Vertical smelting device

Through the sealed DC resistance heating and automatic lifting device of the vertical smelting device, combined with the environmentally friendly dust removal device, the problems of high energy consumption and heavy pollution of the boron carbide preparation device are solved, and efficient and environmentally friendly boron carbide product production is achieved to meet the needs of the engineering ceramics field. quality requirements.

CN221802541UActive Publication Date: 2024-10-01ZHENGZHOU UNIV +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202323602120.2
Authority / Receiving Office
CN · China
Patent Type
Utility models(China)
Current Assignee / Owner
Priority Date
2023-07-20
Filing Date
2023-12-28
Publication Date
2024-10-01
Estimated Expiration
2033-12-28

AI Technical Summary

Technical Problem

The existing boron carbide preparation equipment has problems such as uncontrollable smelting temperature and process, high energy consumption, heavy pollution, low product purity and low production efficiency, making it difficult to achieve energy conservation, environmental protection and large-scale production.

Method used

It adopts a vertical smelting device, achieves high temperature treatment through sealed DC resistance heating, and combines an automatic lifting device and an environmentally friendly dust removal device to dynamically adjust the graphite electrode position and raw material heating to avoid oxidation, improve utilization, and achieve continuous production through a bottom unloading device.

Benefits of technology

It achieves fast heating speed, uniform temperature, high product purity, good crystallinity and uniform particle size, reduces energy consumption and pollution, is suitable for large-scale production, and meets the quality requirements in the field of engineering ceramics.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN221802541U_ABST
    Figure CN221802541U_ABST
Patent Text Reader

Abstract

Two exhaust devices communicated with the interior of a furnace body are symmetrically arranged on the side wall of the upper portion of the furnace body, a furnace top sealing cover is arranged on a furnace top of the upper portion of the furnace body, two feeding grooves communicated with the interior of the furnace body are symmetrically arranged on the furnace top sealing cover, and a graphite electrode is inserted in the center of the furnace top sealing cover. A graphite electrode located outside the furnace top sealing cover is connected with an automatic lifting device, the upper end of the graphite electrode is connected with a positive electrode of a power supply device through a first wire, a negative electrode of the power supply device is connected with a bottom valve plate of a discharging device through a second wire, and the discharging device is located outside the bottom of the furnace body and communicated with a discharging port in the bottom of the furnace body. The device has the advantages of simple structure, high temperature rising speed, large-scale production and the like, products prepared by the device are high in purity, good in crystallinity, uniform in granularity and stable and controllable in quality, and the quality requirement of the engineering ceramic field on boron carbide powder is met.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The utility model relates to the field of smelting devices, and specifically provides a vertical smelting device. Background Art

[0002] Boron carbide (B4C), also known as black diamond, has high melting point, high strength, low density, large neutron capture surface, excellent thermal properties, electrical properties and chemical corrosion resistance. It is the hardest material after diamond and cubic boron nitride. Therefore, boron carbide is widely used in various industrial fields such as mechanical grinding, refractory materials, engineering ceramics, nuclear industry and military. The preparation methods of B4C mainly include element direct synthesis method, carbon thermal reduction synthesis method, self-propagating high temperature synthesis method (using magnesium as initiator), chemical vapor deposition method (CVD), sol-gel method, mechanical alloying method and precursor cracking method. At present, the industrial preparation of boron carbide mainly adopts the AC arc furnace carbon thermal reduction method, usually using boric acid or boric anhydride as raw material, carbon as reducing agent, using three-phase AC in the AC arc furnace, and conducting heat transfer through graphite electrodes to carry out high temperature reduction reaction. The chemical reaction equation in the process is:

[0003] 2B2O3+7C=B4C+6CO

[0004] 4H3BO3+7C=B4C+6CO+6H2O

[0005] The AC arc furnace carbon thermal reduction method is used to prepare boron carbide. The equipment required is simple in structure, small in footprint, and fast in construction. However, due to structural deficiencies, the existing equipment has the following disadvantages: 1. The smelting temperature and process are uncontrollable, the heat loss is serious, the temperature difference in the furnace area is large, and the energy consumption is high (the power consumption per ton of boron carbide crystal block is about 27,500~28,500 kwh); 2. The boron carbide smelting process is dusty and polluted, resulting in a poor production environment and low purity of the product; 3. The boron carbide product generated by smelting is taken out from the upper mouth of the furnace body, which takes a long time to be taken out of the furnace and has a large heat loss. Therefore, it is necessary to study and develop a more energy-saving and environmentally friendly preparation device that can produce boron carbide on a large scale.

[0006] At present, there have been some studies on the preparation method of boron carbide, such as "A preparation method of ultrafine boron carbide powder" (CN107758670A). The boron source and the carbon source are mixed to obtain the smelting raw material, the raw material is placed in the smelting furnace, and a voltage is applied at 1500~1900℃ for 24~48 h to obtain ultrafine boron carbide powder. Although it has its advantages, the process energy consumption is high; "A boron carbide smelting device and a method for preparing boron carbide" (CN107954718A) proposes a new boron carbide smelting device, which can prepare boron carbide through a nearly closed high-temperature treatment method, reducing the pollution of impurity elements, and the product has good crystallinity and high purity, but it mainly adopts arc smelting, and the process energy consumption and production cost are high; "A method for preparing boron carbide fine powder" (CN114105144A) mixes boric acid, graphite powder, deionized water and dispersant in a reactor, and then obtains boron carbide fine powder after two heat treatments. Although it has its advantages, the preparation process is complicated, the production efficiency is low, and it cannot be mass-produced; "A method for producing boron carbide crystal blocks in a resistance furnace" (CN106747452A) adds water to boric acid and a carbon reducing agent to press them into pellets, and then puts them into a resistance furnace for heating to 1900~2500℃, smelting for 20~48 h later, boron carbide ingots are obtained. Although this process has its advantages, the smelting temperature is high, the time is long, and the energy consumption of the process is still high. Utility Model Content

[0007] In order to solve the problems existing in the current boron carbide preparation device, the utility model proposes a vertical smelting device.

[0008] To achieve the above-mentioned purpose, the utility model provides the following technical solutions: a vertical smelting device, comprising a furnace body, a discharge device, a power supply device and a graphite electrode, wherein two exhaust devices connected to the interior of the furnace body are symmetrically mounted on the upper side wall of the furnace body, a furnace top closing cover is mounted on the furnace top of the furnace body, two feeding troughs connected to the interior of the furnace body are symmetrically mounted on the furnace top closing cover, a graphite electrode is inserted in the center of the furnace top closing cover, the graphite electrode located outside the furnace top closing cover is connected to the automatic lifting device, the upper end of the graphite electrode is connected to the positive electrode of the power supply device via a first wire, the negative electrode of the power supply device is connected to the bottom valve plate of the discharge device via a second wire, and the discharge device is located outside the bottom of the furnace body and is connected to the discharge port at the bottom of the furnace body.

[0009] Preferably, the automatic lifting device is of gear transmission type or hydraulic transmission type, including a support, a lifting drive, a lifting guide rail and a connecting rod. The support is equipped with a vertical lifting guide rail, and the lifting drive is mounted on the lifting guide rail. The lifting drive is connected to one end of a horizontal connecting rod, and the other end of the connecting rod is connected to the graphite electrode.

[0010] Preferably, the unloading device comprises a bottom valve plate and a hydraulic top, the bottom valve plate is mounted on the hydraulic top, and the bottom valve plate can reciprocate in a vertical direction along the hydraulic top.

[0011] Preferably, the exhaust device is a self-powered, electromagnetic or electric one-way exhaust device, and the exhaust device outlet is connected to the environmental dust removal device.

[0012] Preferably, the outer walls of the furnace body and the furnace top closing cover are both covered with a heat-insulating layer, and the heat-insulating layer is covered with a sealing layer.

[0013] Beneficial effects of the utility model:

[0014] The utility model has a simple structure and a novel and unique design. It uses a sealed vertical DC resistance heating method to perform high-temperature treatment, thereby achieving a fast heating speed and uniform heating temperature. Since the exhaust device is a one-way single-port device, oxidation of the raw materials at high temperatures is avoided, thereby improving the utilization rate of the raw materials. The environmental protection dust removal device is connected, and the volatilized B2O3 can be recycled, which is energy-saving and environmentally friendly. The bottom unloading device allows the boron carbide product generated by the smelting to be taken out from the bottom, thereby saving the furnace time, achieving continuous production, and reducing heat energy loss, and having good social and economic benefits. BRIEF DESCRIPTION OF THE DRAWINGS

[0015] Figure 1 It is a schematic diagram of the structure of the utility model.

[0016] Among them, 1-furnace body, 2-furnace top closing cover, 3-graphite electrode, 4-lifting device, 4a-support, 4b-lifting drive, 4c-lifting guide rail, 4d-connecting rod, 5-unloading device, 5a-bottom valve plate, 5b-hydraulic top, 6-power supply device, 7-first wire, 8-second wire, 9-feeding trough, 10-one-way exhaust device, 10a-environmental protection dust removal device. DETAILED DESCRIPTION

[0017] The technical solution of the utility model is further described below in conjunction with embodiments, but the protection scope of the utility model is not limited thereto.

[0018] In view of the problems existing in the current boron carbide preparation devices, the practical vertical smelting device dynamically adjusts the position of the graphite electrode through an automatic lifting device during the heating process to accurately control the crystallization process and smelting process of boron carbide. The generated boron carbide product is taken out through a bottom unloading device. It has the advantages of simple process, fast heating speed, and large-scale production. The product has high purity, good crystallinity, uniform particle size, and stable and controllable quality, which meets the quality requirements of the engineering ceramics field for boron carbide powder.

[0019] Therefore, the utility model aims at the problems in the prior art and proposes a vertical smelting device, comprising a furnace body 1, a furnace top closed cover 2, an exhaust device 10, a discharge device 5, a power supply device 6 and a graphite electrode 3. Two exhaust devices 10 connected to the interior of the furnace body 1 are symmetrically installed on the upper side wall of the furnace body 1, a furnace top closed cover 2 is installed on the upper furnace top of the furnace body 1, and two feeding troughs 9 connected to the interior of the furnace body 1 are symmetrically installed on the furnace top closed cover 2. The smelting raw materials are loaded into the furnace body 1 through the feeding trough 9. A graphite electrode 3 is inserted in the center of the furnace top closed cover 2. The graphite electrode 3 located outside the furnace top closed cover 2 is connected to the automatic lifting device 4. The upper end of the graphite electrode 3 is connected to the positive electrode of the power supply device 6 through the first wire 7, and the negative electrode of the power supply device 6 is connected to the bottom valve plate 5a of the discharge device 5 through the second wire. The discharge device 5 is located outside the bottom of the furnace body 1 and is connected to the discharge port at the bottom of the furnace body 1.

[0020] The furnace top closing cover 2 is provided with a through hole, and the graphite electrode 3 passes through the through hole and penetrates into the furnace body 1; the power supply device 6 can generate stable and controllable high-voltage direct current or alternating current.

[0021] It should be noted that the power supply device 6 is connected to the graphite electrode 3, the material in the furnace body 1, and the bottom valve plate 5a to form a stable and controllable high-voltage DC loop circuit.

[0022] Furthermore, the automatic lifting device 4 is of gear transmission or hydraulic transmission type, including a support 4a, a lifting drive 4b, a lifting guide rail 4c and a connecting rod 4d. The support 4a is provided with a vertical lifting guide rail 4c, and the lifting guide rail 4c is provided with a lifting drive 4b. The lifting drive 4b is connected to one end of a horizontal connecting rod 4d, and the other end of the connecting rod 4d is connected to the graphite electrode 3. It is a one-way feeding device with a sealing device.

[0023] Furthermore, the unloading device 5 includes a bottom valve plate 5a and a hydraulic top 5b. The bottom valve plate 5a is installed on the hydraulic top 5b. The bottom valve plate 5a can reciprocate in the vertical direction along the hydraulic top 5b. The boron carbide material obtained by smelting is quickly unloaded by adjusting the bottom valve plate 5a to rise and fall through the hydraulic top 5b to achieve continuous production.

[0024] Furthermore, the exhaust device 10 is a self-powered, electromagnetic or electric one-way exhaust device, and the air outlet of the exhaust device 10 is connected to the environmental dust removal device 10a.

[0025] Furthermore, the outer walls of the furnace body 1 and the furnace top closing cover 2 are both covered with a heat-insulating layer, and the heat-insulating layer is covered with a sealing layer.

[0026] When the utility model is used, the following steps are included:

[0027] S1. Weigh the boron source material and the carbon source material in a mass ratio of 3 to 5:1 respectively; the boron source material is one of boron oxide (B2O3) and boric acid (H3BO3) or a mixture of multiple materials in any proportion; the carbon source material is one of coke, activated carbon, petroleum coke or graphite or a mixture of multiple materials in any proportion;

[0028] S2, mixing the weighed boron source material and carbon source material evenly, and grinding them to obtain a smelting raw material;

[0029] S3, the furnace top of the furnace body 1 is equipped with a furnace top closing cover 2, and then the graphite electrode 3 is inserted into the furnace top and contacts with the bottom plate valve 5a;

[0030] S4, after the smelting raw materials are loaded into the furnace body 1 through the feeding trough 9, the voltage and current are adjusted by the power supply device 6 to heat the smelting raw materials;

[0031] S5. During the heating period, as the temperature of the smelting raw materials increases, the graphite electrode 3 is lifted by the automatic lifting device 4 according to different temperature stages, and the insertion depth of the graphite electrode 3 is dynamically adjusted;

[0032] S6. After heating the smelting raw materials to 1900-2300°C, the boron carbide material can be obtained;

[0033] S7, the boron carbide material produced by smelting is taken out through the bottom unloading device 5;

[0034] S8. Crush and grind the synthetic boron carbide material, wash and filter it 2 to 4 times, and obtain boron carbide powder after graded drying.

[0035] In the description of the present utility model, unless otherwise specified, "plurality" means two or more than two; the terms "upper", "lower", "left", "right", "inner", "outer", "front end", "rear end", "head", "tail" and the like indicate positions or positional relationships based on the positions or positional relationships shown in the accompanying drawings, which are only for the convenience of describing the present utility model and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation on the present utility model. Moreover, the terms "include", "comprise" or any other variant thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device.

[0036] Although the embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A vertical smelting device, comprising a furnace body (1), a discharge device (5), a power supply device (6) and a graphite electrode (3), characterized in that: Two exhaust devices (10) connected to the interior of the furnace body (1) are symmetrically mounted on the upper side wall of the furnace body (1); a furnace top sealing cover (2) is mounted on the upper furnace top of the furnace body (1); two feeding troughs (9) connected to the interior of the furnace body (1) are symmetrically mounted on the furnace top sealing cover (2); a graphite electrode (3) is inserted in the center of the furnace top sealing cover (2); the graphite electrode (3) located outside the furnace top sealing cover (2) is connected to the automatic lifting device (4); the upper end of the graphite electrode (3) is connected to the positive electrode of the power supply device (6) via a first wire (7); the negative electrode of the power supply device (6) is connected to the bottom valve plate (5a) of the discharge device (5) via a second wire; the discharge device (5) is located outside the bottom of the furnace body (1) and is connected to the discharge port at the bottom of the furnace body (1).

2. The vertical smelting device according to claim 1, characterized in that: The automatic lifting device (4) is of gear transmission type or hydraulic transmission type, and comprises a support (4a), a lifting drive member (4b), a lifting guide rail (4c) and a connecting rod (4d). The support (4a) is provided with a vertical lifting guide rail (4c), the lifting drive member (4b) is mounted on the lifting guide rail (4c), the lifting drive member (4b) is connected to one end of a horizontal connecting rod (4d), and the other end of the connecting rod (4d) is connected to the graphite electrode (3).

3. The vertical smelting device according to claim 1, characterized in that: The unloading device (5) comprises a bottom valve plate (5a) and a hydraulic top (5b). The bottom valve plate (5a) is mounted on the hydraulic top (5b). The bottom valve plate (5a) can reciprocate in the vertical direction along the hydraulic top (5b).

4. The vertical smelting device according to claim 1, characterized in that: The exhaust device (10) is a self-powered, electromagnetic or electric one-way exhaust device, and the exhaust device (10) has an air outlet connected to the environmental dust removal device (10a).

5. The vertical smelting device according to claim 1, characterized in that: The outer walls of the furnace body (1) and the furnace top sealing cover (2) are both covered with a heat-insulating layer, and the heat-insulating layer is covered with a sealing layer.