30. This enables more effective suppression of gas generation and, even in cases where tin dissolves in the electrolyte due to repeated charging and discharging, appropriate control of tin dissolution is achieved. It should be noted that the amount of tin adhered can be determined by performing fluorescence X-ray diffraction and ICP emission spectroscopy analysis on the surface-treated metal plate 10 for the battery. It should be noted that the above-mentioned amount of tin adhered represents the amount adhered to a single surface of the metal substrate 20.
[0062] The thickness of the tin layer 30 is preferably 0.15 μm or more, more preferably 0.30 μm or more, even more preferably 0.50 μm or more, and particularly preferably 1.00 μm or more. The upper limit of the thickness of the tin layer 30 is not particularly limited, but it is preferably 5.00 μm or less, more preferably 3.00 μm or less, even more preferably 2.50 μm or less, and particularly preferably 2.00 μm or less. By setting the thickness of the tin layer 30 within the above range, gas generation during charging and discharging can be effectively suppressed, and durability can be improved. In particular, by setting the thickness of the tin layer 30 to 1.00 μm or more, the gas generation suppression effect and durability can be further improved. On the other hand, if the thickness of the tin layer 30 is below the lower limit of the above range, the crystal orientation index of the tin layer 30 cannot be properly controlled, and there is a tendency for gas generation to become significant. It should be noted that the thickness of the tin layer 30 can be determined based on the density of tin (g / cm³). 3 The thickness of the tin layer 30 is calculated by converting the amount of tin deposited as obtained by the above method into the thickness (tin deposited amount divided by density), but the method for determining the thickness of the tin layer 30 is not limited to this. Other methods for determining the thickness of the tin layer 30 include thickness measurement based on cross-sectional observation using a scanning electron microscope (SEM), thickness measurement based on a transmission electron microscope (TEM), and measurement based on a high-frequency glow discharge emission spectroscopy analysis device.
[0063] It should be noted that, in this embodiment, in order to further improve the gas generation suppression effect, the ratio of the crystal orientation index Sn(200) of the (200) facet of the tin layer to the thickness (μm) of the tin layer (Sn(200) / thickness (μm) of the tin layer) is preferably 6.00 or less. The inventors have found that the thickness of the tin layer 30 is closely related to the crystal orientation index Sn(200) of the tin layer 30 regarding the gas generation suppression effect of the surface-treated metal plate 10 for batteries. That is, the inventors have found that by controlling the gas generation suppression effect to satisfy the above-mentioned range for the crystal orientation index Sn(200) relative to the thickness of the tin layer 30, the gas generation suppression effect can be improved more appropriately. It should be noted that, in order to significantly improve the gas generation suppression effect, the ratio of the crystal orientation index Sn(200) of the (200) facet of the tin layer to the thickness (μm) of the tin layer (Sn(200) / thickness (μm) of the tin layer) is more preferably 4.00 or less, and particularly preferably 3.00 or less. The lower limit of the ratio of the crystal orientation index Sn(200) of the (200) plane of the tin layer to the thickness (μm) of the tin layer (Sn(200) / thickness (μm) of the tin layer) is not particularly limited, but is usually above 0.01.
[0064] In the surface-treated metal plate 10 for batteries in this embodiment, the ratio of the crystal orientation index MI(200) of the (200) facet of the metal substrate 20 to the crystal orientation index MI(211) of the (211) facet of the metal substrate 20 (MI(200) / MI(211)) is 1.1 or more, and the crystal orientation index Sn(200) of the (200) facet of the tin layer 30 is 2.95 or less. The reasons for this preferred configuration are as follows.
[0065] As mentioned above, one of the issues in the practical application of alkaline secondary batteries is the generation of hydrogen gas. Hydrogen gas is generated, for example, under conditions where a chemical reaction (self-discharge) occurs between dissimilar metals within the battery, leading to a localized battery formation, and the reaction conditions for hydrogen generation are met. For instance, in nickel-zinc batteries, zinc is deposited as zinc or zinc oxide during charging and dissolves during discharge. However, zinc is also one of the metals with a low electrical potential used in aqueous batteries, resulting in a high discharge rate when a localized battery state is formed between zinc and other metals used in the battery, easily satisfying the conditions for hydrogen generation.
[0066] Excessive hydrogen production can lead to decreased battery performance and leakage. Specifically, when hydrogen is generated due to self-discharge, electrons that would otherwise contribute to the battery reaction are consumed, resulting in reduced battery performance. Furthermore, the greater the amount of hydrogen produced, the lower the battery performance. Additionally, leakage may occur due to increased internal pressure, reducing safety. It's important to note that self-discharge here includes both side reactions during charging / discharging (including the chemical reactions involved in hydrogen production) and chemical reactions that occur outside of charging / discharging, i.e., under natural storage conditions.
[0067] To avoid such battery performance degradation and leakage problems, it is necessary to suppress hydrogen production as much as possible. In particular, current collector materials are more prone to hydrogen production and self-discharge because zinc and other electrolytes are deposited on their surfaces and come into direct contact with the electrolyte.
[0068] To address this problem, materials with high hydrogen overvoltage are known to be used as one method for suppressing hydrogen generation. In this embodiment, the tin (Sn) in the tin layer can be considered a material with high hydrogen overvoltage. However, the inventors have confirmed that even when using tin with high hydrogen overvoltage, the suppression effect on hydrogen generation varies depending on the crystal orientation state of the tin layer. Furthermore, the inventors have discovered that by controlling the crystal orientation index Sn(200) of the (200) face of the tin layer 30 to 2.95 or less, defects with low local tin adhesion (hereinafter also referred to as poor plating areas) can be suppressed on the surface of the tin layer 30, thereby suppressing gas generation on the surface-treated metal plate 10 for batteries.
[0069] Furthermore, the inventors have discovered that even battery surface-treated metal plates, where the surface of the apparent metal substrate is coated with a tin layer through tin plating, can expose a portion of the metal substrate in a high-concentration electrolyte environment (hereinafter also referred to as the electrolyte) due to surface dissolution of the tin layer caused by repeated charging and discharging, potentially generating gas. The reason for this problem is as follows: Even when there are no apparent defects on the outermost surface of the tin layer, and the metal substrate appears to be sufficiently covered by the tin layer, there are sometimes localized defects with low tin adhesion within the tin layer. When using battery surface-treated metal plates with such defects, repeated long-term charging and discharging promotes tin dissolution due to these defects, exposing the metal substrate to the electrolyte. Therefore, it is believed that when using metals with low hydrogen overvoltage (such as iron, copper, or nickel) as the metal substrate, the corrosion current increases, potentially generating gas.
[0070] To address this problem, the inventors have discovered that by making the ratio of the crystal orientation index MI(200) of the (200) facet of the metal substrate 20 to the crystal orientation index MI(211) of the (211) facet of the metal substrate 20 (MI(200) / MI(211)) 1.1 or higher, gas generation can be suppressed for a long time and excellent durability can be achieved in the surface-treated metal plate 10 for batteries. The reason for this is not yet clear, but it is believed to be as follows. That is, the electrodeposition state of tin on the metal substrate 20 varies depending on the crystal facet of the metal substrate 20. It is believed that by controlling the crystal facet of the metal substrate 20 such that the ratio of the crystal orientation index MI(200) / MI(211) is 1.1 or higher, the uniform electrodeposition during tin plating of the metal substrate 20 (at the initial electrodeposition stage) can be improved, and thus defects in the tin layer 30 can be suppressed. Therefore, it is believed that in the surface-treated metal plate 10 for batteries in this embodiment, even if tin dissolves on the surface of the tin layer 30 due to repeated charging and discharging, the exposure of the metal substrate 20 on the surface can be suppressed, thereby improving the durability of the battery.
[0071] The inventors conducted in-depth research on the material that has the above-mentioned gas generation suppression effect and excellent durability. The results showed that by controlling the gas generation by ensuring that the ratio of the crystal orientation index of the metal substrate 20 (MI(200) / MI(211)) is 1.1 or more and the crystal orientation index Sn(200) of the tin layer 30 is 2.95 or less, the defects in the tin layer 30 are suppressed as a whole, thus suppressing gas generation and achieving excellent durability.
[0072] On the other hand, when the crystal orientation index ratio (MI(200) / MI(211)) of the metal substrate 20 is less than 1.1, or the crystal orientation index Sn(200) of the tin layer 30 exceeds 2.95, defects are formed in the tin layer 30. Therefore, during repeated charge-discharge cycles, these defects promote tin dissolution, exposing a portion of the metal substrate 20 to the electrolyte, thus creating a tendency for gas to be generated during charge-discharge. In particular, the inventors have confirmed that when the crystal orientation index ratio (MI(200) / MI(211)) is less than 1.1, the initial plating amount (especially tin adhesion amount less than 2.0 g / m²) is significantly reduced. 2 The electrodeposition properties of the tin layer 30 become uneven, resulting in more irregularities on the surface of the initial tin layer 30. Since plating tends to concentrate on the protrusions, it is believed that by continuing plating under uneven surface conditions, the uniformity of the plating further deteriorates, and defects with low tin adhesion are locally formed in the tin layer 30.
[0073] <Method for manufacturing surface-treated metal plate 10 for batteries>
[0074] The surface-treated metal plate 10 for batteries in this embodiment can be manufactured by tin-plating both sides of the metal substrate 20 to form a tin layer 30. In this embodiment, a tin layer 30 is formed on both sides of the metal substrate 20, but it is not particularly limited to this method; a tin layer 30 can be formed on at least one side of the metal substrate 20.
[0075] First, a metal substrate 20 is prepared in such a way that the ratio of the crystal orientation index MI(200) of the (200) face of the metal substrate 20 to the crystal orientation index MI(211) of the (211) face of the metal substrate 20 (MI(200) / MI(211)) is 1.1 or higher. The method for preparing such a metal substrate 20 is not particularly limited, and for example, the following methods can be used: a method of cold rolling a metal sheet (method 1); a method of continuously annealing a metal sheet after cold rolling (method 2); a method of continuously annealing a metal sheet after cold rolling and then cold rolling it again (hereinafter also referred to as re-rolling) (method 3). As described above, a metal sheet based on one of iron, copper, and nickel is preferred, an iron-based metal sheet is more preferred, a steel sheet is more preferred, and a steel sheet formed of low-carbon steel or very low-carbon steel is particularly preferred.
[0076] In the first method, the metal substrate 20 is prepared by cold rolling (single-stage cold rolling) a metal sheet. From the viewpoint of easily and appropriately controlling the crystal orientation index of the metal substrate 20, the reduction rate (%) during cold rolling of the metal sheet is preferably 80% or more and 99% or less, more preferably 83% or more and 99% or less, and particularly preferably 85% or more and 95% or less. If the reduction rate exceeds the lower or upper limit mentioned above, it is difficult to control the crystal orientation index of the metal substrate 20, and therefore it is not preferred. It should be noted that the reduction rate (%) refers to the reduction rate (%) of the thickness of the metal sheet before and after cold rolling, which can be obtained by dividing the change in the thickness of the metal sheet before and after cold rolling by the thickness of the metal sheet before cold rolling.
[0077] In the second method, a metal substrate 20 is prepared by cold rolling a metal sheet followed by continuous annealing. The reduction rate (%) of the cold rolling is set to the same conditions as in the first method described above. As for the heat treatment conditions in the continuous annealing, it is preferable to set the heat treatment temperature to 550°C or higher and 850°C or lower, and the heat treatment time to 10 seconds or higher and 5 minutes or lower. By setting the heat treatment conditions as described above, it is easy to appropriately control the ratio of crystal orientation indices (MI(200) / MI(211)) of the metal substrate 20, and the metal substrate can be moderately softened. It should be noted that, in order to further soften the metal substrate 20, it is more preferable to set the heat treatment temperature to 650°C or higher and 850°C or lower, and the heat treatment time to 10 seconds or higher and 5 minutes or lower. It should be noted that as long as the ratio of crystal orientation indices (MI(200) / MI(211)) is in the range of 1.1 or higher, after the above heat treatment, surface finishing rolling with a reduction rate (%) of more than 0% and less than 10% can be performed.
[0078] When the heat treatment temperature exceeds 850°C or the heat treatment time exceeds 5 minutes, it becomes difficult to control the crystal orientation index of the metal substrate 20, and therefore it is not preferred. In particular, heat treatment based on box annealing requires a long heat treatment time, making it extremely difficult to control the crystal orientation index of the metal substrate 20. In addition, the strength of the metal substrate 20 may also be drastically reduced, and therefore it is not preferred.
[0079] In the third method, the metal substrate 20 is prepared by cold rolling the metal sheet, followed by continuous annealing and re-rolling (secondary cold rolling). The conditions for the first cold rolling (single cold rolling) and continuous annealing can be set to be the same as in the first and second methods. The reduction rate (%) in the re-rolling of the metal sheet is preferably 10% or more and 90% or less, more preferably 10% or more and 85% or less, and even more preferably 10% or more and 80% or less. In particular, by setting the reduction rate (%) as described above, it is possible to appropriately control the crystal orientation indices MI (200) and MI (211) while making the thickness of the metal substrate 20 thin, and to improve the strength of the metal substrate 20. Therefore, it is more suitable for the case where the surface-treated metal sheet 10 for batteries is used as a current collector. It should be noted that, in order to further improve the strength of the metal substrate 20, it is more preferable to set the reduction rate (%) to 45% or more and 85% or less, even more preferably to 45% or more and 80% or less, and particularly preferably to 50% or more and 80% or less.
[0080] When the reduction rate (%) in re-rolling exceeds 90%, it is difficult to control the crystal orientation index of the metal substrate 20. Furthermore, there is a tendency for the elongation of the metal substrate 20 to decrease, making it excessively hard. Therefore, depending on the processing conditions used in battery applications, cracks may occur in the surface-treated metal sheet 10 for battery applications, or due to vibration, thermal expansion, etc., during use as a battery component. Therefore, a rolling rate (%) exceeding 90% in re-rolling is not preferable.
[0081] It should be noted that in the third method, after one cold rolling, at least one of continuous annealing or re-rolling can be performed in two or more processes. In this case, it is preferable to alternate between continuous annealing and re-rolling. When performing at least one of continuous annealing or re-rolling in two or more processes, the heat treatment conditions for continuous annealing in the final process of obtaining the metal substrate 20, or the reduction rate (%) conditions for re-rolling, can be the same as those in the second method described above. For example, in the case of continuous annealing in two processes, the heat treatment conditions for continuous annealing in the second process are preferably set to a heat treatment temperature of 550°C or higher and 850°C or lower, and a heat treatment time of 10 seconds or higher and 5 minutes or lower. In addition, in the case of re-rolling in two processes, the conditions for re-rolling (three-stage cold rolling) in the second process are preferably set to 10% or higher and 90% or lower, more preferably 10% or higher and 85% or lower, and even more preferably 10% or higher and 80% or lower. As for the heat treatment conditions in continuous annealing processes other than the final continuous annealing process when two or more continuous annealing processes are performed, there are no particular limitations. It is preferable to set the heat treatment temperature to 550°C or higher and 850°C or lower, and the heat treatment time to 10 seconds or higher and 5 minutes or lower. In addition, when two or more re-rolling processes are performed, the rolling percentage (%) in the re-rolling processes other than the final re-rolling process is preferably 10% or higher and 90% or lower, more preferably 10% or higher and 85% or lower, and even more preferably 10% or higher and 80% or lower.
[0082] Alternatively, as a third method, continuous annealing and re-rolling can be performed in two or more separate processes. In this case, it is preferable to alternate between performing continuous annealing and re-rolling twice. When performing continuous annealing and re-rolling in two or more separate processes, the heat treatment conditions for continuous annealing and the reduction rate (%) conditions for re-rolling in the final process of obtaining the metal substrate 20 are the same as those in the second method described above. For example, as the heat treatment conditions for continuous annealing in the second process, the heat treatment temperature is preferably set to 550°C or higher and 850°C or lower, the heat treatment time is preferably set to 10 seconds or higher and 5 minutes or lower, and the re-rolling (third cold rolling) conditions in the second process are preferably set to 10% or higher and 90% or lower, more preferably 10% or higher and 85% or lower, and even more preferably 10% or higher and 80% or lower. As for the heat treatment conditions in continuous annealing processes other than the final continuous annealing process when two or more continuous annealing processes are performed, there are no particular limitations. It is preferable to set the heat treatment temperature to 550°C or higher and 850°C or lower, and the heat treatment time to 10 seconds or higher and 5 minutes or lower. In addition, when two or more re-rolling processes are performed, the rolling percentage (%) in the re-rolling processes other than the final re-rolling process is preferably 10% or higher and 90% or lower, more preferably 10% or higher and 85% or lower, and even more preferably 10% or higher and 80% or lower.
[0083] As a third method, when obtaining the metal substrate 20 by sequentially performing continuous annealing, re-rolling (secondary cold rolling), continuous annealing, and re-rolling (tertiary cold rolling) after a single cold rolling, each process is preferably performed under the following conditions: The rolling percentage (%) in the first cold rolling is preferably 80% or more and 99% or less, more preferably 83% or more and 99% or less, and even more preferably 85% or more and 95% or less. In the continuous annealing after the first cold rolling, the heat treatment temperature is preferably set to 550°C or more and 850°C or less, and the heat treatment time is preferably 10 seconds or more and 5 minutes or less. The rolling percentage (%) in the re-rolling (secondary cold rolling) is preferably 10% or more and 90% or less, more preferably 20% or more and 80% or less, and even more preferably 30% or more and 60% or less. In the continuous annealing after the secondary cold rolling, the heat treatment temperature is preferably set to 550°C or more and 850°C or less, and the heat treatment time is preferably 10 seconds or more and 5 minutes or less. The rolling rate (%) in the re-rolling (third cold rolling) is preferably 10% or more and 90% or less, more preferably 30% or more and 85% or less, and particularly preferably 50% or more and 80% or less.
[0084] It should be noted that the heat treatment conditions for continuous annealing up to the final process and the reduction rate (%) conditions for re-rolling can be appropriately selected based on the characteristics required for the battery application (e.g., the strength and thickness of the metal substrate 20). For example, if either continuous annealing or re-rolling is performed in two processes, or if continuous annealing and re-rolling are performed separately, the heat treatment conditions for continuous annealing in the first process and the reduction rate (%) conditions for re-rolling (secondary cold rolling) can be adjusted in such a way that the strength and thickness of the final metal substrate 20 are within the preferred range. Preferably, the continuous annealing and re-rolling in the first process can be performed under the same conditions as in the second method described above.
[0085] It should be noted that the methods 1 to 3 above can be selected appropriately based on the characteristics required by the battery application (such as thickness, strength, etc.).
[0086] Next, a tin layer 30 is formed by tin plating on the surface of the metal substrate 20, thereby obtaining a surface-treated metal plate 10 for batteries. As long as the crystal orientation index Sn(200) of the (200) plane of the tin layer 30 is controlled to be 2.95 or less, the method of forming the tin layer 30 is not particularly limited. For example, the following methods can be used: adding additives to the tin plating bath used to form the tin layer 30; or controlling the process by adjusting the current density and processing time of the tin plating.
[0087] As the tin plating bath for forming the tin layer 30, a tin plating bath containing additives can be used, such as a Ferrostan bath, MSA bath, halogen bath, or sulfuric acid bath. Among these, as a sulfuric acid bath, it is preferable that the bath composition, containing 10-60 g / L of tin ions and 25-110 mL / L of sulfuric acid, further contains additives. Furthermore, it is particularly preferable that the bath composition, containing 10-60 g / L of tin ions and 25-60 mL / L of sulfuric acid, further contains the aforementioned additives.
[0088] Examples of additives that can be added to the tin plating bath include ethoxylated naphthol and ethoxylated naphthol sulfonic acid. Commercially available examples include Technistan TP Additive manufactured by Technic Japan Inc. and UTB230R manufactured by ISHIARA CHEMICALCO., LTD. The preferred amount of additive added to the tin plating bath is 5 to 100 mL / L, more preferably 10 to 100 mL / L, and even more preferably 15 to 50 mL / L.
[0089] In the plating conditions for forming the tin layer 30, the preferred current density is 1.0~30.0 A / dm³. 2 More preferably, it is 2.0~15.0 A / dm 2More preferably, it is 4.0~15.0 A / dm 2 Furthermore, the temperature of the plating bath is preferably 25~60°C, more preferably 35~55°C. Additionally, the pH of the plating bath is preferably 1.0 or lower.
[0090] In the plating conditions for forming the tin layer 30, the processing time can be controlled by appropriately selecting the above-mentioned plating conditions and within a range that corresponds to the tin adhesion amount. That is, the tin adhesion amount is preferably 1.0 g / m². 2 The above, and more preferably 2.0 g / m 2 The above, further optimized to 3.0 g / m 2 The above, especially the preferred value, is 5.0 g / m 2 The processing time can be adjusted using the methods described above. Additionally, a tin adhesion amount of 35.0 g / m² is preferred. 2 The following, more preferably, is 25.0 g / m 2 The following is a further optimization to achieve 20.0 g / m 2 The following is a preferred value of 15.0 g / m 2 The processing time can be adjusted as follows. Specifically, the processing time is set based on a tin adhesion amount of 5.0 g / m. 2 The above method of tin plating can appropriately control the crystal orientation index Sn(200) of the (200) face of the tin layer 30, can more effectively suppress gas generation, and can appropriately control the tin dissolved in the electrolyte, and is therefore preferred.
[0091] It should be noted that in the surface-treated metal plate 10 for batteries in this embodiment, as long as the ratio of the crystal orientation index of the metal substrate 20 (MI(200) / MI(211)) and the crystal orientation index Sn(200) of the tin layer 30 are controlled within the above range, heat treatment (e.g., reflow soldering) can be performed after the tin layer 30 is formed on the metal substrate 20.
[0092] Example
[0093] The present invention will be described in more detail below with examples, but the present invention is not limited to these examples.
[0094] It should be noted that the evaluation methods for each characteristic are as follows.
[0095] <X-ray diffraction (XRD) determination (crystal orientation index of metal substrate 20 and tin layer 30)>
[0096] X-ray diffraction (XRD) measurements were performed on the surface-treated metal plate 10 for batteries obtained in each embodiment and comparative example to confirm the crystal orientation index of the metal substrate 20 and the tin layer 30. A SmartLab device manufactured by Rigaku Corporation was used as the X-ray diffraction apparatus. The obtained surface-treated metal plate 10 for batteries was cut into 30mm × 30mm pieces and used as the measurement samples. It should be noted that the specific measurement conditions for the X-ray diffraction (XRD) measurements are as follows.
[0097] (Device Composition)
[0098] X-ray source: CuKα
[0099] • Goniometer radius: 300mm
[0100] Optical system: lumped method
[0101] (Incident-side slit system)
[0102] Soler Slit: 5°
[0103] • Length-limiting slit: 5mm
[0104] • Diverging slit: 1 / 2°
[0105] (Light-receiving side slit system)
[0106] • Scattering slit: 1 / 2°
[0107] Soler Slit: 5°
[0108] • Light-receiving slit: 0.3mm
[0109] Monochromatic method: Counter monochromator method
[0110] • Detector: Blink Counter
[0111] (Measurement parameters)
[0112] • Tube voltage - tube current: 45kV 200mA
[0113] • Scan axis: 2θ / θ
[0114] • Scanning mode: Continuous
[0115] • Measurement range: 2θ 30~90°
[0116] • Scanning speed: 10° / min
[0117] • Step size: 0.05°
[0118] The obtained peak intensity values were analyzed using Rigaku Corporation's comprehensive powder X-ray analysis software PDXL for background removal.
[0119] For the surface-treated metal plate 10 for batteries obtained in each embodiment and comparative example, the diffraction intensity of each crystal plane of iron on the surface of the metal substrate 20 was measured by the above-described X-ray diffraction (XRD) method. Then, using the obtained diffraction intensity of iron and the diffraction intensity of standard iron powder, the crystal orientation indices of the (200) and (211) planes on the surface of the metal substrate 20 were calculated, and the ratio of the crystal orientation indices (MI(200) / MI(211)) was calculated. It should be noted that the diffraction angles of each crystal plane of iron and the diffraction angles of each crystal plane of standard iron powder are the diffraction angles described in 03-065-4899 of the diffraction ICDD PDF-2 2014 database.
[0120] For the surface-treated metal plate 10 for batteries obtained in each embodiment and comparative example, the diffraction intensity of each crystal plane of tin on the surface of the tin layer 30 was measured by the above-described X-ray diffraction (XRD) method. Then, the crystal orientation index of the (200) plane of the surface of the tin layer 30 was determined using the obtained diffraction intensity of tin and the diffraction intensity of standard tin powder. It should be noted that the diffraction angles of each crystal plane of tin and the diffraction angles of each crystal plane of standard tin powder are those described in 00-004-0673 of the diffraction ICDD PDF-2 2014 database.
[0121] <Thickness Measurement of Metal Substrate 20>
[0122] The surface-treated metal plate 10 for batteries obtained in each embodiment and comparative example was cut, and the cross-section was ground. The thickness of the metal substrate 20 was determined from the image obtained using a scanning electron microscope (JEOL Ltd., model: JSM-IT500).
[0123] <Determination of tin adhesion amount and calculation of thickness of tin layer 30>
[0124] The amount of tin deposited in the surface-treated metal plate 10 for batteries obtained in each example and comparative example was quantified using X-ray fluorescence (XRF) measurement and a standard curve method. The X-ray fluorescence apparatus used was a Rigaku Corporation ZSXPrimus IV. In the X-ray fluorescence measurement, it was confirmed that the metal elements contained in the tin layer 30 of the surface-treated metal plate 10 for batteries could be quantified using the standard curve method. It should be noted that the thickness of the tin layer 30 was determined based on the density of tin (g / cm³). 3 The tin adhesion amount obtained by the above method is converted into thickness (tin adhesion amount divided by density) and then calculated.
[0125] <Evaluation of Gas Generation Suppression Based on Corrosion Current Density Measurement>
[0126] For the surface-treated metal plate 10 for batteries obtained in each embodiment and comparative example, the gas suppression effect was evaluated by measuring the corrosion current density when immersed in an alkaline solution. Specifically, as a test simulating a localized battery with zinc deposition, a zinc plate was used as the electrode. The obtained surface-treated metal plate 10 for batteries was immersed in an alkaline solution, and the corrosion current density was measured using an electrochemical measurement system to evaluate the gas suppression effect. The lower the corrosion current density after 30 seconds of immersion in the alkaline solution, the higher the gas suppression effect is considered. The gas suppression effect was evaluated based on the corrosion current density value as follows.
[0127] A+: Corrosion current density 200 μA / cm² 2 the following
[0128] A: Corrosion current density exceeds 200 μA / cm 2 And it is 300 μA / cm 2 the following
[0129] B: Corrosion current density exceeds 300 μA / cm 2 And it is 600 μA / cm 2 the following
[0130] C: Corrosion current density exceeds 600 μA / cm 2
[0131] It should be noted that the corrosion current density measurement was performed under the following conditions, measuring the corrosion current density (unit: μA / cm) generated between the test electrode and the counter electrode in a 30% (w / w) potassium hydroxide solution. 2 ).
[0132] • Measuring device: HZ7000 manufactured by Beidou Electric Co., Ltd.
[0133] • Test electrode: Zinc plate (evaluation area 20×20mm, thickness 0.5mm)
[0134] • Counter electrode: for measuring the sample (diameter φ6mm)
[0135] • Measurement method: Non-resistance galvanometer
[0136] <Defect Evaluation in Tin Layer 30 Based on Salt Spray Test (SST)>
[0137] For the surface-treated metal plate 10 for batteries obtained in each embodiment and comparative example, a test piece with a width of 60 mm and a length of 130 mm was prepared. Next, a salt spray test (SST) was performed according to JIS Z 2371, and the state of rust formation on the surface at the center (30 mm × 30 mm) of the surface-treated metal plate 10 for batteries was visually observed to evaluate the defects in the tin layer 30. The neutral salt spray test was performed under the following conditions.
[0138] • Spray chamber temperature: 35℃±2℃
[0139] • Salt concentration: 50g / L ± 5g / L
[0140] • Test duration: 24 hours
[0141] The smaller the maximum diameter of the rust (in the width direction of the test piece) and the fewer the number of rust spots, the fewer defects with low local tin adhesion in the tin layer 30, indicating excellent durability of the surface-treated metal plate 10 for batteries. The durability of the surface-treated metal plate 10 for batteries is evaluated as follows.
[0142] A: The maximum diameter of the rust is less than 2mm and the number of rust spots is less than 10.
[0143] B: The maximum diameter of the rust is less than 2mm, and the number of rust spots is more than 10 but less than 35.
[0144] C: The maximum diameter of the rust exceeds 2mm, or the number of rust rusts exceeds 35.
[0145] The reasons why the battery surface-treated metal plate 10 can be evaluated as a battery through a salt spray test are as follows. The battery surface-treated metal plate 10 has a tin layer 30 formed on a metal substrate 20. Therefore, even if salt water is sprayed onto it, the salt water will not come into contact with the metal substrate 20, and rust should hardly form on the surface of the battery surface-treated metal plate 10. Through a salt spray test, rust can be visually observed, indicating the presence of defects (poor plating) in the tin layer 30, meaning the metal substrate 20 is partially exposed to the salt water. In a battery surface-treated metal plate 10 with defects in the tin layer 30, if repeated charging and discharging are performed under harsh electrolyte conditions, it is expected that a portion of the metal substrate will be exposed due to these defects, leading to increased gas generation. Based on the above, it can be evaluated that the more rust forms in the salt spray test, the more defects are in the tin layer 30, and the worse the battery durability. Conversely, the less rust forms in the salt spray test, the fewer defects are in the tin layer 30, and the better the battery durability.
[0146] <Example 1>
[0147] First, prepare a substrate of low-carbon aluminum-killed steel with the chemical composition shown below.
[0148] C: 0.04 wt%, Mn: 0.32 wt%, Si: 0.01 wt%, P: 0.012 wt%, S: 0.014 wt%, Balance: Fe and unavoidable impurities.
[0149] Next, the prepared substrate is cold rolled with a reduction rate of 85% to 95%, and then subjected to continuous annealing heat treatment at a heat treatment temperature of 700°C, a soaking time of 60 seconds, and a reducing atmosphere.
[0150] Next, after re-rolling (secondary cold rolling) with a reduction rate of 40%~50%, a heat treatment based on continuous annealing is performed at a heat treatment temperature of 700℃, a soaking time of 30 seconds, and a reducing atmosphere. Then, a third cold rolling is performed with a reduction rate of 60%~70% to obtain metal substrate 20 (thickness 0.06 mm). The rolling and heat treatment conditions are shown in Table 1.
[0151] Next, the obtained metal substrate 20 was subjected to electrolytic degreasing and acid pickling with sulfuric acid immersion, and then tin plating was performed under the following conditions, thereby forming tin layers 30 on both sides of the metal substrate 20. It should be noted that the tin plating conditions were set as described below. Furthermore, the tin plating treatment time was set to a condition where the tin adhesion amount was the amount shown in Table 2, resulting in a surface-treated metal plate 10 for batteries. Then, the obtained surface-treated metal plate 10 for batteries was subjected to the aforementioned measurements. The results are shown in Table 2.
[0152] (Bath composition)
[0153] Stannous sulfate: 80g / L
[0154] Sulfuric acid: 80g / L
[0155] Additive (product name "UTB230R", manufactured by ISHIARA CHEMICAL CO., LTD.): 15 mL / L
[0156] (Plating conditions)
[0157] pH: below 1.0
[0158] Bath temperature: 45℃
[0159] Current density: 5.0 A / dm 2
[0160] <Example 2-4>
[0161] Tin plating was performed under the conditions described in Table 2, and otherwise, a surface-treated metal plate 10 for batteries was obtained in the same manner as in Example 1. The aforementioned measurements were then performed on the obtained surface-treated metal plate 10 for batteries. The results are shown in Table 2.
[0162] <Example 5>
[0163] First, prepare a substrate of very low carbon aluminum killed steel with the chemical composition shown below.
[0164] C: 0.002 wt%, Mn: 0.2 wt%, Si: 0.01 wt%, P: 0.012 wt%, S: 0.014 wt%, Balance: Fe and unavoidable impurities.
[0165] Next, the prepared substrate was cold-rolled with a reduction rate of 85% to 95%, and then subjected to continuous annealing heat treatment at a heat treatment temperature of 700°C, a soaking time of 30 seconds, and a reducing atmosphere. It was then re-rolled (secondary cold rolling) with a reduction rate of 60% to 70% to obtain metal substrate 20 (thickness 0.06 mm). The rolling and heat treatment conditions are shown in Table 1.
[0166] Next, the obtained metal substrate 20 was tin-plated under conditions specified in Table 2, and otherwise, a surface-treated metal plate 10 for batteries was obtained in the same manner as in Example 1. Then, the obtained surface-treated metal plate 10 for batteries was subjected to the aforementioned measurements. The results are shown in Table 2.
[0167] <Example 6>
[0168] Except for changing the thickness of the substrate, a substrate of low-carbon aluminum-killed steel with the same chemical composition as in Example 1 was prepared. This substrate was cold-rolled with a reduction rate of 85% to 95%, and then subjected to continuous annealing heat treatment at a heat treatment temperature of 700°C, a soaking time of 30 seconds, and a reducing atmosphere. It was then re-rolled with a reduction rate of 70% to 80% to obtain metal substrate 20 (thickness 0.04 mm). The rolling conditions and heat treatment conditions are shown in Table 1.
[0169] Next, the obtained metal substrate 20 was subjected to electrolytic degreasing and acid pickling with sulfuric acid immersion, and then tin plating was performed under the following conditions, thereby forming tin layers 30 on both sides of the metal substrate 20. It should be noted that the tin plating conditions were set as described below. Furthermore, the tin plating treatment time was set to a condition where the tin adhesion amount was the amount shown in Table 2, resulting in a surface-treated metal plate 10 for batteries. Then, the obtained surface-treated metal plate 10 for batteries was subjected to the aforementioned measurements. The results are shown in Table 2.
[0170] (Bath composition)
[0171] Tin ions: 20g / L
[0172] Sulfuric acid: 45 mL / L
[0173] Additive (product name "Technistan TP Additive", manufactured by Technic Japan Inc): 25 mL / L
[0174] (Plating conditions)
[0175] pH: below 1.0
[0176] Bath temperature: 45℃
[0177] Current density: 1.0 A / dm 2
[0178] <Example 7-11>
[0179] Tin plating was performed under the conditions described in Table 2, and otherwise, a surface-treated metal plate 10 for batteries was obtained in the same manner as in Example 6. The aforementioned measurements were then performed on the obtained surface-treated metal plate 10 for batteries. The results are shown in Table 2.
[0180] <Examples 12-14>
[0181] The additive in the tin plating bath was changed to "Technistan TPAdditive" manufactured by Technic Japan Inc., and the tin plating conditions were changed as described in Table 2. Otherwise, the surface-treated metal plate 10 for batteries was obtained in the same manner as in Example 5. Then, the surface-treated metal plate 10 for batteries was subjected to the above-described measurements. The results are shown in Table 2.
[0182] <Example 15>
[0183] For a substrate of low-carbon aluminum killed steel prepared in the same manner as in Example 1, cold rolling was performed at a reduction rate of 80% to 90% to obtain metal substrate 20 (thickness 0.30 mm). The rolling conditions are shown in Table 1.
[0184] Next, for the obtained metal substrate 20, the tin plating conditions were changed as described in Table 2, and the surface-treated metal plate 10 for batteries was obtained in the same manner as in Example 6. Then, the obtained surface-treated metal plate 10 for batteries was subjected to the above-described measurements. The results are shown in Table 2.
[0185] <Example 16>
[0186] Tin plating was performed under the conditions described in Table 2, and otherwise, a surface-treated metal plate 10 for batteries was obtained in the same manner as in Example 15. The aforementioned measurements were then performed on the obtained surface-treated metal plate 10 for batteries. The results are shown in Table 2.
[0187] <Example 17>
[0188] For a low-carbon aluminum killed steel substrate prepared in the same manner as in Example 1, after cold rolling with a reduction rate of 80% to 90%, a heat treatment based on continuous annealing was performed under the conditions of heat treatment temperature of 800°C, soaking time of 60 seconds, and reducing atmosphere to obtain metal substrate 20 (thickness 0.35 mm). The rolling conditions and heat treatment conditions are shown in Table 1.
[0189] Next, for the obtained metal substrate 20, the tin plating conditions were changed as described in Table 2, and the surface-treated metal plate 10 for batteries was obtained in the same manner as in Example 6. Then, the obtained surface-treated metal plate 10 for batteries was subjected to the above-described measurements. The results are shown in Table 2.
[0190] <Example 18>
[0191] Tin plating was performed with the conditions specified in Table 2, and otherwise, a surface-treated metal plate 10 for batteries was obtained in the same manner as in Example 17. The aforementioned measurements were then performed on the obtained surface-treated metal plate 10 for batteries. The results are shown in Table 2.
[0192] <Comparative Examples 1-4>
[0193] As described in Table 2, the tin plating conditions were changed, but otherwise, the surface-treated metal plate 10 for batteries was obtained in the same manner as in Example 5. Then, the obtained surface-treated metal plate 10 for batteries was subjected to the aforementioned measurements. The results are shown in Table 2.
[0194] <Comparative Examples 5-7>
[0195] For the low-carbon aluminum killed steel substrate prepared in the same manner as in Example 1, after cold rolling with a reduction rate of 80% to 90%, heat treatment based on continuous annealing is performed under the conditions of heat treatment temperature of 700°C, soaking time of 30 seconds, and reducing atmosphere.
[0196] Next, after re-rolling (secondary cold rolling) with a reduction rate of 40%~50%, a box-type annealing heat treatment was performed at a heat treatment temperature of 600℃, a soaking time of 36000 seconds, and a reducing atmosphere to obtain metal substrate 20 (thickness 0.11mm). The rolling conditions and heat treatment conditions are shown in Table 1.
[0197] Next, the obtained metal substrate 20 was tin-plated under conditions specified in Table 2, and otherwise, a surface-treated metal plate 10 for batteries was obtained in the same manner as in Comparative Example 1. Then, the aforementioned measurements were performed on the obtained surface-treated metal plate 10 for batteries. The results are shown in Table 2.
[0198] <Comparative Examples 8-9>
[0199] For a low-carbon aluminum killed steel substrate prepared in the same manner as in Example 1, after cold rolling with a reduction rate of 80% to 90%, a box-type annealing heat treatment was performed under the conditions of heat treatment temperature of 700°C, soaking time of 54,000 seconds, and reducing atmosphere to obtain metal substrate 20 (thickness 0.30 mm). The rolling conditions and heat treatment conditions are shown in Table 1.
[0200] Next, for the obtained metal substrate 20, the tin plating conditions were changed as described in Table 2, and the surface-treated metal plate 10 for batteries was obtained in the same manner as in Example 6. Then, the obtained surface-treated metal plate 10 for batteries was subjected to the above-described measurements. The results are shown in Table 2.
[0201] <Comparative Example 10>
[0202] As described in Table 2, the tin plating conditions were changed, but otherwise, the surface-treated metal plate 10 for batteries was obtained in the same manner as in Example 6, and the evaluation was performed in the same manner. The results are shown in Table 2.
[0203] [Table 1]
[0204]
[0205] [Table 2]
[0206]
[0207] As shown in Table 1, the surface-treated metal plate 10 for batteries has a crystal orientation index MI(200) of the (200) facet of the metal substrate 20 relative to the crystal orientation index MI(211) of the (211) facet (MI(200) / MI(211)) of 1.1 or more, and a crystal orientation index Sn(200) of the (200) facet of the tin layer 30 of 2.95 or less. This reduces the corrosion current density, effectively suppresses gas generation, and results in less rust generation after the salt spray test. Defects in the tin layer 30 are suppressed, thus it can be judged as a material with excellent battery durability (Examples 1-18).
[0208] More specifically, in Examples 1-18, the ratio of the crystal orientation indices of the metal substrate 20 (MI(200) / MI(211)) is 1.1 or higher, and the crystal orientation index Sn(200) of the tin layer 30 is 2.95 or lower, thus the corrosion current density is 600 μm / cm. 2 The gas generation suppression effect is excellent, and the amount of rust generated after the salt spray test is small, thus confirming that the defects in the tin layer 30 are suppressed.
[0209] Furthermore, in Examples 1-11 and 13-18, the metal substrate 20 and the tin layer 30 satisfy the above-mentioned range of crystal orientation indices, and the ratio of the crystal orientation index Sn(200) of the (200) plane of the tin layer 30 to the thickness (μm) of the tin layer 30 (Sn(200) / thickness (μm) of the tin layer) is 6.00 or less, therefore the corrosion current density becomes 300 μm / cm. 2 The following confirms that the gas generation suppression effect is superior. Furthermore, in Examples 1-11 and 14-18, the ratio of the crystal orientation index Sn(200) of the (200) plane of the tin layer 30 to the thickness (μm) of the tin layer 30 (Sn(200) / thickness (μm) of the tin layer) is 3.00 or less, therefore the corrosion current density is 200 μm / cm. 2 The following confirms that the gas generation suppression effect is more significant and superior.
[0210] Furthermore, in Examples 2-11, 14, 16, and 18, the metal substrate 20 and the tin layer 30 satisfy the aforementioned crystal orientation index range, and the tin adhesion amount in the tin layer 30 is 7.4 g / m². 2 As shown above (the thickness of the tin layer 30 is 1.0 μm or more), it is confirmed that the overall defects in the tin layer 30 are more appropriately suppressed, the gas generation suppression effect is improved, and the battery durability is significantly better.
[0211] On the other hand, in Comparative Examples 1-10, since either the ratio of the crystal orientation index MI(200) of the (200) face of the metal substrate 20 to the crystal orientation index MI(211) of the (211) face (MI(200) / MI(211)) or the crystal orientation index Sn(200) of the (200) face of the tin layer 30 is outside the above range, it is confirmed that the surface-treated metal plate 10 for batteries cannot simultaneously achieve the suppression of gas generation and the durability of the battery.
[0212] More specifically, in Comparative Examples 1-7 and 10, where the crystal orientation index Sn(200) of the (200) facet of the tin layer 30 exceeds 2.95, the corrosion current density is high, gas generation is significant, rust formation is abundant, and battery durability is poor. In contrast, in Comparative Examples 8-9, where the crystal orientation index Sn(200) of the (200) facet of the tin layer 30 is less than 2.95, but the ratio of the crystal orientation indices of the metal substrate 20 (MI(200) / MI(211)) is less than 1.1, the corrosion current density is suppressed to a lower level. However, the tin layer 30 has defects, resulting in abundant rust formation after the salt spray test, leading to poor battery durability.
[0213] Explanation of reference numerals in the attached figures
[0214] 10…Surface-treated metal plates for batteries
[0215] 20…metal substrate
[0216] 30… Tin layer
Claims
1. A surface-treated metal plate for batteries, comprising: Metal substrate; and A tin layer disposed on at least one side of the metal substrate. The ratio of the crystal orientation index MI(200) of the (200) face of the metal substrate to the crystal orientation index MI(211) of the (211) face of the metal substrate, i.e., MI(200) / MI(211), is 1.1 or more. The crystal orientation index Sn(200) of the (200) plane of the tin layer is less than 2.
95.
2. The surface-treated metal plate for batteries according to claim 1, wherein, The metal substrate is an iron-based metal substrate.
3. The surface-treated metal plate for batteries according to claim 2, wherein, The iron-based metal substrate is a steel plate.
4. The surface-treated metal plate for batteries according to claim 3, wherein, The steel plate is low-carbon steel or very low-carbon steel.
5. The surface-treated metal plate for batteries according to any one of claims 1 to 4, wherein, The thickness of the metal substrate is 0.01mm to 1.2mm.
6. The surface-treated metal plate for batteries according to any one of claims 1 to 5, wherein, The tin deposition amount in the tin layer is 1.0 g / m. 2 Above and 35.0g / m 2 the following.
7. The surface-treated metal plate for batteries according to any one of claims 1 to 6, wherein, The thickness of the tin layer is greater than 0.15 μm and less than 5.00 μm.
8. The surface-treated metal plate for batteries according to any one of claims 1 to 7, wherein, The ratio of the crystal orientation index Sn(200) of the (200) plane of the tin layer to the thickness (μm) of the tin layer, i.e., Sn(200) / thickness (μm) of the tin layer, is 6.00 or less.
9. The surface-treated metal plate for batteries according to claim 8, wherein, The ratio of the crystal orientation index Sn(200) of the (200) plane of the tin layer to the thickness (μm) of the tin layer, i.e., Sn(200) / thickness (μm) of the tin layer, is 3.00 or less.
Citation Information
Patent Citations
Negative electrode for zinc battery and zinc battery
JP2019139986A